A method for preparing porous carbon electrode materials based on electrostatic self-assembly and its application
By using wet ball milling and electrostatic self-assembly techniques, alkali metal carbonates were nano-sized and modified with charges before electrostatic self-assembly with carbon-based materials. This solved the problems of etchant size mismatch and agglomeration in the preparation of porous carbon materials, and enabled the preparation of efficient and uniform porous carbon electrode materials, thereby improving the electrochemical performance of supercapacitors.
Patent Information
- Application Number
- CN202611262107.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-19
- Publication Date
- 2026-11-17
AI Technical Summary
In existing technologies, the preparation of porous carbon materials has long relied on strong alkalis (KOH/NaOH) as etchants. These etchants react extremely violently at high temperatures, and the resulting gases easily damage the carbon framework, making it difficult to form micro/mesopores and limiting the contribution of the double-layer capacitance. While using K₂CO₃ as an alternative etchant can improve the etching path, commercially available K₂CO₃ particles are micrometer-sized, resulting in an order-of-magnitude size mismatch with nanoscale carbon-based materials. This leads to a small solid-solid contact area, low etching efficiency, and extremely uneven distribution. Furthermore, if K₂CO₃ is nanoscaled, the nanoparticles spontaneously aggregate during subsequent drying or mixing due to their extremely high surface energy, negating the advantages of nanoscale formation.
Alkali metal carbonates were nano-sized into nanoscale particles by wet ball milling, and then positively modified with cationic surfactants and negatively modified with anionic surfactants. Electrostatic self-assembly technology was used to uniformly distribute the nano-etching agent and carbon-based material. Combined with low-temperature drying and high-temperature sintering, a porous carbon electrode material was formed.
This method achieves a controllable ordering of etching paths from severe disorder, improves the specific surface area and pore structure uniformity of porous carbon materials, enhances electrochemical performance, and is suitable for the fabrication of electrodes for high-energy-density supercapacitors.
Smart Images

Figure CN123120519A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of electrochemical energy storage material preparation technology, specifically relating to a method for preparing porous carbon electrode materials based on electrostatic self-assembly and its application. Background Technology
[0002] Supercapacitors, as important electrochemical energy storage devices, possess advantages such as high power density, long cycle life, and fast charge / discharge speed, and are widely used in new energy, smart grids, and consumer electronics. Among these, the specific surface area and pore structure of the electrode material are key factors determining its electrochemical performance. Porous carbon materials, due to their wide availability, good chemical stability, and excellent conductivity, have become the preferred electrode material for supercapacitors. How to construct a rich and uniform microporous structure in carbon materials to maximize the ion-accessible specific surface area is currently a core research topic.
[0003] Currently, chemical activation is the mainstream method for preparing porous carbon materials with high specific surface area. Traditionally, potassium hydroxide (KOH) is often used as an activator / etcher. However, KOH reacts extremely violently at high temperatures of 600~800℃, and the gas produced by the reaction causes mesopores or even macropores to form on the material surface. The etching process is uncontrollable, the carbon skeleton collapses severely in some areas, and the effective specific surface area utilization rate is low.
[0004] Potassium carbonate (K₂CO₃), as a strong base-weak acid salt, is a milder alternative etchant. During thermal etching, it can be converted into a highly reactive β-K₂CO₃ intermediate, making the reaction process more controllable. However, commercially available K₂CO₃ particles are typically micrometer-sized (hundreds of micrometers), while the carbon-based material (OMG_Li) used in this invention has a nanometer-scale thin-layer structure, resulting in a severe size mismatch. The solid-solid contact area between the micrometer-sized etchant particles and the nanometer-scale carbon sheet is extremely small, leading to low etching efficiency and highly uneven distribution, resulting in localized over-etching while other areas show almost no etching.
[0005] To address the aforementioned scale mismatch issue, one approach is to nanoscale K2CO3 using methods such as ball milling. However, nanoparticles possess extremely high surface energy, leading to spontaneous aggregation during subsequent drying or mixing processes, reverting to large particles and completely negating the advantages of nanoscale formation. This nanoparticle aggregation problem is a common technical bottleneck in the application of nanoscale etchants. Therefore, achieving a uniform and orderly distribution of K2CO3 on the surface of carbon-based materials while maintaining its nanoscale dispersion is a pressing technical challenge.
[0006] The present invention aims to overcome the problem of disordered pore structure formed by the violent reaction of strong alkali thermal etching, and thus achieve precise control of the pore structure of graphene nanosheets, in order to construct porous carbon electrode materials with uniform size and controllable hierarchical pore system. Summary of the Invention
[0007] The purpose of this section is to outline some aspects of embodiments of the present invention and to briefly describe some preferred embodiments. Simplifications or omissions may be made in this section, as well as in the abstract and title of this application, to avoid obscuring the purpose of these documents; however, such simplifications or omissions should not be construed as limiting the scope of the invention.
[0008] In view of the problems existing in the prior art, the present invention is proposed.
[0009] Therefore, the problem this invention aims to solve is that the preparation of porous carbon materials has long relied on strong alkalis (KOH / NaOH) as etchants. These etchants react extremely violently at high temperatures, and the resulting gases easily damage the carbon framework, making it difficult to form micro / mesopores and limiting the contribution of the double-layer capacitance. While using K₂CO₃ as an alternative etchant can improve the etching path, commercially available K₂CO₃ particles are micrometer-sized, resulting in an order-of-magnitude size mismatch with nanoscale carbon-based materials. This leads to a small solid-solid contact area, low etching efficiency, and extremely uneven distribution. If K₂CO₃ is nano-sized, the nanoparticles spontaneously agglomerate during subsequent drying or mixing due to their extremely high surface energy, thus negating some of the advantages of nano-sizing. This technical predicament prevents existing preparation methods from simultaneously achieving mild and controllable etchant properties, size matching, and uniform dispersion against agglomeration.
[0010] To solve the above-mentioned technical problems, the present invention provides the following technical solution: waste graphite is thoroughly mixed with stainless steel grinding balls and then subjected to high-energy ball milling. After ball milling, the grinding balls are separated by sieving to obtain carbon-based material OMG_Li. Alkali metal carbonates were obtained as nano-alkali metal carbonate powders by wet ball milling. A positively charged nano-etching agent was obtained by dispersing nano-alkali metal carbonate powder and cationic surfactant in a non-aqueous solvent and then undergoing dispersion treatment. Carbon-based material OMG_Li and anionic surfactant were dispersed in a non-aqueous solvent, and a negatively charged carbon-based dispersion was obtained after dispersion treatment. Positively charged nano-etching agents are added to negatively charged carbon-based dispersions, and electrostatic self-assembly is achieved by relying on the Coulomb force of positive and negative charges to obtain a self-assembled mixture. The self-assembled mixture was dried at low temperature to obtain a self-assembled precursor; the self-assembled precursor was then subjected to high-temperature calcination under an inert nitrogen atmosphere, followed by acid washing, water washing, and drying to obtain the porous carbon electrode material.
[0011] In a preferred embodiment of the preparation method described in this invention, the alkali metal carbonate is potassium carbonate.
[0012] As a preferred embodiment of the preparation method described in this invention, the cationic surfactant is a quaternary ammonium salt type cationic surfactant with a carbon chain length of not less than C14, preferably hexadecyltrimethylammonium bromide (CTAB), and the amount added is 1% to 5% of the mass of carbonate.
[0013] In a preferred embodiment of the preparation method described in this invention, the anionic surfactant is a sulfonate-type anionic surfactant, preferably sodium dodecylbenzenesulfonate (SDBS); and the non-aqueous solvent is anhydrous ethanol.
[0014] As a preferred embodiment of the preparation method described in this invention, the wet ball milling is performed using a high-energy ball mill, the ball milling media are stainless steel beads with a particle size of 5 mm, the ball-to-material mass ratio is 10:~20:1, the ball milling frequency is 20~30 Hz, and the cumulative grinding time is 16~24 h.
[0015] In a preferred embodiment of the preparation method described in this invention, the mass ratio of alkali metal carbonate to carbon-based material in the electrostatic self-assembled composite is 1 to 3:1; the mixing direction is that the positively charged nano-alkali metal carbonate suspension is added dropwise to the negatively charged carbon-based material dispersion; the criterion for successful self-assembly is that the mixture shows obvious flocculation and precipitation and the supernatant becomes clear and transparent.
[0016] As a preferred embodiment of the preparation method described in this invention, the low-temperature drying temperature is 40-60°C to prevent the anhydrous ethanol from boiling out and damaging the self-assembled interface structure; during the drying process, the carbon-based material sheet structure acts as a physical isolation barrier, and the synergistic electrostatic anchoring effect prevents the spontaneous aggregation of nano-etchant particles.
[0017] As a preferred embodiment of the preparation method described in this invention, the atmosphere for high-temperature firing is nitrogen; the heating rate is 5-15 °C / min; the target temperature is 500-800 °C, preferably 650 °C; the holding time is 1-4 h; an excessively fast heating rate will result in excessively rapid gas release, which will easily cause the carbon skeleton to break.
[0018] As a preferred embodiment of the preparation method described in this invention, the acid washing is performed by soaking in 0.5-2 mol / L dilute hydrochloric acid for 1-3 h; after washing with water until neutral, it is vacuum dried at 80-120 ℃ for 8-16 h.
[0019] Another objective of this invention is to overcome the shortcomings of existing technologies and provide a system for preparing porous carbon electrode materials based on electrostatic self-assembly, comprising: preparation of a nano-sized positively charged etchant by wet ball milling with anhydrous ethanol to obtain a nano-carbonate suspension, adding a cationic surfactant and dispersing it to achieve a positively charged nano-potassium carbonate dispersion; a negatively charged carbon-based dispersion preparation module for dispersing carbon-based materials and anionic surfactants in anhydrous ethanol (a non-aqueous solvent); and an electrostatic self-assembly and heat treatment module for self-assembly composite driven by Coulomb force, low-temperature drying, high-temperature sintering, and post-treatment to finally obtain the porous carbon electrode material.
[0020] Another objective of this invention is to overcome the shortcomings of the prior art and provide an application of the porous carbon electrode material obtained by the above preparation method in a supercapacitor. The porous carbon electrode material is mixed with a conductive agent and a binder at a mass ratio of 8:1:1, and then prepared into a 1*1cm... 2 Electrode sheets, loaded onto nickel foam, are pressed and dried to form the working electrode. Using a 6 mol / L KOH aqueous solution as the electrolyte, a three-electrode system is employed. The specific capacitance, rate performance, and cycle stability of the electrode material are comprehensively evaluated by cyclic voltammetry (CV), galvanostatic charge-discharge (GCD), and electrochemical impedance spectroscopy (EIS). The porous carbon electrode material possesses high specific surface area, high micro / mesoporous ratio (40%–55%), and excellent electrochemical performance, making it suitable for the preparation of electrodes for high-energy-density supercapacitors.
[0021] Beneficial effects of this invention: (1) Etching path from severe disorder to controllable order: This invention uses K2CO3, a strong base-weak acid salt, instead of the traditional strong base KOH as the etchant precursor, which solves the problems of carbon skeleton structure destruction and pore disorder caused by strong base etching. Under optimized conditions, K2CO3, compared with KOH, increases the specific surface area of the etching product, improves the total pore volume and the proportion of micropores, and constructs an ideal hierarchical pore structure dominated by micropores and assisted by mesopores.
[0022] (2) Wet ball milling to control the scale matching between etchant and carbon precursor: K2CO3 was shrunk from the micrometer scale to the 100 nm scale by wet ball milling, so that it matched the scale of the nano-sized OMG_Li carbon precursor, increasing the effective solid-solid contact area. The specific capacitance and rate performance of PM-Nano (nano-sized physical hybrid group) were better than those of PM-Micro (micrometer-sized physical hybrid group), proving that the nano-sizing method effectively improves the electrochemical performance of porous carbon materials by increasing the contact area between etchant and carbon-based materials.
[0023] (3) Self-assembly system construction solves the bottleneck of nanoparticle aggregation: This invention innovatively adopts a nano-coupled electrostatic self-assembly synergistic strategy, using the cationic surfactant CTAB to simultaneously perform surface positive electrochemical modification on K2CO3 nanoparticles during wet ball milling. The modified product is denoted as CTAB@K2CO 3, By loading the anionic surfactant SDBS onto the negatively charged surface of OMG_Li, the modified product, denoted as SDBS@OMG_Li, utilizes the Coulomb force between positive and negative charges to drive the nano-etchant to be uniformly anchored in a single-particle state on the carbon precursor surface. The specific capacitance, rate performance, and cycling stability of SA-Nano (electrostatically self-assembled nanoparticles) are significantly superior to PM-Nano, demonstrating that the electrostatic self-assembly method effectively improves the novel electrochemical properties of nanoporous carbon materials. Furthermore, the layered structure of OMG_Li, to some extent, isolates the etchant nanoparticles from agglomeration during drying, synergistically overcoming the technical bottleneck of high specific surface energy nanoparticles' tendency to aggregate.
[0024] (4) Self-assembly system construction solves the bottleneck of nanoparticle agglomeration: This invention innovatively adopts a nano-coupled electrostatic self-assembly synergistic strategy. During wet ball milling, the K2CO3 nanoparticles are simultaneously positively charged using the cationic surfactant CTAB, while the OMG_Li surface is negatively charged using the anionic surfactant SDBS. The Coulomb force between the positive and negative charges drives the nano-etchant to be uniformly anchored on the carbon precursor surface in a single-particle state. The specific capacitance, rate performance, and cycle stability of SA-Nano (electrostatically self-assembled nanoparticles) are significantly better than PM-Nano, demonstrating that the electrostatic self-assembly method effectively improves the electrochemical properties of nanoporous carbon materials. Furthermore, the OMG_Li layered structure isolates the etchant nanoparticles from agglomeration to some extent during drying, thus overcoming the technical bottleneck of high specific surface energy nanoparticles easily agglomerating through the synergistic electrostatic self-assembly method.
[0025] (5) The process is green, low-cost, and has promising prospects for industrial scale-up: K2CO3 is a common inorganic salt with wide availability and low cost. The electrostatic self-assembly process can be completed in the range of room temperature to low temperature. The wet ball milling nano-sizing uses a high-energy ball mill, which is a mature device in both laboratories and industries. The thermal etching temperature is moderate, the heating rate is mild, and it can be achieved in a tube furnace. The entire process flow is simple, the steps are clear, and each step can be independently optimized and scaled up, which has good potential for industrial promotion. Attached Figure Description
[0026] To more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings used in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort. Wherein: Figure 1 This is a schematic diagram of the process of an embodiment of the present invention.
[0027] Figure 2 This is a diagram illustrating an electrochemical application scenario of an embodiment of the present invention.
[0028] Figure 3 The mechanism of the self-assembly method in this invention is demonstrated by showing that positively charged potassium carbonate nanoparticles and negatively charged carbon precursors spontaneously assemble through Coulomb attraction between positive and negative charges.
[0029] Figure 4 These are SEM images of embodiments and comparative examples 1-3 of the present invention. Figure 4 (a) For the characterization of Comparative Example 1, micron-sized KOH directly etched carbon precursor products, the carbon skeleton was destroyed and the formed channels were mainly macropores. Figure 4 (b) For the characterization of Comparative Example 2, micron-sized K2CO3 directly etched carbon precursor products. The figure shows that compared with Comparative Example 1, a small number of macropores were formed at 1µm and the carbon skeleton of the product remained stable. Figure 4 (c) Characterization of Comparative Example 3, where nanoscale K2CO3 directly etches carbon precursor products. The figure shows the formation of etched micro / mesopores at 400 nm compared to Comparative Example 2. Figure 4 (d) is a characterization of OMG_Li self-assembled etching product of nanoscale K2CO3 modified with positive and negative charge, which has more micro / mesopores at 400 nm.
[0030] Figure 5 The CV curves of the embodiments and Comparative Example 1 before and after etching are analyzed at voltage scan rates of 5, 10, 20, 50, and 100 mV / s, respectively. Figure 5 (a) CV analysis of the carbon precursor OMG_Li at various scan rates. Figure 5 (b) Comparative Example 1: CV analysis at various scan rates. Figure 5 (c) shows the CV analysis of Example 1 at various scan rates.
[0031] Figure 6 The specific capacitance of the present invention and Comparative Example 1 before and after etching at voltage scan rates of 5, 10, 20, 50, and 100 mV / s are shown.
[0032] Figure 7The GCD curves of the embodiments and Comparative Example 1 before and after etching are analyzed at current densities of 0.2, 0.5, 1, 2, 5, and 10 A / g, respectively. Figure 7 (a) GCD analysis of the carbon precursor OMG_Li at various current densities. Figure 7 (b) is a comparative example 1 with GCD analysis at various current densities. Figure 7 (c) GCD analysis of Example 1 at various current densities.
[0033] Figure 8 The specific capacitance of the embodiments and comparative example 1 of the present invention before and after etching at current densities of 0.2, 0.5, 1, 2, 5, and 10 A / g. Detailed Implementation
[0034] To make the above-mentioned objects, features and advantages of the present invention more apparent and understandable, the specific embodiments of the present invention will be described in detail below with reference to the examples in the specification.
[0035] Many specific details are set forth in the following description in order to provide a full understanding of the invention. However, the invention may also be practiced in other ways different from those described herein, and those skilled in the art can make similar extensions without departing from the spirit of the invention. Therefore, the invention is not limited to the specific embodiments disclosed below.
[0036] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The phrase "in one embodiment" appearing in different places in this specification does not necessarily refer to the same embodiment, nor is it a single or selective embodiment that is mutually exclusive with other embodiments.
[0037] Unless otherwise specified, all raw materials used in the embodiments of this invention are commercially available. See Table 1 for details.
[0038] Table 1
[0039] The instruments involved in this invention are shown in Table 2.
[0040] Table 2
[0041] Example 1 This embodiment provides a method for preparing electrostatically self-assembled nanogroups SA-Nano, specifically as follows: (1) Preparation of substrate OMG_Li: 6g of waste graphite and 84g of stainless steel grinding balls were weighed, with a ball-to-material ratio of 14:1. After thorough mixing, the mixture was placed in a stainless steel ball mill jar for high-energy ball milling. The ball milling parameters were 20.5h and 25hz. After ball milling, the balls were separated by sieve, and the resulting material was named OMG_Li.
[0042] (2) Preparation of nano-etching agent: 1 g of potassium carbonate and 25 mL of anhydrous ethanol were added to a zirconia ball mill jar containing zirconia grinding beads (5 mm, total weight about 50 g). The mixture was ball-milled at a frequency of 24 Hz in a high-energy ball mill for a total of 24 h to achieve the preparation of nano-etching agent (after wet ball milling and nano-sizing, the particle size of the nano-potassium carbonate was on the order of 500 nm to 1 µm), yielding Nano-K2CO3. (3) Preparation of positively charged nano-etching agent: Nano-K2CO3 powder was taken, and hexadecyltrimethylammonium bromide with a mass fraction of 3% Nano-K2CO3 was weighed and dispersed in anhydrous ethanol for surface positive electrochemical treatment. The Zeta potential of the supernatant was tested. If it was >+30 mV, Nano-K2CO3 achieved negative charge loading. This negatively charged nano-etching agent was named CTAB@K2CO3. Then, the supernatant was taken and the concentration was determined by dry weight method.
[0043] (4) Preparation of negatively charged carbon-based dispersion: OMG_Li powder was taken, and sodium dodecylbenzenesulfonate (SDBS) powder with a mass fraction of 5% OMG_Li was weighed and dispersed in anhydrous ethanol for surface negative electrochemical treatment. The Zeta potential of the supernatant was tested. If it was <-30 mV, the carbon-based material achieved negative charge loading. This negatively charged nano-etchant was named SDBS@OMG_Li. The supernatant was then taken and the concentration was determined by dry weight method.
[0044] (5) Electrostatic self-assembly: Based on the concentration measured by the dry weight method, calculate the required volume. Add the positively charged nano-potassium carbonate suspension dropwise to the negatively charged OMG_Li dispersion at a mass ratio of 1:1 (potassium carbonate: OMG_Li). During mixing, observe obvious flocculation and precipitation. The supernatant should become clear and transparent, indicating that the positive and negative charges have neutralized, and self-assembly is successful. The Zeta potential of the mixed system is close to 0 mV.
[0045] (6) Low temperature drying: The above self-assembled mixture is placed in a 50°C oven and dried to obtain the self-assembled precursor.
[0046] (7) Firing and post-treatment: The self-assembled precursor was placed in a tube furnace and heated to 650℃ at 10℃ / min under a nitrogen atmosphere and held for 2 h. After natural cooling, the resulting solid was successively soaked in 1 mol / L dilute hydrochloric acid for 2 h for acid washing, washed with water until neutral, and vacuum dried at 80℃ for 12 h. The resulting product was designated SA-Nano-650-1-1.
[0047] Figure 1 This is a schematic diagram of the process of an embodiment of the present invention. Figure 2 This is a diagram illustrating an electrochemical application scenario of an embodiment of the present invention.
[0048] Figure 3 This invention demonstrates the mechanism of the self-assembly method, showing the spontaneous assembly of positively charged modified potassium carbonate nanoparticles and negatively charged modified carbon precursors through Coulomb attraction. This embodiment is a key example of the invention, achieving a uniform and orderly distribution of nano-etchant on the surface of carbon-based materials through electrostatic self-assembly driven by positive and negative charges. Combined with the physical isolation effect of carbon layers, the problem of nanoparticle aggregation is effectively overcome, ultimately obtaining porous carbon nanomaterials with uniform micropore distribution. Characterization analysis is shown below. Figure 4 (d) and Figure 5 (c). The area enclosed by the CV curve is positively correlated with the charge discharge rate of the electrode material; as the area increases, the charge discharge process of the electrode material is faster. Example 1 shows the largest enclosed area, indicating that under the same etching conditions at the same temperature, the material exhibits superior electrochemical performance.
[0049] Comparative Example 1 (1) Preparation of substrate OMG_Li: 6g of waste graphite and 84g of stainless steel grinding balls were weighed, with a ball-to-material ratio of 14:1. After thorough mixing, the mixture was placed in a stainless steel ball mill jar for high-energy ball milling. The ball milling parameters were 20.5h and 25hz. After ball milling, the balls were separated by sieve, and the resulting material was named OMG_Li.
[0050] (2) Preparation and mixing: Take 1g each of commercial-grade micron-sized KOH and OMG_Li, i.e., a mass ratio of 1:1, and dry grind and mix KOH and OMG_Li in a mortar for about 15 min to obtain a mixture.
[0051] (3) Calcination and post-treatment: The mixture of KOH and OMG_Li was placed in a tube furnace and heated to 650℃ at 10℃ / min under a nitrogen atmosphere and held for 2 h. After natural cooling, the resulting solid was successively soaked in 1 mol / L dilute hydrochloric acid for 2 h for acid washing, washed with water until neutral, and vacuum dried at 80℃ for 12 h. The resulting product was denoted as Micro(KOH)-650-1-1.
[0052] The difference between this comparative example and Example 1 is that the nano-sizing, surface charge modification and electrostatic self-assembly process of potassium carbonate in steps (2) to (5) of Example 1 are omitted. Micron-sized potassium hydroxide (KOH) and OMG_Li are physically mixed in a mortar. The mass ratio and amount of KOH to OMG_Li are the same as those of potassium carbonate and OMG_Li in Example 1. The firing and post-treatment are the same as those of Example 1.
[0053] Results: The etching activation reaction with strong base KOH was extremely vigorous, and the etchant scale was mismatched with OMG_Li. Therefore, the carbon framework structure is severely damaged, the specific surface area of the product is low, and the generated pore structure is mainly macropores, which limits its contribution to the double-layer capacitance of the material. Characterization analysis is shown in [see below]. Figure 4 (a) Etching with strong alkali causes damage to the carbon framework. Comparative Example 1 demonstrates that replacing the strong alkali KOH with K2CO3 can avoid severe damage to the carbon framework and obtain a better pore structure. Figure 6 The specific capacitance of the embodiments and Comparative Example 1 before and after etching at voltage scan rates of 5, 10, 20, 50, and 100 mV / s are shown. The specific capacitance value of Embodiment 1 is the highest at all scan rates. At 5 mV / s, the specific capacitance of Embodiment 1 reaches 93.60 F / g, OMG_Li is 82.11 F / g, and Comparative Example 1 Micro(KOH)-650-1-1 is 64.44 F / g. At a high scan rate of 100 mV / s, the specific capacitance of Embodiment 1 still reaches 74.48 F / g. Figure 7 The GCD curves of the embodiments and Comparative Example 1 before and after etching are analyzed at current densities of 0.2, 0.5, 1, 2, 5, and 10 A / g, respectively. Figure 7 (a) GCD analysis of the carbon precursor OMG_Li at various current densities. Figure 7 (b) is a comparative example 1 with GCD analysis at various current densities. Figure 7 (c) GCD analysis of Example 1 at various current densities. As the current density increases from 0.1 A / g to 10 A / g, the scan time decreases, indicating that the material charges and discharges faster at higher current densities. Among them, Example 1 had the longest scan time at 0.2 A / g, indicating that the material exhibits superior electrochemical performance under the same etching conditions at the same temperature. Figure 8 The specific capacitance of the embodiments and comparative example 1 before and after etching at current densities of 0.2, 0.5, 1, 2, 5, and 10 A / g are shown. The specific capacitance value of embodiment 1 is the highest at all current densities.
[0054] Comparative Example 2 (1) Preparation of substrate OMG_Li: 6g of waste graphite and 84g of stainless steel grinding balls were weighed, with a ball-to-material ratio of 14:1. After thorough mixing, the mixture was placed in a stainless steel ball mill jar for high-energy ball milling. The ball milling parameters were 20.5h and 25hz. After ball milling, the balls were separated by sieve, and the resulting material was named OMG_Li.
[0055] (2) Preparation and mixing: Take 1g each of commercial-grade micron-sized K2CO3 and OMG_Li, i.e., a mass ratio of 1:1. Place K2CO3 and OMG_Li in a mortar and dry grind and mix for about 15 min to obtain a mixture.
[0056] (3) Calcination and post-treatment: The mixture of K2CO3 and OMG_Li was placed in a tube furnace and heated to 650℃ at 10℃ / min under a nitrogen atmosphere and held for 2 h. After natural cooling, the resulting solid was successively soaked in 1 mol / L dilute hydrochloric acid for 2 h for acid washing, washed with water until neutral, and vacuum dried at 80℃ for 12 h. The resulting product was denoted as Micro-650-1-1.
[0057] The difference between this comparative example and Example 1 is that the wet ball milling of potassium carbonate for nano-sizing is not performed, and CTAB and SDBS are not added for surface charge modification and electrostatic self-assembly. Instead, commercial-grade micron-sized potassium carbonate and OMG_Li are directly dry-milled and mixed in a mortar at a mass ratio of 1:1 for about 15 min. The resulting mixture is then directly subjected to subsequent calcination and post-treatment.
[0058] Results: Due to the order-of-magnitude scale mismatch between the micron-scale etchant and the nanoscale thin-film carbon material, solid- The solid-solid contact area is extremely small. The material etching efficiency is extremely low and unevenly distributed, resulting in localized over-etching and poor channel uniformity. Characterization analysis is shown below. Figure 4 (b) The alkali metal carbonate etching used in this invention is relatively controllable, without the formation of a strongly alkali-activated carbon framework that causes damage, resulting in large-channel pore formation. Comparative Example 2 is used to demonstrate the necessity of nano-sizing the etchant to match the scale of carbon-based materials.
[0059] Comparative Example 3 (1) Preparation of substrate OMG_Li: 6g of waste graphite and 84g of stainless steel grinding balls were weighed, with a ball-to-material ratio of 14:1. After thorough mixing, the mixture was placed in a stainless steel ball mill jar for high-energy ball milling. The ball milling parameters were 20.5h and 25hz. After ball milling, the balls were separated by sieve, and the resulting material was named OMG_Li.
[0060] (2) Preparation of nano-etching agent: 1 g of potassium carbonate and 25 mL of anhydrous ethanol were added to a zirconia ball mill jar containing zirconia grinding beads (5 mm, total weight about 50 g). The mixture was ball-milled at a frequency of 24 Hz in a high-energy ball mill for a total of 24 h to achieve the preparation of nano-etching agent (after wet ball milling and nano-sizing, the particle size of the nano-potassium carbonate was on the order of 500 nm to 1 µm), yielding Nano-K2CO3. (3) Preparation and mixing: Take 1g of Nano-K2CO3 and 1g of OMG_Li respectively, i.e., the mass ratio is 1:1. Place Nano-K2CO3 and OMG_Li in a mortar and dry grind and mix for about 15 min to obtain a mixture.
[0061] (4) Calcination and post-treatment: The mixture of Nano-K2CO3 and OMG_Li was placed in a tube furnace and heated to 650℃ at 10℃ / min under a nitrogen atmosphere and held for 2 h. After natural cooling, the resulting solid was successively soaked in 1 mol / L dilute hydrochloric acid for 2 h for acid washing, washed with water until neutral, and vacuum dried at 80℃ for 12 h. The resulting product was designated as Nano-650-1-1.
[0062] The difference between this comparative example and Example 1 is that the wet ball milling of potassium carbonate is retained, but the positive electrochemical modification of K2CO3 by CTAB in step (3) and the negative electrochemical modification of OMG_Li by SDBS in step (4) are omitted. Electrostatic self-assembly is not performed. Instead, nano-K2CO3 and OMG_Li are directly physically mixed under no-charge guidance. The calcination and post-treatment are the same as in Example 1.
[0063] Results: Although wet ball milling of K2CO3 nanoparticles improved the contact area, the lack of positive and negative charges hindered the improvement of the contact area. Due to the electro-anchoring effect, the high surface energy nanoparticles underwent secondary agglomeration during drying in step (4), reforming into larger particles. This partially offset the advantages of nano-sized particles, resulting in uneven pore size distribution in the product and failing to achieve the significant gains brought by uniform anchoring of single particles as described in the example. Figure 4 (c). Comparative Example 3 is used to demonstrate the necessity of electrostatic self-assembly anchoring for suppressing nanoparticle aggregation and achieving uniform distribution.
[0064] Comparative Example 4 The difference between this comparative example and the embodiment is that: the cetyltrimethylammonium bromide in step (3) is removed. (CTAB) was replaced with dodecyltrimethylammonium bromide (DTAB), and the remaining steps were the same as in the example. The resulting positively charged nano-etchant was named DTAB@K2CO3.
[0065] Results: Due to the short carbon chain of DTAB, it is impossible to establish effective spatial sites on the surface of nano-potassium carbonate particles. The etchant failed to provide sufficient positive electrochemical modification, and the zeta potential test results are shown in Table 3. In the example, the positive electrochemical modification of K₂CO₃ by CTAB resulted in a zeta potential > +30 mV, while the positive electrochemical modification of DTAB in the comparative example resulted in a zeta potential < 1 mV. The example more readily exhibited spontaneous positive and negative charge attraction with the negatively modified OMG_Li, achieving self-assembly of the etchant and the carbon precursor. Comparative Example 4 was used to demonstrate the necessity of the cationic surfactant carbon chain length (≥ C14) for establishing effective positive electrochemical modification.
[0066] Table 3
[0067] In Table 3, SDBS@OMG_Li is the negatively charged nano-etching agent in the examples, CTAB@K2CO3 is the positively charged nano-etching agent in the examples, and DTAB@K2CO3 is the positively charged nano-etching agent in Comparative Example 4.
[0068] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention, and all such modifications or substitutions should be covered within the scope of the present invention.
Claims
1. A method for preparing porous nanocarbon electrode materials based on electrostatic self-assembly, characterized in that: include, Waste graphite was thoroughly mixed with stainless steel grinding balls and then ball-milled at high energy. After ball milling, the grinding balls were separated by sieving to obtain carbon-based material OMG_Li. Alkali metal carbonates were obtained as nano-alkali metal carbonate powders by wet ball milling. A positively charged nano-etching agent was obtained by dispersing nano-alkali metal carbonate powder and cationic surfactant in a non-aqueous solvent and then undergoing dispersion treatment. Carbon-based material OMG_Li and anionic surfactant were dispersed in a non-aqueous solvent, and a negatively charged carbon-based dispersion was obtained after dispersion treatment. Positively charged nano-etching agents are added to negatively charged carbon-based dispersions, and electrostatic self-assembly is achieved by relying on the Coulomb force of positive and negative charges to obtain a self-assembled mixture. The self-assembled mixture was dried at low temperature to obtain a self-assembled precursor; the self-assembled precursor was then subjected to high-temperature calcination under an inert nitrogen atmosphere, followed by acid washing, water washing, and drying to obtain the porous carbon electrode material.
2. The preparation method according to claim 1, characterized in that: The alkali metal carbonate is potassium carbonate.
3. The preparation method according to claim 1, characterized in that: The cationic surfactant is a quaternary ammonium salt type cationic surfactant with a carbon chain length of not less than C14; including hexadecyltrimethylammonium bromide, the amount added is 1% to 5% of the mass of alkali metal carbonate.
4. The preparation method according to claim 1, characterized in that: The anionic surfactant is a sulfonate-type anionic surfactant, including sodium dodecylbenzenesulfonate.
5. The preparation method according to claim 1, characterized in that: The non-aqueous solvent is anhydrous ethanol.
6. The preparation method according to claim 1, characterized in that: The wet ball milling media are stainless steel beads with a particle size of 5 mm; the ball-to-material mass ratio is 10~20:1; the ball milling frequency is 20~30 Hz; and the cumulative grinding time is 16~24h.
7. The preparation method according to claim 1, characterized in that: The mass ratio of the alkali metal carbonate to the carbon-based material OMG_Li is 1~3:1; the stirring time is 15~30 minutes.
8. The preparation method according to claim 1, characterized in that: The low-temperature drying temperature is 40~60℃; the high-temperature firing temperature is 500~800℃, the heating rate is 5~15℃ / min, and the holding time is 2~4 h; the acid washing involves soaking in 1mol / L dilute hydrochloric acid for 1~3 h, washing with water until neutral, and then vacuum drying at 80~120℃ for 16~24 h.
9. The application of a porous carbon electrode material prepared by the method according to any one of claims 1 to 8 in a supercapacitor.