A sulfide all-solid-state battery using citric acid-modified silicon anode material

By forming a lithium citrate layer on the surface of the silicon anode, the volume expansion and interface stability issues of the silicon anode in sulfide all-solid-state batteries are solved, thereby improving the cycle life and safety of the battery.

CN123120835APending Publication Date: 2026-11-17LIYANG ZHONGKE GUNENG NEW ENERGY TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611549144.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-08
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Silicon anodes in sulfide all-solid-state batteries face problems of severe volume expansion and poor interface stability, leading to battery performance degradation and safety hazards.

Method used

Citric acid-modified silicon anode material is used. A citric acid coating layer is formed on the surface of micron-sized silicon particles through esterification reaction, which is converted into a lithium citrate layer. This layer has ionic conductivity and interface isolation functions, which can alleviate volume changes and suppress side reactions.

Benefits of technology

It improves the battery's cycle life, rate performance, and safety, reduces interface impedance, maintains electrode structure integrity, and adapts to changes in silicon particle volume.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120835A_ABST
    Figure CN123120835A_ABST
Patent Text Reader

Abstract

This invention discloses a sulfide all-solid-state battery using a citric acid-modified silicon anode material, relating to the field of solid-state battery technology. The battery includes a cathode, a sulfide solid electrolyte, and a citric acid-modified silicon anode material. The citric acid-modified silicon anode material comprises micron-sized silicon particles and a citric acid coating layer on their surface. The citric acid coating layer is formed through an esterification reaction between the natural hydroxyl groups on the surface of the micron-sized silicon particles and the carboxyl groups in the citric acid molecules, and transforms into a lithium citrate layer during charge and discharge, providing both lithium-ion conduction and isolation functions. This invention effectively suppresses the volume expansion of the silicon anode and interfacial side reactions, significantly improving the cycle stability and rate performance of the sulfide all-solid-state battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of solid-state battery technology, and more specifically, to a sulfide all-solid-state battery using citric acid-modified silicon anode material. Background Technology

[0002] Lithium-ion batteries have long been the dominant battery technology in various industries, including new energy vehicles and portable electronic devices. However, their inherent instability poses safety hazards, and limitations in material selection have become a bottleneck for improving energy density. Under abnormal conditions such as high temperature, overcharging, and short circuits, liquid electrolytes may decompose and generate gas, leading to a rapid increase in internal pressure, causing battery swelling, leakage, and even fire and explosion. In contrast, all-solid-state batteries (ASSBs) offer a promising alternative solution to these limitations. Using non-flammable solid electrolytes (SEs) can ultimately solve safety issues and potentially improve battery energy density. Among all types of solid electrolytes (SEs), sulfide SEs have the highest ionic conductivity at room temperature (10⁻⁶). -3 ~10 -2 Its S / cm ratio and ideal mechanical properties make it the most ideal SEs for large-scale ASSB applications.

[0003] Silicon boasts a theoretical specific capacity of up to 4200 mAh / g, exceeding that of lithium metal (3860 mAh / g) and more than ten times that of commercially available graphite (372 mAh / g). Furthermore, it exhibits a relatively low lithium intercalation potential (relative to Li). + The silicon anode (with a Li / V of 0.4 V) can mitigate lithium deposition and reduce lithium dendrite growth. Furthermore, silicon is abundant in the Earth's crust and cost-effective. Given these advantages, silicon anodes have been extensively studied for developing high-energy-density and high-safety ASSBs. However, silicon anodes experience significant volume expansion (300%) during lithium insertion and extraction, leading to electrode cracking and delamination during cycling. In addition, side reactions between silicon and sulfide SEs can severely degrade battery performance.

[0004] It is evident that sulfide solid electrolytes have attracted significant attention in the all-solid-state battery technology roadmap due to their high ionic conductivity and good mechanical ductility. While silicon-based anode materials possess extremely high theoretical specific capacity, they face severe challenges in practical applications within sulfide all-solid-state batteries. On one hand, silicon undergoes significant volume expansion and contraction during charging and discharging, and repeated stress can easily lead to active particle pulverization, electrode structure collapse, and solid-solid interface contact failure. On the other hand, there is thermodynamic instability between silicon and sulfide solid electrolytes; direct contact can trigger severe interfacial side reactions, generating a high-resistivity interfacial layer and consuming active lithium, resulting in decreased battery cycle life and deterioration of high-rate performance. Existing physical mixing or simple coating modification methods often fail to form a uniform and strongly bonded protective layer on the surface of micron-sized silicon particles, failing to simultaneously meet the dual requirements of volume buffering and interfacial chemical stability.

[0005] In order to address the issues of volume expansion and reaction with sulfide SEs in silicon anodes, this invention utilizes citric acid to coat modified silicon particles to improve the performance of silicon anodes in sulfide ASSBs. Therefore, this invention aims to design a sulfide all-solid-state battery using citric acid-modified silicon anode material. Summary of the Invention

[0006] This invention provides a sulfide all-solid-state battery using citric acid-modified silicon anode material, achieving in-situ optimization and structural stabilization of the silicon anode interface, thereby solving the technical problems of severe volume expansion and poor interface stability of silicon anodes in sulfide all-solid-state batteries mentioned in the background art.

[0007] To achieve the above objectives, the present invention adopts the following technical solution: In a first aspect, the present invention provides a sulfide all-solid-state battery, comprising: a positive electrode; a sulfide solid electrolyte; and a citric acid-modified silicon negative electrode material, wherein the citric acid-modified silicon negative electrode material comprises micron-sized silicon particles; and a citric acid coating layer coated on the surface of the micron-sized silicon particles; wherein the citric acid coating layer is formed by an esterification reaction between the natural hydroxyl groups on the surface of the micron-sized silicon particles and the carboxyl groups in the citric acid molecules; the citric acid coating layer is converted into a lithium citrate layer during battery charging and discharging, and the lithium citrate layer simultaneously has the functions of lithium-ion conduction and isolating silicon from the sulfide solid electrolyte; The above-described scheme constructs a uniform organic coating layer on the surface of silicon particles through chemical bonding. This coating layer transforms in situ into a lithium-ion-rich lithium citrate interface layer during electrochemical cycling. This in-situ formed interface layer not only possesses ionic conductivity and reduces interfacial impedance, but also acts as a physical barrier to effectively prevent direct contact between the silicon active material and the sulfide solid electrolyte, thereby suppressing interfacial side reactions. Simultaneously, this interface layer exhibits a certain degree of mechanical flexibility, enabling it to adapt to volume changes in the silicon particles and maintain the integrity of the electrode structure.

[0008] In one embodiment of the sulfide all-solid-state battery according to the present invention, the sulfide solid electrolyte is Li6PS5Cl, and the positive electrode is lithium cobalt oxide or LiNi. 0.8 Co 0.1 Mn 0.1 O2; This preferred scheme uses a high-ionic-conductivity silver-germanium ore-type electrolyte matched with a high-voltage cathode material, combined with a citric acid-modified silicon anode, to construct a high-energy-density and interface-compatible all-solid-state battery system.

[0009] In one embodiment of the sulfide all-solid-state battery according to the present invention, the micron-sized silicon particles have a particle size of micron, and the citric acid coating layer is formed by treating with a citric acid aqueous solution with a concentration of 5% to 20%, preferably, the concentration of the citric acid aqueous solution is 10%; This preferred embodiment defines the formation conditions of the coating layer. Within this concentration range, citric acid can form a coating layer of moderate thickness and uniform distribution on the silicon surface through esterification, avoiding the problems of incomplete coating due to too low concentration or agglomeration and excessively thick insulating layer due to too high concentration. In addition, the preferred embodiment further optimizes the concentration of the reaction precursor, so that the formed citric acid coating layer achieves the best balance between density and uniformity, thereby obtaining the best electrochemical performance in subsequent cycles.

[0010] In one embodiment of the sulfide all-solid-state battery according to the present invention, the capacity retention rate of the citric acid modified silicon anode material after 1000 cycles at 2 C rate is not less than 93.57%. This preferred scheme characterizes the excellent structural stability of the modified silicon anode under high-rate long-cycle conditions through this performance index, indicating that the lithium citrate interface layer effectively alleviates the accumulation of mechanical stress caused by repeated volume changes.

[0011] In one embodiment of the sulfide all-solid-state battery according to the present invention, the citric acid modified silicon anode material exhibits a capacity decay of 18% when the rate is increased from 0.5 C to 5 C. This preferred solution reflects the good lithium-ion transport kinetics of the modified interface layer through this performance indicator. It can maintain low interface polarization even at high current densities, thus ensuring the fast charging capability of the battery.

[0012] In one embodiment of the sulfide all-solid-state battery according to the present invention, the citric acid modified silicon anode material has an areal capacity of 3 to 10 mAh / cm². 2 Under these conditions, the initial coulomb efficiency is no less than 77%; This preferred solution demonstrates through this performance indicator that, under high load conditions, the citric acid coating can effectively reduce irreversible lithium loss caused by the large specific surface area, thereby improving the energy efficiency of all-solid-state batteries in practical applications.

[0013] In one embodiment of the sulfide all-solid-state battery according to the present invention, the citric acid modified silicon anode material exhibits no short circuit after 30 cycles at a 0.2 C rate. This preferred solution verifies through this performance indicator that the modified layer has a good suppressive effect on micro-short circuits caused by lithium dendrite growth or local stress concentration, thereby improving the safety and reliability of the battery.

[0014] In one embodiment of the sulfide all-solid-state battery according to the present invention, the volume expansion rate of the citric acid modified silicon anode material after 1000 cycles is 155%; This preferred solution directly quantifies the constraint effect of the citric acid coating layer on the volume expansion of the silicon anode through this performance index, proving that as a buffer layer it significantly suppresses the excessive growth of electrode thickness and helps maintain tight contact at the solid-solid interface.

[0015] In one embodiment of the sulfide all-solid-state battery according to the present invention, the preparation method of the citric acid modified silicon anode material includes the following steps: a) placing micron-sized silicon powder in an aqueous citric acid solution, heating and stirring at 50-70°C for 8-16 hours, during which periodic ultrasonic dispersion is performed; b) filtering and washing the product obtained in step a) to remove unreacted citric acid; c) vacuum drying and grinding to obtain the citric acid modified silicon anode material; The preparation method in this preferred embodiment utilizes a mild aqueous esterification reaction, combined with the synergistic effect of a thermal field and an acoustic field, to promote the uniform adsorption and chemical bonding of citric acid molecules on the surface of silicon particles. Periodic ultrasonic dispersion effectively prevents the agglomeration of micron-sized silicon powder, ensuring the uniformity of the coating layer; subsequent washing and drying steps remove excess physically adsorbed organic matter, ensuring the purity and electrochemical activity of the final product.

[0016] In one embodiment of the sulfide all-solid-state battery according to the present invention, the concentration of the citric acid aqueous solution in step a) is 5%~20%, the heating and stirring temperature is 60°C, the time is 12 hours, and the ultrasonic dispersion is performed once every 2 hours for 20 minutes each time. This preferred scheme provides a specific process window under which the reaction rate and coating quality can be precisely controlled, ensuring the full progress of the esterification reaction while avoiding damage to the silicon surface structure that may be caused by prolonged high-temperature treatment, making it suitable for large-scale preparation.

[0017] Compared with the prior art, the beneficial effects of the present invention are: The sulfide all-solid-state battery and its preparation method provided by this invention achieve synergistic effects through the construction of a chemically bonded citric acid coating layer on the surface of micron-sized silicon particles, which is then converted in situ into a lithium citrate functional layer during cycling. First, the lithium citrate layer, acting as an ion conductor, reduces the charge transfer impedance at the silicon / sulfide electrolyte interface, improving rate performance. Second, this interface layer, as a flexible buffer medium, effectively absorbs the volume expansion stress of silicon during alloying, suppressing particle fragmentation and electrode delamination, significantly extending cycle life. Third, the dense coating layer physically isolates silicon from the sulfide electrolyte, blocking harmful interfacial side reaction pathways and improving coulombic efficiency and safety. Compared to traditional physical mixing or carbon coating strategies, the aqueous esterification modification process used in this invention is simple, environmentally friendly, and low-cost, providing an effective solution for the practical application of high-energy-density silicon-based all-solid-state batteries. Attached Figure Description

[0018] Figure 1 Figure (a) is a process flow diagram of citric acid modified silicon particles, and Figure (b) is a process flow diagram of dry preparation of citric acid modified silicon anode. Figure 2Figure (a) is a SEM image of 5% CA@Si citric acid modified silicon particles in an embodiment of the present invention; Figure (b) is a SEM image of 10% CA@Si citric acid modified silicon particles in an embodiment of the present invention; Figure (c) is a SEM image of 20% CA@Si citric acid modified silicon particles in an embodiment of the present invention; Figure (d) is an EDS spectrum of 5% CA@Si citric acid modified silicon particles in an embodiment of the present invention; Figure (e) is an EDS spectrum of 10% CA@Si citric acid modified silicon particles in an embodiment of the present invention; Figure (f) is an EDS spectrum of 20% CA@Si citric acid modified silicon particles in an embodiment of the present invention; Figure (g) is a TEM image of 5% CA@Si citric acid modified silicon particles in an embodiment of the present invention; Figure (h) is a TEM image of 10% CA@Si citric acid modified silicon particles in an embodiment of the present invention; and Figure (i) is a TEM image of 20% CA@Si citric acid modified silicon particles in an embodiment of the present invention. Figure 3 The image shows the C1s spectrum of the 5% CA@Si citric acid modified silicon particles in the embodiment of the present invention. Figure 4 The image shows the C1s spectrum of the 10% CA@Si citric acid modified silicon particles in the embodiment of the present invention. Figure 5 The image shows the C1s spectrum of the 20% CA@Si citric acid modified silicon particles in the embodiment of the present invention. Figure 6 The image shows the O1s spectrum of the 5% CA@Si citric acid modified silicon particles in the embodiment of the present invention. Figure 7 The image shows the O1s spectrum of the 10% CA@Si citric acid modified silicon particles in the embodiment of the present invention. Figure 8 The image shows the O1s spectrum of the 20% CA@Si citric acid modified silicon particles in the embodiment of the present invention. Figure 9 The image shows the Si2p spectrum of the 5%CA@Si citric acid modified silicon particles in the embodiment of the present invention. Figure 10 The image shows the Si 2p spectrum in the X-ray photoelectron spectroscopy of 10% CA@Si citric acid modified silicon particles in the embodiments of the present invention. Figure 11 The image shows the Si 2p spectrum in the X-ray photoelectron spectroscopy of 20% CA@Si citric acid modified silicon particles in the embodiments of the present invention. Figure 12Different types of silicon anode materials in the embodiments of the present invention are used in sulfide solid electrolytes (SASSB) at 2 C (1 mA cm⁻¹). -2 The cycling performance diagram is shown below, and the silicon anode material includes Li-Si, Li-5%CA@Si, Li-10%CA@Si and Li-20%CA@Si; Figure 13 This is a charge-discharge curve diagram for different cycle numbers when the silicon anode material is Li-Si in the embodiments of the present invention; Figure 14 This is a charge-discharge curve diagram of different cycle numbers when the silicon anode material is Li-5%CA@Si in the embodiments of the present invention; Figure 15 These are charge-discharge curves at different cycle numbers when the silicon anode material in this embodiment of the invention is Li-10%CA@Si; Figure 16 These are charge-discharge curves at different cycle numbers when the silicon anode material in this embodiment of the invention is Li-20%CA@Si; Figure 17 The diagram shows the rate performance of different types of modified silicon anode materials in sulfide solid electrolyte (SASSB) in embodiments of the present invention (0.5 C, 1 C, 2 C, 3 C, 5 C). The silicon anode materials include Li-Si, Li-5%CA@Si, Li-10%CA@Si and Li-20%CA@Si. Figure 18 These are charge-discharge curves at different rates when the silicon anode material in this embodiment of the invention is Li-Si. Figure 19 These are charge-discharge curves at different rates when the silicon anode material in this embodiment of the invention is Li-5%CA@Si. Figure 20 These are charge-discharge curves at different rates when the silicon anode material in this embodiment of the invention is Li-10%CA@Si. Figure 21 These are charge-discharge curves at different rates when the silicon anode material in this embodiment of the invention is Li-20%CA@Si. Figure 22 The differential capacity curves (0.1C rate) of different types of silicon anode materials in sulfide solid electrolyte (SASSB) in embodiments of the present invention are shown. The silicon anode materials include Li-Si, Li-5%CA@Si, Li-10%CA@Si and Li-20%CA@Si. Figure 23The differential capacity curves (2C rate) of different types of silicon anode materials in sulfide solid electrolyte (SASSB) in embodiments of the present invention are shown. The silicon anode materials include Li-Si, Li-5%CA@Si, Li-10%CA@Si and Li-20%CA@Si. Figure 24 These are charge-discharge curves for different cycle numbers when the silicon anode material in this embodiment of the invention is Li-Si. Figure 25 This is a charge-discharge curve diagram of different cycle numbers when the silicon anode material is Li-5%CA@Si in the embodiments of the present invention; Figure 26 These are charge-discharge curves at different cycle numbers when the silicon anode material in this embodiment of the invention is Li-10%CA@Si; Figure 27 These are charge-discharge curves at different cycle numbers when the silicon anode material in this embodiment of the invention is Li-20%CA@Si; Figure 28 The image shows the XRD pattern of the silicon anode material in this embodiment of the invention after a certain number of cycles. Figure 29 The images show the EIS spectra of different types of silicon anode materials in the embodiments of the present invention before cycling in a sulfide solid electrolyte (SASSB). The silicon anode materials include Li-Si, Li-5%CA@Si, Li-10%CA@Si and Li-20%CA@Si. Figure 30 The images show the EIS spectra of different types of silicon anode materials in the embodiments of the present invention after 50, 300 and 600 cycles in a sulfide solid electrolyte (SASSB), wherein the silicon anode material is Li-Si; Figure 31 The images show the EIS spectra of different types of silicon anode materials in the embodiments of the present invention after 50, 300 and 600 cycles in a sulfide solid electrolyte (SASSB), wherein the silicon anode material is Li-5%CA@Si; Figure 32 The images show the EIS spectra of different types of silicon anode materials in the embodiments of the present invention after 50, 300 and 600 cycles in a sulfide solid electrolyte (SASSB), wherein the silicon anode material is Li-10%CA@Si; Figure 33 The images show the EIS spectra of different types of silicon anode materials in the embodiments of the present invention after 50, 300 and 600 cycles in a sulfide solid electrolyte (SASSB), wherein the silicon anode material is Li-20%CA@Si; Figure 34Figure (a) shows the cracking and pulverization process of unmodified silicon during repeated lithium insertion and extraction; Figure (b) shows the process by which the citric acid-coated silicon in the embodiment of the present invention maintains its structural integrity during repeated lithium insertion and extraction. Figure 35 Figure (a) is a SEM image of the cross-section of the silicon anode material Li-Si in the embodiment of the present invention after long-term cycling in a sulfide solid electrolyte (SASSB); Figure (b) is a SEM image of the cross-section of the silicon anode material Li-5%CA@Si in the embodiment of the present invention after long-term cycling in a sulfide solid electrolyte (SASSB); Figure (c) is a SEM image of the cross-section of the silicon anode material Li-10%CA@Si in the embodiment of the present invention after long-term cycling in a sulfide solid electrolyte (SASSB); Figure (d) is a SEM image of the cross-section of the silicon anode material Li-20%CA@Si in the embodiment of the present invention after long-term cycling in a sulfide solid electrolyte (SASSB). Figure 36 The image shows the silicon anode material Li-10%CA@Si in this embodiment of the invention, in a sulfide solid electrolyte (SASSB) with a high areal capacity (3 mAh / cm²). 2 Ratio performance chart under ) Figure 37 The image shows the silicon anode material Li-10%CA@Si in this embodiment of the invention, in a sulfide solid electrolyte (SASSB) with a high areal capacity (3 mAh / cm²). 2 Cyclic performance plot under ) Figure 38 The figure shows the charge-discharge curves of the silicon anode material Li-10%CA@Si in the embodiments of the present invention under different areal capacities in a sulfide solid electrolyte (SASSB). Figure 39 The figure shows the solid-state cycling performance of the NCM811||LPSCL||Li-10%CA@Si sulfide full cell in the embodiments of the present invention. Detailed Implementation

[0019] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0020] Unless otherwise specified, all raw materials used in the embodiments of the present invention are commercially available or obtainable by those skilled in the art; unless otherwise specified, all methods used in the embodiments of the present invention are methods mastered by those skilled in the art.

[0021] Based on this, the present invention proposes a sulfide all-solid-state battery, comprising a positive electrode, a sulfide solid electrolyte, and a citric acid-modified silicon anode material. In the battery's stacked structure, the sulfide solid electrolyte is located between the positive electrode and the citric acid-modified silicon anode material, serving the functions of ion transport and electronic insulation. It should be understood that although a specific stacking order is shown in the figure, in other embodiments, as long as effective ion pathways between each functional layer are maintained, the specific assembly form can be adjusted according to the actual battery design requirements.

[0022] The citric acid-modified silicon anode material comprises micron-sized silicon particles and a citric acid coating layer on the surface of the micron-sized silicon particles. Specifically, the micron-sized silicon particles serve as the main active material, providing high specific capacity; while the citric acid coating layer is not simply a physical attachment, but is formed through an esterification reaction between the natural hydroxyl groups on the surface of the micron-sized silicon particles and the carboxyl groups in the citric acid molecules. This chemical bonding method creates a stable Si-OC covalent bond between the coating layer and the silicon substrate. As shown in X-ray photoelectron spectroscopy (XPS), the characteristic peak appearing at approximately 289.2 eV in the C 1s spectrum corresponds to C=O-(OR) in the ester bond, and a corresponding Si-O-(O)R signal was also observed at approximately 103.4 eV in the Si 2p spectrum. This fully confirms that the citric acid is fixed to the surface of the silicon particles through a chemical reaction rather than physical mixing. Compared to physical coating, this chemically bonded interface is less prone to detachment under the mechanical stress of long-term battery cycling, providing a solid structural foundation for the subsequent realization of interface functions.

[0023] Furthermore, the citric acid coating transforms into a lithium citrate layer during battery charging and discharging. Specifically, during the first few lithium intercalation cycles, the organic citric acid molecules coating the silicon surface react in situ with lithium ions to generate a lithium-ion-rich lithium citrate inorganic-organic hybrid layer. This transformation is irreversible and is accompanied by the stabilization of the solid electrolyte interphase (SEI) film. Because this transformation occurs in situ under electrochemical driving, the resulting lithium citrate layer perfectly conforms to the surface morphology of the silicon particles, avoiding the uneven coverage or interfacial voids common in traditional manual coating processes.

[0024] This lithium citrate layer simultaneously functions as a lithium-ion conductor and an isolator between silicon and the sulfide solid-state electrolyte. On one hand, lithium citrate, as a lithium-containing organic salt, possesses a certain lithium-ion conductivity, providing a channel for rapid lithium-ion transport at the silicon / electrolyte interface and effectively reducing interfacial charge transfer impedance. On the other hand, the dense lithium citrate layer acts as a physical barrier, separating the micron-sized silicon particles from the sulfide solid-state electrolyte, blocking direct contact between them, and thus significantly suppressing active lithium loss and electrolyte decomposition caused by interfacial side reactions. During repeated lithium insertion and extraction processes, the lithium citrate layer also exhibits excellent mechanical flexibility, adapting to the volume breathing effect of silicon particles, maintaining the integrity of the electrode structure, and preventing particle fragmentation and interfacial failure due to volume expansion. This multifunctional interface design, integrating ion conduction, chemical isolation, and mechanical buffering, is the key to overcoming the bottleneck in the application of silicon anodes in sulfide all-solid-state batteries.

[0025] Based on the above embodiments, this embodiment further optimizes and verifies the battery material system and the process parameters of the citric acid coating layer. As a specific implementation, the sulfide solid electrolyte is Li6PS5Cl, and the cathode is lithium cobalt oxide or LiNi. 0.8 Co 0.1 Mn 0.1 O2. Specifically, Li6PS5Cl is a sulfide-germanium ore type electrolyte, possessing high room temperature ionic conductivity and good mechanical ductility, which is beneficial for forming a tight solid-solid contact with electrode materials during cold pressing; while lithium cobalt oxide (LCO) and LiNi... 0.8 Co 0.1 Mn 0.1 O2 (NCM811) is a high-voltage, high-specific-capacity cathode material, which, when matched with a modified silicon anode, can construct a high-energy-density all-solid-state battery system. It should be understood that although this embodiment lists the specific electrolyte and cathode material described above, in other embodiments, as long as the high ion conductivity characteristics of the sulfide electrolyte and the potential matching requirements of the cathode material are met, other similar materials can also be selected, without departing from the scope of protection of this invention.

[0026] To investigate the impact of citric acid coating thickness and uniformity on battery performance, a gradient comparison experiment was conducted in this embodiment. The silicon particles were micron-sized, and the citric acid coating was formed by treating the silicon particle surface with a 5%–20% citric acid aqueous solution. Within this concentration range, the thickness and density of the organic coating on the silicon particle surface could be precisely controlled by adjusting the concentration of the precursor solution. As a preferred embodiment, the concentration of the citric acid aqueous solution was 10%. This concentration has been shown to achieve an optimal balance between coating integrity and ion transport kinetics.

[0027] Combining the microscopic morphology characterization results, the structural differences under different concentrations of treatment can be clearly observed. As shown in the energy-dispersive X-ray spectroscopy (EDS) surface distribution map, the sample treated with 10% citric acid solution (10% CA@Si) exhibits the most uniform and dense carbon element distribution on its surface, indicating the formation of a continuous and complete coating layer. In contrast, the carbon signal of the 5% CA@Si sample is relatively sparse, indicating that the coating layer is too thin and may have local exposed areas, resulting in insufficient buffering capacity against silicon volume expansion during cycling. The 20% CA@Si sample shows obvious carbon element agglomeration bright spots, and the transmission electron microscopy (TEM) image shows that its coating layer thickness is significantly uneven. This uneven structure easily introduces stress concentration points during repeated expansion and contraction of silicon particles, inducing coating layer cracking or even detachment. Therefore, a concentration of 10% is a critical process window for achieving high-quality chemical bonding coating.

[0028] Electrochemical performance testing further verified the direct impact of the aforementioned microstructural differences on macroscopic performance. Unmodified pure silicon anodes were used as a control (Li-Si), and all-solid-state batteries were assembled with modified samples of different concentrations for testing. As shown in the cycle performance curves, after 1000 cycles at 2C, the battery using the 10% CA@Si anode maintained a capacity retention of 95.37%, which fully demonstrates that the citric acid-modified silicon anode material maintains a capacity retention of no less than 93.57% after 1000 cycles at 2C. In comparison, the 5% CA@Si sample maintained a capacity retention of 93.57%, which is better than the control but still slightly lower than the 10% sample; while the unmodified Li-Si anode experienced rapid capacity decay due to severe volume expansion and interfacial side reactions. Notably, when the concentration reached 20%, the capacity retention plummeted to 74.08%, attributed to the excessively thick and uneven coating layer increasing interfacial impedance and being prone to mechanical failure during cycling, thus hindering the effective transport of lithium ions. This non-linear performance change trend strongly supports the innovative approach of using a 10% concentration as the preferred value.

[0029] In terms of rate performance, the 10%CA@Si system exhibits excellent fast-charging adaptability. When the test rate is increased from 0.5 C to 5 C, its discharge capacity only decreases by 18%, indicating that the in-situ formed lithium citrate interface layer not only plays a physical isolation role but also constructs an efficient lithium-ion transport channel, significantly reducing interface polarization under high current density. In contrast, the unmodified sample shows severe polarization under the same conditions, with a capacity decay rate far exceeding that of the modified sample.

[0030] Furthermore, regarding the critical issue of volume expansion in silicon anodes, this embodiment employed cross-sectional scanning electron microscopy (SEM) for quantitative characterization. After 1000 long cycles, the electrode thickness of the unmodified Li-Si anode increased significantly, and obvious cracks and delamination appeared; while the electrode structure of the 10% CA@Si anode remained intact, maintaining close contact with the solid electrolyte layer. Calculations showed its volume expansion rate was only 155%. This result directly confirms that an appropriate amount of citric acid coating can effectively absorb the volume change stress of silicon particles through its flexibility, suppressing electrode structure pulverization and failure, thereby ensuring the long-cycle stability of the battery. In summary, 10% citric acid treatment is the optimal solution for achieving high-performance applications of silicon anodes in sulfide all-solid-state batteries, avoiding insufficient protection at low concentrations while overcoming the kinetic deterioration and stress concentration problems at high concentrations.

[0031] Furthermore, this embodiment provides a method for preparing a citric acid-modified silicon anode material. This method constructs a uniform organic coating layer on the surface of micron-sized silicon particles through an aqueous esterification reaction. Specifically, the preparation method includes the following steps: In step S100, micron-sized silicon powder is placed in an aqueous citric acid solution and heated and stirred at 50-70°C for 8-16 hours, during which periodic ultrasonic dispersion is performed. In this step, heating and stirring provide the thermodynamic conditions required for the esterification reaction, promoting the dehydration condensation reaction between the natural hydroxyl groups on the surface of the micron-sized silicon particles and the carboxyl groups in the citric acid molecules, forming stable chemical bonds. It should be understood that although this embodiment provides a temperature range of 50-70°C and a reaction time window of 8-16 hours, in other embodiments, as long as the esterification reaction can proceed sufficiently without damaging the bulk structure of the silicon particles, the specific temperature and time can be adaptively adjusted according to the scale of the reaction system and the concentration of citric acid. Periodic ultrasonic dispersion is a key process feature of this step, its function being to overcome the physical characteristic of micron-sized silicon powder's tendency to agglomerate in an aqueous medium. Through intermittent high-energy ultrasonic treatment, soft agglomerates can be continuously broken up, allowing fresh silicon surfaces to be continuously exposed to the citric acid solution, thereby ensuring the uniformity and integrity of the coating layer. Without this periodic dispersion step, high-concentration citric acid solutions are prone to localized supersaturation precipitation or uneven coating on the surface of aggregates, leading to stress concentration and performance degradation issues as seen in the 20% concentration sample in the previous examples.

[0032] In a preferred embodiment, the concentration of the citric acid aqueous solution in step S100 is 5% to 20%, the heating and stirring temperature is 60°C, the time is 12 hours, and ultrasonic dispersion is performed every 2 hours for 20 minutes each time. Under these preferred conditions, the esterification reaction kinetics reach an optimal equilibrium point: 60°C ensures a sufficient reaction rate while avoiding excessive evaporation of the aqueous solvent or excessive oxidation of the silicon surface that may result from excessively high temperatures; the 12-hour reaction time is sufficient to allow chemical bonding to approach saturation; and the rhythm design of "ultrasonic dispersion for 20 minutes every 2 hours" achieves a good trade-off between maintaining the particle dispersion state and avoiding mechanical damage to the silicon particles caused by prolonged continuous ultrasonication. Experiments show that the 10%CA@Si material prepared using this preferred process has the most uniform and dense distribution of carbon elements on its surface, laying a solid materials science foundation for the subsequent electrochemical performance.

[0033] Step S200 involves filtering and washing the product obtained in step S100 to remove unreacted citric acid. Specifically, this step typically employs Buchner funnel filtration or centrifugation to achieve solid-liquid separation, followed by repeated washing with deionized water. This step is crucial for ensuring the electrochemical activity of the final product. Residual free citric acid not only introduces impurities during battery assembly but may also undergo uncontrollable decomposition reactions during subsequent electrochemical cycles, consuming active lithium and increasing interfacial impedance. Only through thorough washing can it be ensured that only a chemically bonded citric acid coating layer remains on the silicon surface, rather than physically adsorbed excess organic matter, thus guaranteeing the purity and stability of the electrode interface.

[0034] Step S300 involves vacuum drying and grinding to obtain citric acid-modified silicon anode material. Drying in a vacuum environment effectively lowers the boiling point of water, preventing damage to the heat-sensitive organic coating layer caused by high-temperature drying, while thoroughly removing moisture to prevent hydrolysis failure of the sulfide electrolyte during subsequent battery assembly. The grinding process depolymerizes any slight hard agglomerates that may occur during drying, restoring the powder's flowability and dispersibility to meet the process requirements for electrode slurry preparation or dry electrode film formation. Through the synergistic process flow of steps S100 to S300, this invention successfully achieves the preparation of high-quality chemically bonded citric acid-coated silicon anode material in a mild aqueous system. This method has significant advantages such as simple operation, environmental friendliness, low cost, and ease of large-scale scaling.

[0035] Based on the above embodiments, this embodiment further verifies the electrochemical performance and reliability of the citric acid-modified silicon anode material in near-real-world commercial application scenarios, such as high areal capacity and high voltage cathode matching. As a specific implementation method, the citric acid-modified silicon anode material has an areal capacity of 3~10 mAh / cm². 2Under these conditions, the initial coulombic efficiency is no less than 77%. Specifically, when assembling an all-solid-state battery using a 10% CA@Si anode, as the electrode areal capacity increases from 3 mAh / cm², the efficiency is significantly improved. 2 Gradually increase to 10 mAh / cm 2 Although the initial coulombic efficiency of the battery shows a certain downward trend, it still reaches as high as 10 mAh / cm². 2 Under extreme loading conditions, its initial coulombic efficiency remains at 77%, with a corresponding discharge capacity of 131 mAh / g. This result demonstrates that even with a significant increase in specific surface area due to high-activity material loading, the in-situ formed lithium citrate interface layer can effectively reduce irreversible lithium loss caused by side reactions. The underlying mechanism is that the uniform and dense lithium citrate layer not only provides ample lithium-ion transport channels but also acts as an artificial SEI film to pre-stabilize the silicon anode surface, preventing direct contact and decomposition of the fresh silicon surface with the sulfide electrolyte at high potentials, thus ensuring energy conversion efficiency under high energy density designs.

[0036] Meanwhile, as a specific implementation method, the citric acid-modified silicon anode material showed no short-circuit phenomenon after 30 cycles at a 0.2 C rate. As shown in the cycle test curve, the areal capacity is 3 mAh / cm². 2 Under these conditions, the battery operated stably at a 0.2 C rate for 30 cycles, during which the voltage curve remained smooth without abnormal fluctuations, and no micro-short circuits or internal short circuit failures occurred. This fully demonstrates that the citric acid coating layer still possesses excellent mechanical integrity and interface stability under high load conditions. It should be understood that high areal capacity electrodes are often accompanied by greater local stress concentration and more significant volume changes, which can easily induce internal short circuits caused by lithium dendrite penetration or particle pulverization. In this invention, the flexible buffering properties and chemical isolation function of the lithium citrate layer play a crucial role, effectively suppressing electric field distortion and dendrite growth at the interface, ensuring the safety and reliability of the battery under practical thick electrode conditions.

[0037] To further evaluate the practical application potential of this technology in a full-cell system, this embodiment also replaces the cathode material with a high-nickel ternary material, LiNi. 0.8 Co 0.1 Mn 0.1 An all-solid-state battery system, NCM811|Li6PS5Cl|Li-10%CA@Si, was constructed using O2 (NCM811) and validated through long-term cycling at high current density. The system achieved a current density of 3.31 mA / cm². 2At a high current density (approximately 2C rate), the full cell retains a capacity retention of 78.1% after 1000 cycles, with a coulombic efficiency consistently above 99.9%. This performance significantly outperforms traditional unmodified silicon anode systems and is even comparable to some graphite-based all-solid-state batteries. This demonstrates that the citric acid coating modification strategy is not only suitable for laboratory-level half-cell or low-load testing but also withstands the multiple challenges of high-voltage cathode oxidation, high-current-density shocks, and long-cycle mechanical stress. In summary, this invention confirms that the citric acid-modified silicon anode material exhibits excellent comprehensive performance in practical applications such as high areal capacity, high rate, and full-cell matching, possessing extremely high industrial application value.

[0038] Furthermore, to further verify the performance of the materials in this invention in detail, the present invention provides the following embodiments: First, the preparation methods of the materials, the preparation methods of the battery, and the detection methods of each material in this embodiment are as follows: Material preparation: Li 5.5 PS 4.5 Cl 1.5 The powder was provided by Zhongke Sol Energy Technology Co., Ltd. The silicon particles were provided by Tianmu Energy Anode Materials Co., Ltd. The vapor-grown carbon fiber (VGCF) used in the cathode composite material was purchased from Showa Denko Co., Ltd. The PTFE binder was provided by Daikin Fluorochemicals (China) Co., Ltd. Citric acid was provided by Sinopharm Chemical Reagent Co., Ltd.

[0039] Solid-state battery fabrication and electrochemical testing: Negative electrode preparation: The lithium metal negative electrode is made by manually punching a 30μm thick lithium strip using a 9mm diameter circular punch. The silicon negative electrode is prepared by mixing micron-sized silicon and PTFE in a 98:2 ratio, first pre-grinding it into a block in a mortar, then rolling it into a 40μm thick silicon film using a rolling mill, and finally manually punching it using a 10mm diameter circular punch.

[0040] Preparation of composite cathode powder: LiNi cathode active material 0.8 Co 0.1 Mn 0.1 O2 (NMC811) or LiCoO2 (LCO), Li 5.5 PS 4.5 Cl 1.5 The positive electrode active material and VGCF are mixed uniformly at a ratio of 60:35:5. The mixing process first involves thoroughly mixing the positive electrode active material and the electrolyte, and then adding VGCF for uniform mixing.

[0041] Assembly of sulfide-based all-solid-state batteries: Take 80 mg Li 5.5 PS 4.5 Cl 1.5Electrolyte powder was placed in a mold. Pre-compression was performed for 1 minute at 124 MPa (1 ton). Positive electrode powder was evenly distributed on one side of the solid electrolyte and compacted at 124 MPa (1 ton). Subsequently, silicon and lithium metal negative electrode sheets were placed sequentially on the other side of the solid electrolyte, and the mold was assembled. The pressure was maintained at 868 MPa (7 tons) for 3 minutes, then depressurized to 248 MPa (2 tons) and the battery screws were tightened to fabricate the all-solid-state battery. All preparation steps were performed in an argon-filled glove box (O2 < 0.1 ppm, H2O < 0.1 ppm). The battery was tested at 55°C with a voltage range set between 2.5 and 4.2 V.

[0042] like Figure 1 As shown in Figures (a) and (b), three citric acid aqueous solutions with concentrations of 5%, 10%, and 20% were prepared. Equal masses of micron-sized silicon powder were placed in each of the three different citric acid aqueous solutions, and then heated / stirred at 60°C for 12 hours. The natural hydroxyl groups on the surface of the silicon particles reacted with the carboxyl groups in the citric acid molecules, causing small-molecule citric acid to coat the surface of the silicon particles. During this process, ultrasonic dispersion was performed for 20 minutes every 2 hours to inhibit the agglomeration of silicon particles and ensure a more uniform coating of citric acid on the surface of the silicon particles. After heating and stirring, the citric acid solution containing silicon powder was filtered using a Buchner funnel, and deionized water was repeatedly added to remove excess citric acid solution. The resulting product was vacuum dried and ground to obtain citric acid-coated modified silicon particles. Subsequently, the silicon particles were mixed and ground with PTFE as a binder, and then rolled to obtain a silicon anode electrode film.

[0043] The morphology of micron-sized silicon powder and its coatings treated with citric acid solutions of different concentrations was studied using scanning electron microscopy (SEM), energy-dispersive X-ray spectroscopy (EDS), and transmission electron microscopy (TEM). Morphological characteristics are as follows: Figure 2 Figures (a), (b), and (c) show the micron-sized silicon powder particles. These particles consist of irregular polyhedral particles. No significant morphological differences were observed between the three samples and the original micron-sized silicon, indicating that the citric acid aqueous solution treatment did not alter the microstructure of the silicon particles. EDS analysis revealed… Figure 2Figures (d), (e), and (f) show the distribution of carbon (C) on the silicon surface, where the C originates from the citric acid coating. These results indicate that the C distribution is most uniform and dense in 10%CA@Si, while 5%CA@Si and 20%CA@Si exhibit different problems. The insufficient citric acid distribution on the 5%CA@Si surface may lead to insufficient buffering capacity against silicon volume expansion during battery cycling. The EDS spectrum of 20%CA@Si shows significant C bright spots, indicating inhomogeneity and significant agglomeration in the citric acid coating. This may introduce stress gradients into the coating during silicon volume changes, leading to coating failure. Finally, TEM measurements were performed to further analyze the citric acid coating on the silicon surface. Figure 2 As shown in Figures (g), (h), and (i), the coating thickness gradually increases with increasing citric acid solution concentration. Figure 1 As clearly seen in Figure (i), the coating layer exhibits significant thickness inhomogeneity after treatment with 20% citric acid solution.

[0044] To verify that citric acid is coated onto the silicon particle surface through a reaction between hydroxyl and carboxyl groups via heating and stirring, rather than simple mechanical mixing, X-ray photoelectron spectroscopy (XPS) was performed on 5% CA@Si, 10% CA@Si, and 20% CA@Si. The results showed that carbon-containing chemical bonds were clearly present on the silicon particle surface. Figure 3 , Figure 4 , Figure 5 The C 1s energy spectra of 5% CA@Si, 10% CA@Si, and 20% CA@Si are shown. The peak at approximately 289.2 eV originates from the esterification reaction between the carboxyl group of citric acid and the silicon surface, forming C=O-(OR). Analysis of the Si 2p energy spectrum (…) Figure 6 , Figure 7 , Figure 8 Similar verification results can be obtained. The peak at approximately 103.4 eV corresponds to Si-O-(O)R. The formation of additional Si-O-(O)R peaks further confirms a significant esterification reaction between silicon particles and the carboxyl functional groups of citric acid. The O 1s(O)R peaks at 532.5 eV and 534 eV also show similar results. Figure 9 , Figure 10 , Figure 11 The peak reflects the natural oxide layer formed when silicon and carbon are exposed to air.

[0045] To verify the differences in electrochemical performance of 5%CA@Si, 10%CA@Si, and 20%CA@Si anodes in sulfide ASSBs, this invention used a Li6PS5Cl (LPSCl) SE layer, an LCO composite cathode, and Li-Si, Li-5%CA@Si, Li-10%CA@Si, and Li-20%CA@Si anodes. The assembled ASSBs were first activated by cycling once at 0.1C to initially alloy the lithium foil with the silicon anode sheet. Subsequently, they were activated at 2C (1 mA / cm²). 2 The battery was cycled under these conditions. In the initial cycling phase, the coulombic efficiency was low because the CA coating layer formed lithium citrate during early cycles, which contributed to the formation of the SEI layer and consumed some active lithium. However, as cycling progressed, the SEI layer gradually stabilized, and lithium from the lithium citrate could leach out and participate in the reaction. Therefore, after a certain number of cycles, the coulombic efficiency stabilized above 99.9%. Furthermore, the lithium citrate layer mitigated the rapid reaction between silicon and sulfide SEs, promoting the formation of a stable SEI layer and enhancing the battery's long-term cycling performance. Figures 12-16 As shown, full cells assembled using Li-5%CA@Si and Li-10%CA@Si anodes exhibited better cycling performance at 2C rate, with capacity retention of 93.57% and 95.37% respectively after 1000 cycles. The average specific discharge capacity of the Li-10%CA@Si system was slightly higher than that of the Li-5%CA@Si system. However, when using Li-20%CA@Si as the anode, the cycling performance showed a significant decline, with a capacity retention of only 74.08% after 1000 cycles. Nevertheless, compared with the unmodified Li-Si anode system, all three systems showed significantly improved cycling performance, which is attributed to the optimizing effect of the citric acid coating on the silicon anode. Although the results indicate that the coating of Si particles treated with 5% CA solution is not as dense as that with 10% concentration, the volume change of Si is relatively small at low current densities. Therefore, the cycling performance of Li-5%CA@Si and Li-10%CA@Si ASSBs is similar. However, compared with the Li-Si system without CA coating, the performance of ASSBs is significantly improved.

[0046] To further verify the enhancing effect of the CA coating layer on the electrochemical performance of silicon anodes in ASSBs, rate performance tests were conducted on full cells with different anode systems. For example... Figure 17As shown, the Li-10%CA@Si system exhibits the best rate performance, with the specific discharge capacity decreasing from 158 mAh / g to 130 mAh / g, a drop of only 18%. The ASSBs of the Li-5%CA@Si and Li-10%CA@Si systems show little difference in discharge capacity at different rates, but with increasing current density, the capacity decay of the Li-5%CA@Si system is more pronounced than that of the Li-10%CA@Si system, while the Li-Si system exhibits the worst rate performance. (See the voltage-specific capacity curves at different rates.) Figures 18-21 The CA coating can alleviate the polarization of ASSBs at high current densities. This is because CA enables the formation of lithium citrate and a stable SEI in silicon during the initial charge-discharge cycles. This optimized silicon interface is beneficial for Li... + The rate performance results are in high agreement with the cycling performance results described above, indicating that the CA coating significantly enhances the electrochemical performance of the silicon anode in ASSBs.

[0047] Furthermore, the differential capacity curves reflect the changes in electrode performance during battery charge and discharge. When the battery is activated at a 0.1C rate, the differential capacity curves of the Li-Si, Li-5%CA@Si, Li-10%CA@Si, and Li-20%CA@Si anode systems in ASSBs (e.g.) are shown below. Figure 22 The results show that the peak positions in the positive potential region (upper half) are basically the same. The positive potential region usually corresponds to the intercalation and deintercalation process of active ions in the cathode material. Since the same cathode material is used, the intercalation and deintercalation potentials are the same, so the peak positions are consistent. In the negative potential region (lower half), the presence of the CA coating layer, combined with the differences in the coating layer caused by different concentrations of CA solution, leads to changes in the lithium intercalation potential, thus causing differences in peak positions. When the rate increases to 2C, the current density increases, and the peak positions of ASSBs in the Li-Si, Li-5%CA@Si, Li-10%CA@Si, and Li-20%CA@Si anode systems all show slight changes compared to 0.1C (e.g., ...). Figure 23 As cycling time at 2C increases, their differential capacity curves show significant differences. For Li-Si anode ASSBs (such as...), Figure 24 With increasing cycle number, the oxidation peak significantly decreased until it was almost nonexistent. The reduction peak initially sharpened but broadened significantly after 400 cycles. The peak value also decreased rapidly, mainly due to the significant volume expansion of silicon. Although the lithium foil used can form a lithium-silicon alloy, the initial sharpening of the reduction peak is attributed to the improved lithium-ion transport efficiency due to lithium-silicon alloying. However, the limited amount of lithium foil had little effect on suppressing volume expansion. The broadening of the reduction peak also indicates that the structural damage caused by volume expansion reduces lithium-ion transport efficiency. Differential capacity curves of the Li-5%CA@Si and Li-10%CA@Si anode systems (e.g.) Figures 25-26 Similar changes were observed with increasing cycle number. The oxidation peak shifted significantly to the lower voltage region, while the reduction peak showed a trend towards the higher voltage region. The voltage difference between the two peaks decreased significantly, indicating a significant reduction in the polarization of the ASSBs. Furthermore, the width of the reduction peak remained stable during cycling, indicating that no significant volume expansion led to damage to the anode structure and a subsequent decrease in the ion diffusion rate. For Li-20%CA@Si anode ASSBs (such as... Figure 27 Excessive and uneven CA coating leads to additional side reactions in the later stages of the cycle, resulting in decreased peak intensity and the appearance of impurity peaks.

[0048] Furthermore, using electrochemical impedance spectroscopy (EIS), the impedance changes of ASSBs with Li-Si, Li-5%CA@Si, Li-10%CA@Si, and Li-20%CA@Si anodes were recorded before cycling and after different cycles. Before cycling, the impedance differences among the four types of cells were relatively small (e.g., ...). Figure 29 However, after a certain number of cycles, significant differences in impedance emerged. Full cells using unmodified Li-Si anodes without CA coating showed no significant change in impedance during cycling (e.g., ...). Figure 30 Although silicon wafers continue to alloy under the influence of lithium ions during battery cycling. Figure 28 As shown, the XRD pattern of the negative electrode after cycling not only shows obvious Si peaks, but also shows Li peaks. 13 Si4 and Li 12 The characteristic peaks of Si7 indicate that the lithium-silicon alloying process continues throughout the cycle. Compared to the alloying effect under pressure during battery assembly, the Li in XRD... 13 Si4 and Li 12 Si7 exhibits significantly lower characteristic peak intensities. The lithium-silicon alloying process improves lithium-ion transport efficiency on the anode side, thereby reducing battery impedance. However, the unmodified silicon anode exhibits significant volume expansion during cycling, leading to electrode structure damage and contact failure between the anode sheet and the electrolyte membrane, resulting in poor contact and increased battery impedance. For Li-5%CA@Si, Li-10%CA@Si, and Li-20%CA@Si anodes, the introduction of the CA coating layer suppresses silicon volume expansion to maintain electrode structural integrity. Furthermore, CA participates in the formation of a stable SEI layer, ensuring good interfacial contact between the electrode sheet and the electrolyte, thus continuously improving Li-ion transport efficiency. + Transmission efficiency. This causes the battery resistance to decrease as cycling progresses (e.g., ...). Figures 31-33In contrast, the Li-10%CA@Si anode exhibits the densest and most uniform CA coating layer, demonstrating the most significant modification effect and resulting in the most pronounced reduction in impedance during battery cycling. This allows the battery capacity to remain stable, preventing significant performance degradation that occurs with cycling.

[0049] Furthermore, the treated Si undergoes repeated expansion and contraction during lithium deintercalation and intercalation, leading to gradual cracking and eventual pulverization into powder (e.g. Figure 34 (As shown in Figure (a)). However, after coating with a citric acid layer, the citric acid layer forms a stable lithium citrate layer during the initial few lithium deintercalation and intercalation cycles, thereby protecting the silicon (as shown in Figure (a)). Figure 34 As shown in Figure (b)). On the negative electrode side, this protection manifests as protecting the structural integrity of the negative electrode and suppressing its volume change. To more clearly demonstrate the role of the citric acid coating in suppressing volume expansion, SEM measurements were performed on the cross-section of the negative electrode after 1000 cycles, as shown in Figure (b). Figure 35 As shown, after 1000 cycles, the thickness of the Li-Si anode increased to 62 μm. Due to mechanical stress caused by volume change, the anode separated from the SE layer, and obvious cracks appeared in the cross-section of the anode, severely impairing lithium-ion transport—a key factor in the rapid capacity decay of the battery. The thickness changes of Li-5%CA@Si and Li-10%CA@Si were relatively small, at 59.9 μm and 45.7 μm respectively, and the electrode structure remained intact with good contact with the SE layer. The Li-20%CA@Si anode exhibited uneven CA coating, resulting in uneven stress distribution and obvious volume expansion and microcracks. However, due to the participation of the citric acid layer in the formation of a stable SEI, no separation occurred between the electrode and the SE layer. To provide a clearer comparison, SEM and EDS tests were also performed on the cross-section of the anode side without any electrochemical testing. Before cycling, the thickness of the lithium-silicon alloy anode under pressure was only 29.4 μm, and due to the lack of SEI layer formation, it did not have good adhesion to the electrolyte. Compared with the cycled sample, the volume expansion rates of Li-Si, Li-5%CA@Si, Li-10%CA@Si, and Li-20%CA@Si were 211%, 203%, 155%, and 241%, respectively. In conclusion, an appropriate citric acid coating can indeed improve the volume expansion problem of silicon anodes.

[0050] Furthermore, CA coating modification also improves the performance of silicon anodes at high areal capacities, such as... Figure 36 , Figure 37 As shown. The Li-10%CA@Si anode ASSBs have an areal capacity of 3 mAh / cm². 2It exhibited 81.2% capacity retention, but the capacity decreased from 145.33 mAh / g to 117.98 mAh / g as the test rate increased from 0.1C to 1C. No short circuit occurred after 30 cycles at 0.2C. The surface capacity is 3 mAh / cm². 2 5 mAh / cm 2 and 8 mAh / cm 2 At that time, the initial efficiency of SASSB was above 90%. When the capacity reached 10 mAh / cm³, 2 At that time, the initial efficiency dropped significantly to 77%, but it still had a discharge capacity of 131 mAh / g. Figure 38 This indicates that the CA-modified silicon anode exhibits stable charge-discharge performance under high areal capacity conditions.

[0051] To further verify its cycling stability at high current densities, the cathode material was replaced with NCM811, and the best-performing Li-10%CA@Si anode was used. The assembled full cell achieved a cycle stability of 3.31 mA / cm². 2 Cycling at a current density of 1000 times yielded the following results: Figure 39 As shown, the coulombic efficiency remained consistently above 99.9%, and the capacity retention reached 78.1%.

[0052] In summary, this invention uses citric acid as a coating material to modify the silicon surface. The degree of coating is controlled by adjusting the concentration of the citric acid solution. An appropriate amount of citric acid coating can form a stable lithium citrate layer on the silicon anode surface during battery operation, suppressing volume expansion and reducing side reactions between silicon and SE, thereby forming a stable SEI layer. This ensures that the silicon anode maintains its structural integrity after long-term cycling, significantly improving the rate performance of ASSBs. However, when the citric acid solution concentration is too high, it leads to an excessively thick and uneven coating layer, negatively impacting the anode and affecting the electrochemical performance of ASSBs.

[0053] Using a lithium cobalt oxide cathode, ASSBs assembled from LPSCl solid electrolyte and Li-10%CA@Si exhibited a high capacity retention of 95.26% after 1000 cycles at 2C rate, with only a 18% capacity decrease as the rate increased from 0.5C to 5C. High-load ASSBs also showed a reversible capacity exceeding 130 mAh / g at 1C rate. Even when NCM811 was used instead of the lithium cobalt oxide cathode, the capacity remained at 3.31 mA / cm². 2 After 1000 cycles at a current density, the capacity retention rate remained at 78%. This invention demonstrates that inexpensive and readily available citric acid, as a surface coating layer for silicon anodes, can effectively solve the volume expansion problem of silicon anodes, thus opening up new possibilities for the practical application of silicon anodes in ASSBs.

[0054] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A sulfide all-solid-state battery, characterized in that, include: positive electrode; Sulfide solid electrolytes; as well as Citric acid modified silicon anode material, wherein the citric acid modified silicon anode material comprises micron-sized silicon particles; And a citric acid coating layer covering the surface of the micron-sized silicon particles; wherein the citric acid coating layer is formed by an esterification reaction between the natural hydroxyl groups on the surface of the micron-sized silicon particles and the carboxyl groups in the citric acid molecules; the citric acid coating layer is converted into a lithium citrate layer during battery charging and discharging, and the lithium citrate layer has both lithium-ion conduction function and the function of isolating silicon from sulfide solid electrolyte.

2. The sulfide all-solid-state battery according to claim 1, characterized in that, The sulfide solid electrolyte is Li6PS5Cl, and the cathode is lithium cobalt oxide or LiNi. 0.8 Co 0.1 Mn 0.1 O2.

3. The sulfide all-solid-state battery according to claim 1, characterized in that, The micron-sized silicon particles have a particle size of micron, and the citric acid coating layer is formed by treating with a citric acid aqueous solution with a concentration of 5% to 20%, preferably, the concentration of the citric acid aqueous solution is 10%.

4. The sulfide all-solid-state battery according to claim 3, characterized in that, The citric acid-modified silicon anode material retains no less than 93.57% of its capacity after 1000 cycles at a 2C rate.

5. The sulfide all-solid-state battery according to claim 3, characterized in that, The citric acid-modified silicon anode material exhibits a capacity decay of 18% when the rate of change is increased from 0.5 C to 5 C.

6. The sulfide all-solid-state battery according to claim 3, characterized in that, The citric acid-modified silicon anode material has an areal capacity of 3 ~ 10 mAh / cm². 2 Under these conditions, the initial coulomb efficiency is no less than 77%.

7. The sulfide all-solid-state battery according to claim 3, characterized in that, The citric acid-modified silicon anode material showed no short circuit after 30 cycles at a 0.2 C rate.

8. The sulfide all-solid-state battery according to claim 3, characterized in that, The volume expansion rate of the citric acid modified silicon anode material after 1000 cycles is 155%.

9. The sulfide all-solid-state battery according to claim 1, characterized in that, The preparation method of the citric acid modified silicon anode material includes the following steps: a) Place micron-sized silicon powder in an aqueous citric acid solution and heat and stir at 50-70°C for 8-16 hours, during which periodic ultrasonic dispersion is performed; b) Filter and wash the product obtained in step a) to remove unreacted citric acid; c) Vacuum drying and grinding are performed to obtain the citric acid modified silicon anode material.

10. The sulfide all-solid-state battery according to claim 9, characterized in that, The concentration of the citric acid aqueous solution in step a) is 5%~20%, the heating and stirring temperature is 60℃, the time is 12 hours, and the ultrasonic dispersion is performed once every 2 hours for 20 minutes each time.