A copper-doped Prussian blue cathode material and its freeze-drying preparation method
By combining copper ion doping and freeze-drying technology, the problems of difficult removal of crystal water and structural instability of Prussian blue materials were solved, and high-capacity, structurally stable copper-doped Prussian blue cathode materials were prepared, which improved the electrochemical performance and cycle life of sodium-ion batteries.
Patent Information
- Application Number
- CN202611148777.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-31
- Publication Date
- 2026-11-17
AI Technical Summary
Existing Prussian blue cathode materials suffer from problems such as difficulty in effectively removing water of crystallization and structural instability, which affect their electrochemical performance and cycle life.
By combining copper ion doping with freeze-drying technology, copper ions partially replace the transition metal sites in the Prussian blue framework, and low-temperature freeze-drying technology removes the water of crystallization, forming a copper-doped Prussian blue material with a loose and porous structure.
A Prussian blue cathode material with high capacity, excellent structural stability and low water of crystallization content was achieved, which significantly improved the electrochemical performance and cycle stability of sodium-ion batteries.
Smart Images

Figure CN123120718A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the technical field of sodium-ion battery cathode materials, specifically relating to a copper-doped Prussian blue cathode material and its freeze-drying preparation method. Background Technology
[0002] With the accelerated development of electric vehicles and smart grids, energy storage technology has become one of the most closely watched research areas. Sodium-ion batteries, due to their abundant sodium resources and low cost, are considered one of the most promising technologies for large-scale energy storage applications. Prussian blue and its analogues (PBAs), as cathode materials for sodium-ion batteries, have attracted widespread attention due to their stable, open three-dimensional framework structure, abundant raw materials, high theoretical capacity, and ease of synthesis. However, the synthesis of high-performance Prussian blue-based cathode materials still faces significant challenges, mainly in the following two aspects.
[0003] Firstly, there is the issue of water of crystallization. During the conventional aqueous synthesis of Prussian blue analogues, a large amount of coordinated water and free water (collectively referred to as water of crystallization) is inevitably introduced into the crystal lattice. Water of crystallization can be further divided into adsorbed water, interstitial water, and bound water. Adsorbed water can be relatively easily removed by heating, but interstitial and bound water are more difficult to remove. Traditional processes commonly use high-temperature ovens for direct drying. High-temperature evaporation of moisture easily causes grain melting and agglomeration, pore closure, and insufficient removal of water from the crystal lattice, resulting in a high residual amount of water of crystallization. For example, in the study "Control of Co-precipitation Reaction of Iron-Based Prussian Blue Sodium-Ion Battery Cathode Material," the water of crystallization content of NaFeHCF after drying at 60℃ for 12 hours was still 12.22~19.21 wt%, as measured by TG. The presence of water of crystallization severely deteriorates the electrochemical performance of the material: water molecules occupy the active storage sites of sodium ions, reducing reversible capacity; under the battery operating voltage, the water of crystallization will convert into Na(H2O). + When the cell enters the electrolyte, it undergoes a side reaction with the electrolyte, consuming the active sodium source and generating gas, which can cause the battery to swell or even fail. At the same time, the water of crystallization can occupy the interstitial sites in Prussian blue materials, which hinders the migration of sodium ions during charging and discharging, affects the sodium ion migration kinetics, and significantly reduces the rate performance of the material.
[0004] Secondly, there is the issue of structural instability. Manganese-based Prussian blue materials exhibit a severe Jahn-Teller effect during charge and discharge, leading to structural distortion and rapid capacity decay. This structural instability severely limits the material's cycle life and practical applications.
[0005] To address the aforementioned issues, researchers have explored various modification strategies. In terms of elemental doping, copper (Cu) has been extensively studied due to its excellent electrical conductivity and structural stability. Research (https: / / doi.org / 10.1021 / acssuschemeng.5c09858) shows that copper ion doping can effectively improve the structural stability of manganese-based Prussian blue and enhance the low-spin Fe... 2+ / Fe 3+ The redox activity of copper-doped Prussian blue analogues is shown. At 1C rate, they provide 109.6 mAh / g. -1 The reversible capacity was achieved, with a capacity retention of 89.6% after 100 cycles. The ternary Cu-Mn-Fe Prussian blue analog CuMnFePBA, with a Cu / Mn molar ratio of 1:1, exhibited optimal overall performance, balancing high capacity, rate performance, and long-term cycling stability. The chemical formula of the product is Na2Cu1Mn1[Fe(CN)6]2·□ 0.09 ·2.14H2O (DOI: 10.1002 / adma.202417876) can achieve 132.4 mAh·g -1 The specific capacity of the Cu-Mn-Fe Prussian blue analogue was 73.3% after 1000 cycles; the capacity retention of the Cu-Mn-Fe Prussian blue analogue-based 18650 cylindrical battery reached 73.54% after 850 cycles. Furthermore, copper doping stabilizes the PBA framework structure, improving cycle stability through the synergistic effect of iron vacancies and copper doping. Regarding the drying process, the ternary Cu-Mn-Fe Prussian blue analogue prepared by co-precipitation was dried in a 120 ℃ vacuum oven for 12 h. TG analysis showed that the water content of the ternary Cu-Mn-Fe Prussian blue analogue was 11.5 wt%. Existing patents, such as CN116375054A, disclose a method for reducing crystal water through freeze-drying. Freeze-drying technology can remove moisture from materials at low temperatures, avoiding structural collapse caused by high-temperature drying.
[0006] However, there is currently a lack of existing technologies that combine copper ion doping with freeze-drying technology in the preparation of Prussian blue cathode materials.
[0007] Therefore, a new method needs to be developed that can combine the advantages of chemical modification by copper doping with the advantages of physical protection by freeze drying. Summary of the Invention
[0008] The purpose of the present invention is to overcome the defects of insufficient capacity, unstable structure and difficulty in effectively removing crystal water of Prussian blue materials in the prior art, and provide a copper-doped Prussian blue cathode material and a freeze-drying preparation method thereof. In the present invention, copper ions partially replace the transition metal sites in the Prussian blue framework to introduce additional capacity contribution and stabilize the crystal structure; meanwhile, freeze-drying technology is adopted to remove the crystal water in the material at low temperature, so as to preserve the framework structure optimized by copper doping. The synergistic effect of copper doping and freeze-drying finally obtains the Prussian blue cathode material with high capacity, excellent structural stability and low crystal water content.
[0009] To solve the above technical problems, the present invention adopts the following technical solutions: The present invention provides a copper-doped Prussian blue cathode material, the chemical general formula of which is: Na x Cu y M 1-y [Fe(CN)₆] z ·nH₂O, where M is Mn or Fe, 0<x≤2, 0<z≤1, 0<y≤0.1, 0≤n≤5; the material has a cubic crystal form, the powder is in a loose and porous structure, and the residual crystal water content is ≤5wt%.
[0010] Further, the molar ratio of metal elements in the copper salt and the transition metal salt is y:(1-y), and y=0.05.
[0011] The present invention also provides a preparation method of the copper-doped Prussian blue cathode material. The method uses a raw material system comprising a copper salt, a transition metal salt and a ferrocyanide to prepare a copper-doped Prussian blue wet filter cake through a co-precipitation reaction. The molar ratio of metal elements in the copper salt and the transition metal salt is y:(1-y), 0<y≤0.1, and the following steps are sequentially performed on the obtained wet filter cake: S1. Spread the wet filter cake on a pre-cooled metal carrier to form a thin-layer material; S2. Immerse the entire metal carrier carrying the thin-layer material in liquid nitrogen for deep cooling and quick freezing; S3. Perform vacuum freeze-drying on the quick-frozen material to obtain primary dry powder; S4. Place the primary dry powder in a vacuum environment for heat treatment to prepare the copper-doped Prussian blue cathode material with low crystal water content.
[0012] Further, the specific steps of the co-precipitation reaction are as follows: add sodium ferrocyanide decahydrate, copper sulfate, transition metal salt and sodium citrate into a solvent, mix them and carry out the co-precipitation reaction to obtain the copper-doped Prussian blue wet filter cake; the molar ratio of the copper sulfate to the transition metal salt is y:(1-y), the transition metal salt includes ferrous sulfate or manganese chloride, and the solvent is deionized water.
[0013] Furthermore, in step S1, the metal carrier is copper foil or aluminum foil; the thickness of the thin material layer is less than 5 mm. This step aims to increase the contact area between the material and the cold source, laying the foundation for subsequent rapid and uniform freezing.
[0014] Furthermore, in step S2, the liquid nitrogen rapid freezing time is 30 seconds to 3 minutes. The extremely low temperature of liquid nitrogen and the high thermal conductivity of the metal carrier work together to freeze the moisture in the wet filter cake instantly, forming micro- and nano-scale ice crystals. This rapid freezing minimizes the expansion damage to the material's microstructure caused by ice crystal growth.
[0015] Furthermore, in step S3, the pressure inside the freeze-drying chamber is ≤0.02 mbar, the cold trap temperature is below -50℃, and the drying time is 24–72 hours. Under these conditions, the solid ice in the material sublimates directly into water vapor without passing through a liquid state, and the water vapor is captured and condensed by the cold trap. This sublimation process lasts for 24–72 hours until the material mass no longer changes, resulting in a primary dried powder. Under these conditions, the solid ice in the material sublimates directly into water vapor without passing through a liquid state, removing most of the free water and some weakly bound water at low temperatures.
[0016] Furthermore, step S4 involves heat treatment at 120°C for 4–10 hours. This step aims to remove strongly coordinated water that is difficult to remove through freeze-drying, resulting in a final product with extremely low water of crystallization content.
[0017] Furthermore, steps S1 and S2 are carried out in an inert atmosphere (such as an argon glove box) to prevent the material from being oxidized in humid air.
[0018] Furthermore, in step S3, to reduce the reheating during material transfer, the sample rack of the freeze dryer can be pre-cooled.
[0019] The above steps form an organic whole, and each step is closely related and inseparable, jointly affecting the morphology, structure, and electrochemical performance of the final copper-doped Prussian blue cathode material.
[0020] The present invention provides a Prussian blue cathode material prepared by the above method, characterized by having a highly loose and porous microstructure, extremely low particle agglomeration, and extremely low residual water of crystallization content.
[0021] The present invention also provides a sodium-ion battery positive electrode sheet comprising the above-mentioned positive electrode material and a sodium-ion battery.
[0022] Compared with the prior art, the present invention has the following advantages: 1. Copper ion doping of Prussian blue achieves dual capacity optimization. Copper ions replace some transition metal sites within the lattice, thereby achieving capacity optimization through Cu doping. 2+ / Cu +The redox couple additionally contributes sodium storage capacity; the strongly coordinated Cu-N bond effectively suppresses Mn in manganese-based materials 3+ induced Jahn-Teller lattice distortion, buffers the volume deformation during charge and discharge, stabilizes the crystal framework, and simultaneously activates low-spin Fe 2+ / Fe 3 + redox activity, essentially improving the reversible specific capacity and structural durability of the material
[0023] 2. The preservation effect of liquid nitrogen flash freezing combined with vacuum drying on the copper-doped structure. After the wet Prussian blue filter cake is spread into a layer and rapidly frozen by liquid nitrogen, the moisture instantly forms tiny ice crystals, preventing large ice crystals from piercing the crystal lattice and destroying the copper-doped optimized framework; low-temperature sublimation dehydration replaces traditional high-temperature drying, avoiding the problems of grain melting and agglomeration and cubic structure collapse, which can stably control the crystal water of the material within 5wt%, reduce electrolyte hydrolysis side reactions and irreversible loss of active sodium, and preserve and consolidate the structural optimization effect brought by copper doping
[0024] 3. Synergistic effect of copper doping and freeze drying. Copper doping is an intrinsic chemical modification of the material, which supplements sodium storage capacity through Cu 2 + / Cu + couple, suppresses lattice distortion through strong coordination bonds, and improves the capacity and structural stability of the material. Liquid nitrogen flash freezing-vacuum freeze drying is a physical regulation at the preparation process level, which removes moisture under low-temperature and no thermal damage conditions, and completely preserves the loose cubic framework optimized by copper doping. The two are mutually adapted and indispensable: the single use of copper doping combined with traditional high-temperature drying will lose the modification advantage due to framework collapse; if only the freeze-drying process is used without copper doping, the intrinsic lattice stability and sodium storage capacity of the material cannot be improved
[0025] Meanwhile, the present invention defines a reasonable copper doping range of 0<y≤0.1: when the doping ratio is within this range, the doping gain effect is far greater than the negative lattice disturbance; however, if the doping ratio approaches the upper limit y=0.1, excess copper ions will introduce a large number of lattice defects and coordination-bound water sites, the negative deterioration effect at the component level will exceed the structural gain brought by the freeze-drying process compared with traditional drying, and excess Cu 2+ will occupy a large number of sodium ion intercalation and deintercalation sites, increase lattice coordination water sites, and bring negative effects such as intensified lattice distortion, increased crystal water, and greatly deteriorated electrochemical performance. There will be a phenomenon that the undoped traditional dried sample is superior to the highly doped freeze-dried sample in terms of water content and electrochemical performance. This boundary rule is an unexpected technical effect verified by the control experiments of the present application, which also proves the necessity and rationality of the doping parameter range of the present invention. The synergistic effect of the two finally achieves a technical improvement of 1+1>2, which is significantly better than any single modification means
[0026] 4. Outstanding electrochemical performance. The material prepared by this process has regular, loose, and porous grains with unobstructed ion transport channels. After being assembled into a sodium-ion battery, the optimal sample can achieve a specific capacity of 138.8 mAh / g in the first discharge cycle at 0.1C, and retain 88% of its capacity after 200 cycles at 1C. Compared with existing technologies, it has better capacity and cycle stability under the same 2C fast charge cycle conditions, and its rate adaptability and long-cycle service capability are significantly improved.
[0027] 5. The process is simple and has industrialization potential. The overall process revolves around co-precipitation, centrifugation, freeze drying, and vacuum heat treatment. Centrifuges, freeze dryers, and vacuum ovens are all standard equipment commonly used in the battery industry. By optimizing the carrier and batch pre-freezing method, it can transition to pilot-scale and even large-scale production; the process has low barriers to entry and high feasibility for large-scale implementation. Attached Figure Description
[0028] Figure 1 The images shown are SEM images of Examples 1 to 7 of the present invention, where (a) is Example 1, (b) is Example 2, (c) is Example 3, (d) is Example 4, (e) is Example 5, (f) is Example 6, and (g) is Example 7. Figure 2 XRD patterns of Examples 1 to 7; Figure 3 The results of thermogravimetric tests for Examples 1 to 5; Figure 4 The graph shows a comparison of the cycle performance of the Prussian blue materials obtained in Examples 1 to 5 after being assembled into sodium-ion half-cells.
[0029] Figure 5 The first charge-discharge curves of sodium-ion half-cells assembled from the Prussian blue materials obtained in Examples 1 to 5 are shown. Detailed Implementation
[0030] To make the objectives, technical solutions, and advantages of the embodiments of this application clearer, the technical solutions in the embodiments of this application are described clearly and completely below. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. Based on the embodiments in this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.
[0031] Example 1
[0032] This embodiment provides a copper-doped Prussian blue cathode material (Na). x Cu y Mn 1-y [Fe(CN)6] z The preparation method of nH2O is as follows: Step S1: Wet sample pretreatment. This includes the following steps: Weigh 4.48 g of ferrous sulfate heptahydrate (FeSO4·7H4O), 0.224 g of copper sulfate pentahydrate (CuSO4·5H2O), and 12.7047 g of sodium citrate (Na3C6H5O7·2H2O), and dissolve them in deionized water to prepare 1000 mL of solution A. Weigh 7.6516 g of sodium ferrocyanide decahydrate (Na4Fe(CN)6·10H2O), and dissolve it in deionized water to prepare 1000 mL of solution B. The molar ratio of Cu doping is 0.05.
[0033] Stir solutions A and B at 850 rpm for 40 mins respectively.
[0034] Solution A is slowly added dropwise to solution B using a peristaltic pump while stirring slowly and evenly. After the addition is complete, continue stirring until the mixture is homogeneous and reacted for 30 minutes, then let it stand for 24 hours.
[0035] After 24 hours of settling, the supernatant was removed, and the mixture was centrifuged and washed three times with deionized water. The final product was a copper-doped Prussian blue precursor precipitate filter cake.
[0036] Step S2, Cryogenic Freezing. In an argon glove box, take a pre-cooled copper foil (approximately 10cm x 10cm) with a thickness of 0.1mm and place it on a cold table at a temperature below -50℃. Spread the centrifuged precursor precipitate evenly on the copper foil to form a thin layer with a thickness of approximately 2mm. Hold the edge of the copper foil with tweezers and quickly immerse it entirely into a liquid nitrogen Dewar flask for 60 seconds until no more bubbles are generated and the material is completely frozen.
[0037] Step S3: Freeze-drying. Quickly transfer the frozen "copper foil-ice cake" composite to the sample rack of the freeze dryer, which has been pre-cooled to -60°C. Close the chamber, start the vacuum pump, maintain the pressure inside the chamber below 0.02 mbar, keep the cold trap temperature at -64°C, and sublimate dry for 48 hours to obtain the primary dried product.
[0038] Step S4, Post-processing. The freeze-dried primary product, a loose blue powder, is transferred to a vacuum oven and heat-treated at 120°C under vacuum for 4-10 hours to finally obtain a copper-doped Prussian blue cathode material with low water of crystallization content.
[0039] Example 2
[0040] In this embodiment, the raw material ratio, co-precipitation synthesis steps, and Cu doping ratio are the same as in Example 1. Only the drying post-treatment process is modified. Steps S2, cryogenic quick-freezing, and S3, freeze-drying, which were in Example 1, are omitted. The wet filter cake after centrifugation and washing is directly placed in a 120°C vacuum oven for constant temperature drying for 12 hours (traditional hot drying). Other conditions are exactly the same as in Example 1.
[0041] Example 3
[0042] The preparation process is the same as in Example 1, except that copper sulfate pentahydrate is not added in step S1 (i.e., no copper doping). Other conditions are exactly the same as in Example 1, and the complete process of liquid nitrogen quick-freezing, 48h freeze-drying, and 120℃ vacuum heat treatment is adopted.
[0043] Example 4
[0044] The preparation process is the same as in Example 1, except that copper sulfate pentahydrate is not added in step S1 (i.e., no copper doping), and steps S2, deep freezing and S3, and freeze drying in Example 1 are omitted. The wet filter cake after centrifugation and washing is directly placed in a vacuum oven at 120°C for constant temperature drying for 12 hours (traditional heat drying). Other conditions are exactly the same as in Example 1.
[0045] Example 5
[0046] The difference between this embodiment and Embodiment 1 is that the amount of copper sulfate pentahydrate added in step S1 is 0.448g (that is, to increase the amount of copper doping, the Cu / (Cu+Fe) molar ratio is about 0.1, and other conditions are exactly the same as in Embodiment 1, and the complete set of processes of liquid nitrogen quick-freezing, 48h freeze-drying and 120℃ vacuum heat treatment is adopted.
[0047] Example 6
[0048] In Example 1, equimolar amounts of ferrous sulfate heptahydrate were replaced with manganese chloride to prepare a copper-doped manganese-based Prussian blue Fe-Mn system. The molar proportion of Cu doping was 0.05. The remaining raw material ratios, thin-layer liquid nitrogen quick-freezing, 48-hour high-vacuum freeze-drying, and 120°C vacuum heat treatment were the same as in Example 1.
[0049] Example 7
[0050] Using the preparation scheme in Example 6, steps S2 and S3 were replaced with the traditional hot drying method to process the same batch of centrifuged samples: the centrifuged samples were placed in a 120°C vacuum oven and dried at a constant temperature for 12 hours.
[0051] The resulting material had a water content of 10.8 wt%. SEM showed that the particles were severely agglomerated into large clumps, making it difficult to discern the initial cubic morphology.
[0052] Example 8
[0053] The difference between this embodiment and Embodiment 6 is that copper sulfate pentahydrate is not added (i.e., no copper doping), while the other conditions are exactly the same as in Embodiment 6.
[0054] Example 9
[0055] The difference between this embodiment and Example 6 is that copper sulfate pentahydrate is not added (i.e., no copper doping), and the liquid nitrogen quick-freezing + freeze-drying is replaced by drying in a 120°C vacuum oven for 12 hours (conventional hot drying). All other conditions are exactly the same as in Example 6. This embodiment is used to compare and verify the synergistic effect of copper doping and freeze-drying.
[0056] Example 10
[0057] The difference between this embodiment and Example 6 is that the amount of copper sulfate pentahydrate added is 0.448g (i.e., the amount of copper doping is increased, and the Cu / (Cu+Mn) molar ratio is about 0.1, while other conditions are exactly the same as in Example 1).
[0058] The following are the structural characterization, water of crystallization content testing, and electrochemical performance testing of the above-mentioned embodiments. 1. Microstructure like Figure 1 These are SEM images of the samples prepared in Examples 1-7 of this invention. Examples 1 and 6 include the complete preparation process, which can generate well-dispersed cubic grains with complete edges and corners, and the material has a rich porous structure. In Examples 2 and 7, after drying in a traditional oven, the grains broke up and agglomerated, and the pores were blocked. In Example 3, without copper doping, the grain defects increased. In Example 4, the double blank control group showed the most significant structural deterioration. In Example 5, after the doping ratio reached the upper limit, the grain uniformity deteriorated and the defects increased. The SEM characterization of this group clearly shows the regulatory effect of the copper doping ratio and the freeze-drying process on the microscopic crystal morphology, particle dispersion state and pore structure of the material, explaining the fundamental reason for the differences in the crystal water content and electrochemical performance of different groups of samples from the microstructural level. Figure 2 As shown, the XRD diffraction peaks of Examples 1-7 all correspond to the characteristic peaks of cubic Prussian blue analogues, indicating that each sample successfully formed a PBA framework structure and no obvious impurity phase was detected.
[0059] 2. Test for water of crystallization content The total water of crystallization (including surface adsorbed free water, interstitial water, and metal coordination bound water) of the samples from Examples 1 to 7 was quantitatively determined by segmented weight loss and the total water content was calculated using simultaneous thermogravimetric analysis (TG) under a nitrogen atmosphere. The Karl Fischer coulometric method with a solid heating furnace was used for precise verification in a low dew point glove box. Both test methods were performed in accordance with the "T / CIET705-2024 Determination of Water Content in Prussian Blue Electrode Materials".
[0060] The thermogravimetric analysis (TGA) was performed using a NETZSCH STA449F3 simultaneous thermal analyzer, with a high-purity nitrogen carrier gas flow rate of 40 mL / min, and the temperature was uniformly increased from room temperature to 400℃ at a rate of 10℃ / min. Within this temperature range, the Prussian blue cyanide framework does not undergo thermal decomposition, and the sample mass loss is solely due to moisture removal.
[0061] The thermogravimetric (TG) curve is divided into weight loss stages: weight loss within the range of room temperature to 120°C is attributed to the removal of free water adsorbed on the material surface; weight loss within the range of 150°C to 250°C is attributed to the removal of bound water within the crystal lattice (i.e., water of crystallization), which is the water of crystallization referred to in this invention. The proportion of water of crystallization is calculated based on the remaining mass retention rate of the material at 250°C on the TG curve, using the following formula: The mass fraction of water of crystallization, w(H2O), is calculated as 100% - the percentage of sample mass retained at 250℃.
[0062] Figure 3 The TG thermogravimetric curves for Examples 1 to 5 are shown in the figure. The retention rate corresponding to the 250°C mark can be directly calculated: the water of crystallization content of Examples 1 to 5 is 3.9wt%, 11.5wt%, 8.7wt%, 11.2wt%, and 13.2wt%, respectively.
[0063] The Karl Fischer test environment has a glove box dew point of ≤-20℃ and a sample heating release temperature of 180℃. The total moisture mass is calculated and converted into mass fraction according to Faraday's law of electrolysis. The data is considered valid when the deviation between the two test results for the same sample is ≤0.5wt%.
[0064] In the manganese-based system, the crystal water content of Example 6, which uses the complete process of this invention, is 4.2 wt%. The water content of Example 7, which is dried in a conventional 120°C vacuum oven, is 10.8 wt% as measured by Karl Fischer method. The moisture change trends of Examples 8, 9, and 10 are completely consistent with the corresponding groups of the iron-based system.
[0065] The overall moisture content variation pattern can be explained by combining the aforementioned SEM microstructure results: When relying on liquid nitrogen cryogenic quick-freezing to form a loose, porous, and complete cubic structure, the internal water vapor escape channels of the material are unobstructed, and interstitial water and weakly coordinated water can be fully removed without damaging the crystal framework. Therefore, the moisture content of samples with both copper doping modification and complete freeze-drying post-processing can be stably controlled within 5 wt%. If copper doping modification is cancelled, the binding effect of the crystal lattice on water molecules is enhanced, and even if the freeze-drying process is used, the moisture content will exceed the standard significantly. If the traditional high-temperature direct drying process is used instead, although some coordinated water can be forcibly removed by strong heating to obtain extremely low moisture values, it will cause particle agglomeration, pore closure, and even collapse of the cubic framework. After the microstructure fails, the electrochemical performance of the material will deteriorate significantly. In addition, when the copper doping ratio is increased to the upper limit y=0.1, the excessive copper ions introduce lattice defects and add a large number of coordinated water sites, which will lead to a rebound in the crystal water content and a decrease in the overall performance of the material.
[0066] 3. Electrochemical performance testing Samples 1-10 were used as positive electrode active materials, and electrode sheets were prepared by mixing them with conductive carbon black and PVDF binder in a 7:2:1 ratio. Sodium metal was used as the counter electrode, and CR2032 coin cells were assembled for testing. The electrolyte was 1M NaClO4 inEC / DEC (1:1) with 5% FEC.
[0067] Table 1
[0068] Note: In order to achieve the same conditions for comparison with the prior art CN116375054A, the optimal sample examples 1 and 6 were selected and supplemented with 0.2C specific capacity and 2C rate 200-cycle test according to the test specifications of the literature; the other samples adopted the conventional 0.1C activation calibration and 1C rate long cycle characterization scheme of this application.
[0069] In Example 1 (iron-based Cu doping and complete freeze-drying process), the water of crystallization was 3.9 wt%, and in Example 6 (manganese-based Cu doping and complete freeze-drying process), the water of crystallization was 4.2 wt%. Both samples consistently maintained a water of crystallization below 5 wt%. SEM characterization results showed that both samples were prepared by first spreading the wet filter cake into a thin layer, then rapidly freezing it with liquid nitrogen to generate uniformly sized micro-ice crystals. After freeze-drying, the samples retained well-defined cubic grains with dispersed, non-agglomerated particles and abundant intergranular and internal pores. This loose, porous microstructure allows interstitial water and weakly coordinated water to escape smoothly during the preparation stage, achieving controllable removal of low-crystal-water content. Furthermore, it establishes a continuous, rapid sodium ion transport channel during battery charging and discharging, significantly reducing ion diffusion polarization.
[0070] In terms of composition, a low proportion of copper ions are uniformly embedded in the crystal lattice, and the addition of Cu... 2+ / Cu + The redox couple increases the number of sodium ion storage sites, resulting in maximum capacities of 138.8 mAh / g and 137.4 mAh / g at 0.1C, respectively. Compared to existing technologies under 0.2C testing conditions, their specific capacities are 136.5 mAh / g and 135.6 mAh / g, significantly higher than the existing benchmark capacity of 120.0 mAh / g. Simultaneously, the strong coordination Cu-N bond stabilizes the crystal framework, suppressing the typical Jahn-Teller lattice distortion of manganese-based materials. Combined with low water of crystallization, it significantly reduces side reactions such as electrolyte hydrolysis and irreversible consumption of active sodium during charging and discharging. Under 2C fast charging cycling conditions (200 cycles), the capacity retention rates are 91.1% and 91.3%, respectively, both superior to the existing technology's 85.0%. The capacity retention rates under conventional 1C 200-cycle cycling are also excellent, exceeding other samples in the same group, demonstrating optimal long-cycle structural stability.
[0071] Example 2 contained 11.5 wt% water of crystallization, while Example 7 contained only 10.8 wt%. The doping ratios of both were consistent with the optimal sample, differing only in the drying process, which was replaced with high-temperature drying in a 120°C vacuum oven. However, the electrochemical performance significantly decreased. In Example 2, the capacity retention after 200 cycles at 1C was only 82.6%, compared to only 82.8% in Example 7. SEM morphology revealed that traditional high-temperature drying lacked an ice crystal formation process; the grains adhered and melted upon heating, resulting in broken cubic edges and large-area closure and blockage of internal pores. Although Example 7 achieved a low water content by forcibly removing some coordinated water through high-temperature heating, the material's microscopic three-dimensional crystal framework had collapsed and shattered, destroying the structural carriers for sodium ion insertion and extraction. In Example 2, the pores were closed, preventing the removal of interstitial and coordinated water within the crystal lattice. During charge and discharge, side reactions continuously consumed active sodium ions, and the dense agglomeration structure elongated the sodium ion diffusion path, increasing polarization and causing a simultaneous decrease in reversible capacity and cycle life. This control group directly demonstrates that simply relying on high temperature to forcibly reduce the water of crystallization cannot improve electrochemical performance. First, a complete and loose cubic microstructure is required, and only low water content has a positive effect.
[0072] Examples 3 and 8 employed the liquid nitrogen freeze-drying process entirely, but without copper doping modification. SEM observation of Example 3 revealed that while the material maintained its basic cubic crystal profile, grain regularity decreased, and the number of fine crystallites and lattice defects significantly increased. There were no Cu-N coordination bonds binding water molecules, resulting in a stronger lattice water-holding capacity and a crystal water content exceeding the 5wt% limit. This indicates a lack of Cu... 2+ / Cu + While redox couples can be used to enhance sodium storage capacity, Cu-N coordination bonds cannot be used to suppress lattice distortion and irreversible side reactions during charge and discharge. Therefore, the reversible specific capacity and long-cycle stability show a significant decline compared to the best doped samples in Examples 1 and 6 of the same matrix.
[0073] Examples 4 and 9 served as double blank control groups, without copper doping modification and using traditional high-temperature drying treatment. Microscopically, the grains were severely broken and agglomerated, and the pores were completely closed and blocked. The water content was much higher than that of Examples 1 and 6. The sodium ion diffusion channels were missing, the electrolyte side reactions caused by water were the most intense, and there were no additional sodium storage active sites brought by copper doping. All electrochemical indicators decreased significantly.
[0074] Examples 5 and 10 increased the copper doping ratio to the upper limit of 0.1, and although a complete freeze-drying process was used, the performance deteriorated significantly. Excessive copper ions disrupt the uniformity of the crystal lattice. The SEM image of Example 5 shows large differences in grain size and a large number of deformed fragments. Simultaneously, the excessive Cu... 2+ It will form numerous coordination bonds with cyanide ions and water molecules, creating a large number of new water-binding sites and causing an increase in the water of crystallization content. Excess Cu 2+ It also crowds out sodium ion insertion / extraction sites, reducing the material's sodium storage capacity and simultaneously exacerbating lattice distortion. The degradation effect at this component level outweighs the structural optimization benefits of freeze-drying compared to traditional drying; ultimately, the reversible capacity and cycle durability are significantly degraded compared to the optimal low-doped sample. Therefore, a low copper doping ratio is crucial, falling below the requirements of existing technologies.
[0075] The three sets of control samples mentioned above, from the three dimensions of no doping, process replacement, and excessive doping, demonstrate that only through the synergistic cooperation of copper doping components, doping ratio range, and liquid nitrogen multi-stage freeze-drying process can the microstructure, water of crystallization content, and electrochemical performance be simultaneously optimized.
[0076] The above embodiments fully demonstrate that the freeze-drying dehydration method provided by the present invention can effectively solve the problems of structural damage and particle agglomeration in the dehydration process of Prussian blue materials, and significantly improve its comprehensive electrochemical performance as a cathode material for sodium-ion batteries.
[0077] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A copper-doped Prussian blue cathode material, characterized in that, Its general chemical formula is: Na x Cu y M 1-y [Fe(CN)6] z ·nH2O; wherein, M is Mn or Fe, 0<x≤2, 0<z≤1, 0<y≤0.1, 0≤n≤5; the material is of cubic crystal form, the powder has a loose and porous structure, and the residual crystal water content is ≤5wt%.
2. The copper-doped Prussian blue cathode material according to claim 1, characterized in that, y is 0.
05.
3. A method for preparing the copper-doped Prussian blue cathode material according to any one of claims 1 or 2, comprising preparing a copper-doped Prussian blue wet filter cake by co-precipitation reaction using a raw material system containing copper salt, transition metal salt and ferrocyanide, characterized in that, The molar ratio of the metal elements in the copper salt and the transition metal salt is y:(1-y), where 0<y≤0.1, and the following steps are sequentially performed on the obtained wet filter cake: S1. Spreading the wet filter cake on a pre-cooled metal carrier to form a thin-layer material; S2. Fully immersing the metal carrier carrying the thin-layer material in liquid nitrogen for deep-cooling quick freezing; S3. Subjecting the quick-frozen material to vacuum freeze-drying to obtain a primary dried powder; S4. Subjecting the primary dried powder to heat treatment in a vacuum environment to prepare a copper-doped Prussian blue positive electrode material with low crystal water content.
4. The preparation method according to claim 3, characterized in that, The co-precipitation reaction step is: adding sodium ferrocyanide decahydrate, copper sulfate, a transition metal salt and the chelating agent sodium citrate into deionized water for mixing, and performing post-treatment after the co-precipitation reaction to obtain a copper-doped Prussian blue wet filter cake; the transition metal salt is ferrous sulfate or manganese chloride.
5. The preparation method according to claim 3, characterized in that, In step S1, the metal carrier is a copper foil or an aluminum foil; the spreading thickness of the thin-layer material is less than 5 mm.
6. The preparation method according to claim 3, characterized in that, In step S2, the liquid nitrogen quick freezing time is 30 s to 3 min.
7. The preparation method according to claim 3, characterized in that, In step S3, the pressure in the freeze-drying chamber is ≤0.02 mbar, the cold trap temperature is lower than -50°C, and the drying duration is 24 to 72 h.
8. The preparation method according to claim 3, characterized in that, In step S4, the heat treatment temperature is 120°C, and the holding time is 4 to 10 h.
9. A positive electrode sheet for a sodium-ion battery, characterized in that, Comprising the copper-doped Prussian blue positive electrode material according to claim 1; the positive electrode sheet is prepared by mixing the positive electrode material, a conductive agent and a binder to form a slurry, and coating the slurry on a current collector.
10. A sodium-ion battery, characterized in that, Comprising a housing, a separator, an electrolyte, a negative electrode, and the sodium ion battery positive electrode sheet according to claim 9, wherein the positive electrode sheet, the separator and the negative electrode are stacked in sequence and immersed in the electrolyte.
Citation Information
Patent Citations
Preparation method of sodium ion battery positive electrode Prussian blue material
CN116375054A