Electrode for rechargeable lithium battery and rechargeable lithium battery including the electrode

By using an organic-inorganic composite layer of polysilsesquioxane fibers containing crosslinkable functional groups in the electrodes of rechargeable lithium batteries, the deficiencies of electrodes in terms of tensile strength, air permeability, and adhesion have been solved, achieving efficient manufacturing and improved stability of the batteries.

CN123120618APending Publication Date: 2026-11-17SAMSUNG SDI CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202610624550.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2025-05-16
Filing Date
2026-05-08
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing rechargeable lithium battery electrodes have shortcomings in terms of tensile strength, air permeability, adhesion, electrolyte wettability and heat resistance, and the use of traditional separators increases manufacturing complexity and cost.

Method used

The organic-inorganic composite layer, which integrates fibers containing polysilsesquioxane (PSSQ) with crosslinkable functional groups, improves tensile strength, air permeability and adhesion, and enhances the stability and reliability of the electrode through multi-layer composite layers, thus replacing traditional diaphragms.

Benefits of technology

It improves the mechanical strength of the electrodes and the reliability of the battery, simplifies the manufacturing process, reduces the cell defect rate and electrode volume expansion, and enhances the stability and lifespan of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120618A_ABST
    Figure CN123120618A_ABST
Patent Text Reader

Abstract

Provided are an electrode for a rechargeable lithium battery and a rechargeable lithium battery including the same. The electrode for a rechargeable lithium battery includes an active material layer for a rechargeable lithium battery; and an organic-inorganic composite layer integrated with the active material layer, and the organic-inorganic composite layer includes a fiber including a polysilsesquioxane having a cross-linkable functional group.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application claims priority to Korean Patent Application No. 10-2025-0064099, filed on May 16, 2025, with the Korean Intellectual Property Office; Korean Patent Application No. 10-2025-0064101, filed on May 16, 2025, with the Korean Intellectual Property Office; Korean Patent Application No. 10-2025-0064098, filed on May 16, 2025, with the Korean Intellectual Property Office; and Korean Patent Application No. 10-2025-0064100, filed on May 16, 2025, with the entire disclosure of the aforementioned Korean patent applications is incorporated herein by reference. Technical Field

[0002] This disclosure relates to an electrode for a rechargeable lithium battery and a rechargeable lithium battery including the electrode. Background Technology

[0003] Recently, with the rapid proliferation of battery-powered electronic devices such as mobile phones, laptops, and electric vehicles, the demand for rechargeable batteries with high energy density and high capacity is increasing rapidly. Therefore, research and development to improve the performance of rechargeable lithium batteries is actively underway.

[0004] A rechargeable lithium battery is a battery that includes a positive electrode and a negative electrode containing active materials capable of inserting and deintercalating lithium ions, and generates electrical energy through oxidation and reduction reactions when lithium ions are deintercalated from the negative electrode and inserted into the positive electrode, and deintercalated from the positive electrode and inserted into the negative electrode. Summary of the Invention

[0005] This disclosure aims to provide an electrode for a rechargeable lithium battery, the electrode comprising an organic-inorganic composite layer integrated with an active material layer and having improved tensile strength and improved air permeability.

[0006] This disclosure also aims to provide an electrode for a rechargeable lithium battery, the electrode comprising an organic-inorganic composite layer integrated with an active material layer and having improved tensile strength and improved adhesion.

[0007] This disclosure also aims to provide an electrode for a rechargeable lithium battery, the electrode comprising an organic-inorganic composite layer integrated with an active material layer and having excellent electrolyte wettability.

[0008] This disclosure also aims to provide an electrode for a rechargeable lithium battery, the electrode comprising an organic-inorganic composite layer integrated with an active material layer and having stability against foreign matter.

[0009] This disclosure also aims to provide an electrode for a rechargeable lithium battery, the electrode comprising an organic-inorganic composite layer integrated with an active material layer and providing improved tensile strength, improved electrolyte wettability and turn-off effect.

[0010] This disclosure also aims to provide an electrode for a rechargeable lithium battery, the electrode comprising an organic-inorganic composite layer integrated with an active material layer and having improved adhesion to the active material layer and improved heat resistance.

[0011] This disclosure also aims to provide a rechargeable lithium battery including the electrodes described above for a rechargeable lithium battery.

[0012] One embodiment provides an electrode for a rechargeable lithium battery.

[0013] The electrode for the rechargeable lithium battery includes: an active material layer for the rechargeable lithium battery; and an organic-inorganic composite layer integrated with the active material layer, wherein the organic-inorganic composite layer includes fibers comprising polysilsesquioxane (PSSQ) having crosslinkable functional groups.

[0014] The electrode for the rechargeable lithium battery includes: an active material layer for the rechargeable lithium battery; and an organic-inorganic composite layer integrated with the active material layer, wherein the organic-inorganic composite layer includes fibers comprising PSSQ having crosslinkable functional groups and aromatic polyamide polymers.

[0015] The electrode for the rechargeable lithium battery includes: an active material layer for the rechargeable lithium battery; and a multilayer organic-inorganic composite layer integrated with the active material layer for the rechargeable lithium battery, wherein the multilayer organic-inorganic composite layer includes a first organic-inorganic composite layer and a second organic-inorganic composite layer. The difference between the PSSQ content in the first organic-inorganic composite layer and the PSSQ content in the second organic-inorganic composite layer is 10 wt% or greater.

[0016] Another embodiment provides an electrode assembly for a rechargeable lithium battery.

[0017] The electrode assembly for the rechargeable lithium battery includes a positive electrode active material layer for the rechargeable lithium battery, a negative electrode active material layer for the rechargeable lithium battery, and a multilayer organic-inorganic composite layer located between the positive electrode active material layer for the rechargeable lithium battery and the negative electrode active material layer for the rechargeable lithium battery.

[0018] 1. Electrodes used in rechargeable lithium batteries include: Active material layer for rechargeable lithium batteries; and The organic-inorganic composite layer is integrated with the active material layer. The organic-inorganic composite layer includes fibers, which contain polysilsesquioxanes with crosslinkable functional groups.

[0019] 2. The electrode according to item 1, wherein at least some of the crosslinkable functional groups in the fiber are crosslinked with each other.

[0020] 3. The electrode according to items 1-2, wherein the crosslinkable functional group is one or more of (meth)acryloyl, (meth)acryloyloxy, and (meth)acryloyloxyalkyl.

[0021] 4. The electrodes according to items 1-3, wherein the polysilsesquioxane having crosslinkable functional groups also has substituted or unsubstituted aromatic groups.

[0022] 5. The electrodes according to items 1-4, wherein the polysilsesquioxanes having crosslinkable functional groups include random, ladder, cage or partially cage types.

[0023] 6. Based on the electrodes in items 1-5, the polysilsesquioxane is ladder-shaped and represented by the following chemical formula 3: [Chemical Formula 3]

[0024] In chemical formula 3, R 3 R 4 R 5 and R 6 Each of these components is independently hydrogen, hydroxyl, C1 to C20 alkyl, C2 to C20 alkenyl, C2 to C20 alkynyl, C3 to C20 cycloalkyl, C6 to C20 aryl, C7 to C20 aralkyl, crosslinkable functional group, or a combination thereof. R 3 R 4 R 5 and R 6 At least one of them includes a crosslinkable functional group, and n is the number of moles in the unit.

[0025] 7. Based on the electrodes in items 1-6, where R is in chemical formula 3. 3 R 4 R 5 and R 6 Each is independently phenyl or (meth)acryloyl, and R 3 R 4 R 5 and R 6 At least one of them includes (meth)acryloyl.

[0026] 8. The electrode according to items 1-7, wherein the content of polysilsesquioxane having crosslinkable functional groups is in the range of 10wt% to 100wt% of the fiber.

[0027] 9. The electrode according to items 1-8, wherein the fiber further comprises a polymer, and the polymer comprises polyvinylidene fluoride, polyacrylonitrile, polyamide-imide, polyvinylpyrrolidone, polyacrylic acid, polyvinyl alcohol, aromatic polyamide or combinations thereof.

[0028] 10. The electrode according to items 1-9, wherein the polymer comprises a mixture of polyvinylidene fluoride and polyacrylonitrile.

[0029] 11. The electrode according to items 1-10, wherein, relative to 100 parts by weight of the mixture, polyvinylidene fluoride and polyacrylonitrile are included in the range of 10 parts by weight to 90 parts by weight: 90 parts by weight to 10 parts by weight.

[0030] 12. The electrode according to items 1-11, wherein, relative to 100 parts by weight of polymer, the fiber comprises 10 to 50 parts by weight of polysilsesquioxane.

[0031] 13. The electrode according to items 1-12, wherein the polysilsesquioxane has a weight-average molecular weight in the range of 2,000 g / mol to 100,000 g / mol.

[0032] 14. The electrode according to items 1-13, wherein the active material layer for the rechargeable lithium battery includes a positive electrode active material layer.

[0033] 15. The electrodes according to items 1-14, wherein the fibers also include aromatic polyamide polymers.

[0034] 16. The electrode according to items 1-15, wherein a polysilsesquioxane having crosslinkable functional groups and an aromatic polyamide polymer are included in the fiber in a weight ratio ranging from 1:1 to 20:1.

[0035] 17. The electrode according to items 1-16, wherein the fiber further comprises a polymer, and the polymer comprises polyvinylidene fluoride, polyacrylonitrile, polyamide-imide, polyvinylpyrrolidone, polyacrylic acid, polyvinyl alcohol or combinations thereof.

[0036] 18. The electrode according to items 1-17, wherein the polymer comprises a mixture of polyvinylidene fluoride and polyacrylonitrile.

[0037] 19. The electrode according to items 1-18, wherein, relative to 100 parts by weight of the mixture, polyvinylidene fluoride and polyacrylonitrile are included in the range of 10 parts by weight to 90 parts by weight: 90 parts by weight to 10 parts by weight.

[0038] 20. The electrode according to items 1-19, wherein, relative to 100 parts by weight of polymer, the fiber comprises 1 to 40 parts by weight of polysilsesquioxane and 0.1 to 30 parts by weight of aromatic polyamide polymer.

[0039] 21. Electrodes used in rechargeable lithium batteries include: Active material layer for rechargeable lithium batteries; and The organic-inorganic composite layer is integrated with the active material layer. The organic-inorganic composite layer includes fibers, which contain polyvinylidene fluoride polymers, polyacrylonitrile polymers, and polysilsesquioxane.

[0040] 22. According to the electrode in item 21, the fiber is an island fiber.

[0041] 23. The electrode according to items 21-22, wherein the island fiber has a sea region and an island region, the sea region being composed of a polyvinylidene fluoride polymer, and the island region having a core-shell structure having a core composed of a polyacrylonitrile polymer and a shell surrounding the core and composed of polysilsesquioxane.

[0042] 24. The electrodes according to items 21-23, wherein, in the island fiber, the island regions are randomly arranged in the sea region.

[0043] 25. The electrodes according to items 21-24, wherein, in the cross-section of the island fiber, the area ratio of the island region is 30% to 50%.

[0044] 26. The electrode according to items 21-25, wherein the polysilsesquioxane has substituted or unsubstituted aromatic groups.

[0045] 27. The electrode according to items 21-26, wherein the polysilsesquioxane has crosslinkable functional groups.

[0046] 28. The electrode according to items 21-27, wherein at least some of the crosslinkable functional groups in the fiber are crosslinked with each other.

[0047] 29. The electrode according to items 21-28, wherein the crosslinkable functional group includes one or more of epoxy group, glycidyl group, glycidyloxy group and glycidyloxyalkyl group.

[0048] 30. The electrodes according to items 21-29, wherein the polysilsesquioxane includes random, ladder, cage or partially cage-like types.

[0049] 31. According to the electrodes in items 21-30, the polysilsesquioxane is ladder-shaped and represented by the following chemical formula 8: [Chemical Formula 8]

[0050] In chemical formula 8, R 7 R 8 R 9 and R 10 Each of these components is independently hydrogen, hydroxyl, C1 to C20 alkyl, C2 to C20 alkenyl, C2 to C20 alkynyl, C3 to C20 cycloalkyl, C6 to C20 aryl, C7 to C20 aralkyl, crosslinkable functional group, or a combination thereof. R 7 R 8 R 9 and R 10 At least one of them includes a crosslinkable functional group, and n is the number of moles in the unit.

[0051] 32. According to the electrodes in items 21-31, where R is in chemical formula 8. 7 R 8 R 9 and R 10 Each is independently phenyl, epoxy, glycidyl, glycidyloxy, or glycidyloxyalkyl, and R 7 R 8 R 9 and R 10 At least one of them includes an epoxy group, a glycidyl group, a glycidyloxy group, or a glycidyloxyalkyl group.

[0052] 33. The electrode according to items 21-32, wherein, relative to the total amount of 100 parts by weight of polyvinylidene fluoride polymers and polyacrylonitrile polymers, the polyvinylidene fluoride polymers and polyacrylonitrile polymers are included in the range of 50 parts by weight to 90 parts by weight and 50 parts by weight to 10 parts by weight.

[0053] 34. The electrode according to items 21-33, wherein the content of polysilsesquioxane is in the range of 5 parts by weight to 50 parts by weight relative to the total amount of 100 parts by weight of polyvinylidene fluoride polymers and polyacrylonitrile polymers.

[0054] 35. The electrode according to items 21-34, wherein the active material layer for the rechargeable lithium battery includes a negative electrode active material layer.

[0055] 36. Electrodes used in rechargeable lithium batteries include: Active material layer for rechargeable lithium batteries; and A multi-layered organic-inorganic composite layer is integrated with the active material layer used in rechargeable lithium batteries. The multilayer organic-inorganic composite layer includes a first organic-inorganic composite layer and a second organic-inorganic composite layer, and The difference in polysilsesquioxane content between the first organic-inorganic composite layer and the second organic-inorganic composite layer is 10 wt% or greater.

[0056] 37. The electrode according to item 36, wherein the multilayer organic-inorganic composite layer has a total of 2 to 8 first organic-inorganic composite layers and second organic-inorganic composite layers.

[0057] 38. The electrode according to items 36-37, wherein the second organic-inorganic composite layer has a higher polysilsesquioxane content than the first organic-inorganic composite layer.

[0058] 39. The electrode according to items 36-38, wherein the second organic-inorganic composite layer is integrated with the active material layer for the rechargeable lithium battery, and the active material layer for the rechargeable lithium battery is the negative electrode active material layer.

[0059] 40. The electrode according to items 36-39, wherein the content of polysilsesquioxane in the second organic-inorganic composite layer is 10 wt% or more, and the content of polysilsesquioxane in the first organic-inorganic composite layer is 0 wt% or more.

[0060] 41. The electrode according to items 36-40, wherein a first organic-inorganic composite layer and a second organic-inorganic composite layer are stacked alternately.

[0061] 42. The electrode according to items 36-41, wherein the polysilsesquioxane content of the multilayer organic-inorganic composite layer is in the range of 10 wt% to 30 wt% relative to 100 parts by weight of polymer.

[0062] 43. The electrode according to items 36-42, wherein the multilayer organic-inorganic composite layer has a thickness in the range of 0.5 μm to 20 μm.

[0063] 44. The electrodes according to items 36-43, wherein the polysilsesquioxane has substituted or unsubstituted aromatic groups.

[0064] 45. The electrode according to items 36-44, wherein the polysilsesquioxane has crosslinkable functional groups.

[0065] 46. ​​The electrode according to items 36-45, wherein the crosslinkable functional group includes one or more of (meth)acryloyl, (meth)acryloyloxy, (meth)acryloyloxyalkyl, epoxy, glycidyl, glycidoxy and glycidoxyalkyl.

[0066] 47. According to the electrodes in items 36-46, the polysilsesquioxane includes a ladder-type structure and is represented by the following chemical formula 8: [Chemical Formula 8]

[0067] In chemical formula 8, R 7 R 8 R 9 and R 10 Each of these components is independently hydrogen, hydroxyl, C1 to C20 alkyl, C2 to C20 alkenyl, C2 to C20 alkynyl, C3 to C20 cycloalkyl, C6 to C20 aryl, C7 to C20 aralkyl, crosslinkable functional group, or a combination thereof. R 7 R 8 R 9 and R 10 At least one of them includes a crosslinkable functional group, and n is the number of moles in the unit.

[0068] 48. The electrode according to claims 36-47, wherein at least one of the first organic-inorganic composite layer and the second organic-inorganic composite layer comprises fibers containing polysilsesquioxane.

[0069] 49. The electrodes according to items 36-48, wherein the fibers containing polysilsesquioxane also include polyvinylidene fluoride polymers and polyacrylonitrile polymers.

[0070] 50. According to the electrodes in items 36-49, the fiber is an island fiber.

[0071] 51. The electrode according to items 36-50, wherein the island fiber has a sea region and an island region, the sea region being composed of a polyvinylidene fluoride polymer, and the island region having a core-shell structure having a core composed of a polyacrylonitrile polymer and a shell surrounding the core and composed of polysilsesquioxane.

[0072] 52. The electrode according to items 36-51, wherein, relative to the total amount of 100 parts by weight of polyvinylidene fluoride polymers and polyacrylonitrile polymers, the polyvinylidene fluoride polymers and polyacrylonitrile polymers are included in the range of 50 parts by weight to 90 parts by weight and 50 parts by weight to 10 parts by weight.

[0073] 53. The electrode according to items 36-52, wherein the content of polysilsesquioxane is in the range of 5 parts by weight to 50 parts by weight relative to the total amount of 100 parts by weight of polyvinylidene fluoride polymers and polyacrylonitrile polymers.

[0074] Another embodiment provides a rechargeable lithium battery.

[0075] The rechargeable lithium battery includes the electrode for the rechargeable lithium battery; and an electrode for the rechargeable lithium battery facing the electrode for the rechargeable lithium battery.

[0076] 54. Rechargeable lithium batteries include: Electrodes for rechargeable lithium batteries according to items 1 to 53; and Electrodes for rechargeable lithium batteries, facing the electrodes for rechargeable lithium batteries.

[0077] 55. The rechargeable lithium battery according to item 54, wherein the rechargeable lithium battery does not have a separator.

[0078] In an electrode for a rechargeable lithium battery according to one embodiment, an organic-inorganic composite layer is integrated with the active material layer. Therefore, a lamination process for combining the separator and the active material layer is unnecessary, allowing for economical battery manufacturing. Since the permeability and tensile strength of the organic-inorganic composite layer in the electrode for a rechargeable lithium battery according to one embodiment are improved, the organic-inorganic composite layer can replace a conventional separator, thereby also improving the mechanical strength of the electrode.

[0079] In an electrode for a rechargeable lithium battery according to one embodiment, the adhesion and tensile strength of the organic-inorganic composite layer can be improved, thus allowing the organic-inorganic composite layer to replace a conventional separator, thereby improving electrode reliability. In an electrode for a rechargeable lithium battery according to one embodiment, the electrode wettability of the organic-inorganic composite layer can be improved, thereby enhancing the reliability of the electrode in the battery.

[0080] In an electrode for a rechargeable lithium-ion battery according to one embodiment, an organic-inorganic composite layer is integrated with the active material layer. Therefore, a stacking process for combining the separator and active material layers is unnecessary, allowing for economical battery manufacturing. In one embodiment, the electrode for the rechargeable lithium-ion battery can exhibit improved permeability and improved stability against foreign matter. This can reduce resistance associated with lithium-ion migration and decrease cell defect rates caused by foreign matter during the manufacture of rechargeable lithium-ion batteries (such as stacked cells) or electrode volume expansion during charging and discharging. The electrode for a rechargeable lithium-ion battery according to one embodiment can exhibit improved tensile strength, improved electrolyte wettability, improved adhesion, and improved heat resistance, and includes an organic-inorganic composite layer exhibiting a turn-off effect, thereby improving the reliability of the rechargeable battery without a conventional separator. Attached Figure Description

[0081] The above and other objects, features, and advantages of this disclosure will become more apparent to those skilled in the art from the detailed description of exemplary embodiments with reference to the accompanying drawings, in which: Figure 1 This is a cross-sectional view of an electrode for a rechargeable lithium battery according to the first, second, or third embodiment; Figure 2 The results of line scan analysis of the surface of the organic-inorganic composite layer according to the first embodiment using transmission electron microscopy (TEM) are shown. Figure 3 TEM results of the surface of the fibers of the organic-inorganic composite layer according to the first embodiment are shown; Figure 4 TEM results of a cross-section of the fibers of the organic-inorganic composite layer according to the first embodiment are shown; Figure 5 TEM results of the surface of the fibers of the organic-inorganic composite layer according to the second embodiment are shown; Figure 6 TEM results of a cross-section of the fibers of the organic-inorganic composite layer according to the second embodiment are shown; Figure 7 The results of transverse analysis of the fibers included in the organic-inorganic composite layer according to the third embodiment are shown; Figure 8 The results of high-angle annular dark-field scanning transmission electron microscopy (HAADF-STEM) analysis of silicon and carbon in the cross-section of the fiber according to the third embodiment are shown. Figure 9 The results of HAADF-STEM for the fibers according to the third embodiment are shown; Figure 10 The results of transmission electron microscopy-energy dispersive spectroscopy (TEM-EDS) of the fiber according to the third embodiment are shown; Figure 11 This is a schematic cross-sectional view of the island fiber according to the third embodiment; Figures 12 to 15 This is a cross-sectional view of an electrode for a rechargeable lithium battery according to the fourth embodiment. Figure 16 The HAADF-STEM results of the fibers according to the fourth embodiment are shown; Figure 17 The results of scanning transmission electron microscopy-energy dispersive spectroscopy (STEM-EDS) of the fiber according to the fourth embodiment are shown; Figure 18 This is a schematic cross-sectional view of the island fiber according to the fourth embodiment; Figure 19This is a cross-sectional view of an electrode assembly for a rechargeable lithium battery according to a fourth embodiment. Figures 20 to 23 A rechargeable lithium battery according to one embodiment is schematically shown; Figure 24 The SEM results of the organic-inorganic composite layer before the shutdown evaluation of Example 7 are shown; Figure 25 The SEM results of the organic-inorganic composite layer after the shutdown evaluation of Example 7 are shown. Figure 26 The SEM results obtained after hot-pressing the organic-inorganic composite layer of Example 7 are shown. Figure 27 The SEM results obtained after hot-pressing the organic-inorganic composite layer of Comparative Example 7 are shown; and Figure 28 A diagram is shown illustrating a method for measuring short-circuit strength during compression after foreign body injection. Detailed Implementation

[0082] Preferred exemplary embodiments of the present disclosure are described in detail below with reference to the accompanying drawings. Prior to this, the terms or words used in this specification and claims should not be construed as limited to their typical or dictionary meanings, but rather should be interpreted based on the principle that the inventor can appropriately define the concepts of the terms to best interpret his own disclosure, using meanings and concepts consistent with the technical spirit of the present disclosure. Therefore, it should be understood that the exemplary embodiments described in this specification and the constructions shown in the accompanying drawings are only some of the most preferred exemplary embodiments of the present disclosure and do not represent all the technical spirit of the present disclosure, and various equivalents and modifications may exist at the time of filing this application. Furthermore, when used in this specification, "comprising" and "including" and / or variations thereof indicate the presence of the mentioned shapes, quantities, steps, operations, elements, components, and / or groups thereof, without excluding the presence or addition of one or more other shapes, quantities, operations, elements, components, and / or groups thereof. Additionally, when describing exemplary embodiments of the present disclosure, "may" and "may be" may include "one or more exemplary embodiments of the present disclosure".

[0083] Example embodiments of this disclosure are described in detail below. However, these are presented by way of example and are not intended to limit the disclosure, which is defined only by the scope of the claims.

[0084] Unless otherwise stated herein, when a component such as a layer, film, region, or plate is described as being “on” another component, this includes not only the case where the component is “directly on” the other component, but also the case where there is another component between them.

[0085] Unless otherwise specified, a singular expression may also include a plural expression. Furthermore, unless otherwise specified, "A or B" may mean "including A, including B, or including both A and B".

[0086] In the specification, "the combination of them" can refer to mixtures, laminates, complexes, copolymers, alloys, blends, and reaction products of the components.

[0087] When the terms “about” or “substantially” are used in conjunction with numerical values ​​in this specification, it is intended that the relevant numerical values ​​include a tolerance of ±10% around the stated value. When a range is specified, the range includes all values ​​within that range, such as increments of 0.1%.

[0088] In this specification, "particle size (D50)" refers to the average particle size representing the size of particles that constitute 50% of the cumulative volume in a particle size distribution. The particle size distribution can be measured using methods well-known to those skilled in the art. For example, it can be measured using a particle size analyzer or by transmission electron microscopy or scanning electron microscopy. Alternatively, by using a measuring device that utilizes dynamic light scattering, particle size can be measured using dynamic light scattering. The number of particles in each particle size range can be counted through data analysis, and the D50 value can be calculated from this. Optionally, the number of particles can be measured using laser diffraction. When measured by laser diffraction, more specifically, the particles to be measured can be dispersed in a dispersion medium and irradiated with ultrasound at approximately 28 kHz at a 60 W output using a commercially available laser diffraction particle size measuring device (e.g., Microtrac MT 3000). The D50 can then be calculated using the measuring device based on 50% of the particle size distribution.

[0089] If the particles described above are spherical, then the dimensions described above can represent the diameter.

[0090] When describing numerical ranges in this specification, “X to Y” means “X or greater and Y or less (greater than or equal to X and less than or equal to Y)”.

[0091] The following description will primarily focus on rechargeable lithium batteries. However, this disclosure is applicable not only to rechargeable lithium batteries but also to other types of rechargeable batteries.

[0092] An electrode for a rechargeable lithium battery (hereinafter also referred to as an "electrode") according to one embodiment includes an active material layer for the rechargeable lithium battery and an organic-inorganic composite layer integrated with the active material layer, wherein the organic-inorganic composite layer includes fibers comprising polysilsesquioxane (PSSQ).

[0093] Figure 1This is a cross-sectional view of an electrode for a rechargeable lithium battery according to a first embodiment, a second embodiment, or a third embodiment.

[0094] Reference Figure 1 Electrode 1 may include an active material layer 2 for a rechargeable lithium battery and an organic-inorganic composite layer 3 integrated on one surface of the active material layer 2 for a rechargeable lithium battery. Figure 1 The diagram shows the active material layer 2 and the organic-inorganic composite layer for rechargeable lithium batteries formed as separate layers, but the dashed line indicates the integration of the active material layer 2 and the organic-inorganic composite layer 3 for rechargeable lithium batteries.

[0095] The first electrode for rechargeable lithium batteries An electrode for a rechargeable lithium battery (hereinafter also referred to as an "electrode") includes an active material layer for the rechargeable lithium battery and an organic-inorganic composite layer integrated with the active material layer, wherein the organic-inorganic composite layer includes fibers containing PSSQ having crosslinkable functional groups.

[0096] The fiber can be a core-shell fiber having a core and a shell surrounding the core. The shell can include PSSQ having crosslinkable functional groups. The core can include non-silicone polymers as described below.

[0097] Organic-inorganic composite layers can exhibit improved tensile strength and improved air permeability. In one embodiment, the organic-inorganic composite layer can have a tensile strength of 250 kgf / cm². 2 Or greater (e.g., 450 kgf / cm²) 2 Or even higher, for example, 450 kgf / cm² 2 Up to 800 kgf / cm 2 The tensile strength is [specified]. Within the above range, the reliability of the electrode can be improved. In one embodiment, the organic-inorganic composite layer can have an air permeability of 120 sec / 100 cc or less (e.g., 10 sec / 100 cc to 120 sec / 100 cc). Within the above range, the organic-inorganic composite layer can replace a conventional diaphragm. Tensile strength and air permeability can be measured by the methods described below.

[0098] Organic-inorganic composite layer Organic-inorganic composite layers can be used as a separator between the active material layer for rechargeable lithium batteries and the electrode facing the active material layer for rechargeable lithium batteries to prevent short circuits.

[0099] Rechargeable lithium batteries that include this electrode may not require a separate separator. Therefore, during battery manufacturing (such as stacked cells), the electrode does not require the lamination process used to combine the separator and electrode, enabling battery manufacturing with a simpler and more economical process. Furthermore, the electrode does not suffer from the thermal shrinkage issues associated with conventional separators, thus improving battery stability and lifespan.

[0100] Organic-inorganic composite layers can be integrated with the active material layer used in rechargeable lithium batteries. Here, "integration" can refer to the state where the organic-inorganic composite layer is formed directly on the active material layer without the intervention of any other layer, that is, the organic-inorganic composite layer is more firmly bonded to the active material layer.

[0101] Scanning electron microscopy (SEM) or transmission electron microscopy (TEM) can be used to confirm the integration of the active material layer and the organic-inorganic composite layer. According to one embodiment, SEM or TEM results clearly show that the active material layer can be distinguished from the organic-inorganic composite layer, but the interface (boundary) between them is not clearly defined and appears to be non-uniform.

[0102] Organic-inorganic composite layers can be formed by infiltrating into the active material layer, drying, and cross-linking. This prevents the increase in resistance during lithium-ion migration. The process for forming organic-inorganic composite layers is described in detail below.

[0103] The organic-inorganic composite layer can be a single layer. Here, "single layer" can mean that fibers containing PSSQ with crosslinkable functional groups are electrospun onto an active material layer to form a single layer in which the organic and inorganic components are not included in separate layers but are included in a single layer.

[0104] Organic-inorganic composite layers can have a nonwoven state, such as a network structure of multiple fibers. The network structure can be advantageous for minimizing resistance during lithium-ion migration. The network structure can refer to a porous layer with pores randomly formed between the fibers. According to one embodiment, the diameter of the pores can be in the range of 500 nm or smaller (e.g., 10 nm to 300 nm).

[0105] Based on their average diameter, the fibers can be microfibers or nanofibers. The average diameter of the fibers can be in the range of 500 nm or smaller (e.g., 10 nm to 350 nm or 10 nm to 300 nm). Within the above range, organic-inorganic composite layers can be readily formed. Here, the “average diameter” of the nanofibers can be the average calculated from the diameters measured from multiple (approximately 100) nanofibers selected from SEM images.

[0106] Organic-inorganic composite layers include fibers containing PSSQ with crosslinkable functional groups.

[0107] Even when mixed with the polymers described below, PSSQ can be electrospun as is and uniformly dispersed in the polymer. Therefore, PSSQ can achieve the effect of an organic-inorganic composite layer even at any location within the organic-inorganic composite layer, thereby improving reliability.

[0108] Figure 2 The results are based on line scan analysis of the surface of the fibers in the organic-inorganic composite layer of the first embodiment. (Refer to...) Figure 2 This confirms that silicon is distributed within the organic-inorganic composite layer. Figure 2 In this context, silicon (Si) can represent the position of PSSQ within the fiber. Figure 2 In the diagram, solid lines represent carbon, dashed lines represent high-angle annular dark field (HAADF), and dotted lines represent silicon.

[0109] Figure 3 and Figure 4 TEM results of the surface and cross-section of the fibers of the organic-inorganic composite layer according to the first embodiment are shown. (Refer to...) Figure 3 and Figure 4 The white portion is silicon, indicating that silicon is evenly distributed throughout the fiber.

[0110] PSSQ possesses crosslinkable functional groups. At least some of these crosslinkable functional groups can crosslink with each other during the formation of the organic-inorganic composite layer. This improves the tensile strength of the organic-inorganic composite layer not only by increasing the degree of connection between PSSQs within the same fiber, but also by increasing the degree of connection between PSSQs in adjacent fibers within the organic-inorganic composite layer. Furthermore, the tensile strength of the organic-inorganic composite layer can be further enhanced by the interaction of PSSQs with polymers described below.

[0111] In one embodiment, the fiber may include at least a crosslinked product of PSSQ having crosslinkable functional groups.

[0112] The crosslinkable functional group can be a functional group that can be crosslinked by heat and / or light. For example, the crosslinkable functional group can include one or more of (meth)acryloyl, (meth)acryloyloxy, and (meth)acryloyloxyalkyl.

[0113] The crosslinkable functional group can be represented by the following chemical formula 1, but this disclosure is not limited thereto: [Chemical Formula 1]

[0114] In chemical formula 1, It is the connecting part of the elements. R1 It is hydrogen or methyl, and R 2 It is a single bond or a C1 to C20 alkylene group.

[0115] Crosslinkable functional groups can be included at any location on the PSSQ. For example, crosslinkable functional groups can be included at the ends of the PSSQ.

[0116] PSSQ with crosslinkable functional groups can also have substituted or unsubstituted aromatic groups. Compared to epoxy, substituted or unsubstituted aromatic groups (e.g., phenyl) have lower crosslinking rates and higher energy requirements for crosslinking. Therefore, after electrospinning, the process can be carried out at higher temperatures compared to PSSQ with epoxy as a functional group. When post-processing is performed at high temperatures after spinning, the crystallinity of the polymer used together increases due to recrystallization and annealing effects. Therefore, PSSQ with substituted or unsubstituted aromatic groups can have higher mechanical strength than PSSQ with epoxy as a functional group. Here, "substituted or unsubstituted aromatic group" can refer to substituted or unsubstituted C6 to C10 monocyclic or heterocyclic aromatic groups. Here, "substituted or unsubstituted" can mean that one or more hydrogen atoms of the functional group are substituted by C1 to C10 alkyl, halogen, hydroxyl, amino, or C6 to C10 aryl. For example, the substituted or unsubstituted aromatic group can be phenyl, and the crosslinkable functional group can be (meth)acryloyl. For example, substituted or unsubstituted aromatic groups can be bonded to the silicon of PSSQ.

[0117] PSSQs with crosslinkable functional groups can be random, ladder-shaped, cage-shaped, or partially cage-shaped. For example, PSSQs with crosslinkable functional groups can be ladder-shaped.

[0118] In one embodiment, the PSSQ having crosslinkable functional groups can have units of the following chemical formula 2: [Chemical Formula 2] [RSiO 2 / 3 ] n In chemical formula 2, R is hydrogen, hydroxyl, C1 to C20 alkyl, C2 to C20 alkenyl, C2 to C20 alkynyl, C3 to C20 cycloalkyl, C6 to C20 aryl, C7 to C20 aralkyl, crosslinkable functional group or a combination thereof, n is the number of moles of the unit, and at least one of R is a crosslinkable functional group.

[0119] n can be from 1 to 1,000,000.

[0120] In one embodiment, the PSSQ having crosslinkable functional groups is ladder-shaped and can be represented by the following chemical formula 3, but this disclosure is not limited thereto.

[0121] [Chemical Formula 3]

[0122] In chemical formula 3, R 3 R 4 R 5 and R 6 Each of these components is independently hydrogen, hydroxyl, C1 to C20 alkyl, C2 to C20 alkenyl, C2 to C20 alkynyl, C3 to C20 cycloalkyl, C6 to C20 aryl, C7 to C20 aralkyl, crosslinkable functional group, or a combination thereof. R 3 R 4 R 5 and R 6 At least one of them is a crosslinkable functional group, and n is the number of moles in the unit.

[0123] n can be from 1 to 1,000,000.

[0124] In chemical formula 3, the crosslinkable functional groups can be the same as those defined in chemical formula 1.

[0125] In chemical formula 3, R 3 R 4 R 5 and R 6 Each is independently a hydroxyl group, a C6 to C20 aryl group, a crosslinkable functional group, or a combination thereof, and R 3 R 4 R 5 and R 6 At least one of them can be a crosslinkable functional group.

[0126] PSSQs with crosslinkable functional groups can have concentrations from 2,000 g / mol to 100,000 g / mol (e.g., 2000 g / mol, 3000 g / mol, 4000 g / mol, 5000 g / mol, 6000 g / mol, 7000 g / mol, 8000 g / mol, 9000 g / mol, 10000 g / mol, 11000 g / mol, 12000 g / mol, 13000 g / mol, 14000 g / mol, 15000 g / mol, 16000 g / mol, 17000 g / mol, 18000 g / mol, 190 g / mol). The weight-average molecular weights (MAMs) of PSSQ are 0.00 g / mol, 20000 g / mol, 25000 g / mol, 30000 g / mol, 35000 g / mol, 40000 g / mol, 45000 g / mol, 50000 g / mol, 55000 g / mol, 60000 g / mol, 65000 g / mol, 70000 g / mol, 75000 g / mol, 80000 g / mol, 85000 g / mol, 90000 g / mol, 95000 g / mol, 100000 g / mol, or 15,000 g / mol to 20,000 g / mol. Within these ranges, the viscosity of PSSQ can be easily adjusted. The weight-average molecular weight can be obtained as a standard conversion value for polystyrene using gel permeation chromatography.

[0127] The fiber can be formed solely from PSSQ having crosslinkable functional groups. However, the fiber may also include polymers to facilitate electrospinning for fiber formation.

[0128] In one embodiment, the content of PSSQ having crosslinkable functional groups can be from 10 wt% to 80 wt% of the fiber, for example, 10 wt%, 11 wt%, 12 wt%, 13 wt%, 14 wt%, 15 wt%, 16 wt%, 17 wt%, 18 wt%, 19 wt%, 20 wt%, 21 wt%, 22 wt%, 23 wt%, 24 wt%, 25 wt%, 26 wt%, 27 wt%, 28 wt%, 29 wt%, 30 wt%, 31 wt%, 32 wt%, 33 wt%, 34 wt%, 35 wt%, 36 wt%, 37 wt%, 38 wt%, 39 wt%, 40 wt%, 41 wt%, 42 wt%. The concentrations of organic-inorganic composite layers can be 43wt%, 44wt%, 45wt%, 46wt%, 47wt%, 48wt%, 49wt%, 50wt%, 51wt%, 52wt%, 53wt%, 54wt%, 55wt%, 56wt%, 57wt%, 58wt%, 59wt%, 60wt%, 61wt%, 62wt%, 63wt%, 64wt%, 65wt%, 66wt%, 67wt%, 68wt%, 69wt%, 70wt%, 71wt%, 72wt%, 73wt%, 74wt%, 75wt%, 76wt%, 77wt%, 78wt%, 79wt%, or 80wt%, or 10wt% to 70wt%. Within the above ranges, the aforementioned effects of organic-inorganic composite layers can be easily achieved.

[0129] There are no particular restrictions on the type of polymer, provided that it is suitable for electrospinning and does not adversely affect the dispersion and function of PSSQ with crosslinkable functional groups. For example, the polymer is a non-silicone polymer (excluding silicon) and may include polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), polyamide-imide (PAI), polyvinylpyrrolidone (PVP), polyacrylic acid (PAA), polyvinyl alcohol (PVA), aromatic polyamides, or combinations thereof.

[0130] In one embodiment, the polymer may be a mixture of PVDF and PAN. This mixture is suitable for electrospinning when combined with PSSQ having crosslinkable functional groups, and can exhibit the effect of improving the dispersibility of PSSQ having crosslinkable functional groups. Relative to 100 parts by weight of the mixture, PVDF and PAN may be included in a ratio of 10 parts by weight to 90 parts by weight: 90 parts by weight to 10 parts by weight (e.g., 10 parts by weight: 90 parts by weight, 15 parts by weight: 85 parts by weight, 20 parts by weight: 80 parts by weight, 25 parts by weight: 75 parts by weight, 30 parts by weight: 70 parts by weight, 35 parts by weight: 65 parts by weight, 40 parts by weight: 60 parts by weight, 45 parts by weight: 55 parts by weight, 50 parts by weight: 50 parts by weight, 55 parts by weight: 45 parts by weight, 60 parts by weight: 40 parts by weight, 65 parts by weight: 35 parts by weight, 70 parts by weight: 30 parts by weight, 75 parts by weight: 25 parts by weight, 80 parts by weight: 20 parts by weight, 85 parts by weight: 15 parts by weight, 90 parts by weight: 10 parts by weight, or 20 parts by weight to 60 parts by weight: 80 parts by weight to 40 parts by weight). Within the aforementioned range, PSSQ with crosslinkable functional groups can exhibit high dispersibility in mixtures.

[0131] In one embodiment, the fiber may comprise 1 to 50 parts by weight relative to 100 parts by weight of the polymer (e.g., 1 part by weight, 2 parts by weight, 3 parts by weight, 4 parts by weight, 5 parts by weight, 6 parts by weight, 7 parts by weight, 8 parts by weight, 9 parts by weight, 10 parts by weight, 11 parts by weight, 12 parts by weight, 13 parts by weight, 14 parts by weight, 15 parts by weight, 16 parts by weight, 17 parts by weight, 18 parts by weight, 19 parts by weight, 20 parts by weight, 21 parts by weight, 22 parts by weight, 23 parts by weight, 24 parts by weight, 25 parts by weight). PSSQ is available in the following weight ranges: 26 parts by weight, 27 parts by weight, 28 parts by weight, 29 parts by weight, 30 parts by weight, 31 parts by weight, 32 parts by weight, 33 parts by weight, 34 parts by weight, 35 parts by weight, 36 parts by weight, 37 parts by weight, 38 parts by weight, 39 parts by weight, 40 parts by weight, 41 parts by weight, 42 parts by weight, 43 parts by weight, 44 parts by weight, 45 parts by weight, 46 parts by weight, 47 parts by weight, 48 parts by weight, 49 parts by weight, or 50 parts by weight, or 10 to 50 parts by weight, or 5 to 30 parts by weight. Within these ranges, PSSQ exhibits high dispersibility.

[0132] The organic-inorganic composite layer can have a thickness of 1 μm to 30 μm (e.g., 5 μm to 15 μm). Within this range, the organic-inorganic composite layer can be used in batteries.

[0133] Organic-inorganic composite layers can be prepared by forming a fiber-containing layer on at least one surface of an active material layer and crosslinking the fiber-containing layer.

[0134] First, a layer containing fibers is formed on at least one surface of the active material layer.

[0135] According to one embodiment, the fiber-containing layer can be formed by electrospinning a solution for forming the fiber-containing layer on one surface of an active material layer. The solution may include PSSQ having crosslinkable functional groups and also includes a polymer.

[0136] Electrospinning can be performed as follows: a nozzle assembly consisting of needle tips with a gauge size of 23G to 30G and a collection roller are positioned at regular intervals; a solution is injected into the nozzle assembly; an active material layer is placed on the collection roller; and a voltage of 35kV to 90kV is applied to the needle tips. The distance between the nozzle assembly and the active material layer can be 10cm to 20cm. A needle tip size of 25G to 30G is preferred because it allows for the formation of an organic-inorganic composite layer in the desired shape.

[0137] During the electrospinning process, the solution is spun and stretched into a fibrous shape, thereby forming a fiber-containing layer on the active material layer. The solution is suspended as droplets at the tip due to surface tension, and when a voltage is applied, charges accumulate on the surface of the solution, generating repulsive forces. When a critical voltage is reached where the repulsive force between the charges becomes higher than the surface tension of the solution, a Taylor cone is generated, and a polymer solution jet is ejected from the tip of the cone and highly stretched to form fibers, which collect on the active material layer to form a fiber-containing layer.

[0138] According to one embodiment, the electrospinning process can be carried out at temperatures ranging from 15°C to 40°C and relative humidity ranging from 40% to 60%. When the electrospinning process is carried out under the above-mentioned temperature and relative humidity conditions, it has the advantage of maintaining a constant fiber diameter during spinning.

[0139] The solution may also include an initiator for promoting crosslinking of PSSQ having crosslinkable functional groups. The initiator may include one or more of a thermal initiator and a photoinitiator. The thermal initiator and photoinitiator may be any conventional type known to those skilled in the art.

[0140] The solution may also include a solvent, and the solvent may include, for example, dimethylacetamide, dimethyl sulfoxide, dimethylformamide, tetrahydrofuran, carbon tetrachloride, methylpyrrolidone, water, ethanol, acetone, or combinations thereof. The solvent may be included as a residue in the organic-inorganic composite layer.

[0141] In the solution, the content of PSSQ with crosslinkable functional groups or a mixture of PSSQ with crosslinkable functional groups and a polymer can be from 5 wt% to 40 wt% relative to 100 wt% of the total solution. Within the above range, the organic-inorganic composite layer can be formed to a suitable thickness.

[0142] In one embodiment, a drying process can be performed at 50°C to 100°C after the electrospinning process.

[0143] The fiber-containing layer can be pressed or hot-pressed after cross-linking. Pressing can increase the density between fibers in the fiber-containing layer and reduce the thickness of the organic-inorganic composite layer.

[0144] According to one embodiment, hot pressing can be performed by pressing a fiber-containing layer at 50°C or higher (e.g., 50°C to 100°C). The purpose of pressing is to control the thickness of the fiber layer, therefore the shape and size of the pressing equipment are not limited, as long as the desired thickness can be obtained. In one embodiment, hot pressing rollers are used for pressing, and the desired thickness can be achieved by adjusting the distance between the rollers.

[0145] Furthermore, the fibers can be cross-linked by heat-treating the fiber-containing layer under certain conditions. For heat treatment, the heat treatment temperature and / or heat treatment time can be adjusted according to the PSSQ or polymer content in the fibers. Heat treatment can be carried out at 50°C to 200°C (e.g., 100°C to 150°C) for 5 to 60 minutes.

[0146] Active material layer for rechargeable lithium batteries The active material layer used in a rechargeable lithium battery can be either a positive electrode active material layer or a negative electrode active material layer. For example, the active material layer used in a rechargeable lithium battery can be a positive electrode active material layer.

[0147] The positive electrode active material layer may include a positive electrode active material, and may also include a binder and / or a conductive material. In one example, the positive electrode active material layer may also include an additive that can be used as a sacrificial positive electrode.

[0148] The content of positive electrode active material can be 90 wt% to 99.5 wt% relative to 100 wt% of positive electrode active material layer, and the content of binder and conductive material can be 0.5 wt% to 5 wt% respectively relative to 100 wt% of positive electrode active material layer.

[0149] As the positive electrode active material, compounds capable of reversibly inserting and deintercalating lithium (lithium-intercalating compounds) can be used. Specifically, one or more composite oxides of lithium with at least one metal selected from cobalt, manganese, nickel, and combinations thereof can be used.

[0150] The composite oxide can be a lithium transition metal composite oxide, specifically, lithium nickel oxide, lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate compound, cobalt-free lithium nickel manganese oxide, or a combination thereof.

[0151] In one example, a compound represented by any of the following chemical formulas can be used: Li a A 1-b X b O 2- c D c (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05); Li a Mn 2-b X b O 4-c D c (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05); Li a Ni 1-b-c Co b X c O 2-α D α (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<α<2); Li a Ni 1-b- c Mn b X c O 2-α D α (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<α<2); Li a Ni b Co c L 1 d G e O2 (0.90≤a≤1.8, 0≤b≤0.9, 0≤c≤0.5, 0≤d≤0.5, 0≤e≤0.1); Li a NiG b O2 (0.90≤a≤1.8, 0.001≤b≤0.1); Li a CoG b O2 (0.90≤a≤1.8, 0.001≤b≤0.1); Li a Mn 1-b G b O2 (0.90≤a≤1.8, 0.001≤b≤0.1); Li a Mn2G b O4 (0.90≤a≤1.8, 0.001≤b≤0.1); Li aMn 1-g G g PO4 (0.90≤a≤1.8, 0≤g≤0.5); Li (3-f) Fe2(PO4)3 (0≤f≤2); and Li a FePO4 (0.90≤a≤1.8).

[0152] In the above chemical formulas, A is Ni, Co, Mn, or a combination thereof; X is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, rare earth metals, or a combination thereof; D is O, F, S, P, or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, or a combination thereof; and L 1 It is Mn, Al, or a combination thereof.

[0153] In one example, the positive electrode active material can be a high-nickel positive electrode active material, in which the nickel content is 80 mol% or more, 85 mol% or more, 90 mol% or more, 91 mol% or more, 94 mol% or more, or 99 mol% or less relative to 100 wt% of metals other than lithium in the lithium transition metal composite oxide. Such a high-nickel positive electrode active material can exhibit high capacity and therefore can be used in high-capacity, high-density rechargeable lithium batteries.

[0154] The binder enables the positive electrode active material particles to adhere well to each other and also enables the positive electrode active material to adhere well to the current collector. Representative examples of binders may include PVA, carboxymethyl cellulose, hydroxypropyl cellulose, cellulose diacetate, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, PVP, polyurethane, polytetrafluoroethylene, PVDF, polyethylene, polypropylene, styrene-butadiene rubber, (meth)acrylated styrene-butadiene rubber, epoxy resin, (meth)acrylate resin, polyester resin, nylon, but this disclosure is not limited thereto.

[0155] Conductive materials are used to impart conductivity to electrodes and can be any electrically conductive material that does not cause chemical changes in the battery in which it is not used. Examples of conductive materials include: carbon-based materials such as natural graphite, synthetic graphite, carbon black, acetylene black, Ketjen black, carbon fibers, carbon, and nanofibers; metallic materials, including copper, nickel, aluminum, silver, etc., in the form of metal powders or metal fibers; conductive polymers, such as polyphenylene derivatives; or mixtures thereof.

[0156] The negative electrode active material layer may include a negative electrode active material, and may further include a binder and / or a conductive material. For example, the negative electrode active material layer may include 90 wt% to 99 wt% of the negative electrode active material, 0.5 wt% to 5 wt% of the binder, and 0 wt% to 5 wt% of the conductive material.

[0157] The negative electrode active material includes a material capable of reversibly intercalating / deintercalating lithium ions, lithium metal, an alloy of lithium and a metal, a material capable of doping and dedoping lithium, or a transition metal oxide.

[0158] The material capable of reversibly intercalating / deintercalating lithium ions may be a carbon-based negative electrode active material, such as crystalline carbon, amorphous carbon, or a combination thereof. The crystalline carbon may be graphite, such as amorphous, plate-like, flake-like, spherical or fibrous natural graphite or artificial graphite, and the amorphous carbon may be soft carbon or hard carbon, mesophase pitch carbide, or calcined coke.

[0159] The alloy of lithium and a metal may be an alloy of lithium and at least one of metals Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, and Sn.

[0160] The material capable of doping and dedoping lithium may be a Si-based negative electrode active material or a Sn-based negative electrode active material. The Si-based negative electrode active material may be silicon, a silicon-carbon composite, SiO x (0<x≤2), a Si-Q alloy (Q is one of an alkali metal, an alkaline earth metal, a Group 13 element, a Group 14 element (excluding Si), a Group 15 element, a Group 16 element, a transition metal, a rare earth element, and combinations thereof), or a combination thereof. The Sn-based negative electrode active material may be Sn, SnO₂, a Sn-based alloy, or a combination thereof.

[0161] The silicon-carbon composite may be a composite of silicon and amorphous carbon. According to an embodiment, the silicon-carbon composite may be silicon particles coated with amorphous carbon. For example, the silicon-carbon composite may include secondary particles (core) assembled from primary silicon particles and an amorphous carbon coating (shell) located on the surface of the secondary particles. Amorphous carbon is also located between the primary silicon particles, so that the primary silicon particles may be coated with, for example, amorphous carbon. The secondary particles may be dispersed in an amorphous carbon matrix.

[0162] The silicon-carbon composite may further include crystalline carbon. For example, the silicon-carbon composite may include a core containing crystalline carbon and silicon particles, and an amorphous carbon coating located on the surface of the core.

[0163] The Si-based negative electrode active material or the Sn-based negative electrode active material may be used after being mixed with the carbon-based negative electrode active material.

[0164] The binder enables the negative electrode active material particles to adhere well to each other and to the current collector. Non-aqueous binders, aqueous binders, dry binders, or combinations thereof can be used as binders.

[0165] Non-aqueous adhesives may be polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene-propylene copolymer, polystyrene, polyurethane, polytetrafluoroethylene, PVDF, polyethylene, polypropylene, PAI, polyimide, or combinations thereof.

[0166] The waterborne adhesive may be at least one of styrene-butadiene rubber, (meth)acrylated styrene-butadiene rubber, (meth)acrylonitrile-butadiene rubber, (meth)acryloyl rubber, butyl rubber, fluorinated elastomer, polyethylene oxide, PVP, polyepoxygenated alcohol, polyphosphazene, poly(meth)acrylonitrile, ethylene-propylene-diene copolymer, polyvinylpyridine, chlorosulfonated polyethylene, latex, polyester resin, (meth)acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol, and combinations thereof.

[0167] When using an aqueous binder as the negative electrode binder, it may also include a cellulose-based compound capable of imparting viscosity. As a cellulose-based compound, one or more of carboxymethyl cellulose, hydroxypropyl methyl cellulose, methyl cellulose, and their alkali metal salts may be mixed and used. The alkali metal may be Na, K, or Li.

[0168] Dry binders are polymeric materials capable of being fibrous and can be, for example, polytetrafluoroethylene, PVDF, vinylidene fluoride-hexafluoropropylene copolymer, polyethylene oxide, or combinations thereof.

[0169] Conductive materials are used to impart conductivity to electrodes and can be any electrically conductive material that does not cause chemical changes in the battery in which it is not used. Specific examples of conductive materials include carbon-based materials such as natural graphite, synthetic graphite, carbon black, acetylene black, Ketjen black, carbon fibers, carbon, and nanofibers; metallic materials, including copper, nickel, aluminum, silver, etc., in the form of metal powders or metal fibers; conductive polymers, such as polyphenylene derivatives; or mixtures thereof.

[0170] Electrodes used in rechargeable lithium batteries may also include current collectors.

[0171] The current collector may be located on one surface of the active material layer. According to one embodiment, the electrode may include an active material layer, a current collector located on one surface of the active material layer, and an organic-inorganic composite layer located on the other surface of the active material layer. According to one embodiment, the organic-inorganic composite layer may be formed on the other surface of the current collector.

[0172] The current collector used for the positive electrode active material layer may include an aluminum current collector. The current collector used for the negative electrode active material layer may be at least one of copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal, and combinations thereof.

[0173] The second electrode is used in rechargeable lithium batteries. An electrode for a rechargeable lithium battery (hereinafter also referred to as an "electrode") comprises an active material layer for the rechargeable lithium battery and an organic-inorganic composite layer integrated with the active material layer, wherein the organic-inorganic composite layer comprises fibers containing PSSQ and aromatic polyamide polymers having crosslinkable functional groups.

[0174] The fiber can be a core-shell fiber having a core and a shell surrounding the core. The shell can include PSSQ having crosslinkable functional groups. The core can include non-silicone polymers as described below.

[0175] Aromatic polyamide polymers can improve the electrolyte wettability of organic-inorganic composite layers. In one embodiment, the electrolyte wetting rate of the organic-inorganic composite layer can be 5.0 mm. 2 / s or greater.

[0176] Organic-inorganic composite layers may include aromatic polyamide polymers and PSSQ with crosslinkable functional groups, thereby providing not only improved electrolyte wettability but also improved tensile strength and adhesion. Aromatic polyamide polymers are well known as materials with high mechanical strength. The introduction of such materials can improve the strength of fibrous membranes. However, due to their poor adhesive properties, such materials are difficult to use in composites. This disclosure aims to improve tensile strength and adhesion by using PSSQ with crosslinkable functional groups in aromatic polyamide polymers. When both aromatic polyamide polymers and PSSQ with crosslinkable functional groups are used, the polymer chains of PSSQ insert between the chains of the aromatic polyamide polymer due to the low molecular weight of PSSQ, resulting in entanglement of the aromatic polyamide polymer. Therefore, since PSSQ exerts an elongation effect on the aromatic polyamide polymer, the tensile strength can be improved when the two materials are mixed. Furthermore, PSSQ has highly adhesive epoxy groups as functional groups, resulting in improved adhesion of the fibrous membrane. Furthermore, the main chain of PSSQ has -Si-O-, and this structure exhibits a high affinity for the electrolyte. That is, due to this structure, the electrolyte permeation properties of the fiber membrane are also improved. This effect is thought to improve the tensile strength and adhesion of the organic-inorganic composite layer, but this disclosure is not limited thereto.

[0177] Organic-inorganic composite layers can have a strength of 900 kgf / cm². 2 Or greater (e.g., 1300 kgf / cm²) 2Or even higher, for example, 1300 kgf / cm² 2 Up to 3000 kgf / cm 2 The tensile strength of the electrode is within the above range, which can improve the reliability of the electrode.

[0178] The organic-inorganic composite layer can have a dry adhesion to the active material layer of 0.8 gf / mm or greater (e.g., 1.1 gf / mm or greater, e.g., 1.1 gf / mm to 5 gf / mm). Within the above range, the reliability of the electrode can be improved. Each of tensile strength and dry adhesion can be measured by the methods described below.

[0179] Organic-inorganic composite layer Organic-inorganic composite layers can be used as a separator between the active material layer for rechargeable lithium batteries and the electrode facing the active material layer for rechargeable lithium batteries to prevent short circuits.

[0180] A rechargeable lithium battery including electrodes according to one embodiment may not require a separate separator. Therefore, when manufacturing the battery (such as stacked cells), the electrodes do not require a lamination process combining the electrodes with the separator, thus allowing for a simpler and more economical battery manufacturing process. The electrodes may not have the thermal shrinkage issues caused by conventional separators, thereby improving battery stability and lifespan.

[0181] Organic-inorganic composite layers can be integrated with active material layers used in rechargeable lithium batteries. Here, "integration" can mean that the organic-inorganic composite layer is formed directly on the active material layer without the intervention of any other layers, and that the organic-inorganic composite layer is more firmly bonded to the active material layer.

[0182] The integration of the active material layer and the organic-inorganic composite layer can be confirmed using scanning electron microscopy (SEM) or transmission electron microscopy (TEM). According to one embodiment, it can be clearly seen from the SEM or TEM results that the active material layer and the organic-inorganic composite layer are distinct from each other, but the interface (boundary) between the active material layer and the organic-inorganic composite layer is not clearly defined and appears to be non-uniform.

[0183] Organic-inorganic composite layers can be formed by infiltrating into the active material layer, drying, and cross-linking. This prevents the increase in resistance during lithium-ion migration. The process for forming organic-inorganic composite layers is described in detail below.

[0184] The organic-inorganic composite layer can be a single layer. Here, "single layer" can mean that fibers containing an aromatic polyamide polymer and PSSQ having crosslinkable functional groups are electrospun onto an active material layer to form a single layer in which the organic and inorganic components are not included in separate layers but are included in a single layer.

[0185] Organic-inorganic composite layers can have a nonwoven state, such as a network structure of multiple fibers. The network structure can be advantageous for minimizing resistance during lithium-ion migration. The network structure can refer to a porous layer with pores randomly formed between the fibers. According to one embodiment, the diameter of the pores can be 500 nm or smaller, for example, 10 nm to 300 nm.

[0186] Based on their average diameter, the fibers can be microfibers or nanofibers. The average diameter of the fibers can be in the range of 500 nm or smaller (e.g., 10 nm to 350 nm or 50 nm to 300 nm). Within the above range, organic-inorganic composite layers can be readily formed. Here, the “average diameter” of the nanofibers can be the average calculated from the diameters measured from multiple (approximately 100) nanofibers selected from SEM images.

[0187] The organic-inorganic composite layer includes fibers containing PSSQ with crosslinkable functional groups and aromatic polyamide polymers.

[0188] Even when mixed with aromatic polyamide polymers, PSSQ can be electrospun as is and uniformly dispersed in the fibers. Therefore, PSSQ can achieve the effect of an organic-inorganic composite layer even at any location in the organic-inorganic composite layer, thereby improving reliability.

[0189] Figure 5 and Figure 6 These are the TEM analysis results of the surface and cross-section of the fibers in the organic-inorganic composite layer, respectively. (Refer to...) Figure 5 and Figure 6 As can be seen, the relatively white parts are silicon, indicating that silicon is evenly distributed throughout the fiber.

[0190] The fibers include PSSQ with crosslinkable functional groups and aromatic polyamide polymers. In the absence of PSSQ, the adhesion of the organic-inorganic composite layer may be significantly reduced, and the electrolyte impregnation properties may also be compromised.

[0191] PSSQs possess crosslinkable functional groups. At least some of these crosslinkable functional groups can crosslink with each other during the formation of the organic-inorganic composite layer. This not only increases the degree of connection between PSSQs within the same fiber but also increases the degree of connection between PSSQs in adjacent fibers within the organic-inorganic composite layer, thereby improving the adhesion of the organic-inorganic composite layer.

[0192] In one embodiment, the fiber may include at least a crosslinked product of PSSQ having crosslinkable functional groups.

[0193] The crosslinkable functional group can be a functional group that can be crosslinked by heat and / or light. For example, the crosslinkable functional group can include one or more of epoxy, glycidyl, glycidyloxyalkyl, (meth)acryloyl, (meth)acryloyloxy, and (meth)acryloyloxyalkyl.

[0194] PSSQs with crosslinkable functional groups may also have substituted or unsubstituted aromatic groups. Substituted or unsubstituted aromatic groups can further impart improved adhesion of the organic-inorganic composite layer. Here, "substituted or unsubstituted aromatic groups" can refer to substituted or unsubstituted C6 to C10 monocyclic or heterocyclic aromatic groups. "Substituted or unsubstituted" can mean that one or more hydrogen atoms of the functional group are substituted by C1 to C10 alkyl, halogen, hydroxyl, amino, or C6 to C10 aryl groups. For example, the substituted or unsubstituted aromatic group can be phenyl, and the crosslinkable functional group can be (meth)acryloyl. For example, the substituted or unsubstituted aromatic groups can be bonded to the silicon of the PSSQ.

[0195] PSSQs can be random, ladder-shaped, cage-shaped, or partially cage-shaped. For example, a PSSQ can be ladder-shaped.

[0196] PSSQ with crosslinkable functional groups can have units of chemical formula 2.

[0197] PSSQ with crosslinkable functional groups is ladder-shaped and can be represented by chemical formula 3, but this disclosure is not limited thereto.

[0198] In chemical formula 3, R 3 R 4 R 5 and R 6 Each is independently a hydroxyl group, a C6 to C20 aryl group, a crosslinkable functional group, or a combination thereof, and R 3 R 4 R 5 and R 6 At least one of them can be a crosslinkable functional group.

[0199] The crosslinkable functional group may be represented by chemical formula 1 or chemical formula 4, but this disclosure is not limited thereto: [Chemical Formula 1]

[0200] In chemical formula 1, It is the connecting part of the elements. R 1 It is hydrogen or methyl. R 2 It is a single bond or a C1 to C20 alkylene group.

[0201] [Chemical Formula 4]

[0202] In chemical formula 4, It is the connecting part of the elements, and R 7 and R 8 Each is independently a single bond or an alkylene group having 1 to 20 carbon atoms.

[0203] For example, crosslinkable functional groups can be represented by chemical formula 4. Compared to chemical formula 1, chemical formula 4 can further improve the adhesion of organic-inorganic composite layers.

[0204] Crosslinkable functional groups can be included at any location on the PSSQ. For example, crosslinkable functional groups can be included at the ends of the PSSQ.

[0205] PSSQs with crosslinkable functional groups can have concentrations from 2,000 g / mol to 100,000 g / mol (e.g., 2000 g / mol, 3000 g / mol, 4000 g / mol, 5000 g / mol, 6000 g / mol, 7000 g / mol, 8000 g / mol, 9000 g / mol, 10000 g / mol, 11000 g / mol, 12000 g / mol, 13000 g / mol, 14000 g / mol, 15000 g / mol, 16000 g / mol, 17000 g / mol, 18000 g / mol, 190 g / mol). The weight-average molecular weights (MAMs) are 20,000 g / mol, 25,000 g / mol, 30,000 g / mol, 35,000 g / mol, 40,000 g / mol, 45,000 g / mol, 50,000 g / mol, 55,000 g / mol, 60,000 g / mol, 65,000 g / mol, 70,000 g / mol, 75,000 g / mol, 80,000 g / mol, 85,000 g / mol, 90,000 g / mol, 95,000 g / mol, or 100,000 g / mol, or 15,000 g / mol up to 20,000 g / mol. Within these ranges, the viscosity of PSSQ with crosslinkable functional groups can be easily adjusted. The MLM values ​​can be obtained as a standard conversion value for polystyrene using gel permeation chromatography.

[0206] Aromatic polyamide polymers can be aromatic polyamide polymers.

[0207] Aromatic polyamide polymers may include units of the following chemical formula 5: [Chemical Formula 5]

[0208] In chemical formula 5, It is the connecting part of the elements. R 21 and R 22 Each is independently C1 to C5 alkyl, hydroxyl, or C6 to C10 aryl. a and b are each independent integers from 0 to 3, and R 23 and R 24 It is hydrogen, C1 to C5 alkyl, hydroxyl or C6 to C10 aryl.

[0209] Aromatic polyamide polymers can have values ​​from 3000 g / mol to 500000 g / mol (e.g., 3000 g / mol, 4000 g / mol, 5000 g / mol, 6000 g / mol, 7000 g / mol, 8000 g / mol, 9000 g / mol, 10000 g / mol, 11000 g / mol, 12000 g / mol, 13000 g / mol, 14000 g / mol, 15000 g / mol, 16000 g / mol, 17000 g / mol, 18000 g / mol, 19000 g / mol, 20000 g / mol, 25000 g / mol, 30000 g / mol). The weight-average molecular weights (MMW) of aromatic polyamide polymers can be easily adjusted within the above ranges (1000 g / mol, 35000 g / mol, 40000 g / mol, 45000 g / mol, 50000 g / mol, 55000 g / mol, 60000 g / mol, 65000 g / mol, 70000 g / mol, 75000 g / mol, 80000 g / mol, 85000 g / mol, 90000 g / mol, 95000 g / mol, 100000 g / mol, 150000 g / mol, 200000 g / mol, 300000 g / mol, 400000 g / mol, or 500000 g / mol, or from 5000 g / mol to 100000 g / mol).

[0210] Aromatic polyamide polymers can be prepared by conventional methods known to those skilled in the art, or they can be commercially available products.

[0211] PSSQ and aromatic polyamide polymers with crosslinkable functional groups can be included in the fiber in a weight ratio of 1:1 to 20:1 (e.g., 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, 11:1, 12:1, 13:1, 14:1, 15:1, 16:1, 17:1, 18:1, 19:1, 20:1, 3:1, or 10:1). Within the above range, the effect of an organic-inorganic composite layer can be easily achieved.

[0212] The type of polymer is not limited, as long as it is conducive to electrospinning and does not affect the dispersion and function of aromatic polyamide polymers and PSSQ. For example, the polymer can be a non-silicone polymer that does not contain silicon, and can include PVDF, PAN, PAI, PVP, PAA, PVA, or combinations thereof.

[0213] In one embodiment, the polymer may be a mixture of PVDF and PAN. When combined with PSSQ, this mixture can facilitate electrospinning and impart an effect that increases the dispersibility of PSSQ. PVDF and PAN may be included in a ratio of 10 to 90 parts by weight : 90 to 10 parts by weight (e.g., 20 to 60 parts by weight : 80 to 40 parts by weight) relative to 100 parts by weight of the mixture. Within the above range, PSSQ can exhibit high dispersibility in the mixture.

[0214] In one embodiment, the fiber may comprise 1 to 40 parts by weight (1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, or 40 parts by weight, or for example 5 to 30 parts by weight) of PSSQ relative to 100 parts by weight of the polymer. Within the above range, PSSQ can exhibit high dispersibility.

[0215] In one embodiment, the fiber may comprise 0.1 to 30 parts by weight (e.g., 0.1, 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, or 30 parts by weight, or 0.5 to 10 parts by weight) of an aromatic polyamide polymer relative to 100 parts by weight of the polymer. Within the above range, the aromatic polyamide polymer can exhibit high dispersibility.

[0216] The organic-inorganic composite layer can have a thickness of 1 μm to 30 μm (e.g., 5 μm to 15 μm). Within this range, the organic-inorganic composite layer can be applied in batteries.

[0217] Organic-inorganic composite layers can be prepared by forming a fiber-containing layer on at least one surface of an active material layer and crosslinking the fiber-containing layer.

[0218] First, a layer containing fibers is formed on at least one surface of the active material layer.

[0219] According to one embodiment, the fiber-containing layer can be formed by electrospinning a solution used to form the fiber-containing layer onto a surface of an active material layer. The solution may include an aromatic polyamide polymer and PSSQ having crosslinkable functional groups, and also includes polymers.

[0220] Electrospinning can be performed as follows: a nozzle assembly consisting of needle tips with a gauge size of 23G to 30G and a collection roller are positioned at regular intervals; a solution is injected into the nozzle assembly; an active material layer is placed on the collection roller; and a voltage of 35kV to 90kV is applied to the needle tips. The distance between the nozzle assembly and the active material layer can be 10cm to 20cm. A needle tip size of 25G to 30G is preferred because it allows for the formation of an organic-inorganic composite layer in the desired shape.

[0221] During the electrospinning process, the solution is spun and stretched into a fibrous shape, thereby forming a fiber-containing layer on the active material layer. The solution is suspended as droplets at the tip due to surface tension, and when a voltage is applied, charges accumulate on the surface of the solution, generating repulsive forces. When a critical voltage is reached where the repulsive force between the charges becomes higher than the surface tension of the solution, a Taylor cone is generated, and a polymer solution jet is ejected from the tip of the cone and highly stretched to form fibers, which collect on the active material layer to form a fiber-containing layer.

[0222] According to one embodiment, the electrospinning process can be carried out at temperatures ranging from 15°C to 40°C and relative humidity ranging from 40% to 60%. When the electrospinning process is carried out under the above-mentioned temperature and relative humidity conditions, it has the advantage of maintaining a constant fiber diameter during spinning.

[0223] The solution may also include an initiator for promoting crosslinking of PSSQ having crosslinkable functional groups. The initiator may include one or more of a thermal initiator and a photoinitiator. The thermal initiator and photoinitiator may be any conventional type known to those skilled in the art.

[0224] The solution may also include a solvent, and the solvent may include, for example, dimethylacetamide, dimethyl sulfoxide, dimethylformamide, tetrahydrofuran, carbon tetrachloride, methylpyrrolidone, water, ethanol, acetone, or combinations thereof. The solvent may be included as a residue in the organic-inorganic composite layer.

[0225] In the solution, the content of PSSQ with crosslinkable functional groups or a mixture of PSSQ with crosslinkable functional groups and a polymer can be from 5 wt% to 40 wt% relative to 100 wt% of the total solution. Within the above range, the organic-inorganic composite layer can be formed to a suitable thickness.

[0226] In one embodiment, a drying process can be performed at 30°C to 80°C after the electrospinning process.

[0227] The fiber-containing layer can be hot-pressed after cross-linking. Pressing can increase the density between fibers in the fiber-containing layer and reduce the thickness of the organic-inorganic composite layer.

[0228] According to one embodiment, hot pressing can be performed at a temperature of 50°C or higher (e.g., 50°C to 150°C) by a roll pressing process.

[0229] Active material layer for rechargeable lithium batteries The active material layer used in a rechargeable lithium battery can be either a positive electrode active material layer or a negative electrode active material layer. For example, the active material layer used in a rechargeable lithium battery can be a positive electrode active material layer.

[0230] Since the active material layer used in the rechargeable lithium battery is substantially the same as the active material layer described in "First Electrode for Rechargeable Lithium Battery", its detailed description is omitted.

[0231] The third electrode is used in rechargeable lithium batteries. The electrode for a rechargeable lithium battery (hereinafter also referred to as the “electrode”) includes an active material layer for the rechargeable lithium battery and an organic-inorganic composite layer integrated with the active material layer, wherein the organic-inorganic composite layer includes fibers comprising PVDF-type polymers, PAN-type polymers and PSSQ.

[0232] Organic-inorganic composite layer Organic-inorganic composite layers can be used as a separator between the active material layer for rechargeable lithium batteries and the electrode facing the active material layer for rechargeable lithium batteries to prevent short circuits.

[0233] Rechargeable lithium batteries that include this electrode may not require a separate separator. Therefore, when manufacturing batteries (such as stacked cells), the electrode does not need to undergo a lamination process combining it with a separator, allowing for simpler and more economical battery manufacturing. The electrode may also avoid the thermal shrinkage issues caused by conventional separators, thus improving battery stability and lifespan.

[0234] The organic-inorganic composite layer is integrated with the active material layer used in rechargeable batteries. Here, "integration" can mean that the organic-inorganic composite layer is formed directly on the active material layer without the intervention of any other layer, and the organic-inorganic composite layer is more firmly bonded to the active material layer.

[0235] The integration of the active material layer and the organic-inorganic composite layer can be confirmed using scanning electron microscopy (SEM) or transmission electron microscopy (TEM). According to one embodiment, it can be clearly seen from the SEM or TEM results that the active material layer and the organic-inorganic composite layer are distinct from each other, but the interface (boundary) between the active material layer and the organic-inorganic composite layer is not clearly defined and appears to be non-uniform.

[0236] Organic-inorganic composite layers can be formed by permeation into an active material layer and drying. This prevents an increase in resistance during lithium-ion migration. Besides drying, the formation of organic-inorganic composite layers can also involve cross-linking and / or hot pressing. The process for forming organic-inorganic composite layers is described in detail below.

[0237] The organic-inorganic composite layer can be a single layer. Here, "single layer" can mean that the fiber is electrospun onto the active material layer to form a single layer in which the organic and inorganic components are not included in separate layers but are included in a single layer.

[0238] Organic-inorganic composite layers can have a nonwoven state, such as a network structure of multiple fibers. The network structure can be advantageous for minimizing resistance during lithium-ion migration. The network structure can refer to a porous layer with pores randomly formed between the fibers. According to one embodiment, the diameter of the pores can be in the range of 90 nm or smaller (e.g., 10 nm to 90 nm).

[0239] Based on the average diameter, the fiber can be a micron-fiber or a nanofiber. In one embodiment, the average diameter of the fiber can be 300 nm or less, for example, 10 nm to 200 nm or 10 nm to 100 nm. Within the above range, organic-inorganic composite layers can be readily formed. Here, the “average diameter” of the nanofiber can be the average calculated from the diameters measured from multiple (approximately 100) nanofibers selected from SEM images.

[0240] The organic-inorganic composite layer includes fibers containing PVDF-type polymers, PAN-type polymers, and PSSQ.

[0241] When mixed with PVDF and PAN polymers, PSSQ can be electrospun as is and dispersed uniformly. Therefore, PSSQ can achieve the effect of an organic-inorganic composite layer at any location within the layer, thereby improving electrode reliability. Specifically, when PSSQ is mixed with PVDF and PAN polymers and electrospun to form fibers, the PSSQ is uniformly distributed within the fibers, significantly improving the tensile strength of the organic-inorganic composite layer.

[0242] Figure 7 The results are from a transverse analysis of the fibers included in the organic-inorganic composite layer. Figure 7 The results obtained by measurement using the HAADF-STEM-EDS method are shown.

[0243] Reference Figure 7 Blue represents carbon, and red represents silicon. It can be seen that silicon is evenly distributed throughout the fiber. Figure 7 In the image, white represents silicon, and it can be seen that silicon is evenly distributed throughout the fiber.

[0244] Figure 8 The results of high-angle annular dark-field scanning transmission electron microscopy (HAADF-STEM) analysis of silicon and carbon in fiber profiles are shown. Figure 8 It is Figure 7 The distribution of silicon and carbon in the scanning direction (black line in the green box on the image) after a line scan (the direction orthogonal to the fiber axis) in the right-hand image is shown as an intensity graph.

[0245] Reference Figure 8 It can be seen that silicon is uniformly distributed in Figure 7 The cross-section of the fiber is shown. Figure 8 In the diagram, solid lines represent carbon, dotted lines represent silicon, and dashed lines represent high-angle annular dark field (HAADF).

[0246] Because the fibers include PVDF-type polymers, PAN-type polymers, and PSSQ, they can be formed into island-island fibers. Specifically, island-island fibers include a marine region and multiple island regions included within that marine region.

[0247] The island region can be composed of PVDF-based polymers. The island region can have a core-shell structure, with a core composed of PAN-based polymers and a shell surrounding the core composed of PSSQ. Compared to fibers comprising PVDF-based polymers, PAN-based polymers, and PSSQ as independent components in the fiber, island fibers can significantly improve the tensile strength of the organic-inorganic composite layer by enhancing the interaction between the three components. The specific mechanism by which the combination of PVDF-based polymers, PAN-based polymers, and PSSQ forms island fibers during electrospinning has not been elucidated, but is believed to be due to the specific combination of the three components. However, this disclosure is not limited thereto.

[0248] In island-island fibers, island regions can be randomly distributed within the sea area. For example, in the cross-section of an island-island fiber, the area ratio of island regions can be 30% to 70%, such as 30% to 50% or 40% to 60%. Within these ranges, the effect of an organic-inorganic composite layer can be easily achieved. The area ratio of island regions can refer to the ratio of the total area of ​​island regions to the cross-sectional area of ​​the fiber.

[0249] Sea island fibers can be identified using scanning transmission electron microscopy-energy dispersive spectroscopy (STEM-EDS).

[0250] Figure 9 The results of HAADF-STEM analysis of the fibers are shown. (Refer to...) Figure 9 It can identify the PAN core and the silicon surrounding the core.

[0251] Figure 10 The TEM-EDS results of the fibers are shown. (Reference) Figure 10 It can be confirmed that the fibers included in the organic-inorganic composite layer are island fibers.

[0252] Figure 11 This is a schematic diagram of island fiber. (Refer to...) Figure 11 The island fiber consists of a marine region 4 and an island region with a core-shell structure. The marine region 4 is composed of PVDF-type polymers. The island region may include a core 6 composed of PAN-type polymers and a shell 5 surrounding the core and composed of PSSQ.

[0253] In one embodiment, the organic-inorganic composite layer can have a strength of 600 kgf / cm². 2 Or greater (e.g., 1000 kgf / cm²) 2 Or even higher, for example, 1000 to 2000 kgf / cm³ 2 The tensile strength of the electrode can be improved within the above range.

[0254] Fibers can improve the electrolyte wettability of organic-inorganic composite layers by incorporating PVDF-based polymers, PAN-based polymers, and PSSQ. The improved electrolyte wettability can be further enhanced by adding the inorganic component PSSQ to the organic components, PVDF-based polymers, and PAN-based polymers. It can be considered that since the fibers are prepared by electrospinning, electrolyte wettability can be improved, but PSSQ, due to its Si-O bonds, can further improve the electrolyte wettability of the organic-inorganic composite layer. However, this disclosure is not limited thereto.

[0255] In one embodiment, the organic-inorganic composite layer can have a thickness of 5.0 mm. 2 / s or greater, 7.5mm 2 / s or greater, such as 7.5mm 2 / s to 10mm 2 The electrolyte wetting rate is [value] / s. Within the above range, the impregnation properties of the organic-inorganic composite layer in the battery can be improved.

[0256] The fibers can be imparted with a shutdown effect by including PVDF-based polymers, PAN-based polymers, and PSSQ. The organic-inorganic composite layer includes pores as described above. Therefore, when the battery is at a high temperature, the PVDF-based polymer can melt and block the pores, thereby providing a shutdown effect. As described above, the fibers including PVDF-based polymers, PAN-based polymers, and PSSQ are island fibers, wherein the sea-like regions are composed of PVDF-based polymers. Therefore, at high temperatures, the PVDF-based polymer melts rapidly, thereby further increasing the shutdown effect.

[0257] In this embodiment, the electrode can be applied to a battery having an electrolyte containing a carbonate solvent. When placed in a carbonate electrolyte at high temperatures, the PVDF polymer can easily provide a shut-off effect through swelling and melting.

[0258] Because the fibers comprise PVDF-based polymers, PAN-based polymers, and PSSQ, the organic-inorganic composite layer can provide improved adhesion to the active material layer. As described above, the fibers comprising PVDF-based polymers, PAN-based polymers, and PSSQ are island fibers, wherein the sea-like region is composed of PVDF-based polymers. Therefore, since the PVDF-based polymers are included in the sea-like region of the fiber, improved adhesion can be provided. Specifically, the fibers can increase adhesion to the positive electrode active material layer, which includes a PVDF-based binder as a binder.

[0259] In one embodiment, the PSSQ may have crosslinkable functional groups. These crosslinkable functional groups can crosslink with each other during the process of preparing the organic-inorganic composite layer to increase the degree of bonding between fibers and with the electrode plate, thereby significantly improving adhesion.

[0260] In one embodiment, the organic-inorganic composite layer may have a dry adhesion to the active material layer for a rechargeable battery of 0.7 gf / mm or greater, 1.1 gf / mm or greater, or 1.2 gf / mm or greater, for example, 1.2 gf / mm to 5 gf / mm. In one embodiment, the organic-inorganic composite layer may have a wet adhesion to the active material layer for a rechargeable battery of 0.6 gf / mm or greater, or 1.4 gf / mm or greater, for example, 1.4 gf / mm to 5 gf / mm.

[0261] When the fibers include PVDF-based polymers, PAN-based polymers, and PSSQ, the heat resistance of the organic-inorganic composite layer can be improved. PSSQ includes the inorganic component Si. Therefore, the fibers of this disclosure can further improve heat resistance compared to fibers containing only PVDF-based polymers and PAN-based polymers as organic components.

[0262] In one embodiment, the PSSQ may have crosslinkable functional groups. These crosslinkable functional groups can crosslink with each other during the process of preparing the organic-inorganic composite layer to fix the fiber structure, thereby significantly improving the heat resistance of the organic-inorganic composite layer.

[0263] In one embodiment, the organic-inorganic composite layer may have a thermal shrinkage rate of 5% or less (e.g., 0 to 3%) in the electrolyte in each of the longitudinal (MD, mechanical direction) and transverse (TD) directions.

[0264] Here, the MD shrinkage rate can be 5% or less, for example, 0 to 3%, and the TD shrinkage rate can be 5% or less, for example, 0 to 3%.

[0265] The various components included in the fiber are described in detail below.

[0266] PVDF polymers PVDF polymers can be homopolymers or copolymers of monomer mixtures including vinylidene fluoride.

[0267] In one embodiment, the polymer may be PVDF. In another embodiment, the polymer may be a copolymer comprising a mixture of monomers including vinylidene fluoride and comonomers, such as PVDF-hexafluoropropylene (PVDF-HPF).

[0268] PVDF polymers can have concentrations ranging from 100,000 g / mol to 500,000 g / mol (e.g., 100,000 g / mol, 110,000 g / mol, 120,000 g / mol, 130,000 g / mol, 140,000 g / mol, 150,000 g / mol, 160,000 g / mol, 170,000 g / mol, 180,000 g / mol, 190,000 g / mol, 200,000 g / mol, 210,000 g / mol, 220,000 g / mol, 230,000 g / mol, 240,000 g / mol, 250,000 g / mol, 260,000 g / mol, 270,000 g / mol, 280,000 g / mol, 290,000 g / mol, 30...). The weight-average molecular weights of 0000 g / mol, 310000 g / mol, 320000 g / mol, 330000 g / mol, 340000 g / mol, 350000 g / mol, 360000 g / mol, 370000 g / mol, 380000 g / mol, 390000 g / mol, 400000 g / mol, 410000 g / mol, 420000 g / mol, 430000 g / mol, 440000 g / mol, 450000 g / mol, 460000 g / mol, 470000 g / mol, 480000 g / mol, 490000 g / mol, or 500000 g / mol, or 150,000 g / mol to 500,000 g / mol. Within the above range, the viscosity of the electrospinning solution can be easily adjusted.

[0269] PAN polymers PAN polymers can be homopolymers or copolymers of monomer mixtures including acrylonitrile.

[0270] In one embodiment, the polymer may be PAN. PAN-based polymers may have concentrations from 100,000 g / mol to 300,000 g / mol (e.g., 100,000 g / mol, 110,000 g / mol, 120,000 g / mol, 130,000 g / mol, 140,000 g / mol, 150,000 g / mol, 160,000 g / mol, 170,000 g / mol, 180,000 g / mol, 190,000 g / mol, 200...). The weight-average molecular weights are 2000 g / mol, 210000 g / mol, 220000 g / mol, 230000 g / mol, 240000 g / mol, 250000 g / mol, 260000 g / mol, 270000 g / mol, 280000 g / mol, 290000 g / mol, or 300000 g / mol, or 100,000 g / mol to 200,000 g / mol. Within these ranges, the viscosity of the electrospinning solution can be easily adjusted.

[0271] PSSQ PSSQ may include alkyl groups (R) bonded to the main chain of silicon.

[0272] The alkyl group of PSSQ can be a substituted or unsubstituted aromatic group. Substituted or unsubstituted aromatic groups can further provide dimensional stability by maintaining the spacing between the molecular chains of PSSQ, thereby preventing volume changes in the organic-inorganic composite layer even during crosslinking. Here, "substituted or unsubstituted aromatic group" can refer to a substituted or unsubstituted C6 to C10 monocyclic or heterocyclic aromatic group. "Substituted or unsubstituted" can mean that one or more hydrogen atoms of the functional group are substituted by a C1 to C10 alkyl, halogen, hydroxyl, amino, or C6 to C10 aryl group. For example, a substituted or unsubstituted aromatic group can be phenyl. For example, a substituted or unsubstituted aromatic group can be bonded to the silicon of PSSQ.

[0273] PSSQs can be random, ladder-shaped, cage-shaped, or partially cage-shaped. For example, a PSSQ can be ladder-shaped.

[0274] PSSQ may include silicon-based compounds having units with the following chemical formula 6: [Chemical Formula 6] [R'SiO 3 / 2 ] n In chemical formula 6, R' is hydrogen, hydroxyl, C1 to C20 alkyl, C2 to C20 alkenyl, C2 to C20 alkynyl, C3 to C20 cycloalkyl, C6 to C20 aryl, C7 to C20 aralkyl, crosslinkable functional group or combination thereof, and n is the number of moles of the unit.

[0275] n can be from 1 to 1,000,000.

[0276] In one embodiment, the PSSQ is ladder-shaped and represented by the following chemical formula 7, but this disclosure is not limited thereto: [Chemical Formula 7]

[0277] In chemical formula 7, R 1 R 2 R 3 and R 4 Each is independently hydrogen, hydroxyl, C1 to C20 alkyl, C2 to C20 alkenyl, C2 to C20 alkynyl, C3 to C20 cycloalkyl, C6 to C20 aryl, C7 to C20 aralkyl, crosslinkable functional group or combination thereof, and n is the number of moles of the unit.

[0278] n can be from 1 to 1,000,000.

[0279] In one embodiment, the PSSQ may have crosslinkable functional groups. At least some of these crosslinkable functional groups can be crosslinked during the process of forming the organic-inorganic composite layer. This can further improve the strength, adhesion, and heat resistance of the organic-inorganic composite layer by increasing the degree of bonding between PSSQs within the same fiber.

[0280] In one embodiment, the fiber may include at least a crosslinked product of PSSQ having crosslinkable functional groups.

[0281] The crosslinkable functional group can be a functional group capable of being crosslinked by heat and / or light. For example, the crosslinkable functional group can include one or more of epoxy group, glycidyl group, glycidyloxy group, and glycidyloxyalkyl group.

[0282] The crosslinkable functional group can be represented by chemical formula 4, but this disclosure is not limited thereto.

[0283] Crosslinkable functional groups can be included at any location on the PSSQ. For example, crosslinkable functional groups can be included at the ends of the PSSQ.

[0284] In one embodiment, PSSQ is ladder-shaped and may be represented by the following chemical formula 8, but this disclosure is not limited thereto.

[0285] [Chemical Formula 8]

[0286] In chemical formula 8, R 7 R 8 R 9 and R 10 Each of these components is independently hydrogen, hydroxyl, C1 to C20 alkyl, C2 to C20 alkenyl, C2 to C20 alkynyl, C3 to C20 cycloalkyl, C6 to C20 aryl, C7 to C20 aralkyl, crosslinkable functional group, or a combination thereof. R 7 R 8 R 9 and R 10 At least one of them is a crosslinkable functional group, and n is the number of moles in the unit.

[0287] n can be from 1 to 1,000,000.

[0288] In Formula 8, the crosslinkable functional groups can be the same as those defined in Formula 4.

[0289] In one embodiment, the crosslinkable functional groups in Formula 8 can be from 20 mol% to 50 mol% of the total functional groups of silicon, for example, 20 mol%, 21 mol%, 22 mol%, 23 mol%, 24 mol%, 25 mol%, 26 mol%, 27 mol%, 28 mol%, 29 mol%, 30 mol%, 31 mol%, 32 mol%, 33 mol%, 34 mol%, 35 mol%, 36 mol%, 37 mol%, 38 mol%, 39 mol%, 40 mol%, 41 mol%, 42 mol%, 43 mol%, 44 mol%, 45 mol%, 46 mol%, 47 mol%, 48 mol%, 49 mol%, or 50 mol%, or 30 mol% to 50 mol%. Within the above range, the organic-inorganic composite layer can have the effect of improving adhesion and heat resistance.

[0290] In chemical formula 8, R 7 R 8 R 9 and R 10 Each is independently a hydroxyl group, a C6 to C20 aryl group, a crosslinkable functional group, or a combination thereof, and R 7 R 8 R 9 and R 10 At least one of them can be a crosslinkable functional group.

[0291] PSSQ can have a weight-average molecular weight of 5,000 g / mol to 30,000 g / mol (e.g., 5,000 g / mol, 6,000 g / mol, 7,000 g / mol, 8,000 g / mol, 9,000 g / mol, 10,000 g / mol, 11,000 g / mol, 12,000 g / mol, 13,000 g / mol, 14,000 g / mol, 15,000 g / mol, 16,000 g / mol, 17,000 g / mol, 18,000 g / mol, 19,000 g / mol, 20,000 g / mol, 25,000 or 30,000 g / mol, or 10,000 g / mol to 20,000 g / mol). Within this range, the viscosity of PSSQ can be easily adjusted.

[0292] Relative to the total amount of 100 parts by weight of PVDF and PAN polymers, the PVDF and PAN polymers can be included in a ratio of 50 to 90 parts by weight: 50 to 10 parts by weight (e.g., 50 parts by weight: 50 parts by weight, 55 parts by weight: 45 parts by weight, 60 parts by weight: 40 parts by weight, 65 parts by weight: 35 parts by weight, 70 parts by weight: 30 parts by weight, 75 parts by weight: 25 parts by weight, 80 parts by weight: 20 parts by weight, 85 parts by weight: 15 parts by weight, 90 parts by weight: 10 parts by weight, 60 to 90 parts by weight: 40 to 10 parts by weight). Within the above range, the effect of an organic-inorganic composite layer can be easily achieved.

[0293] The content of PSSQ can be from 5 parts by weight to 50 parts by weight relative to 100 parts by weight of the total amount of PVDF and PAN polymers, for example, 5 parts by weight, 6 parts by weight, 7 parts by weight, 8 parts by weight, 9 parts by weight, 10 parts by weight, 11 parts by weight, 12 parts by weight, 13 parts by weight, 14 parts by weight, 15 parts by weight, 16 parts by weight, 17 parts by weight, 18 parts by weight, 19 parts by weight, 20 parts by weight, 21 parts by weight, 22 parts by weight, 23 parts by weight, and 24 parts by weight. 25 parts by weight, 26 parts by weight, 27 parts by weight, 28 parts by weight, 29 parts by weight, 30 parts by weight, 31 parts by weight, 32 parts by weight, 33 parts by weight, 34 parts by weight, 35 parts by weight, 36 parts by weight, 37 parts by weight, 38 parts by weight, 39 parts by weight, 40 parts by weight, 41 parts by weight, 42 parts by weight, 43 parts by weight, 44 parts by weight, 45 parts by weight, 46 parts by weight, 47 parts by weight, 48 parts by weight, 49 parts by weight, or 50 parts by weight, or 10 parts by weight to 30 parts by weight. Within the above range, the effect of an organic-inorganic composite layer can be easily achieved.

[0294] In one embodiment, the total amount of PVDF polymers, PAN polymers and PSSQ in the fiber can be 95 wt% or more, for example, 95 wt% to 100 wt%.

[0295] The thickness of the organic-inorganic composite layer can be from 1 μm to 20 μm, for example, from 1 μm to 10 μm. Within this range, the organic-inorganic composite layer can be used in batteries.

[0296] An organic-inorganic composite layer can be formed by forming a fiber-containing layer on at least one surface of an active material layer and drying the fiber-containing layer.

[0297] First, a layer containing fibers is formed on at least one surface of the active material layer.

[0298] According to one embodiment, a fiber-containing layer can be prepared by electrospinning a solution for forming a fiber-containing layer on one surface of an active material layer. The solution may include PVDF-based polymers, PAN-based polymers, and PSSQ.

[0299] Electrospinning can be performed as follows: a nozzle assembly consisting of needle tips with a gauge size of 23G to 30G and a collection roller are positioned at regular intervals; a solution is injected into the nozzle assembly; an active material layer is placed on the collection roller; and a voltage of 35kV to 90kV is applied to the needle tips. The distance between the nozzle assembly and the active material layer can be 10cm to 20cm. A needle tip size of 25G to 30G is preferred because it allows for the formation of an organic-inorganic composite layer in the desired shape.

[0300] During the electrospinning process, the solution is spun and stretched into a fibrous shape, thereby forming a fiber-containing layer on the active material layer. The solution is suspended as droplets at the tip due to surface tension, and when a voltage is applied, charges accumulate on the surface of the solution, generating repulsive forces. When a critical voltage is reached where the repulsive force between the charges becomes higher than the surface tension of the solution, a Taylor cone is generated, and a polymer solution jet is ejected from the tip of the cone and highly stretched to form fibers, which collect on the active material layer to form a layer containing nanofibers.

[0301] According to one embodiment, the electrospinning process can be carried out at 20°C to 30°C and 40% to 60% relative humidity. When the electrospinning process is carried out under the above temperature and relative humidity conditions, it has the advantage of maintaining a constant fiber diameter during spinning.

[0302] The electrospinning speed can be adjusted to form an organic-inorganic composite layer of appropriate thickness, and the electrospinning speed can be, for example, from 1 m / min to 3 m / min. In addition, the flow rate of the solution discharged from the tip can be adjusted to a range of 20 μL / min to 1000 μL / min (e.g., 20 μL / min to 200 μL / min).

[0303] The solution may also include an initiator for promoting crosslinking of PSSQ having crosslinkable functional groups. The initiator may include one or more of thermal initiators and photoinitiators. Thermal and photoinitiators may be of conventional types known to those skilled in the art.

[0304] The solution may also include a solvent, and the solvent may include, for example, dimethylacetamide, dimethyl sulfoxide, dimethylformamide, tetrahydrofuran, carbon tetrachloride, methylpyrrolidone, water, ethanol, acetone, or combinations thereof. The solvent may be included as a trace residue in the organic-inorganic composite layer.

[0305] The content of the mixture of PVDF-based polymers, PAN-based polymers, and PSSQ in the solution can be from 5 wt% to 20 wt% relative to the total 100 wt% of the solution. Within this range, the organic-inorganic composite layer can be formed to an appropriate thickness.

[0306] After the electrospinning process, a solvent removal process can be carried out at 80°C to 120°C.

[0307] Subsequently, after the electrospinning process, an organic-inorganic composite layer can be formed by drying the fiber-containing layer. The drying process can be adjusted appropriately according to the boiling point of the solvent.

[0308] Organic-inorganic composite layers can be formed by cross-linking the fiber-containing layers.

[0309] Crosslinking can be performed by heat treatment of the fiber-containing layer under predetermined conditions. For example, the heat treatment can be performed in a vacuum at 50°C to 200°C (e.g., 50°C to 150°C) for 5 to 180 minutes.

[0310] The fiber-containing layer can be hot-pressed before or after drying and / or crosslinking. Hot pressing can increase the density between fibers in the fiber-containing layer and reduce the thickness of the organic-inorganic composite layer. According to one embodiment, hot pressing can be performed by pressing the fiber-containing layer at a pressure of 0.1 MPa to 1 MPa at 70°C or higher (e.g., 70°C to 150°C).

[0311] Active material layer for rechargeable lithium batteries The active material layer used in a rechargeable lithium battery can be either a positive electrode active material layer or a negative electrode active material layer. For example, the active material layer used in a rechargeable lithium battery can be a negative electrode active material layer.

[0312] Since the active material layer used in the rechargeable lithium battery is substantially the same as the active material layer described in "First Electrode for Rechargeable Lithium Battery", its detailed description is omitted.

[0313] The fourth type of electrode is used in rechargeable lithium batteries. An electrode for a rechargeable lithium battery (hereinafter also referred to as an "electrode") comprises an active material layer for the rechargeable lithium battery and a multilayer organic-inorganic composite layer integrated with the active material layer. The multilayer organic-inorganic composite layer comprises a first organic-inorganic composite layer and a second organic-inorganic composite layer, wherein the difference between the PSSQ content in the first organic-inorganic composite layer and the PSSQ content in the second organic-inorganic composite layer is 10 wt% or greater.

[0314] Multilayer organic-inorganic composite layer Multilayer organic-inorganic composite layers can be used as a separator between the active material layer for rechargeable lithium batteries and the electrode facing the active material layer for rechargeable lithium batteries to prevent short circuits.

[0315] Rechargeable lithium batteries that include this electrode may not require a separate separator. Therefore, when manufacturing batteries (such as stacked cells), the electrode does not need to undergo a lamination process combining it with a separator, allowing for simpler and more economical battery manufacturing. Furthermore, the electrode does not suffer from the thermal shrinkage issues caused by conventional separators, thus improving battery stability and lifespan.

[0316] The organic-inorganic composite layer can be integrated with the active material layer used in rechargeable batteries. Here, "integration" can mean that the organic-inorganic composite layer is formed directly on the active material layer without the intervention of any other layer, that is, the organic-inorganic composite layer is more firmly bonded to the active material layer.

[0317] The integration of the active material layer and the organic-inorganic composite layer can be confirmed using scanning electron microscopy (SEM) or transmission electron microscopy (TEM). According to one embodiment, the SEM or TEM results clearly show that the active material layer can be distinguished from the organic-inorganic composite layer; however, the interface (boundary) between the active material layer and the organic-inorganic composite layer is not clearly defined and appears to be non-uniform.

[0318] Multilayer organic-inorganic composite layers can have a structure in which multiple organic-inorganic composite layers are stacked in the thickness direction of the composite layer. Here, each organic-inorganic composite layer can be a single layer. Here, "single layer" can mean that the organic component and the inorganic component are not included in separate layers, but are formed in one layer.

[0319] Organic-inorganic composite layers can be integrated with adjacent organic-inorganic composite layers. Here, "integration" can be the same as the concept mentioned above.

[0320] A multilayer organic-inorganic composite layer may include two or more organic-inorganic composite layers, for example, two to eight organic-inorganic composite layers. For example, a multilayer organic-inorganic composite layer may include four to eight organic-inorganic composite layers. As another example, a multilayer organic-inorganic composite layer may include four organic-inorganic composite layers. When a multilayer organic-inorganic composite layer includes four organic-inorganic composite layers, the effects provided by each organic-inorganic composite layer can be fully realized even when the composite layer is hot-pressed. Each organic-inorganic composite layer in a multilayer organic-inorganic composite layer can be distinguished from each other by energy-dispersive X-ray spectroscopy (EDAX), but this disclosure is not limited thereto.

[0321] In the organic-inorganic composite layer of the multilayer organic-inorganic composite layer, the content of PSSQ can be the same or different.

[0322] The multilayer organic-inorganic composite layer includes a first organic-inorganic composite layer and a second organic-inorganic composite layer, wherein the first organic-inorganic composite layer and the second organic-inorganic composite layer have different contents of PSSQ. The difference in PSSQ content between the first organic-inorganic composite layer and the second organic-inorganic composite layer is 10 wt% or greater.

[0323] The lower the air permeability of the multilayer organic-inorganic composite layer, the lower its resistance to foreign matter compression. Resistance to foreign matter compression represents the load that causes a short circuit between the positive and negative electrodes when a foreign object is forcibly introduced onto the multilayer organic-inorganic composite layer and then compressed. Although this is not always the case, there may be a trade-off between improved air permeability and improved resistance to foreign matter compression. Conversely, when the difference in PSSQ content in the multilayer organic-inorganic composite layer is 10 wt% or greater, the air permeability of the multilayer organic-inorganic composite layer can also be improved, and its stability against foreign matter can also be improved.

[0324] When the permeability of the multilayer organic-inorganic composite layer is reduced, lithium-ion migration can be decreased, thereby reducing the battery resistance. When the stability of the multilayer organic-inorganic composite layer against foreign matter is improved, the cell defect rate caused by foreign matter can be reduced during the manufacture of rechargeable lithium batteries (such as stacked cells), or the electrode volume expansion during charging and discharging can be reduced.

[0325] PSSQ, as an inorganic component, can improve the toughness of organic-inorganic composite layers. However, when the PSSQ content in each organic-inorganic composite layer of a multilayer organic-inorganic composite layer is equal, each layer may have similar toughness and may exhibit fracture (failure) behavior, thereby reducing the resistance to foreign matter. In this disclosure, by adjusting the difference in PSSQ content between the first and second organic-inorganic composite layers to 10 wt% or greater, failure is delayed by exhibiting different failure behaviors caused by foreign matter in each layer, and the frictional delamination between layers increases the resistance to permeation via foreign matter. Therefore, the resistance to foreign matter can be improved, and air permeability is also enhanced.

[0326] The difference in PSSQ content between the first organic-inorganic composite layer and the second organic-inorganic composite layer can be from 10 wt% to 50 wt%, for example, 10 wt%, 11 wt%, 12 wt%, 13 wt%, 14 wt%, 15 wt%, 16 wt%, 17 wt%, 18 wt%, 19 wt%, 20 wt%, 21 wt%, 22 wt%, 23 wt%, 24 wt%, 25 wt%, 26 wt%, 27 wt%, 28 wt%, 29 wt%, 30 wt%, 31 wt%, 32 wt%, 33 wt%, 34 wt%, 35 wt%, 36 wt%, 37 wt%, 38 wt%, 39 wt%, 40 wt%, 41 wt%, 42 wt%, 43 wt%, 44 wt%, 45 wt%, 46 wt%, 47 wt%, 48 wt%, 49 wt%, or 50 wt%, or 10 wt% to 30 wt%, or 10 wt% to 20 wt%. Within the aforementioned range, physical properties other than breathability and resistance to foreign objects remain unaffected, and breathability and resistance can be easily improved.

[0327] The second organic-inorganic composite layer may have a higher PSSQ content than the first organic-inorganic composite layer. In one embodiment, the second organic-inorganic composite layer may contain 10 wt% or more (e.g., 10 wt%, 11 wt%, 12 wt%, 13 wt%, 14 wt%, 15 wt%, 16 wt%, 17 wt%, 18 wt%, 19 wt%, 20 wt%, 21 wt%, 22 wt%, 23 wt%, 24 wt%, 25 wt%, 26 wt%, 27 wt%, 28 wt%, 29 wt%, 30 wt%, 31 wt%, 32 wt%, 33 wt%, 34 wt%, 35 wt%, 36 wt%, 37 wt%, 38 wt%, 39 wt%, 40 wt%, 41 wt%, 42 wt%, 43 wt%, 44 wt%, 45 wt%, 46 wt%, 47 wt%, 48 wt%, 49 wt%, or 50 wt%, 10 wt% to 50 wt%, e.g., 15 wt% to 30 wt% or 20 wt% to 30 wt%) of PSSQ. In one embodiment, the PSSQ content in the first organic-inorganic composite layer can be 0 wt% or greater, for example, 0 wt%, 1 wt%, 2 wt%, 3 wt%, 4 wt%, 5 wt%, 6 wt%, 7 wt%, 8 wt%, 9 wt%, 10 wt%, 11 wt%, 12 wt%, 13 wt%, 14 wt%, 15 wt%, 16 wt%, 17 wt%, 18 wt%, 19 wt%, 20 wt%, 21 wt%, 22 wt%, 23 wt%, 24 wt%, 25 wt%, 26 wt%, 27 wt%, 28 wt%, 29 wt%, 30 wt%, 31 wt%, 32 wt%, 33 wt%, 34 wt%, 35 wt%, 36 wt%, 37 wt%, 38 wt%, 39 wt%, or 40 wt%, 1 wt% to 40 wt%, for example, 5 wt% to 20 wt%, or 10 wt% to 20 wt%.

[0328] The second organic-inorganic composite layer can be integrated with the active material layer for rechargeable lithium batteries, and the active material layer for rechargeable lithium batteries can be the negative electrode active material layer.

[0329] The PSSQ content in the multi-layer organic-inorganic composite layer can be from 10wt% to 50wt%, for example, 10wt%, 11wt%, 12wt%, 13wt%, 14wt%, 15wt%, 16wt%, 17wt%, 18wt%, 19wt%, 20wt%, 21wt%, 22wt%, 23wt%, 24wt%, 25wt%, 26wt%, 27wt%, 28wt%, 29wt%, 30wt%, 31wt%, 32wt%, 33wt%, 34wt%, 35wt%, 36wt%, 37wt%, 38wt%, 39wt%, 40wt%, 41wt%, 42wt%, 43wt%, 44wt%, 45wt%, 46wt%, 47wt%, 48wt%, 49wt% or 50wt%, 10wt% to 30wt%, 15wt% to 30wt%, for example, 20wt% to 30wt%. Within the above range, the effects of improved air permeability and resistance to the compressive force of foreign objects can be achieved.

[0330] The thickness of the multilayer organic-inorganic composite layer can be from 0.5 μm to 20 μm, for example, from 1 μm to 15 μm, or for example, from 5 μm to 15 μm. Within the above range, the multilayer organic-inorganic composite layer can be used in batteries.

[0331] The stacking configuration of the first and second organic-inorganic composite layers is not particularly limited. However, the first and second organic-inorganic composite layers can be stacked alternately. This can provide a complementary effect between the two layers with different PSSQ contents, thereby further improving the electrode performance. Specifically, the multilayer organic-inorganic composite layers are hot-pressed during the battery manufacturing process, and hot pressing can also provide a complementary effect between the two layers.

[0332] Figures 12 to 15 These are cross-sectional views of the electrodes according to one embodiment.

[0333] Reference Figure 12 The electrode may include an active material layer 1 for a rechargeable lithium battery, and a second organic-inorganic composite layer 2a, a first organic-inorganic composite layer 2b, a second organic-inorganic composite layer 2a and a first organic-inorganic composite layer 2b that are integrally formed with one surface of the active material layer 1 and stacked in sequence.

[0334] Reference Figure 13 The electrode may include an active material layer 1 for a rechargeable lithium battery, and a second organic-inorganic composite layer 2a, a first organic-inorganic composite layer 2b, and a second organic-inorganic composite layer 2a that are integrally formed with one surface of the active material layer 1 and stacked in sequence.

[0335] Reference Figure 14The electrode may include an active material layer 1 for a rechargeable lithium battery, and a second organic-inorganic composite layer 2a, a first organic-inorganic composite layer 2b, a second organic-inorganic composite layer 2a, a first organic-inorganic composite layer 2b, a second organic-inorganic composite layer 2a, and a first organic-inorganic composite layer 2b, which are integrally stacked with one surface of the active material layer 1.

[0336] Reference Figure 15 The electrode may include an active material layer 1 for a rechargeable lithium battery, and a second organic-inorganic composite layer 2a, a first organic-inorganic composite layer 2b, a second organic-inorganic composite layer 2a, a first organic-inorganic composite layer 2b, a second organic-inorganic composite layer 2a, a first organic-inorganic composite layer 2b, a second organic-inorganic composite layer 2a, a first organic-inorganic composite layer 2b, a second organic-inorganic composite layer 2a, and a first organic-inorganic composite layer 2b, which are integrally stacked with one surface of the active material layer 1.

[0337] exist Figures 12 to 15 The image shows an active material layer 1, a second organic-inorganic composite layer 2a, a first organic-inorganic composite layer 2b, and a second organic-inorganic composite layer 2a formed in separate layers for a rechargeable lithium battery, but the dashed lines indicate that each layer is integrated.

[0338] The multilayer organic-inorganic composite layer may consist only of a first organic-inorganic composite layer and a second organic-inorganic composite layer. However, the multilayer organic-inorganic composite layer may also include a third organic-inorganic composite layer. The PSSQ content of the third organic-inorganic composite layer may differ from the PSSQ content of the first and second organic-inorganic composite layers.

[0339] At least one of the first and second organic-inorganic composite layers may include fibers containing PSSQ. In this case, the air permeability of the multilayer organic-inorganic composite layer can be easily improved.

[0340] In one embodiment, the first organic-inorganic composite layer, the second organic-inorganic composite layer, and the third organic-inorganic composite layer may each comprise fibers containing PSSQ. Therefore, the description below is limited to the case where the composite layer comprises fibers containing PSSQ.

[0341] Organic-inorganic composite layer The organic-inorganic composite layer may include fibers containing PSSQ and has a nonwoven type, such as a fiber network structure. The network structure can have the advantage of minimizing resistance during lithium-ion migration. The network structure can represent a porous layer with pores randomly formed between the fibers. According to one embodiment, the diameter of the pores can be 90 nm or smaller, for example, from 10 nm to 90 nm.

[0342] In one embodiment, the fiber may be a core-shell fiber having a core and a shell surrounding the core. The shell may include PSSQ having crosslinkable functional groups. The core may include a non-silicone polymer as described below.

[0343] Based on its average diameter, the fiber can be a microfiber or a nanofiber. In one embodiment, the average diameter of the fiber can be in the range of 300 nm or less (e.g., 10 nm to 200 nm or 10 nm to 100 nm). Within the above range, organic-inorganic composite layers can be readily formed. Here, the “average diameter” of the nanofiber can be the average calculated from the diameters measured from multiple (approximately 100) nanofibers selected from SEM images.

[0344] Even when mixed with the polymers described below, PSSQ can be electrospun as is and uniformly dispersed in the polymer. Therefore, PSSQ can achieve the effect of an organic-inorganic composite layer even at any location within the organic-inorganic composite layer, thereby improving reliability.

[0345] PSSQ can include compounds having a T unit, wherein the T unit has a silicon-bonded monovalent organic group R.

[0346] PSSQs can have substituted or unsubstituted aromatic groups. Because substituted or unsubstituted aromatic groups maintain the distance between the molecular chains of the PSSQ, the volume of the organic-inorganic composite layer does not change even when crosslinking occurs, thus further providing a dimensional stability effect. Here, "substituted or unsubstituted aromatic groups" can refer to substituted or unsubstituted C6 to C10 monocyclic or heterocyclic aromatic groups. "Substituted or unsubstituted" can mean that one or more hydrogen atoms of the functional group are substituted by C1 to C10 alkyl, halogen, hydroxyl, amino, or C6 to C10 aryl groups. For example, a substituted or unsubstituted aromatic group can be phenyl. For example, substituted or unsubstituted aromatic groups can be bonded to the silicon of the PSSQ.

[0347] PSSQs can be random, ladder-shaped, cage-shaped, or partially cage-shaped. For example, a PSSQ can be ladder-shaped.

[0348] PSSQ may include silicon-based compounds having a unit of chemical formula 6: In one embodiment, PSSQ is ladder-shaped and may be represented by chemical formula 7, but this disclosure is not limited thereto.

[0349] In one embodiment, the PSSQ may have crosslinkable functional groups. At least some of these crosslinkable functional groups can crosslink with each other during the process of forming the organic-inorganic composite layer. This can further improve the strength, adhesion, and heat resistance of the organic-inorganic composite layer by increasing the degree of bonding between the PSSQs within the same fiber.

[0350] In one embodiment, the fiber may include at least a crosslinked product of PSSQ having crosslinkable functional groups.

[0351] The crosslinkable functional group can be a functional group that can be crosslinked by heat and / or light. For example, the crosslinkable functional group can include one or more of (meth)acryloyl, (meth)acryloyloxy, (meth)acryloyloxyalkyl, epoxy, glycidyl, glycidoxy, and glycidoxyalkyl.

[0352] In one embodiment, the crosslinkable functional group may be represented by chemical formula 4, but this disclosure is not limited thereto.

[0353] Crosslinkable functional groups can be included at any location on the PSSQ. For example, crosslinkable functional groups can be included at the ends of the PSSQ.

[0354] In one embodiment, PSSQ is ladder-shaped and may be represented by chemical formula 8, but this disclosure is not limited thereto.

[0355] In Formula 8, the crosslinkable functional groups can be the same as those defined in Formula 4.

[0356] In one embodiment, in Formula 4, the crosslinkable functional groups may be included in the form of 20 mol% to 50 mol% of the total functional groups of silicon (e.g., 20 mol%, 21 mol%, 22 mol%, 23 mol%, 24 mol%, 25 mol%, 26 mol%, 27 mol%, 28 mol%, 29 mol%, 30 mol%, 31 mol%, 32 mol%, 33 mol%, 34 mol%, 35 mol%, 36 mol%, 37 mol%, 38 mol%, 39 mol%, 40 mol%, 41 mol%, 42 mol%, 43 mol%, 44 mol%, 45 mol%, 46 mol%, 47 mol%, 48 mol%, 49 mol%, or 50 mol% or 30 mol% to 50 mol%). Within the above range, the adhesion and heat resistance of the organic-inorganic composite layer can be improved.

[0357] In chemical formula 8, R 7 R 8 R 9 and R 10 Each is independently a hydroxyl group, a C6 to C20 aryl group, a crosslinkable functional group, or a combination thereof, and R 7 R 8 R 9 and R 10 At least one of them can be a crosslinkable functional group.

[0358] PSSQ can have a weight-average molecular weight of 5,000 g / mol to 30,000 g / mol (e.g., 5,000 g / mol, 6,000 g / mol, 7,000 g / mol, 8,000 g / mol, 9,000 g / mol, 10,000 g / mol, 11,000 g / mol, 12,000 g / mol, 13,000 g / mol, 14,000 g / mol, 15,000 g / mol, 16,000 g / mol, 17,000 g / mol, 18,000 g / mol, 19,000 g / mol, 20,000 g / mol, 25,000 or 30,000 g / mol, or 10,000 g / mol to 20,000 g / mol). Within these ranges, the viscosity of PSSQ can be easily adjusted. In the specification, the weight-average molecular weight can be obtained as a polystyrene standard conversion value using gel permeation chromatography.

[0359] The PSSQ content in the fiber can be basically the same as described above.

[0360] The polymer can be readily electrospun, and its type is unrestricted, as long as it does not affect the dispersion and function of the PSSQ. For example, the polymer can be a non-silicone polymer and can include PVDF, PAN, PAI, PVP, PAA, PVA, or combinations thereof. The polysilsesquioxane content of the multilayer organic-inorganic composite layer can range from 10 wt% to 30 wt% relative to 100 parts by weight of the polymer.

[0361] In one embodiment, the polymer may include PVDF-based polymers and PAN-based polymers. That is, the fiber may include PVDF-based polymers, PAN-based polymers, and PSSQ.

[0362] When mixed with PVDF and PAN polymers and formed into fibers by electrospinning, PSSQ can be uniformly distributed in the fibers, thereby significantly improving the tensile strength of the organic-inorganic composite layer.

[0363] The fibers can be formed into island fibers using polymers including PVDF, PAN, and PSSQ. Specifically, island fibers comprise a marine region and multiple island regions within that marine region.

[0364] The island regions can be composed of PVDF-based polymers. The island regions can have a core-shell structure, with a core composed of PAN-based polymers and a shell surrounding the core composed of PSSQ. Compared to fibers comprising PVDF-based polymers, PAN-based polymers, and PSSQ as individual components, island fibers can significantly improve the tensile strength of the organic-inorganic composite layer by enhancing the interaction between the three components. The specific mechanism by which the combination of PVDF-based polymers, PAN-based polymers, and PSSQ forms island fibers during electrospinning has not yet been elucidated. However, it is believed to be generated by a specific combination of the aforementioned three components, but this disclosure is not limited thereto.

[0365] In island-island fibers, island regions can be randomly distributed within the sea area. For example, the area ratio of island regions in the cross-section of an island-island fiber can be from 30% to 70%, such as 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%, 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49%, 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, or 70 wt%, or 30% to 50%, or 40% to 60%. Within these ranges, the effect of an organic-inorganic composite layer can be easily achieved. The island region area ratio can be expressed as the ratio of the total area of ​​the island regions to the cross-sectional area of ​​the fiber.

[0366] Island fibers can be detected by scanning transmission electron microscopy-energy dispersive spectroscopy (STEM-EDS).

[0367] Figure 16 The HAADF-STEM results for the fibers are shown. (Reference) Figure 16 This allows us to confirm the PAN core and the silicon surrounding it.

[0368] Figure 17 The TEM-EDS results of the fibers are shown. (Reference) Figure 17 It can be confirmed that the fibers included in the organic-inorganic composite layer are island fibers.

[0369] Figure 18 This is a schematic diagram of island fiber. (Refer to...) Figure 18 The island fiber includes a marine region 4 composed of PVDF-type polymers and an island region with a core-shell structure, wherein the island region may include a core 6 composed of PAN-type polymers and a shell 5 surrounding the core and composed of PSSQ.

[0370] In one embodiment, the organic-inorganic composite layer can have a strength of 1000 kgf / cm². 2Or larger (e.g., 1000 kgf / cm) 2 Up to 2000 kgf / cm 2 The tensile strength of the multilayer organic-inorganic composite layer is within the above range. Furthermore, the multilayer organic-inorganic composite layer can also exhibit improved tensile strength, thus the electrode can possess improved mechanical strength.

[0371] Since the fibers include PVDF-type polymers, PAN-type polymers, and PSSQ, the electrode wettability of the organic-inorganic composite layer can be improved, thus the electrode wettability of the multilayer organic-inorganic composite layer can be improved.

[0372] In the fiber, the inorganic component PSSQ is further added to organic components such as PVDF and PAN polymers, thereby exhibiting improved electrode wettability. Since the fiber is electrospun, electrode wettability can be improved. However, since PSSQ has Si-O bonds, it is believed that the electrode wettability of the organic-inorganic composite layer can be further improved, but this disclosure is not limited thereto.

[0373] In one embodiment, the organic-inorganic composite layer can have a thickness of 7.5 mm. 2 / s or greater (e.g., 7.5mm) 2 / s to 10mm 2 The electrolyte wetting rate is [value] / s. Within the above range, the electrode wettability of the multilayer organic-inorganic composite layer can be improved.

[0374] Fibers can provide a shutdown effect by including PVDF-based polymers, PAN-based polymers, and PSSQ. The organic-inorganic composite layer includes pores as described above. Therefore, when the battery is at high temperatures, the PVDF-based polymers can melt and block the pores, thereby providing a shutdown effect. As described above, the fiber containing PVDF-based polymers, PAN-based polymers, and PSSQ is a sea-island fiber, wherein the sea-island region is composed of PVDF-based polymers. Therefore, at high temperatures, the PVDF-based polymers melt rapidly, thereby further increasing the shutdown effect. Therefore, multilayer organic-inorganic composite layers can also provide a shutdown effect.

[0375] In one embodiment, the electrode can be applied to a battery having an electrolyte containing a carbonate solvent. When placed in a carbonate electrolyte at high temperatures, PVDF polymers can readily provide a shut-off effect through swelling and melting.

[0376] Because the fibers include PVDF-based polymers, PAN-based polymers, and PSSQ, the organic-inorganic composite layer can impart improved adhesion to the active material layer. As described above, the fibers comprising PVDF-based polymers, PAN-based polymers, and PSSQ are island fibers, wherein the sea-like regions are composed of PVDF-based polymers. Therefore, since the PVDF-based polymers are included in the sea-like regions of the fibers, improved adhesion can be provided. Specifically, the fibers can increase the adhesion to the positive electrode active material layer, which includes PVDF-based polymers as a binder. Therefore, the multilayer organic-inorganic composite layer can also provide improved adhesion to the active material layer.

[0377] In one embodiment, the PSSQ may have crosslinkable functional groups. These crosslinkable functional groups can crosslink with each other during the process of preparing the organic-inorganic composite layer to increase the bonding between fibers and with the electrode plate, thereby significantly improving adhesion.

[0378] In one embodiment, the dry adhesion of the organic-inorganic composite layer to the active material layer for the rechargeable battery can be 1.2 gf / mm or greater, for example, 1.2 gf / mm to 5 gf / mm. In one embodiment, the wet adhesion of the organic-inorganic composite layer to the active material layer for the rechargeable battery can be 1.4 gf / mm or greater, for example, 1.4 gf / mm to 5 gf / mm.

[0379] Because the fibers include PVDF-based polymers, PAN-based polymers, and PSSQ, the heat resistance of the organic-inorganic composite layer can be improved. Therefore, the multilayer organic-inorganic composite layer can also possess improved heat resistance. PSSQ includes the inorganic component Si. Therefore, compared to fibers that only include PVDF-based polymers and PAN-based polymers as organic components, the fibers of this disclosure can impart higher heat resistance.

[0380] In one embodiment, the PSSQ may have crosslinkable functional groups. These crosslinkable functional groups can crosslink with each other during the process of preparing the organic-inorganic composite layer to fix the fiber structure, thereby significantly improving the heat resistance of the organic-inorganic composite layer.

[0381] In one embodiment, the organic-inorganic composite layer on each of the MD and TD may have a thermal shrinkage rate of 5% or less (e.g., 0 to 3%) in the electrolyte.

[0382] Here, the MD shrinkage rate can be 5% or less, for example, 0 to 3%, and the TD shrinkage rate can be 5% or less, for example, 0 to 3%.

[0383] PVDF polymers can be homopolymers or copolymers of monomer mixtures including vinylidene fluoride.

[0384] In one embodiment, the polymer may be PVDF.

[0385] In another embodiment, the polymer may be a copolymer comprising a mixture of monomers including vinylidene fluoride and comonomers, such as PVDF-HPF.

[0386] PVDF polymers can have a weight-average molecular weight of 100,000 g / mol to 500,000 g / mol (e.g., 150,000 g / mol to 500,000 g / mol). Within this range, the viscosity of the electrospinning solution can be easily adjusted.

[0387] PAN polymers can be homopolymers or copolymers of monomer mixtures including acrylonitrile.

[0388] In one embodiment, the polymer may be PAN.

[0389] PAN-based polymers can have a weight-average molecular weight of 100,000 g / mol to 300,000 g / mol (e.g., 100,000 g / mol to 200,000 g / mol). Within this range, the viscosity of the electrospinning solution can be easily adjusted.

[0390] Relative to a total of 100 parts by weight of PVDF and PAN polymers, the PVDF and PAN polymers can be included in quantities of 50 to 90 parts by weight and 50 to 10 parts by weight (e.g., 60 to 90 parts by weight and 40 to 10 parts by weight). Within the above range, the effect of an organic-inorganic composite layer can be easily achieved.

[0391] The content of PSSQ can be from 5 parts by weight to 50 parts by weight relative to 100 parts by weight of the total amount of PVDF and PAN polymers, for example, 5 parts by weight, 6 parts by weight, 7 parts by weight, 8 parts by weight, 9 parts by weight, 10 parts by weight, 11 parts by weight, 12 parts by weight, 13 parts by weight, 14 parts by weight, 15 parts by weight, 16 parts by weight, 17 parts by weight, 18 parts by weight, 19 parts by weight, 20 parts by weight, 21 parts by weight, 22 parts by weight, 23 parts by weight, and 24 parts by weight. 25 parts by weight, 26 parts by weight, 27 parts by weight, 28 parts by weight, 29 parts by weight, 30 parts by weight, 31 parts by weight, 32 parts by weight, 33 parts by weight, 34 parts by weight, 35 parts by weight, 36 parts by weight, 37 parts by weight, 38 parts by weight, 39 parts by weight, 40 parts by weight, 41 parts by weight, 42 parts by weight, 43 parts by weight, 44 parts by weight, 45 parts by weight, 46 parts by weight, 47 parts by weight, 48 parts by weight, 49 parts by weight, or 50 parts by weight, or 10 parts by weight to 30 parts by weight. Within the above range, the effect of an organic-inorganic composite layer can be easily achieved.

[0392] In one embodiment, the total amount of PVDF polymers, PAN polymers and PSSQ in the fiber may be 95 wt% or less, for example, 95 wt% to 100 wt%.

[0393] The organic-inorganic composite layer can have a thickness of 1 μm to 20 μm (e.g., 1 μm to 10 μm). Within this range, the organic-inorganic composite layer can be used in batteries.

[0394] Preparation of multilayer organic-inorganic composite layers The following describes a method for preparing a multilayer organic-inorganic composite layer according to one embodiment. However, the preparation of the composite layer is not limited to the method described below.

[0395] The multilayer organic-inorganic composite layer can be prepared by: preparing each of an electrospinning solution (first electrospinning solution) for the first organic-inorganic composite layer and an electrospinning solution (second electrospinning solution) for the second organic-inorganic composite layer, and alternately electrospinning the first and second electrospinning solutions onto the surface of the active material layer and drying each solution. Here, the difference in PSSQ content between the first and second electrospinning solutions is 10 wt% or greater.

[0396] Electrospinning can be performed as follows: a nozzle assembly consisting of needle tips with a gauge size of 23G to 30G and a collection roller are positioned at regular intervals; a solution is injected into the nozzle assembly; an active material layer is placed on the collection roller; and a voltage of 35kV to 90kV is applied to the needle tips. The distance between the nozzle assembly and the active material layer can be 10cm to 20cm. A needle tip size of 25G to 30G is preferred because it allows for the formation of an organic-inorganic composite layer in the desired shape.

[0397] During the electrospinning process, the solution is spun and stretched into a fibrous shape, thereby forming a fiber-containing layer on the active material layer. The solution is suspended as droplets at the tip due to surface tension, and when a voltage is applied, charges accumulate on the surface of the solution, generating repulsive forces. When a critical voltage is reached where the repulsive force between the charges becomes higher than the surface tension of the solution, a Taylor cone is generated, and a polymer solution jet is ejected from the tip of the cone and highly stretched to form fibers, which collect on the active material layer to form a fiber-containing layer.

[0398] According to one embodiment, the electrospinning process can be carried out at 20°C to 30°C and 40% to 60% relative humidity. When the electrospinning process is carried out under the above temperature and relative humidity conditions, it has the advantage of maintaining a constant fiber diameter during spinning.

[0399] The electrospinning speed can be adjusted to form an organic-inorganic composite layer of appropriate thickness, and the electrospinning speed can be, for example, from 1 m / min to 3 m / min. In addition, the flow rate of the solution discharged from the tip can be adjusted to a range of 20 μL / min to 1000 μL / min (e.g., 20 μL / min to 200 μL / min).

[0400] Each of the first and second electrospinning solutions may further include an initiator for promoting crosslinking of PSSQ having crosslinkable functional groups. The initiator may include one or more of thermal initiators and photoinitiators. Thermal and photoinitiators may be conventional types known to those skilled in the art.

[0401] The solution may also include a solvent, and the solvent may include, for example, dimethylacetamide, dimethyl sulfoxide, dimethylformamide, tetrahydrofuran, carbon tetrachloride, methylpyrrolidone, water, ethanol, acetone, or combinations thereof. The solvent may be included as a trace residue in the organic-inorganic composite layer.

[0402] The content of the mixture of PSSQ and polymer in the solution can be from 5 wt% to 20 wt% relative to the total solution of 100 wt%. Within the above range, the organic-inorganic composite layer can be formed to an appropriate thickness.

[0403] After the electrospinning process, a solvent removal process can be performed at temperatures ranging from 80°C to 20°C.

[0404] The drying process can be adjusted appropriately based on the boiling point of the solvent.

[0405] Organic-inorganic composite layers can be formed by cross-linking layers including fibers.

[0406] Crosslinking can be performed by heat treatment of the fiber-containing layer under predetermined conditions. For example, the heat treatment can be performed in a vacuum at 50°C to 200°C (e.g., 50°C to 150°C) for 5 to 180 minutes.

[0407] The fiber-containing layer can be hot-pressed before or after drying and / or crosslinking. Hot pressing can increase the density between fibers in the fiber-containing layer and reduce the thickness of the organic-inorganic composite layer. According to one embodiment, hot pressing can be performed by pressing the fiber-containing layer at a pressure of 0.1 MPa to 1 MPa at 70°C or higher (e.g., 70°C to 150°C).

[0408] Active material layer for rechargeable lithium batteries The active material layer used in a rechargeable lithium battery can be either a positive electrode active material layer or a negative electrode active material layer. For example, the active material layer used in a rechargeable lithium battery can be a negative electrode active material layer.

[0409] Since the active material layer used in the rechargeable lithium battery is substantially the same as the active material layer described in "First Electrode for Rechargeable Lithium Battery", its detailed description is omitted.

[0410] Electrode components for rechargeable lithium batteries The electrode assembly for a rechargeable lithium battery includes a positive electrode active material layer for a rechargeable lithium battery, a negative electrode active material layer for a rechargeable lithium battery, and a multilayer organic-inorganic composite layer located between the positive electrode active material layer for a rechargeable lithium battery and the negative electrode active material layer for a rechargeable lithium battery.

[0411] The multilayer organic-inorganic composite layer, the positive electrode active material layer, and the negative electrode active material layer are basically the same as those described above.

[0412] In one embodiment, the second organic-inorganic composite layer can be integrated with the negative electrode active material layer, and the first organic-inorganic composite layer can be integrated with the positive electrode active material layer.

[0413] Figure 19 This is a cross-sectional view of an electrode assembly for a rechargeable lithium battery according to one embodiment.

[0414] Reference Figure 19 The electrode assembly may include: a negative electrode active material layer 1a; a multilayer organic-inorganic composite layer, including a second organic-inorganic composite layer 2a, a first organic-inorganic composite layer 2b, a second organic-inorganic composite layer 2a and a first organic-inorganic composite layer 2b sequentially formed on the negative electrode active material layer 1a; and a positive electrode active material layer 1b, integrated on the multilayer organic-inorganic composite layer.

[0415] Rechargeable lithium batteries A rechargeable lithium battery includes an electrode for rechargeable lithium batteries and another electrode for rechargeable lithium batteries.

[0416] In rechargeable lithium-ion batteries, the electrodes used for the rechargeable lithium-ion battery have different electrical characteristics than the other electrode used for the rechargeable lithium-ion battery. That is, if the electrode assembly for the rechargeable lithium-ion battery includes a positive electrode, the other electrode can be a negative electrode. Furthermore, if the electrode assembly for the rechargeable lithium-ion battery includes a negative electrode, the other electrode can be a positive electrode.

[0417] Rechargeable lithium batteries may also include an electrolyte solution.

[0418] Electrolyte solutions used in rechargeable lithium batteries may include non-aqueous organic solvents and lithium salts.

[0419] Non-aqueous organic solvents can be used as a medium for transporting ions that participate in the electrochemical reactions of a battery.

[0420] Non-aqueous organic solvents can be carbonate solvents, ester solvents, ether solvents, ketone solvents, alcohol solvents, aprotic solvents, or combinations thereof.

[0421] Carbonate solvents can include dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), methyl ethyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), butyl carbonate (BC), etc.

[0422] Ester solvents can include methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, decanoic acid lactone, mevalonate lactone, caprolactone, etc.

[0423] Ether solvents may include dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, dimethoxyethane, 2-methyltetrahydrofuran, 2,5-dimethyltetrahydrofuran, tetrahydrofuran, etc. Additionally, ketone solvents may include cyclohexanone, etc. Alcohol solvents may include ethanol, isopropanol, etc. Aprotic solvents may include: nitriles, such as R-CN (where R is a C2 to C20 straight-chain, branched, or cyclic hydrocarbon group, and may include double bonds, aromatic rings, or ether bonds, etc.); amides, such as dimethylformamide; dioxolane, such as 1,3-dioxolane, 1,4-dioxolane, etc.; sulfolane, etc.

[0424] Non-aqueous organic solvents can be used alone or in combination of two or more.

[0425] Furthermore, when using carbonate solvents, cyclic carbonates and chain carbonates can be mixed and used, and cyclic carbonates and chain carbonates can be mixed in a volume ratio of about 1:1 to about 1:9.

[0426] Lithium salts dissolved in organic solvents supply lithium ions in batteries, enabling basic operation of rechargeable lithium batteries and improving lithium ion transport between the positive and negative electrodes. Examples of lithium salts include those selected from LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiAlO2, LiAlCl4, LiPO2F2, LiCl, LiI, LiN(SO2C2F5)2, Li(FSO2)2N (lithium bis(fluorosulfonyl)imide, LiFSI), LiC4F9SO3, and LiN(C x F 2x+1 SO2)(C y F 2y+1 At least one of the following: (SO2) (where x and y are integers from 1 to 20), lithium trifluoromethane sulfonate, lithium tetrafluoroethane sulfonate, lithium difluoro(oxalate)borate (LiDFOB), lithium difluorobis(oxalate)phosphate (LiDFBOP), and lithium bis(oxalate)borate (LiBOB).

[0427] Rechargeable lithium batteries can be classified according to their shape, such as cylindrical batteries, prismatic batteries, pouch batteries, or coin-shaped batteries.

[0428] Figures 20 to 23 This is a schematic diagram illustrating a rechargeable lithium battery according to an embodiment. Figure 20 A cylindrical battery is shown. Figure 21 A prismatic battery is shown, and Figure 22 and Figure 23 A pouch-type battery is shown. (See reference) Figures 20 to 23 The rechargeable lithium battery 100 may include an electrode assembly 40 and a housing 50. The electrode assembly 40 includes a positive electrode 10 and a negative electrode 20 including a negative electrode active material layer and an organic-inorganic composite layer. The electrode assembly 40 is housed in the housing 50. The positive electrode 10 and the negative electrode 20 may be impregnated with an electrolyte solution (not shown). Figure 20 As shown, the rechargeable lithium battery 100 may include a sealing member 60 of the sealed housing 50. Figure 21 In this context, the rechargeable lithium battery 100 may include a positive electrode lead connector 11, a positive electrode terminal 12, a negative electrode lead connector 21, and a negative electrode terminal 22. For example... Figure 22 and Figure 23 As shown, the rechargeable lithium battery 100 may include electrode terminals 70, which serve as electrical paths for guiding current formed in the electrode assembly 40 to the outside. The electrode terminals 70 may be, for example, a positive electrode terminal 71 and a negative electrode terminal 72.

[0429] As a non-limiting example, the rechargeable lithium battery according to the embodiments can be used in automobiles, mobile phones and / or various types of electronic devices.

[0430] Examples and comparative examples of this disclosure are described below. However, the following examples are merely illustrative of this disclosure, and this disclosure is not limited thereto.

[0431] Example 1 As the positive electrode active material, a positive electrode slurry was prepared by mixing 97.5 wt% lithium cobalt oxide, 1.0 wt% carboxymethyl cellulose, and 1.5 wt% PVDF in N-methyl-2-pyrrolidone as a solvent. The positive electrode slurry was applied to aluminum foil, dried, and rolled to form a positive electrode active material layer.

[0432] The mixture was prepared by mixing 60 parts by weight of PVDF and 40 parts by weight of PAN. Furthermore, an electrospinning solution was prepared by adding 20 parts by weight of PSSQ with crosslinkable functional groups (PSSQ having phenyl and methacrylate groups) relative to 100 parts by weight of the mixture, and then dissolving the resulting mixture in dimethylacetamide as a solvent.

[0433] A layer comprising nanofibers (average diameter: 90 nm) was formed by electrospinning an electrospinning solution onto a prepared positive electrode active material layer. The electrospinning process is as follows: Electrospinning was performed at 20°C by positioning a nozzle assembly consisting of 52 25G needle tips and a collecting roller at 15cm intervals, adding a solution for forming an organic-inorganic composite layer to the tips, and applying a voltage of 40kV to 90kV. Here, the roller speed of the collecting roller was set to 25cm / min, and the flow rate of the solution for forming the organic-inorganic composite layer ejected from the tips was set to 1mL / min.

[0434] The thickness of the layer including nanofibers was adjusted by hot pressing using a roller press. Subsequently, an organic-inorganic composite layer (thickness: 8 μm) with a fiber network structure, including PVDF, PAN and methacrylate-based crosslinked PSSQ, was formed on the positive electrode active material layer, and subjected to a heat treatment at 70°C for 30 minutes for crosslinking to manufacture the positive electrode for rechargeable lithium batteries.

[0435] Example 2 The positive electrode was manufactured in the same manner as in Example 1, except that it underwent a heat treatment at 140°C for 30 minutes for crosslinking.

[0436] Example 3 The positive electrode is manufactured in the same manner as in Example 1, except that it includes 30 parts by weight of PSSQ with crosslinkable functional groups.

[0437] Comparison Example 1 The positive electrode is fabricated in the same manner as in Example 1, except that PSSQ with crosslinkable functional groups is not included in the electrospinning solution.

[0438] Comparison Example 2 The positive electrode is manufactured in the same manner as in Example 1, except that the heat treatment for crosslinking at 70°C for 30 minutes is not performed.

[0439] Comparison Example 3 First, a fiber membrane is formed by electrospinning a solution containing PSSQ (which has only phenyl groups as silicon substituents) that does not have crosslinkable functional groups. Then, a composite layer containing PSSQ is formed by spinning a PSSQ solution onto the previously electrospun fiber membrane. The positive electrode is manufactured in the same manner as in Example 1, except that the spinning solution is separated and spun twice.

[0440] The physical properties of the organic-inorganic composite layers prepared in the example and comparative examples are evaluated below, and the results are shown in Table 1.

[0441] (1) Tensile strength (unit: kgf / cm) 2 ): An organic-inorganic composite positive electrode was manufactured from the various compositions of the example and comparative examples. Subsequently, after the positive electrode was cut into five rectangular pieces, each having a size of 10 mm (width (MD)) × 25 mm (length (TD)), each sample was mounted on a universal testing machine (UTM) with a measurement length of 40 mm, and then the sample was stretched to measure the average tensile strength on MD.

[0442] (2) Air permeability (unit: sec / 100cc): Air permeability is evaluated by measuring the time (unit: sec) required for 100cc of air to pass through the organic-inorganic composite layer using a measuring device (EG01-55-1MR, Asahi Seiko).

[0443] [Setting conditions for the air permeability measuring device] Measured pressure: 0.5 kg / cm 2 Cylinder pressure: 2.5 kg / cm² 2 Time setting: 10 seconds [Table 1]

[0444] As shown in Table 1, it can be seen that the organic-inorganic composite layer of the example exhibits significantly improved tensile strength compared to the organic-inorganic composite layer of the comparative example. This is because the strength is improved due to the uniform distribution and cross-linking of PSSQ in the polymer fibers. In Comparative Example 3, it can be seen that when PSSQ is electrospun alone, the air permeability increases, but the strength is not improved at all.

[0445] Example 4 As the negative electrode active material, a negative electrode slurry was prepared by mixing 97.5 wt% artificial graphite, 1.0 wt% carboxymethyl cellulose, and 1.5 wt% styrene-butadiene rubber in distilled water as a solvent. The negative electrode slurry was applied to copper foil, dried, and rolled to form a negative electrode active material layer.

[0446] A mixture was prepared by mixing 60 parts by weight of PVDF and 40 parts by weight of PAN, and by adding 10 parts by weight of PSSQ with crosslinkable functional groups (PSSQ with phenyl and epoxy groups) and 3 parts by weight of methyl aromatic polyamide polymer (MA; having the following chemical formula, Nomax) relative to 100 parts by weight of the prepared mixture. ® Mix the ingredients, add 1 part by weight of initiator (boron ester initiator), and add dimethylacetamide as a solvent for dispersion to prepare an electrospinning solution.

[0447] [Chemical Formula]

[0448] A layer comprising nanofibers (average diameter: 90 nm) is formed by electrospinning an electrospinning solution onto a negative electrode active material layer. The electrospinning process is as follows: At 20°C, a solution for forming the organic-inorganic composite layer was added to the tips by positioning a nozzle assembly consisting of 40 tips with a needle size of 25G and a collecting roller at 15cm intervals, and a voltage of 40kV to 90kV was applied. Here, the roller speed of the collecting roller was set to 35cm / min, and the initial flow rate of the solution for forming the organic-inorganic composite layer ejected from the tips was set to 1mL / min. After electrospinning, the solution was dried with hot air at 70°C.

[0449] The layer comprising nanofibers is pressed using a hot roller press heated to 90°C. The roller speed is 20 cm / min. A negative electrode for a rechargeable lithium battery is manufactured in which an organic-inorganic composite layer (thickness: 8 μm) having a network structure of fibers comprising PVDF, PAN, aromatic polyamide polymers and epoxy-crosslinked PSSQ fibers is formed on the negative electrode active material layer.

[0450] Example 5 and Example 6 The negative electrode was manufactured in the same manner as in Example 4, except that the contents of PSSQ and aromatic polyamide polymers were varied as shown in Table 2 below.

[0451] Compare Example 4 The negative electrode for a rechargeable lithium battery is manufactured in the same manner as in Example 4, except that PSSQ and aromatic polyamide polymers are not included in the electrospinning solution.

[0452] Compare Example 5 The negative electrode for the rechargeable lithium battery is manufactured in the same manner as in Example 4, except that PSSQ is not included in the electrospinning solution.

[0453] Comparison Example 6 The negative electrode for a rechargeable lithium battery is manufactured in the same manner as in Example 4, except that PSSQ without crosslinkable functional groups (PSSQ with only phenyl as a silicon substituent) is included in the electrospinning solution instead of PSSQ with crosslinkable functional groups.

[0454] The physical properties of the organic-inorganic composite layers prepared in the following evaluation examples and comparative examples are shown in Table 2 below.

[0455] (1) Tensile strength (unit: kgf / cm) 2 ): An organic-inorganic composite negative electrode was manufactured from the various compositions of the example and comparative examples. Subsequently, after the negative electrode was cut into five rectangular pieces, each having a size of 10 mm (width (MD)) × 25 mm (length (TD)), each sample was mounted on a universal testing machine (UTM) with a measurement length of 40 mm, and then the sample was stretched to measure the average tensile strength on MD.

[0456] (2) Dry Adhesion (unit: gf / mm): Samples of each example and comparative example were cut into pieces 25 mm wide and 80 mm long. Subsequently, the negative electrode active material layer was fixed to the upper fixture, and the organic-inorganic composite layer was fixed to the lower fixture. These electrodes were then stretched and peeled using UTM. Here, the speed was 100 mm / min. Dry adhesion was measured three times to obtain an average value.

[0457] (3) Electrolyte wetting rate (unit: mm) 2 / s): The prepared sample was cut into pieces 40 mm wide and 70 mm long. Then, 15 μL of electrolyte (1.5 M LiPF6 dissolved in ethylene carbonate, methyl ethyl carbonate, and dimethyl carbonate (volume ratio 30:50:20)) was dropped onto the sample from a height of 1 cm. After 30 seconds, the wetting rate was measured by measuring the distance the electrolyte diffused from the center.

[0458] [Table 2]

[0459] As shown in Table 2, it can be confirmed that the organic-inorganic composite layers of each example exhibit excellent tensile strength, excellent dry adhesion, and excellent electrolyte wetting rate. Based on Comparative Example 6, it can be seen that the epoxy-containing PSSQ has improved adhesion but insufficient strength.

[0460] For Comparative Example 5, it can be confirmed that the aramid enhances strength but weakens adhesion. In this example, compared to aramid alone, the combination of PSSQ and aramid not only provides high adhesion but also improves strength. Furthermore, this combination also improves electrode wetting rate. When applied to rechargeable batteries, this can contribute to improved battery performance by enhancing electrolyte impregnation.

[0461] Example 7 As the negative electrode active material, a negative electrode slurry was prepared by mixing 97.5 wt% artificial graphite, 1.0 wt% carboxymethyl cellulose, and 1.5 wt% styrene-butadiene rubber in distilled water as a solvent. The negative electrode slurry was applied to copper foil, dried, and rolled to form a negative electrode active material layer.

[0462] An electrospinning solution was prepared by mixing 60 parts by weight of PVDF and 40 parts by weight of PAN, and then by mixing 20 parts by weight of PSSQ (a PSSQ having phenyl and crosslinkable functional groups, R in chemical formula 4) with 100 parts by weight of the mixture. 7 It is n-propylidene, R 8 The mixture is a methylene group, and 0.5 parts by weight of a borate ester initiator is mixed with 100 parts by weight of PSSQ. The resulting mixture is then dissolved in dimethylacetamide as a solvent.

[0463] A layer comprising nanofibers (average diameter: 90 nm) is formed by electrospinning an electrospinning solution onto a negative electrode active material layer. The electrospinning process is as follows: Under conditions of 26°C and 50% relative humidity, an electrospinning solution was added to the tips by positioning a nozzle assembly consisting of 52 tips with a needle size of 25G and a collecting roller at 15cm intervals, and a voltage of 40 to 90 kV was applied. Here, the roller speed of the collecting roller was 1 to 3 m / min, and the flow rate of the solution ejected from the tips for forming the organic-inorganic composite layer was set to 150 μL / min. After electrospinning, drying was performed using hot air at 90°C.

[0464] A layer comprising nanofibers was hot-pressed at 70°C and 0.3 MPa, and subjected to a heat treatment for crosslinking at 140°C in a vacuum for 3 hours to fabricate an integrated negative electrode for a rechargeable lithium battery, wherein an organic-inorganic composite layer (thickness: 8 μm) having a network structure of nanofibers comprising PVDF, PAN and PSSQ with crosslinkable functional groups of phenyl groups is formed on the negative electrode active material layer.

[0465] like Figures 7 to 10 The results show that the prepared nanofibers are indeed island fibers.

[0466] The prepared organic-inorganic composite layer is hot-pressed, and then... Figure 26 The SEM results are shown below. (Refer to...) Figure 26 As can be seen, the organic-inorganic composite layer has a bonded portion due to the cross-linking of the epoxy groups in PSSQ. Cracks are observed on the fiber surface due to the cross-linking, and the fibers are found to maintain their circular cross-sectional shape.

[0467] Example 8 The negative electrode is manufactured in the same manner as in Example 7, except that the mixture of PVDF and PAN includes 10 parts by weight of PSSQ relative to 100 parts by weight.

[0468] Example 9 The negative electrode is manufactured in the same manner as in Example 7, except that the mixture of PVDF and PAN includes 30 parts by weight of PSSQ relative to 100 parts by weight.

[0469] Example 10 The negative electrode was manufactured in the same manner as in Example 7, except that the mixture of PVDF and PAN included 10 parts by weight of PSSQ (PSSQ having phenyl groups and not having crosslinkable functional groups) relative to 100 parts by weight.

[0470] Compare Example 7 The negative electrode is fabricated in the same manner as in Example 7, except that PSSQ is not included in the electrospinning solution.

[0471] The organic-inorganic composite layer was hot-pressed, and then the SEM results were shown. Figure 27 (See also:) Figure 27 This confirms that the fibers have a compressed shape.

[0472] Compare Example 8 The negative electrode is manufactured in the same manner as in Example 7, except that PVDF is not included in the electrospinning solution.

[0473] Compare Example 9 The negative electrode is manufactured in the same manner as in Example 7, except that PAN is not included in the electrospinning solution.

[0474] Compare Example 10 A separator is purchased in which a heat-resistant layer containing boehmite and acrylic binder and an adhesive layer containing PVDF adhesive are sequentially laminated on one surface of a polyethylene film. The negative electrode is manufactured by laminating the separator onto a negative electrode active material layer formed in the same manner as in Example 7.

[0475] Compare Example 11 The negative electrode is fabricated in the same manner as in Example 7, except that PAA is included in the electrospinning solution instead of PAN.

[0476] The physical properties of the organic-inorganic composite layers and / or membranes formed in the example and comparative examples were evaluated. The results are shown in Table 3 below. Figure 24 and Figure 25 middle.

[0477] (1) Tensile strength (unit: kgf / cm) 2 ): After preparing specimens 1 cm wide and 8 cm long, they were attached to clamps with the distance between the clamps (specimen length) set to 2 cm. A tensile test was then performed at a speed of 10 cm / min. The tensile strength (engineering strength) was calculated by dividing the force at the fracture point by the cross-sectional area of ​​the specimen in its original state. Three measurements were taken for each specimen to obtain the average value.

[0478] (2) Electrolyte wettability (unit: mm) 2 / s): 15 μL of electrolyte is dropped from a height of 1 cm onto an electrospun fiber layer or diaphragm, and the wetting rate is calculated by the area of ​​the electrolyte spread on it for 30 seconds.

[0479] (3) Shutdown effect: After separating the 5cm × 5cm electrospun membranes prepared in the various example and comparative examples from the negative electrode, they were attached to the positive electrode by hot pressing. The resulting samples were then sealed in a bag along with the electrolyte and placed at 150°C for 1 hour. The surface of the organic-inorganic composite layer of the samples was observed by SEM to evaluate whether the pores were blocked. When the pores were blocked, it was evaluated as exhibiting a shut-off effect.

[0480] When 50% or more of the pores in the diaphragm are blocked, the rating is ○; when less than 50% of the pores in the diaphragm are blocked, the rating is ×.

[0481] (4) Adhesion (unit: gf / mm): (4-1) Dry adhesion Electrodes prepared in the various example and comparative examples were cut to a size of 2.5 cm × 8 cm to prepare samples. In each sample, the organic-inorganic composite layer was separated from the negative electrode active material layer by approximately 10 mm to 20 mm. The organic-inorganic composite layer was then fixed to the upper clamp, and the negative electrode active material layer to the lower clamp, with a distance of 20 mm between the clamps. The sample was then peeled off by pulling it in a 180° direction. The peeling speed was 20 mm / min. After peeling began, the force required to peel 40 mm was measured three times to obtain an average value. This average value was determined as the mean of the measurements. Adhesion was measured using UTM.

[0482] (4-2) Wet adhesion Electrodes prepared in the various example and comparative examples were cut into 2.5 cm × 8 cm dimensions to prepare samples. The prepared samples were placed in bags. 2.5 g of a mixed solvent (50:50 volume ratio) containing dissolved LiPF6 in ethylene carbonate and methyl ethyl carbonate was injected as the electrolyte, the bag was sealed, and the resulting product was placed at 25°C for 24 hours. Subsequently, the resulting samples were placed in a 50°C chamber under a pressure of 200 kgf for 2 hours. In the samples, after separating the organic-inorganic composite layer from the negative electrode active material layer by approximately 10 mm to 20 mm, the organic-inorganic composite layer was fixed to the upper clamp, and the negative electrode active material layer was fixed to the lower clamp, with a distance of 20 mm between the clamps. The sample was then peeled off by pulling it in a 180° direction. The peeling speed was 20 mm / min. After peeling began, the force required to peel 40 mm was measured three times to obtain the average value. This average value was determined as the mean of the measurements. Adhesion was measured using UTM.

[0483] (5) Electrolyte thermal shrinkage rate (unit: %): The electrodes (including the organic-inorganic composite layer, the negative electrode active material layer, and the copper foil) prepared in each example and comparative example were cut into 5cm × 5cm sizes to prepare samples. After removing the sample from the negative electrode, the sample was hot-pressed onto the positive electrode to seal it in a bag with the electrolyte, and then left for 24 hours to allow the electrolyte to fully impregnate the electrospun membrane. After placing the resulting bag in an oven at 150°C for 1 hour, the sample was removed from the bag to measure how much the size had decreased compared to the initial size (5cm × 5cm) on MD and TD, thereby calculating the thermal shrinkage rate. The thermal shrinkage rate was calculated using the following mathematical expression 1.

[0484] [Mathematical Expression 1] Thermal shrinkage rate = (L0 - L1) / L0 × 100 (L0 is the initial length of the organic-inorganic composite layer (5cm), and L1 is the length of the organic-inorganic composite layer after it has been placed at 150°C for 1 hour.) [Table 3]

[0485] As shown in Table 3, the example organic-inorganic composite layer has improved tensile strength, improved electrode wettability, improved turn-off effect, and improved adhesion and heat resistance to the active material layer.

[0486] Example 11 Preparation of the first electrospinning solution A mixture was prepared by mixing 60 parts by weight of PVDF and 40 parts by weight of PAN, and an electrospinning solution was prepared by: PSSQ (containing phenyl groups and crosslinkable functional groups) was added to the mixture. 7 It is n-propylidene, R 8 The methylene group is mixed with the mixture to make its content in the fiber 10 wt%, and 0.5 parts by weight of borate ester initiator are mixed with 100 parts by weight of PSSQ. The resulting mixture is dissolved in dimethylacetamide as a solvent.

[0487] Preparation of the second electrospinning solution A mixture was prepared by mixing 60 parts by weight of PVDF and 40 parts by weight of PAN, and an electrospinning solution was prepared by: PSSQ (containing phenyl groups and crosslinkable functional groups) was added to the mixture. 7 It is n-propylidene, R 8 The methylene group is mixed with the mixture to make its content in the fiber 20 wt%. 0.5 parts by weight of borate ester initiator are mixed with 100 parts by weight of PSSQ. The resulting mixture is dissolved in dimethylacetamide as a solvent.

[0488] Electrode manufacturing As the negative electrode active material, a negative electrode slurry was prepared by mixing 97.5 wt% artificial graphite, 1.0 wt% carboxymethyl cellulose, and 1.5 wt% styrene-butadiene rubber in distilled water as a solvent. The negative electrode slurry was applied to copper foil, dried, and rolled to form a negative electrode active material layer.

[0489] As the positive electrode active material, a positive electrode slurry was prepared by mixing 97.5 wt% lithium cobalt oxide, 1.0 wt% carboxymethyl cellulose, and 1.5 wt% PVDF in the solvent N-methyl-2-pyrrolidone. The positive electrode slurry was applied to aluminum foil, dried, and rolled to form a positive electrode active material layer.

[0490] The electrode assembly is manufactured as follows: A second electrospinning solution and a first electrospinning solution are alternately electrospinned onto the negative electrode active material layer, dried in a desiccator at 90°C, hot-pressed at 70°C and 0.3 MPa, and heat-treated in a vacuum at 140°C for 180 minutes to crosslink. The prepared positive electrode active material layer is then layered. In the electrode assembly, the negative electrode active material layer, the second organic-inorganic composite layer, the first organic-inorganic composite layer, the second organic-inorganic composite layer, the first organic-inorganic composite layer, and the positive electrode active material layer are stacked sequentially. The difference in PSSQ content between the first and second organic-inorganic composite layers is 10 wt%. The electrode assembly comprises a total of four organic-inorganic composite layers with a thickness of 7 μm to 8 μm.

[0491] The electrospinning process was performed as follows: a nozzle assembly consisting of 40 tips with a needle size of 25G and a collecting roller positioned at 15cm intervals were used. A solution for forming the organic-inorganic composite layer was added to the tips, and a voltage of 40kV to 90kV was applied. Electrospinning was carried out at 26°C and 50% relative humidity. The collecting roller speed was set to 1m / min to 3m / min, and the flow rate of the electrospinning solution ejected from the tips was set to 150μL / min. After electrospinning, the solution was dried using hot air at 90°C.

[0492] Example 12 The electrode assembly is fabricated in the same manner as in Example 11, except that a total of six organic-inorganic composite layers are formed by alternately stacking a first organic-inorganic composite layer and a second organic-inorganic composite layer. The thickness of the six organic-inorganic composite layers is 7 μm to 8 μm.

[0493] Example 13 The electrode assembly is fabricated in the same manner as in Example 11, except that a total of eight organic-inorganic composite layers are formed by alternately stacking a first organic-inorganic composite layer and a second organic-inorganic composite layer. The thickness of the eight organic-inorganic composite layers is 7 μm to 8 μm.

[0494] Example 14 The electrode assembly was manufactured in the same manner as in Example 11, except that the difference in PSSQ content between the first organic-inorganic composite layer (10 wt% PSSQ) and the second organic-inorganic composite layer (40 wt% PSSQ) was changed to 30 wt%. The thickness of the four organic-inorganic composite layers was 7 μm to 8 μm.

[0495] Compare Example 12 Preparation of the first electrospinning solution A mixture was prepared by mixing 60 parts by weight of PVDF and 40 parts by weight of PAN, and an electrospinning solution was prepared by: PSSQ (containing phenyl and crosslinkable functional groups, PSSQ (in chemical formula 4, R)) was added. 7 It is n-propylidene, R 8 The methylene group is mixed with the mixture to make its content in the fiber 10 wt%, and 0.5 parts by weight of borate ester initiator are mixed with 100 parts by weight of PSSQ. The resulting mixture is dissolved in dimethylacetamide as a solvent.

[0496] Preparation of the second electrospinning solution A mixture was prepared by mixing 60 parts by weight of PVDF and 40 parts by weight of PAN, and an electrospinning solution was prepared by: PSSQ (containing phenyl and crosslinkable functional groups, PSSQ (in chemical formula 4, R)) was added. 7 It is n-propylidene, R 8 The methylene group is mixed with the mixture to make its content in the fiber 15 wt%, and 0.5 parts by weight of borate ester initiator are mixed with 100 parts by weight of PSSQ. The resulting mixture is dissolved in dimethylacetamide as a solvent.

[0497] The electrode assembly was fabricated using a first electrospinning solution and a second electrospinning solution in the same manner as in Example 11. The difference in PSSQ content between the first organic-inorganic composite layer and the second organic-inorganic composite layer was 5 wt%. The electrode assembly comprised a total of four organic-inorganic composite layers, and the thickness of the four organic-inorganic composite layers was 7 μm to 8 μm.

[0498] The physical properties of the multilayer organic-inorganic composite layers and electrode assemblies fabricated in the evaluation and comparative examples are assessed.

[0499] (1) Short-circuit strength after foreign body injection (unit: N): After preparing the following samples, the short-circuit strength was measured using the compression mode of an Instron universal testing machine. When manufacturing the electrode assemblies of the example and comparative examples, 10 foreign bodies c were injected at regular intervals between the negative electrode b, which contains a negative electrode active material layer and a multilayer organic-inorganic composite layer h, and the positive electrode a, which contains a positive electrode active material layer. The foreign bodies were made of stainless steel and had an “L” shaped cross-section with a horizontal length of 1000 μm, a vertical length of 1000 μm, and a thickness of 100 μm. The positive electrode a, negative electrode b, multilayer organic-inorganic composite layer h, and foreign bodies c were inserted into bag I, and bag I was placed between iron plates d. Then, the positive electrode terminal e and the negative electrode terminal f were connected to the positive electrode a and the negative electrode b, respectively, to manufacture a short-circuit structure with Figure 28The sample is shown in the cross-section. The positive and negative electrode terminals are then connected to a multimeter g. The sample is placed on a flat lower iron plate positioned on an Instron lower clamp, and the bag is pressed down by an upper clamp with an Instron load cell connected to one side. The pressing force (N) is measured when the multilayer organic-inorganic composite layer h breaks due to the foreign object c and resistance is detected by the multimeter due to the contact between the positive and negative electrodes. The short-circuit strength against foreign object pressing is, for example, 200 N or greater. Within this range, battery safety against foreign objects can be increased when manufacturing actual batteries.

[0500] (2) Air permeability (unit: sec / 100cc): Air permeability is evaluated by measuring the time (unit: sec) required for 100cc of air to pass through the organic-inorganic composite layer using a measuring device (EG01-55-1MR, Asahi Seiko).

[0501] [Setting conditions for the air permeability measuring device] Measured pressure: 0.5 kg / cm 2 Cylinder pressure: 2.5 kg / cm² 2 Time setting: 10 seconds [Table 4]

[0502] As shown in Table 4, the example organic-inorganic composite layer provides improved air permeability, and the example electrode assembly provides high stability against foreign matter.

[0503] However, the organic-inorganic composite layer in Comparative Example 12 exhibits low short-circuit strength and air permeability values.

[0504] Reference Example 1 An electrospinning solution and a positive electrode active material layer were prepared in the same manner as the first electrospinning solution in Example 11. The prepared electrospinning solution was electrospinned onto the positive electrode active material layer in the same manner as in Example 11, and subjected to preheating, heat treatment, and hot pressing to form an organic-inorganic composite layer on the positive electrode active material layer. The organic-inorganic composite layer comprises 60 parts by weight of PVDF, 40 parts by weight of PAN, and 20 parts by weight of PSSQ, as well as nanofibers crosslinked with crosslinkable functional groups of PSSQ.

[0505] Figure 16 and Figure 17 The results shown confirm that the prepared nanofibers are island fibers.

[0506] See Example 2 Except for including 60 parts by weight of PVDF and 40 parts by weight of PAN but excluding PSSQ, the organic-inorganic composite layer is formed in the same manner as in Reference Example 1.

[0507] This confirms that the prepared nanofibers are not island fibers.

[0508] Evaluate the following physical properties of the organic-inorganic composite layer and electrode prepared in Reference Example 1 and Reference Example 2.

[0509] (1) Tensile strength (unit: kgf / cm) 2 After preparing a specimen with a width of 1 cm and a length of 8 cm, attach it to a fixture, setting the distance between the fixtures (the specimen length) to 2 cm, and then perform a tensile test at a speed of 10 cm / min. The tensile strength (engineering strength) is calculated by dividing the force at the fracture point of the specimen by the cross-sectional area of ​​the specimen in its original state. Three measurements are taken for each specimen to obtain the average value.

[0510] (2) Electrolyte wettability (unit: mm) 2 / s): 15 μL of electrolyte is dropped onto the electrospun fiber layer or diaphragm from a height of 1 cm, and the wetting rate is calculated by the area covered by the electrolyte after 30 seconds.

[0511] (3) Shutdown effect: After separating the 5cm × 5cm electrospun membranes prepared in Reference Examples 1 and 2 from the positive electrode, they were attached to the negative electrode by hot pressing. The resulting samples were then sealed in a bag along with the electrolyte and placed at 150°C for 1 hour. The surface of the organic-inorganic composite layer of the samples was observed by SEM to evaluate whether the pores were blocked. When the pores were blocked, it was evaluated as exhibiting a shut-off effect.

[0512] (4) Adhesion (unit: gf / mm): (4-1) Dry adhesion The electrodes prepared in each of Reference Examples 1 and 2 were cut to a size of 2.5 cm × 8 cm to prepare samples. In each sample, after separating the organic-inorganic composite layer from the positive electrode active material layer by approximately 10 to 20 mm, the organic-inorganic composite layer was fixed to the upper clamp, and the positive electrode active material layer was fixed to the lower clamp, with a distance of 20 mm between the clamps. The sample was then peeled off by pulling it in a 180° direction. The peeling speed was 20 mm / min. After peeling began, the force required to peel 40 mm was measured three times to obtain an average value. This average value was determined as the mean of the measurements. Adhesion was measured using UTM.

[0513] (4-2) Wet adhesion The electrodes prepared in each of Reference Examples 1 and 2 were cut into 2.5 cm × 8 cm dimensions to prepare samples. The prepared samples were placed in bags. 2.5 g of a mixed solvent containing dissolved LiPF6 in ethylene carbonate and methyl ethyl carbonate (volume ratio 50:50) was injected as the electrolyte, the bag was sealed, and placed at 25°C for 24 hours. Subsequently, the resulting samples were placed in a 50°C chamber under a pressure of 200 kgf for 2 hours. In the samples, after separating the organic-inorganic composite layer from the positive electrode active material layer by approximately 10 mm to 20 mm, the organic-inorganic composite layer was fixed to the upper clamp, and the positive electrode active material layer was fixed to the lower clamp, with a distance of 20 mm between the clamps. The samples were then peeled off by pulling them in a 180° direction. The peeling speed was 20 mm / min. After peeling began, the force required to peel 40 mm was measured three times to obtain the average value. This average value was determined as the mean of the measurements. Adhesion was measured using UTM.

[0514] (5) Electrolyte thermal shrinkage rate (unit: %): The electrodes (including the organic-inorganic composite layer, the positive electrode active material layer, and the aluminum foil) prepared in each of Reference Example 1 and Reference Example 2 were cut into 5cm × 5cm sizes to prepare samples. After removing the sample from the positive electrode, the sample was hot-pressed onto the negative electrode to seal it in a bag with the electrolyte, and then left for 24 hours to allow the electrolyte to fully impregnate the electrospun membrane. After placing the resulting bag in an oven at 150°C for 1 hour, the sample was removed from the bag to measure how much the size had decreased compared to the initial size (5cm × 5cm) on MD and TD, thereby calculating the thermal shrinkage rate. The thermal shrinkage rate was calculated using the following mathematical expression 1.

[0515] [Mathematical Expression 1] Thermal shrinkage rate = (L0 - L1) / L0 × 100 (L0 is the initial length of the organic-inorganic composite layer (5cm), and L1 is the length of the organic-inorganic composite layer after it has been placed at 150°C for 1 hour.) [Table 5]

[0516] As shown in Table 5, it can be seen that the organic-inorganic composite layer of Reference Example 1 provides favorable effects in terms of tensile strength, electrolyte wetting rate, dry adhesion, wet adhesion, and thermal shrinkage, and also provides a shut-off effect. Therefore, it can be expected that the multilayer organic-inorganic composite layer of the example will also provide favorable effects in terms of tensile strength, electrolyte wetting rate, dry adhesion, wet adhesion, and thermal shrinkage, and also provide a shut-off effect.

[0517] While preferred exemplary embodiments of the present disclosure have been described above, the present disclosure is not limited thereto, and various modifications can be made within the scope of the claims, the detailed description of the present disclosure, and the accompanying drawings. Clearly, these modifications also fall within the scope of the present disclosure.

Claims

1. An electrode for a rechargeable lithium battery, the electrode for the rechargeable lithium battery comprising: Active material layer for rechargeable lithium batteries; as well as The organic-inorganic composite layer is integrated with the active material layer. The organic-inorganic composite layer includes fibers, which contain polyvinylidene fluoride polymers, polyacrylonitrile polymers, and polysilsesquioxane.

2. The electrode according to claim 1, wherein, The fiber is an island fiber.

3. The electrode according to claim 2, wherein, The island fiber has a sea region and an island region. The sea region is composed of a polyvinylidene fluoride polymer, and the island region has a core-shell structure. The core-shell structure has a core composed of a polyacrylonitrile polymer and a shell surrounding the core composed of the polysilsesquioxane.

4. The electrode according to claim 2, wherein, In the island fiber, the island regions are randomly arranged in the sea region.

5. The electrode according to claim 2, wherein, In the cross-section of the island fiber, the area ratio of the island region is 30% to 50%.

6. The electrode according to claim 1, wherein, The polysilsesquioxane has substituted or unsubstituted aromatic groups.

7. The electrode according to claim 1, wherein, The polysilsesquioxane has crosslinkable functional groups.

8. The electrode according to claim 7, wherein, At least some of the crosslinkable functional groups in the fiber are crosslinked with each other.

9. The electrode according to claim 7, wherein, The crosslinkable functional group includes one or more of epoxy, glycidyl, glycidyloxy, and glycidyloxyalkyl groups.

10. The electrode according to claim 1, wherein, The polysilsesquioxane includes random, ladder, cage, or partially cage-like types.

11. The electrode according to claim 1, wherein, The polysilsesquioxane is ladder-shaped and is represented by the following chemical formula 8: [Chemical Formula 8] In chemical formula 8, R 7 R 8 R 9 and R 10 Each of these components is independently hydrogen, hydroxyl, C1 to C20 alkyl, C2 to C20 alkenyl, C2 to C20 alkynyl, C3 to C20 cycloalkyl, C6 to C20 aryl, C7 to C20 aralkyl, crosslinkable functional group, or a combination thereof. R 7 R 8 R 9 and R 10 At least one of them includes a crosslinkable functional group, and n is the number of moles in the unit.

12. The electrode according to claim 11, wherein, In chemical formula 8, R 7 R 8 R 9 and R 10 Each is independently phenyl, epoxy, glycidyl, glycidyloxy, or glycidyloxyalkyl, and R 7 R 8 R 9 and R 10 At least one of them includes an epoxy group, a glycidyl group, a glycidyloxy group, or a glycidyloxyalkyl group.

13. The electrode according to claim 1, wherein, The polyvinylidene fluoride polymer and the polyacrylonitrile polymer are included in the range of 50 to 90 parts by weight and 50 to 10 parts by weight, respectively, relative to a total of 100 parts by weight of the polyvinylidene fluoride polymer and the polyacrylonitrile polymer.

14. The electrode according to claim 13, wherein, The content of polysilsesquioxane is in the range of 5 to 50 parts by weight relative to the total amount of 100 parts by weight of the polyvinylidene fluoride polymer and the polyacrylonitrile polymer.

15. The electrode according to claim 1, wherein, The active material layer for the rechargeable lithium battery includes a negative electrode active material layer.

16. A rechargeable lithium battery, said rechargeable lithium battery comprising: Electrode for a rechargeable lithium battery according to any one of claims 1 to 15; as well as Electrode for rechargeable lithium battery, facing the electrode for rechargeable lithium battery.

17. The rechargeable lithium battery according to claim 16, wherein, The rechargeable lithium battery does not have a separator.

Citation Information

Patent Citations

  • Positive electrode active material for sodium secondary battery, method for preparing the same and sodium secondary battery including the same

    KR1020250064098A

  • Holographic optical device and transparent screen display device having the holographic optical device

    KR1020250064099A

  • Negative electrode active material for secondary battery, method for preparing the same and lithium secondary battery including the same

    KR1020250064100A

  • Method of synthesizing porous silica nanoparticles with transparency and low refractive properties

    KR1020250064101A