A double-layer ultra-thick negative electrode sheet with "bottom reinforcement for crack resistance and top buffer for liquid absorption" and its preparation method
By employing a dual-layer structure design and material partitioning, combined with stepwise pulping and gradient drying processes, the problems of drying cracking and interface failure in ultra-thick negative electrode sheets were solved, achieving a synergistic effect of high flexibility and strong anchoring, thus improving the overall performance of the battery.
Patent Information
- Application Number
- CN202611395420.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-09
- Publication Date
- 2026-11-17
AI Technical Summary
Ultra-thick negative electrode sheets are prone to problems such as drying cracking, rolling breakage, and bottom interface failure during preparation and use. Existing single binder systems cannot take into account both anchoring force and flexibility, resulting in battery performance degradation.
The design employs a dual-layer structure. The lower negative electrode active layer contains large-particle graphite, conductive carbon black, single-walled carbon nanotubes, and polyacrylic acid, forming a rigid and swelling-resistant system. The upper negative electrode active layer contains small-particle graphite, conductive carbon black, carboxymethyl cellulose, and styrene-butadiene rubber, forming a flexible buffer system. Through material partitioning and particle size partitioning design, combined with step-by-step pulping and gradient drying processes, the interfacial bonding strength and flexibility are ensured.
It significantly improves the crack resistance and interfacial stability of the electrode, reduces the microcrack initiation rate and peel strength, improves the cycle life and processing yield of the battery, and enhances the adsorption capacity of the electrolyte.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention relates to the field of lithium-ion battery technology, and in particular to a double-layer ultra-thick negative electrode sheet with "bottom reinforcement for crack resistance and top buffer for liquid absorption" and its preparation method. Background Technology
[0002] With the rapid development of new energy vehicles and the energy storage industry, the market is placing increasingly higher demands on the energy density and cycle life of lithium-ion batteries. Increasing the areal density of the electrode sheets is one of the most direct and effective ways to improve battery energy density; however, ultra-thick electrode sheets with an areal density ≥20 mg / cm³ are challenging to achieve. 2 However, lithium-ion batteries face severe failure issues during preparation and use, which seriously restricts their industrial application. Therefore, developing high-performance ultra-thick negative electrode sheets is of great significance for improving the battery life of lithium-ion batteries and promoting technological iteration in the new energy industry.
[0003] Currently, there are two main types of core failure mechanisms in the preparation and long-term use of ultra-thick negative electrode sheets. The first type is drying cracking and roll forming fracture: During the drying process of thick coating, the solvent evaporates directionally from the inside of the electrode sheet to the surface, and the binder migrates upward with the solvent and accumulates on the surface, resulting in a severe lack of binder in the bottom layer of the electrode sheet, forming a binder-deficient area, and the mechanical brittleness of the bottom material increases significantly; In the subsequent roll forming process, uneven strain occurs in the thickness direction of the electrode sheet, and the copper foil substrate interface has the strongest constraint and the most significant stress concentration. The binder-deficient bottom layer is very prone to microcracks, which extend upward from the interface and eventually cause the entire electrode sheet to fracture. At the same time, it becomes the starting point for active material shedding and performance degradation during battery charge and discharge cycles.
[0004] The second type is the bottom interface failure mode: During long-term battery cycling, byproducts generated by electrolyte decomposition will continuously accumulate on the side near the copper foil current collector; at the same time, the traditional negative electrode binder styrene-butadiene rubber is prone to oxidation and swelling under long-term high potential environment at the current collector interface, which leads to the failure of electrical contact between the active material and the current collector, ultimately causing the coating to peel off from the copper foil surface, forming visible black spots, and causing the battery capacity to drop rapidly.
[0005] To address these issues, the industry has explored various single-material system solutions, but all suffer from irreconcilable contradictions. Specifically, existing technologies have proposed using polyacrylic acid anode adhesive as the primary bonding material, combined with a carbon nanotube system. While the strong adhesion between the polyacrylic acid anode adhesive and the copper foil can mitigate bottom failure to some extent, the high rigidity of the polyacrylic acid anode adhesive's molecular chains leads to poor flexibility in the anode sheet, making it prone to large-area powder shedding during subsequent processing such as winding and stacking. Furthermore, the use of polyacrylic acid anode adhesive combined with carbon nanotubes significantly increases production costs.
[0006] Alternatively, using styrene-butadiene rubber as the main negative electrode binder, combined with a carboxymethyl cellulose composite carbon nanotube system, the resulting negative electrode sheet has good processability and excellent flexibility. However, it cannot compensate for the natural rubber deficiency in the bottom layer caused by the binder floating on the surface. Furthermore, the anchoring force between the bottom layer and the copper foil is insufficient, and the styrene-butadiene rubber has poor swelling resistance, making it difficult to fundamentally solve the problems of bottom layer cracking and black spot failure.
[0007] Therefore, there is an urgent need to develop a new type of negative electrode that can match the different failure characteristics of the upper and lower layers of ultra-thick electrode sheets, specifically address the problems of low-resin-content cracking and interface failure in the lower layer, while ensuring the overall processing performance of the electrode sheet and significantly improving the cycle life of the battery. Summary of the Invention
[0008] The purpose of this invention is to provide a double-layer ultra-thick negative electrode sheet with "bottom reinforcement for crack resistance and top buffer for liquid absorption" and its preparation method, so as to solve the technical problems of dry rolling and bottom layer cracking, black spot peeling at the interface during the cycling process, and the inability of a single binder system to take into account both anchoring force and flexibility in the existing ultra-thick negative electrode sheet.
[0009] The technical problem to be solved by this invention can be achieved through the following technical solution: In a first aspect, the present invention provides a double-layer ultra-thick negative electrode sheet with "bottom reinforcement for crack resistance and top buffer for liquid absorption", comprising a copper foil current collector and a lower negative electrode active layer and an upper negative electrode active layer sequentially stacked on the surface of the copper foil current collector. The ratio of the areal density of the upper negative electrode active layer to that of the lower negative electrode active layer is (5-7):(3-5); The lower negative electrode active layer contains large-particle graphite, conductive carbon black, single-walled carbon nanotubes, polyacrylic acid and 1,3-butanediol; the upper negative electrode active layer contains small-particle graphite, conductive carbon black, carboxymethyl cellulose and styrene-butadiene rubber.
[0010] Preferably, the mass ratio of large-particle graphite, conductive carbon black, single-walled carbon nanotubes, polyacrylic acid and 1,3-butanediol in the lower negative electrode active layer is (96.5-98):(0.4-1.2):(0.005-0.05):(1.0-2.2):(0.1-0.3).
[0011] Preferably, the mass ratio of small-particle graphite, conductive carbon black, carboxymethyl cellulose and styrene-butadiene rubber in the upper negative electrode active layer is (95.5-97.8):(0.2-0.8):(0.6-1.8):(1.4-2.5).
[0012] Preferably, the single-walled carbon nanotubes have a diameter of 1–3 nm, a length of 10–30 μm, an aspect ratio >1000, and a purity >95%.
[0013] Preferably, a single-walled carbon nanotube slurry is first prepared; the solid content of the single-walled carbon nanotube slurry is 0.55±0.1%, wherein the single-walled carbon nanotube content is 0.22±0.04%, and the dispersant content is 0.33±0.06%, wherein the dispersant includes one or more of sodium carboxymethyl cellulose, ammonium polyacrylate, or polyvinylpyrrolidone.
[0014] Preferably, the polyacrylic acid has a weight-average molecular weight of 600,000 to 800,000, a glass transition temperature (Tg) of 90 to 110°C, and a carboxyl content of ≥90%.
[0015] Preferably, the median particle size D50 of large-particle graphite is 10–20 μm; and the median particle size D50 of small-particle graphite is 3–8 μm.
[0016] Preferably, the glass transition temperature (Tg) of the styrene-butadiene rubber is ≤-12℃, the elongation at break is >350%, and the gel content is 60%~70%.
[0017] More preferably, the overall compaction density of the double-layer ultra-thick negative electrode sheet is 1.6–1.7 g / cm³. 3 Total surface density ≥20mg / cm³ 2 .
[0018] By adopting the above technical solution, the negative electrode sheet of the present invention has a bidirectional zero-crossing functional partition structure of "lower layer pure rigid swelling resistant system + upper layer pure flexible buffer system". The lower layer mainly uses polyacrylic acid as the main binder component. The high carboxyl content of polyacrylic acid can form strong hydrogen bond anchoring with the oxide on the surface of copper foil. Its high glass transition temperature ensures that no plastic deformation and swelling degradation occur in the electrolyte environment. It chemically blocks the path of oxidation failure of traditional binders, thereby significantly improving the adhesion between the binder and the copper foil current collector, fundamentally eliminating the problems of bottom layer cracking and interface black spots. The upper layer mainly uses styrene-butadiene rubber as the main binder component. The low glass transition temperature and high gel content of styrene-butadiene rubber provide sufficient elastic deformation space and capillary liquid retention capacity for the upper layer, which can make up for the problem of excessive rigidity of polyacrylic acid binder and avoid the influence of rigid materials on the overall flexibility of the negative electrode sheet.
[0019] In the lower negative electrode active layer, this invention introduces large-particle graphite as a rigid framework to reduce the specific surface area, thereby reducing the need for binder. At the same time, single-walled carbon nanotubes, with their extremely high aspect ratio, interweave and overlap in the interparticle gaps to form a steel-like network, which together with the molecular chains of polyacrylic acid constitutes a "chain-network" composite anchoring system. This system coats the large-particle graphite at multiple points and strongly bonds it to the copper foil interface, fundamentally compensating for the lack of binder in the bottom layer caused by the binder floating during the drying process. Meanwhile, the introduced 1,3-butanediol acts as an anti-cracking agent, playing a plasticizing and slow-release role during solvent evaporation, reducing the drying stress caused by uneven capillary forces, and inhibiting the initiation of microcracks at the copper foil interface.
[0020] In the upper negative electrode active layer, the present invention introduces small-particle graphite. Small-particle graphite can provide a larger specific surface area and more pore channels to enhance the electrolyte adsorption and liquid retention capacity. The flexible bonding system composed of carboxymethyl cellulose and styrene-butadiene rubber has a high elongation at break, which can absorb the volume expansion stress during the charging and discharging process and avoid problems such as powder shedding in subsequent processing due to excessive rigidity of the electrode sheet.
[0021] This invention achieves a synergistic amplification effect through the partitioning design of graphite particle size in the upper and lower layers and the bidirectional isolation of the material system. The large-particle skeleton in the lower layer reduces stress concentration, while the small-particle body in the upper layer improves liquid absorption efficiency. The large-particle graphite has a lower specific surface area, which reduces the consumption of polyacrylic acid. Even if the binder floats to the surface during drying, the remaining amount of adhesive can still maintain the stability of the underlying structure. The small-particle graphite has more pore channels, which can provide more adsorption sites for electrolyte. Combined with the high gelation properties of styrene-butadiene rubber, it can further lock in and retain the electrolyte. The dual combination of particle size partitioning and material partitioning further amplifies the gain effect of functional partitioning, fundamentally solving the contradiction of "insufficient bottom-layer anchoring and insufficient overall flexibility" in ultra-thick electrodes.
[0022] Secondly, the present invention provides a method for preparing the above-mentioned "bottom-reinforced crack-resistant, top-buffered liquid-absorbing" double-layer ultra-thick negative electrode sheet, comprising the following steps: S1. Preparation and Pre-forming of Lower Layer Slurry: Polyacrylic acid powder is added to deionized water to prepare a polyacrylic acid solution with a solid content of 1% to 3%. Single-walled carbon nanotubes and dispersant are added to deionized water to prepare a single-walled carbon nanotube slurry. Large-particle graphite, conductive carbon black, single-walled carbon nanotube slurry and deionized water are kneaded and stirred. 10% to 30% of the total amount of polyacrylic acid solution is added and dispersed at high speed for 0.5 to 2 hours. The remaining polyacrylic acid solution is then added, and the slurry viscosity is adjusted to 4000 to 8000 mPa·s. 1,3-Butanediol, an anti-cracking agent, is added, and the mixture is degassed under vacuum to obtain the lower layer slurry. The lower layer slurry is uniformly coated on the surface of the copper foil current collector and pre-dried at 80 to 100°C until there is no flowing slurry on the surface to form the lower negative electrode active layer. S2. Preparation of upper slurry: Small-particle graphite, carboxymethyl cellulose, conductive carbon black and deionized water are stirred. Styrene and butadiene are added to deionized water and emulsifier, and emulsion polymerization is carried out. The pH is adjusted to 7-9 to prepare a styrene-butadiene rubber emulsion with a solid content of 40%-50%. The emulsion is dispersed by high-speed stirring for 0.5-2 hours. The viscosity of the slurry is adjusted to 3000-6000 mPa·s. Vacuum degassing is performed to obtain the upper slurry. S3. Double-layer coating and post-treatment: The upper slurry is uniformly coated onto the surface of the pre-dried lower negative electrode active layer. It is then dried in stages at 100–120℃ to form the upper negative electrode active layer. After drying, the electrode moisture content is ≤0.1%. Subsequently, cold pressing is performed, controlling the overall compaction density to be 1.6–1.7 g / cm³. 3 .
[0023] Preferably, the segmented drying in step S3 includes: first drying at 100-110°C for 2-4 minutes, and then drying at 110-120°C for 1-3 minutes; the cold pressing is roller pressing, and the roller temperature is 15-25°C.
[0024] By adopting the above technical solution, the preparation method of the present invention employs a stepwise slurry preparation and gradient drying process. Firstly, in the preparation of the slurry for the lower negative electrode active layer, 10%–30% polyacrylic acid is added for pre-dispersion, followed by the addition of the remaining polyacrylic acid to adjust the viscosity. This allows for the initial wetting of the surface of large graphite particles with a small amount of polyacrylic acid, preventing the agglomeration of single-walled carbon nanotubes with the graphite. Subsequent addition of polyacrylic acid adhesive forms a uniform bonding network, ensuring the dispersion stability of the lower slurry. Adding all the polyacrylic acid adhesive at once can easily lead to the agglomeration of graphite and single-walled carbon nanotubes, reducing dispersion uniformity and affecting the consistency of the underlying network. If the initial addition ratio is less than 10%, the pre-dispersion effect is insufficient, and particle agglomeration will still occur. If it is higher than 30%, the slurry viscosity will increase prematurely, which is detrimental to subsequent high-speed dispersion.
[0025] The pre-drying process allows only the surface of the lower negative electrode active layer to be cured, preserving the active groups at the interlayer interface and ensuring the interfacial bonding strength after the upper and lower layers are coated, thus avoiding double-layer peeling. If the pre-drying temperature is below 80℃, the solvent will evaporate too slowly, resulting in low production efficiency. If it is above 100℃, the polyacrylic acid will cure prematurely, leading to a decrease in the interfacial bonding strength between the upper and lower layers and making double-layer peeling more likely.
[0026] Meanwhile, adding 1,3-butanediol in the final stage of the lower slurry avoids its premature participation in the dispersion reaction, thus preserving its stress-relieving function to the greatest extent. Furthermore, the preparation method does not introduce any toxic or harmful solvents throughout the process, is simple and controllable, and is suitable for the large-scale production needs of existing lithium battery production lines.
[0027] During the formation of the upper negative electrode active layer, a segmented drying process is adopted. The initial low-temperature stage prevents surface crusting, while the subsequent high-temperature stage thoroughly removes deep moisture. If the initial drying temperature exceeds 110℃, the surface solvent evaporates too quickly, easily forming a hard shell that hinders the discharge of internal solvent, leading to electrode blistering. If the subsequent drying temperature is below 110℃, the deep solvent cannot be completely removed, resulting in excessive moisture content in the electrode and affecting electrochemical performance. Simultaneously, segmented drying allows for the rapid removal of free solvent from the electrode surface before slowly removing the deep bound water, preventing rapid solvent evaporation that could cause electrode peeling and blistering. Low-temperature cold pressing prevents the styrene-butadiene rubber from softening and sticking to the rollers due to heat, ensuring uniform and controllable compaction density and improving the thickness consistency of the electrode. The beneficial effects of this invention are: 1. The dual-layer functional partition structure constructed in this invention combines the strong anchoring and swelling resistance of the lower polyacrylic acid / single-walled carbon nanotube system with the high flexibility and excellent liquid absorption of the upper carboxymethyl cellulose / styrene-butadiene rubber system. Through strict isolation of the material system, the problem of interface black spots caused by oxidation and swelling of styrene-butadiene rubber is eliminated from the root. At the same time, the processing powdering defect caused by full-layer polyacrylic acid is avoided, and the long-standing problem of bottom-layer cracking and interface peeling coupling failure of ultra-thick electrode sheets is solved.
[0028] 2. This invention utilizes a rigid cross-linked network formed by high aspect ratio single-walled carbon nanotubes and polyacrylic acid in the lower layer, combined with the stress-relieving effect of 1,3-butanediol, to significantly improve the crack resistance of the bottom layer. The microcrack initiation rate during rolling is reduced by more than 60%, the peel strength is increased by more than 20% compared with the existing double-layer scheme, and the thickness rebound rate is reduced by more than 32%, which significantly improves the processing yield and structural stability of the electrode sheet.
[0029] 3. This invention achieves differentiated zoning of graphite particle size by using large-particle graphite to construct the mechanical framework in the lower layer and small-particle graphite to construct the liquid-absorbing body in the upper layer. Large-particle graphite significantly reduces the specific surface area, decreasing the consumption of polyacrylic acid binder, while small-particle graphite has a large specific surface area and abundant pore channels, providing more adsorption sites and wetting paths for the electrolyte. The particle size zoning and the bidirectional isolation of the material system create a synergistic effect, further enhancing the functional effects of lower layer reinforcement against cracking and upper layer buffering and liquid absorption. Detailed Implementation
[0030] The specific embodiments of the present invention will be described in detail below, but it should be understood that the scope of protection of the present invention is not limited to the specific embodiments.
[0031] Example Example 1: A double-layer ultra-thick negative electrode sheet with "bottom reinforcement for crack resistance and top buffer for liquid absorption" was prepared according to the following method: S1. Preparation and Pre-forming of Lower Layer Slurry: Polyacrylic acid powder with a weight-average molecular weight of 700,000, a glass transition temperature of 100℃, and a carboxyl content of 92% was added to deionized water to prepare a polyacrylic acid adhesive with a solid content of 2%. Single-walled carbon nanotubes (diameter 2nm, length 20μm, aspect ratio >1000, purity >95%) and dispersant polyvinylpyrrolidone were added to deionized water to prepare a single-walled carbon nanotube slurry with a solid content of 0.55%, wherein the single-walled carbon nanotube content was 0.22% and the dispersant polyvinylpyrrolidone content was 0.33%. Large-particle graphite with a D50 of 15μm and a specific surface area of 65m² was added. 2 Conductive carbon black and single-walled carbon nanotube slurry with a DBP absorption value of 180 mL / 100 g were kneaded and stirred with deionized water. 20% of the total amount of polyacrylic acid adhesive was added and dispersed at high speed for 1 hour. The remaining polyacrylic acid adhesive was then added, and the slurry viscosity was adjusted to 6000 mPa·s. 0.2% of the total mass of 1,3-butanediol was added, and the mixture was degassed under vacuum to obtain the lower layer slurry. The addition amounts of single-walled carbon nanotubes, polyacrylic acid, and conductive carbon black were controlled to be 0.05% of the total mass of the lower layer, 1.5%, and 0.8%, respectively. The lower layer slurry was uniformly coated onto the surface of an 8 μm copper foil current collector and pre-dried at 90°C until no more slurry flowed on the surface.
[0032] S2. Preparation of the upper slurry: Small-particle graphite with D50=5μm, carboxymethyl cellulose with a viscosity of 800mPa·s, and deionized water were kneaded and stirred; styrene and butadiene were added to deionized water and rosin acid soap and emulsion polymerized, and the pH was adjusted to 8 to prepare a styrene-butadiene rubber emulsion with a solid content of 45%. The styrene-butadiene rubber emulsion (glass transition temperature of -15℃, elongation at break of 400%, gel content of 65%) was dispersed by high-speed stirring for 1h, and the slurry viscosity was adjusted to 4500mPa·s. Vacuum degassing was performed to obtain the upper slurry; the amount of styrene-butadiene rubber added was controlled to be 1.4% of the total mass of the upper layer, the amount of carboxymethyl cellulose added was 1.0% of the total mass of the upper layer, and the amount of conductive carbon black added was 0.8% of the total mass of the upper layer.
[0033] S3. Double-layer coating and post-treatment: The upper slurry is uniformly coated onto the pre-dried lower surface, with an upper layer density to lower layer density ratio of 5:5. It is first dried at 105℃ for 3 minutes, then dried at 115℃ for 2 minutes to form the upper negative electrode active layer. After drying, the electrode moisture content is ≤0.1%. Subsequently, it is cold-pressed at 20℃ to control the overall compaction density to 1.65 g / cm³. 3 The total surface density is 22 mg / cm³. 2 .
[0034] Example 2 is a double-layer ultra-thick negative electrode sheet with "bottom reinforcement for crack resistance and top buffer for liquid absorption". The only difference from Example 1 is that the amount of single-walled carbon nanotube slurry added accounts for 0.005% of the total mass of the lower layer.
[0035] Example 3 is a double-layer ultra-thick negative electrode sheet with "bottom reinforcement for crack resistance and top buffer for liquid absorption". The only difference between it and Example 1 is that the density ratio of the upper layer to the lower layer is 7:3.
[0036] Comparative Example Comparative Example 1: A negative electrode sheet was prepared according to the following method: S1. Preparation and Pre-forming of Lower Layer Slurry: Large-particle graphite with D50=15μm and a specific surface area of 65m² is used... 2 Conductive carbon black with a DBP absorption value of 180 mL / 100 g and deionized water were kneaded and stirred. Carboxymethyl cellulose (viscosity 800 mPa·s) was added, and styrene and butadiene were added to deionized water and rosin soap for emulsion polymerization. The pH was adjusted to 8 to prepare a styrene-butadiene rubber emulsion with a solid content of 45%. The styrene-butadiene rubber emulsion (glass transition temperature -15℃, elongation at break 400%, gel content 65%, solid content 45%) was mixed and dispersed at high speed for 1 h. The viscosity of the slurry was adjusted to 6000 mPa·s, and vacuum degassing was performed to obtain the lower layer slurry. The amount of styrene-butadiene rubber added was controlled to be 1.4% of the total mass of the lower layer, the amount of carboxymethyl cellulose added was 1.0% of the total mass of the lower layer, and the amount of conductive carbon black added was 0.8% of the total mass of the lower layer. The lower layer slurry was uniformly coated on the surface of an 8 μm copper foil current collector and pre-dried at 90℃ until there was no flowing slurry on the surface.
[0037] S2. Preparation of the upper slurry: Single-walled carbon nanotubes (diameter 2nm, length 20μm, aspect ratio >1000, purity >95%) and dispersant polyvinylpyrrolidone were added to deionized water to prepare a single-walled carbon nanotube slurry with a solid content of 0.55%, of which the single-walled carbon nanotube content was 0.22% and the dispersant polyvinylpyrrolidone content was 0.33%. Small-particle graphite with D50=5μm, conductive carbon black, single-walled carbon nanotube slurry, and deionized water were kneaded and stirred, and polyacrylic acid adhesive (weight evenly distributed) was added. 20% of the total mass of the slurry (700,000 molecules, glass transition temperature 100℃, carboxyl content 92%, solid content 2%) was stirred and dispersed at high speed for 1 hour. Then, the remaining polyacrylic acid adhesive was added, and the viscosity of the slurry was adjusted to 4500 mPa·s. 0.2% of the total mass of the upper layer of 1,3-butanediol was added, and the mixture was degassed under vacuum to obtain the upper layer slurry. The amount of single-walled carbon nanotubes added was controlled to be 0.05% of the total mass of the upper layer, the amount of polyacrylic acid added was 1.5% of the total mass of the upper layer, and the amount of conductive carbon black added was 0.8% of the total mass of the upper layer.
[0038] S3. Double-layer coating and post-treatment: The upper slurry is uniformly coated onto the pre-dried lower surface, with an upper layer density to lower layer density ratio of 5:5. It is first dried at 105℃ for 3 minutes, then dried at 115℃ for 2 minutes to form the upper negative electrode active layer. After drying, the electrode moisture content is ≤0.1%. Subsequently, it is cold-pressed at 20℃ to control the overall compaction density to 1.65 g / cm³. 3 The total surface density is 22 mg / cm³. 2 .
[0039] Comparative Example 2: A negative electrode sheet was prepared according to the following method: Single-walled carbon nanotubes (diameter 2 nm, length 20 μm, aspect ratio > 1000, purity > 95%) and dispersant polyvinylpyrrolidone were added to deionized water to prepare a slurry with a solid content of 0.55% single-walled carbon nanotubes, of which the single-walled carbon nanotube content was 0.22% and the dispersant polyvinylpyrrolidone content was 0.33%. Graphite with a D50 of 8 μm and a specific surface area of 65 m² was also added. 2 The following are the ingredients: conductive carbon black with a DBP absorption value of 180 mL / 100 g, single-walled carbon nanotube slurry, polyacrylic acid powder (weight average molecular weight 700,000, glass transition temperature 100℃, carboxyl content 92%), carboxymethyl cellulose (viscosity 800 mPa·s), and styrene-butadiene rubber latex (glass transition temperature -15℃, elongation at break 400%, gel content 65%, solid content 45%). The styrene-butadiene rubber latex is prepared by adding styrene and butadiene to deionized water and rosin acid soap, emulsion polymerization, and adjusting the pH to 8 to prepare a styrene-butadiene rubber latex with a solid content of 45%. Finally, it is kneaded and stirred with deionized water.
[0040] The mixture was stirred and dispersed at high speed for 1 hour, and the viscosity of the slurry was adjusted to 5000 mPa·s. Vacuum degassing was performed to obtain a mixed slurry. The amount of single-walled carbon nanotubes added was controlled to be 0.05% of the total mass, polyacrylic acid to be 1.5% of the total mass, styrene-butadiene rubber to be 1.4% of the total mass, carboxymethyl cellulose to be 1.0% of the total mass, and conductive carbon black to be 0.8% of the total mass.
[0041] The mixed slurry was uniformly coated onto the surface of an 8μm copper foil current collector, and then dried at 105℃ for 3 minutes, followed by drying at 115℃ for 2 minutes to form the upper negative electrode active layer. After drying, the moisture content of the electrode sheet was ≤0.1%. Subsequently, it was cold-pressed by roller pressing at 20℃ to control the overall compaction density to 1.65 g / cm³. 3 The total surface density is 22 mg / cm³. 2 .
[0042] Comparative Example 3, a negative electrode sheet, differs from Example 1 only in that: no single-walled carbon nanotube slurry is added to the lower negative electrode active layer.
[0043] Comparative Example 4, a negative electrode sheet, differs from Example 1 only in that the anti-cracking agent 1,3-butanediol is not added to the lower slurry.
[0044] Comparative Example 5, a negative electrode sheet, differs from Example 1 only in that the upper active layer uses the same large-particle graphite (D50=15μm) as the lower layer.
[0045] Comparative Example 6 is a negative electrode sheet, which differs from Example 1 only in that the particle size division of the upper and lower layers of graphite is reversed, that is, the lower layer uses small-particle graphite (D50=5μm) and the upper layer uses large-particle graphite (D50=15μm).
[0046] Performance testing 1. Peel strength test: The 180° peel test method was used. The negative electrode sheets obtained in the examples and comparative examples were cut into 25mm×100mm samples. The active material layer of the electrode sheet was attached to a stainless steel plate with 3M tape. The sample was peeled along the 180° direction at a speed of 50mm / min using a universal tensile testing machine. The peel force was recorded and divided by the width. The result is expressed in N / m and is used to evaluate the interfacial bonding force between the active material layer and the copper foil current collector.
[0047] 2. Bending performance test: The electrode sheet is cut into 20mm×100mm samples and bent 180° with a cylindrical core with a diameter of 2mm. The maximum number of bends when the active material layer at the bend point of the electrode sheet shows visible cracks or powder falling off is recorded, and is expressed as the number of bends.
[0048] 3. Resistivity test: The surface resistivity and volume resistivity of the electrode are tested using the four-probe method, and the results are expressed in Ω·cm.
[0049] 4. Thickness rebound rate test: Test the change in electrode thickness 48 hours after rolling and after full charge, and calculate the thickness rebound rate. Thickness rebound rate = (thickness after full charge - thickness after rolling) / thickness after rolling × 100%, and the result is expressed as %.
[0050] 5. Rate performance test: The negative electrode obtained from the examples and comparative examples was assembled with the lithium iron phosphate positive electrode to form a 2032 coin cell. Charge and discharge tests were conducted at current densities of 0.2C, 0.5C, 1C, 2C, 3C and 4C respectively. The capacity retention rate at each rate was recorded. The capacity retention rate (%) at each rate was calculated based on the discharge specific capacity at 0.2C.
[0051] 6. Cycle life test: Assemble the negative electrode and the lithium iron phosphate positive electrode into a 2032 coin cell, and conduct constant current charge and discharge cycle test at 25°C with a current density of 1C / 1C. Record the capacity retention rate (%) at different cycle numbers.
[0052] 7. High and low temperature performance test: Assemble the negative electrode and the lithium iron phosphate positive electrode into a 2032 coin cell and conduct discharge tests at temperatures of -20℃, 0℃, 25℃, 45℃ and 60℃ respectively. Record the capacity retention rate (%) at each temperature. Calculate the capacity retention rate (%) at each temperature based on the discharge specific capacity at 25℃.
[0053] The results of the above experiments are shown in Tables 1 to 4: Table 1 Physical performance data
[0054] Table 2 Rate Performance
[0055] Table 3 Cyclic Performance
[0056] Table 4 Temperature Performance
[0057] Based on the physical performance data in Table 1 and in conjunction with Examples 1 to 3, it can be seen that all embodiments of the present invention exhibit excellent comprehensive physical properties. Example 1 shows the best peel strength (195.37 N / m), resistivity (as low as 4.02 Ω·cm), and thickness rebound rate (only 4.6%) among all samples. This is because the lower layer of polyacrylic acid forms strong hydrogen bonds with the copper foil surface, 0.05% single-walled carbon nanotubes construct a continuous conductive reinforcing network to suppress microcrack propagation, 1,3-butanediol moderates the drying stress of the bottom layer, and the upper layer of carboxymethyl cellulose / styrene-butadiene rubber provides high flexibility and buffering. The synergistic effect of the two layers achieves a balance between strong anchoring and high flexibility. In Example 2, the single-walled carbon nanotube content is reduced to 0.005%, the continuity of the conductive network weakens, the resistivity increases to 4.52 Ω·cm, and the peel strength and rebound rate slightly deteriorate. In Example 3, the ratio of the upper and lower layers becomes 7:3, and the increased flexibility of the upper layer leads to a decrease in peel strength to 176.50 N / m.
[0058] Combining Example 1 with Comparative Examples 1 to 3, it can be seen that after the system in Comparative Example 1 was interchanged, the lower layer lacked polyacrylic acid anchoring, and the peel strength was only 162.89 N / m; in Comparative Example 2, the single-layer mixed system of polyacrylic acid and styrene-butadiene rubber interfered with each other, the peel strength was only 85.20 N / m, it cracked and shed powder after one bend, and the rebound rate was as high as 12.8%; in Comparative Example 3, the lower layer lacked single-walled carbon nanotubes, and the resistivity increased to 8.20 Ω·cm.
[0059] As can be seen from Comparative Examples 4 to 6, in Comparative Example 4, without the addition of anti-cracking additives, the microcrack defects in the bottom layer reduced the bending performance to 2-times cracking and increased the rebound rate to 7.5%. In Comparative Example 5, the use of large-particle graphite in the upper layer reduced the liquid absorption capacity, and the bending performance decreased to 2-times cracking. In Comparative Example 6, after the particle size partitioning was reversed, the lower layer of small-particle graphite was densely packed, the mass transfer channels were narrowed, and the resistivity increased to 4.45 Ω·cm. This indicates that the particle size partitioning design of the lower layer of large particles and the upper layer of small particles in this invention has a synergistic effect with the material partitioning design.
[0060] Based on the rate performance data and considering Examples 1 to 3, it can be seen that Example 1 performed best at all rate ratios, maintaining a capacity retention of 46.78% at 4C. This is because the high aspect ratio conductive network of single-walled carbon nanotubes ensures rapid electron transport, large graphite particles provide unobstructed lithium-ion channels in the lower layer, and small graphite particles in the upper layer ensure a high liquid absorption rate. The bilayer structure achieves rapid mass transfer at high rate ratios. In Example 2, the reduction in single-walled carbon nanotubes hindered electron transport at high rate ratios, causing the 4C to drop to 41.5%. In Example 3, the increased proportion of the upper layer improved the liquid absorption rate, achieving 4C at 43.0%, slightly better than Example 2.
[0061] Combining Example 1 with Comparative Examples 1 to 3, it can be seen that after the system of Comparative Example 1 is interchanged, the lower layer lacks polyacrylic acid / single-walled carbon nanotubes to anchor the conductive network, and the 4C is only 40.37%, and the interface deterioration is aggravated at high magnification; the single-layer mixed system of Comparative Example 2 has the worst mass transfer, with a 4C of only 33.5%; the absence of single-walled carbon nanotubes in Comparative Example 3 results in the highest sheet resistance, with a 4C of only 37.5%.
[0062] Comparative Example 4 shows that microcracks in the bottom layer increase interfacial resistance, resulting in a 4C value of 40.8%. Comparative Example 5 shows that the large particles in the upper layer do not absorb enough liquid, causing the 4C value to drop to 40.5%. Comparative Example 6 shows that after the particle size partitioning is reversed, the mass transfer of small particles in the lower layer is hindered, causing the 4C value to drop to 39.5%. This indicates that the SWCNT conductive network and particle size partitioning design have a decisive influence on high-rate performance.
[0063] Based on the cycling performance data, combined with Examples 1 to 3, it can be seen that Example 1 achieved a capacity retention rate of 86.64% after 2500 cycles, the highest among all samples. This is because the strong anchoring of polyacrylic acid ensures that the active material and the current collector maintain electrical contact throughout the long cycle; the single-walled carbon nanotube network inhibits the propagation of microcracks in the underlying layer; 1,3-butanediol eliminates stress defects in the underlying layer; and the upper carboxymethyl cellulose / styrene-butadiene rubber buffers volume expansion. The synergistic effect of the two layers ensures long-term stability of the interface structure. In Example 2, the reduction in single-walled carbon nanotubes led to the gradual failure of the conductive pathways during long cycles, decreasing to 84.2% after 2500 cycles. In Example 3, the thinning of the lower anchoring layer accelerated the decay in the later stages of cycling, reaching 85.2% after 2500 cycles.
[0064] Combining Example 1 with Comparative Examples 1 to 3, it can be seen that in Comparative Example 1, the lower layer lacks polyacrylic acid anchoring and SBR oxidation swelling leads to black spots (8.5%), with only 84.13% after 2500 cycles; in Comparative Example 2, the single-layer mixed system has an uneven bonding network, with only 77.5% after 2500 cycles; and in Comparative Example 3, the lack of single-walled carbon nanotubes leads to a missing conductive network and insufficient crack resistance of the bottom layer, with only 80.0% after 2500 cycles.
[0065] In Comparative Example 4, the bottom layer microcracks continued to propagate under cyclic stress, with only 82.8% remaining after 2500 cycles; in Comparative Example 5, insufficient liquid absorption by the upper large particles led to accelerated long-cycle decay, with 80.5% remaining after 2500 cycles; and in Comparative Example 6, the mass transfer of the lower small particles was hindered after the particle size partitioning was reversed, with 81.0% remaining after 2500 cycles. This indicates that the integrity of the particle size partitioning design is the structural basis for ensuring long-cycle stability.
[0066] Based on the high and low temperature performance data, combined with Examples 1 to 3, it can be seen that the capacity of each sample in the high-temperature region is higher than that at room temperature with little difference. This is because the high temperature increases the ionic conductivity of the electrolyte, partially masking the structural differences. In the low-temperature region, the differences are significantly amplified. Example 1 achieved a capacity retention of 18.24% at -20℃, the best among all samples. This is because the single-walled carbon nanotubes maintain excellent electronic conductivity at low temperatures, PAA anchoring ensures that the interface does not peel off due to thermal shrinkage, 1,3-butanediol eliminates underlying stress defects, and the upper layer of low glass transition temperature styrene-butadiene rubber (-15℃) provides elastic buffering, ensuring structural integrity and smooth charge transport at low temperatures. In Example 2, the reduction in single-walled carbon nanotubes lowered the capacity retention to 16.5% at -20℃; in Example 3, increased upper layer flexibility facilitated low-temperature liquid absorption, reaching 17.2% at -20℃.
[0067] Combining Example 1 with Comparative Examples 1 to 3, it can be seen that the lower layer of Comparative Example 1 uses a carboxymethyl cellulose / styrene-butadiene rubber system. At low temperatures, the carboxymethyl cellulose becomes brittle and the elasticity of the styrene-butadiene rubber decreases, reaching only 12.74% at -20℃. The monolayer mixed system in Comparative Example 2 exhibits the most severe low-temperature polarization, reaching only 11.0% at -20℃. Comparative Example 3, lacking a single-walled carbon nanotube conductive network, suffers severe electron transport obstruction at low temperatures, reaching 15.0% at -20℃.
[0068] In Comparative Example 4, the electrolyte penetration was hindered by microcracks in the bottom layer at low temperatures, reaching 16.8% at -20℃. In Comparative Example 5, the large particles in the upper layer had a small specific surface area and poor liquid absorption capacity, resulting in insufficient electrolyte wetting at low temperatures, dropping to 14.5% at -20℃. In Comparative Example 6, the dense accumulation of small graphite particles in the lower layer led to greater resistance to lithium ion diffusion in the narrow channels at low temperatures, reaching 14.8% at -20℃. This indicates that the synergistic effect of the lower single-walled carbon nanotube / polyacrylic acid conductive anchoring network and the upper low glass transition temperature styrene-butadiene rubber flexible buffer layer is key to ensuring the wide temperature range adaptability of the electrode.
[0069] The above-disclosed embodiments are merely a few specific examples of the present invention. However, the embodiments of the present invention are not limited thereto, and any variations that can be conceived by those skilled in the art should fall within the protection scope of the present invention.
Claims
1. A double-layer ultra-thick negative electrode sheet with "bottom reinforcement for crack resistance and top buffer for liquid absorption", characterized in that, It includes a copper foil current collector and a lower negative electrode active layer and an upper negative electrode active layer sequentially stacked on the surface of the copper foil current collector; The ratio of the areal density of the upper negative electrode active layer to that of the lower negative electrode active layer is (5-7):(3-5); The lower negative electrode active layer comprises large-particle graphite, conductive carbon black, single-walled carbon nanotubes, polyacrylic acid, and 1,3-butanediol; the upper negative electrode active layer comprises small-particle graphite, conductive carbon black, carboxymethyl cellulose, and styrene-butadiene rubber.
2. The double-layer ultra-thick negative electrode sheet with "bottom reinforcement for crack resistance and top buffer for liquid absorption" as described in claim 1, characterized in that, The mass ratio of large-particle graphite, conductive carbon black, single-walled carbon nanotubes, polyacrylic acid and 1,3-butanediol in the lower negative electrode active layer is (96.5-98):(0.4-1.2):(0.005-0.05):(1.0-2.2):(0.1-0.3).
3. The double-layered ultra-thick negative electrode sheet of claim 1, wherein the negative electrode sheet is characterized by the fact that the negative electrode sheet is reinforced at the lower part thereof to prevent cracking and is cushioned at the upper part thereof to absorb liquid. 3 The mass ratio of small-particle graphite, conductive carbon black, carboxymethyl cellulose and styrene-butadiene rubber in the upper negative electrode active layer is (95.5-97.8): (0.2-0.8): (0.6-1.8): (1.4-2.5).
4. The double-layered ultra-thick negative electrode sheet of claim 1, wherein the negative electrode sheet is characterized by the fact that the negative electrode sheet is reinforced at the lower part thereof to prevent cracking and is cushioned at the upper part thereof to absorb liquid. The single-walled carbon nanotubes have a diameter of 1–3 nm, a length of 10–30 μm, an aspect ratio >1000, and a purity >95%.
5. The double-layer ultra-thick negative electrode sheet with bottom reinforcement for crack resistance and top buffer for liquid absorption as described in claim 1, characterized in that, The single-walled carbon nanotubes are first prepared into a single-walled carbon nanotube slurry; the solid content of the single-walled carbon nanotube slurry is 0.55±0.1%, wherein the single-walled carbon nanotube content is 0.22±0.04%, and the dispersant content is 0.33±0.06%, wherein the dispersant includes one or more of sodium carboxymethyl cellulose, ammonium polyacrylate, or polyvinylpyrrolidone.
6. The double-layer ultra-thick negative electrode sheet with "bottom reinforcement for crack resistance and top buffer for liquid absorption" as described in claim 1, characterized in that, The polyacrylic acid has a weight-average molecular weight of 600,000 to 800,000, a glass transition temperature (Tg) of 90 to 110°C, and a carboxyl content of ≥90%.
7. The double-layer ultra-thick negative electrode sheet with "bottom reinforcement for crack resistance and top buffer for liquid absorption" as described in claim 1, characterized in that, The styrene-butadiene rubber has a glass transition temperature Tg ≤ -12℃, an elongation at break >350%, and a gel content of 60% to 70%.
8. The double-layer ultra-thick negative electrode sheet with "bottom reinforcement for crack resistance and top buffer for liquid absorption" as described in claim 1, characterized in that, The median particle size D50 of the large-particle graphite is 10–20 μm; the median particle size D50 of the small-particle graphite is 3–8 μm.
9. A method for preparing a double-layer ultra-thick negative electrode sheet with "bottom reinforcement for crack resistance and top buffer for liquid absorption", characterized in that, Includes the following steps: S1. Preparation and Pre-forming of Lower Layer Slurry: Polyacrylic acid is added to deionized water to prepare a polyacrylic acid solution with a solid content of 1% to 3%. Single-walled carbon nanotubes and dispersants are added to deionized water to prepare a single-walled carbon nanotube slurry. Large-particle graphite, conductive carbon black, single-walled carbon nanotube slurry and deionized water are kneaded and stirred. 10% to 30% of the total amount of polyacrylic acid solution is added and dispersed at high speed for 0.5 to 2 hours. The remaining polyacrylic acid solution is then added, and the slurry viscosity is adjusted to 4000 to 8000 mPa·s. 1,3-Butanediol is added, and the mixture is degassed under vacuum to obtain the lower layer slurry. The lower layer slurry is uniformly coated on the surface of the copper foil current collector and pre-dried at 80 to 100°C until there is no flowing slurry on the surface to form the lower negative electrode active layer. S2. Preparation of upper slurry: Small-particle graphite, carboxymethyl cellulose, conductive carbon black and deionized water are stirred. Styrene and butadiene are added to deionized water and emulsifier, and emulsion polymerization is carried out. The pH is adjusted to 7-9 to prepare a styrene-butadiene rubber emulsion with a solid content of 40%-50%. The emulsion is dispersed by high-speed stirring for 0.5-2 hours. The viscosity of the slurry is adjusted to 3000-6000 mPa·s. Vacuum degassing is performed to obtain the upper slurry. S3. Double-layer coating and post-treatment: The upper slurry is uniformly coated onto the surface of the pre-dried lower negative electrode active layer. It is then dried in stages at 100–120℃ to form the upper negative electrode active layer. After drying, the electrode moisture content is ≤0.1%. Subsequently, cold pressing is performed, controlling the overall compaction density to be 1.6–1.7 g / cm³. 3 .
10. The method for preparing a double-layer ultra-thick negative electrode sheet with "bottom reinforcement for crack resistance and top buffer for liquid absorption" according to claim 9, characterized in that, The segmented drying in step S3 includes: first drying at 100-110℃ for 2-4 minutes, and then drying at 110-120℃ for 1-3 minutes; the cold pressing is roller pressing, and the roller temperature is 15-25℃.