Electrolytes and their use in lithium-based batteries
By designing an electrolyte containing specific lithium salts and carbonate solvents, and combining it with an anion-involved solvation structure, the problem of poor performance of lithium-ion batteries at extreme temperatures was solved, achieving high voltage stability and efficient ion transport, thereby improving the energy density and lifespan of the battery.
Patent Information
- Application Number
- CN202511732979.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2025-09-11
- Filing Date
- 2025-11-24
- Publication Date
- 2026-11-17
AI Technical Summary
Conventional lithium-ion batteries perform poorly under extreme temperatures. Ion transport is hindered at low temperatures, and they are prone to decomposition at high temperatures, producing corrosive byproducts that affect energy density and lifespan.
A ternary lithium salt system comprising lithium tetrafluoroborate, lithium difluorooxalate borate, and lithium difluorodioxalate phosphate is mixed with a carbonate solvent. Through a cation-anion solvation engineering strategy, a stable cathode-electrolyte intermediate phase is formed, optimizing ionic conductivity and high voltage stability.
It maintains good performance over a wide temperature range, stabilizes the cathode interface at high voltage, improves the capacity retention and coulombic efficiency of lithium-ion batteries, and extends battery life.
Smart Images

Figure CN123120867A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an electrolyte, for example, specifically but not exclusively, an electrolyte for lithium-based batteries and the use of said electrolyte in said lithium-based batteries. Background Technology
[0002] The rapid development of consumer electronics and electric vehicles has driven unprecedented demand for lithium-ion batteries (LIBs), which offer high energy density and reliable performance at extreme temperatures—alleviating range anxiety for long-distance EVs and unlocking applications from the cold plains of Northeast China and the deep ocean to the vacuum of space.
[0003] However, conventional lithium-ion batteries (LIBs) rely on ethylene carbonate (EC)-based electrolytes and lithium hexafluorophosphate (LiPF6), which typically perform poorly under harsh conditions. For example, at low temperatures, the high viscosity and desolvation of EC hinder ion transport, thus limiting the performance of low-temperature LIBs. In particular, the capacity retention of conventional LIBs below 0°C often drops to less than 25% of their room-temperature capacity. At high temperatures (≥45°C), LiPF6 is prone to thermal decomposition. This leads to the formation of corrosive byproducts such as phosphorus pentafluoride (PF5) and hydrogen fluoride (HF), subsequently triggering solvent decomposition and structural degradation of the electrode materials. Moreover, the inefficient cathode (positive electrode) surface cathode (positive electrode)-electrolyte interphase (CEI) formed by conventional carbonate-based electrolytes exacerbates the irreversible phase transition of the cathode material at high voltages (e.g., 4.6 V). These problems hinder the overall energy density and lifetime of LIBs.
[0004] Therefore, the present invention attempts to eliminate or at least mitigate these disadvantages by providing new or other improved electrolytes for lithium-based batteries, especially lithium-ion batteries. Summary of the Invention
[0005] In a first aspect of the invention, an electrolyte for a lithium-based battery is provided, comprising a mixture of at least three lithium salts and a carbonate solvent, wherein the at least three lithium salts are selected from the group consisting of lithium tetrafluoroborate (LiBF4), lithium difluorooxalate borate (LiDFOB), lithium difluorodioxalate phosphate (LiDFBP), lithium bis(fluorosulfonyl)imide (LiFSI), and lithium bis(trifluoromethanesulfonyl)imide (LiTFSI).
[0006] Optionally, the at least three lithium salts comprise lithium tetrafluoroborate (LiBF4), lithium difluorooxalate borate (LiDFOB), and lithium difluorodioxalate phosphate (LiDFBP).
[0007] Optionally, lithium tetrafluoroborate (LiBF4), lithium difluorooxalate borate (LiDFOB), and lithium difluorodioxalate phosphate (LiDFBP) have a molar ratio of 4:4:3.
[0008] Optionally, the at least three lithium salts have a total concentration of about 0.5 M to about 1.5 M.
[0009] Optionally, the at least three lithium salts have a total concentration of about 1.1 M.
[0010] Optionally, the carbonate solvent mixture comprises propylene carbonate (PC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), and fluoroethylene carbonate (FEC).
[0011] The optional propylene carbonate (PC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), and fluoroethylene carbonate (FEC) have a volume ratio of a:b:c:d, where a is about 2-5, b is about 3-5, c is about 1-3, d is about 1-2, and a+b+c+d=1.
[0012] Optionally, the electrolyte also includes additives selected from the group consisting of vinylene carbonate (VC), 1,3-propanesulfonate lactone (PS), ethylene difluorocarbonate (DFEC), tri-(trimethylsilane)borate (TMSB), methane disulfonate methylene (MMDS), and tri-(trimethylsilane)phosphate (TMSP) and combinations thereof.
[0013] Optionally, the mass of the additive is 5% or less of the total mass of the electrolyte.
[0014] Optionally, the decomposition voltage of the electrolyte is approximately 4 μA cm⁻¹. -2 The cutoff current density measured by linear sweep voltammetry (LSV) is approximately 4.43 V (relative to Li / Li). + ).
[0015] In an optional embodiment, the electrolyte is kept in liquid form at a temperature of about -80°C to about 45°C.
[0016] Optionally, the electrolyte is stable at temperatures below or equal to about 80°C for at least 140 hours.
[0017] In a second aspect of the invention, a lithium-based battery is provided, comprising: a cathode (positive electrode) including a cathode active material selected from lithium cobalt oxide (LCO), lithium iron phosphate (LFP), lithium manganese oxide (LMO), lithium manganese iron phosphate (LMFP), nickel-cobalt-manganese nickel-rich material (nickel-rich NCM), nickel-cobalt-aluminum nickel-rich material (nickel-rich NCA), and graphite; an anode (negative electrode); and an electrolyte comprising at least three lithium salts selected from lithium tetrafluoroborate (LiBF4), lithium difluorooxalate borate (LiDFOB), and lithium difluorodioxalate phosphate (LiDFBP), and a carbonate solvent mixture selected from propylene carbonate (PC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), and fluoroethylene carbonate (FEC).
[0018] In an optional embodiment, the cathode comprises a cathode active material of lithium cobalt oxide, and the anode comprises an anode active material selected from the group consisting of graphite, silicon, lithium metal, silicon-carbon composites, and silicon dioxide.
[0019] Optionally, the cathode comprises a graphite cathode active material, and the anode comprises an anode active material selected from the group consisting of lithium metal, silicon, silicon-carbon composites, and silicon dioxide.
[0020] Optionally, the cathode comprises a cathode active material of lithium iron phosphate, lithium manganese oxide, lithium manganese iron phosphate, nickel-cobalt-manganese-rich material, or nickel-cobalt-aluminum-rich material, and the anode comprises an anode active material selected from the group consisting of graphite and lithium metal.
[0021] Optionally, the cathode mass loading is approximately 6.6 mg cm⁻¹. -2 .
[0022] Optionally, the mass loading of the anode is approximately 2.0 mg cm⁻¹. -2 Approximately 4.0 mg cm -2 .
[0023] In one optional embodiment, the lithium-based battery has an average coulombic efficiency of at least 99% when operating at a voltage of at least 4.6 V and a temperature of about 45 °C.
[0024] Optionally, the electrolyte is arranged to form a cathode-electrolyte interphase (CEI) on the cathode at a voltage of about 4.6 V to stabilize the interface phase of the cathode at the high voltage.
[0025] Optionally, the cathode-electrolyte intermediate phase is uniformly distributed on the cathode surface, and its thickness is from about 7 nm to about 20 nm.
[0026] Optionally, the cathode-electrolyte intermediate phase includes LiF with a concentration gradient, such that the LiF concentration on the side closer to the cathode surface is higher than the LiF concentration on the side farther from the cathode surface. Attached Figure Description
[0027] The invention will now be described more specifically by way of example only with reference to the accompanying drawings, in which: Figure 1 This is a schematic diagram illustrating the synergistic cation-anion solvation engineering strategy of customized electrolytes, which achieves excellent performance over a wide temperature range and at high voltage by controlling solvent-salt interactions and promoting protective anion-induced CEI. Figure 2 Different carbonate solvents with Li were shown. + The binding energy; Figure 3A The Li-based basis set calculation based on B3LYP / 6-311++G(d,p) is shown. + - Solvent binding energy; Figure 3B This demonstrates Li based on basis set calculations using B3LYP / DGDZVPS. + - Solvent binding energy; Figure 3C The Li-based basis set calculation based on M062X / 6-311++G(d,p) is shown. + - Solvent binding energy; Figure 4 The minimum and maximum electrostatic potentials (ESP) of the solvent are shown. min and ESP max )able; Figure 5 A comparison of the physicochemical properties of different carbonate solvents is shown; Figure 6 The freezing and boiling points of different carbonate solvents are shown; Figure 7 It is a table summarizing the key physical properties of different carbonate solvents; Figure 8 This is a table summarizing and comparing the physical and chemical properties of different solvents. ε refers to dielectric constant; η refers to viscosity; FE refers to freezing point; Li-solvent refers to Li + - Solvent binding energy; HOMO refers to Li + - HOMO energy of the solvent; Figure 9 The HOMO energies of the components in the designed electrolyte system are shown; Figure 10 The radial distribution function (RDF) and corresponding coordination number of the basic electrolyte are shown; Figure 11The radial distribution function (RDF) and corresponding coordination number of the designed electrolyte are shown. Figure 12 Li was shown + Binding energies between different anions. The basis set is B3LYP / 6-311++G(d,p), and single-point energies are calculated using DMSO as an implicit solvent. Figure 13 Different electrolytes are shown 7 Li NMR spectrum; Figure 14 The LSV curves of the basic electrolyte and the designed electrolyte are shown; Figure 15 Li in different solvation structures is shown + Desolvation energy; Figure 16 The results show the base electrolyte before and after storage at 80°C for 144 hours. 19 F NMR spectrum; Figure 17 The results show the base electrolyte before and after storage at 80°C for 144 hours. 1 H NMR spectrum; Figure 18 The designed electrolyte is shown before and after storage at 80°C for 144 hours. 19 F NMR spectrum (left) and 1 1H NMR spectrum (right); Figure 19 The basic electrolyte and designed electrolytes are shown from 30°C to DSC spectrum at 85℃; Figure 20 Optical images of the base electrolyte and the designed electrolyte are shown at different temperatures, where 1 and 2 refer to the base electrolyte and the designed electrolyte, respectively; Figure 21 The temperature-dependent ionic conductivity of the base electrolyte and the designed electrolyte is shown; Figure 22 The long-term cycling performance of the Li||LCO half-cell at 25 °C (2.7–4.6 V) is shown. Compared to Li / Li + ); Figure 23 The cycling performance of different Li||LCO half-cells using different batches of electrolyte is shown; Figure 24 The charging and discharging spectra of Li||LCO half-cells using the basic electrolyte (left) and the designed electrolyte (right) are shown at 25 °C. Figure 25A The charge / discharge profiles and activation cycle CE of the Li||LCO half-cell using the base electrolyte are shown. Figure 25B The charge / discharge profile and activation cycle CE of a Li||LCO half-cell using the designed electrolyte are shown. Figure 25C The CE (Cycles Efficiency) during long-term cycling and the average CE calculated after 200 cycles are shown for Li||LCO half-cells using different electrolytes. The designed electrolyte has an average CE of 99.45% after 400 cycles. Figure 26 The cycling performance of the Li||LCO half-cell at 45°C is shown. Figure 27A The charging and discharging spectra of Li||LCO half-cells using the basic electrolyte (left) and the designed electrolyte (right) are shown at 45 °C. Figure 27B The average voltage of Li||LCO half-cells using different electrolytes is shown when discharged at 45°C. Figure 27C The coulombic efficiency of Li||LCO half-cells using different electrolytes at 45 °C is shown. Figure 28 The capacity retention of the Li||LCO half-cell at 0.33 C at different temperatures is shown; Figure 29 The discharge capacity performance of the Li||LCO half-cell using the designed electrolyte after charging at 25°C is shown at -60°C and 0.05C. Figure 30 The charge / discharge spectra of Li||LCO half-cells using the base electrolyte (left) and the designed electrolyte (right) at different temperatures are shown. Figure 31 The overpotential of Li||LCO half-cells using different electrolytes at different temperatures is shown; Figure 32 The electrochemical performance of the Li|| graphite half-cell is shown; Figure 33 Long-term cycling of Li|| graphite half-cells using different electrolytes at 25 °C (left) and 45 °C (right) is shown; Figure 34 The capacity retention (left) and overpotential (right) of Li|| graphite half-cells using different electrolytes at different temperatures are shown. Figure 35 The cycling performance of graphite||LCO full cells using different batches of electrolyte is shown; Figure 36AThe charge / discharge profiles of a graphite ||LCO full cell using a base electrolyte are shown. Figure 36B The charge / discharge profiles of a graphite || LCO full cell using a designed electrolyte are shown. Figure 37 It is a table summarizing the corresponding battery parameters and calculated energy density of the assembled graphite (Gr)||LCO full cell; Figure 38A The FTIR spectra of EMC solvent, EMC solutions with different lithium salts, and designed electrolytes are shown. Figure 38B FTIR of EMC solvent and EMC solution with 20 wt% LiBF4 is shown; Figure 38C FTIR of EMC solvent and EMC solution with 20 wt% LiDFBP is shown; Figure 38D FTIR of EMC solvent and EMC solution with 20 wt% LiDFOB is shown; Figure 39 The in-situ FTIR spectrum of the designed electrolyte during the first cycle is shown; Figure 40 The experiment showed the use of different electrolytes at 0.2 C (1 C = 200 mAh g⁻¹). -1 SEM images of LCO after two activation cycles at a current density of ) Figure 41 TEM images of LCO particles after 50 cycles with different electrolytes are shown. Figure 42A The atomic percentages of different elements on the LCO surface are shown after 50 cycles in base electrolytes with different etching times. An insert shows the atomic percentages of P and Co in line graph format. Figure 42B The atomic percentages of different elements on the LCO surface are shown after 50 cycles in electrolytes with different etching times. An insert shows the atomic percentages of P and Co in line graph format. Figure 43 The F on the LCO surface after 50 cycles in the base electrolyte is shown. 1s spectrum; Figure 44 The results show F based on etching the LCO surface for 0 seconds, 30 seconds, 60 seconds, and 90 seconds after 50 cycles in the base electrolyte. 1s The percentage of the fitted area of different components in the XPS spectrum; Figure 45 The F on the LCO surface is shown after 50 cycles in the designed electrolyte.1s spectrum; Figure 46 The figure shows F based on etching the LCO surface for 0 seconds, 30 seconds, 60 seconds, and 90 seconds after 50 cycles in the designed electrolyte. 1s The percentage of the fitted area of different components in the XPS spectrum; Figure 47 The B of LCO after 50 cycles at different etching times is shown. 1s (Left) and P 1s (Right) XPS core spectrum; Figure 48 The O2 on the LCO surface is shown after 50 cycles in the base electrolyte. 1s spectrum; Figure 49 The results show O etching on an LCO surface for 0 seconds, 30 seconds, 60 seconds, and 90 seconds after 50 cycles in a base electrolyte. 1s The percentage of the fitted area of different components in the XPS spectrum; Figure 50 The O2 content on the LCO surface is shown after 50 cycles in the designed electrolyte. 1s spectrum; Figure 51 The results show O etching on an LCO surface for 0 seconds, 30 seconds, 60 seconds, and 90 seconds after 50 cycles in the designed electrolyte. 1s The percentage of the fitted area of different components in the XPS spectrum; Figure 52A The C2 of the LCO surface is shown after 50 cycles in a base electrolyte (left) and a designed electrolyte (right) with different etching times. 1s spectrum; Figure 52B The concentration of Li2CO3 on the LCO surface is shown after 50 cycles in different electrolytes with different etching times; Figure 53A The concentrations of selected components on the LCO surface are shown after 50 cycles in base electrolytes with different etching times. Figure 53B The concentrations of selected components on the LCO surface are shown after 50 cycles in electrolytes with different etching times. Figure 54 The HR-TEM patterns of LCO particles after 200 cycles in the base (left) electrolyte and the designed electrolyte (right) are shown. Figure 55A The atomic percentages of different elements on the LCO surface are shown after 200 cycles in a base electrolyte. Figure 55BThe atomic percentages of different elements on the LCO surface are shown after 200 cycles in the designed electrolyte; Figure 56 The image shows HR-TEM images of the LCO surface after 200 cycles of the base (left) electrolyte and the designed (right) electrolyte, including the corresponding FFT patterns. Figure 57 The in-situ Raman spectra of LCO particles during the first cycle are shown; and Figure 58 This is a schematic diagram illustrating the mechanism by which the designed electrolyte improves the electrochemical performance of a graphite||LCO full cell. Detailed Implementation
[0028] Unless the context clearly indicates otherwise, the forms “a” and “the” as used herein are intended to include both singular and plural forms.
[0029] The terms “example” or “exemplary” as used in this invention are intended to be used as instances, examples, or illustrations. Any aspect or design described as “exemplary” in this disclosure is not necessarily to be construed as being more preferred or advantageous than other aspects or designs. Rather, the use of the terms “example” or “exemplary” is intended to present concepts in a specific manner. As used in this application, the term “or” is intended to mean an inclusive “or” rather than an exclusive “or.” That is, unless otherwise specified or the context clearly indicates, “X adopts A or B” is intended to mean any natural inclusive permutation. That is, “X adopts A or B” holds true in any of the foregoing cases if X adopts A, X adopts B, or X adopts both A and B.
[0030] As used herein, the term “about” is intended to refer to a value that deviates slightly from the values described herein. Examples have been described throughout this disclosure.
[0031] Unwilling to be bound by theory, the inventors, through their own research, experimentation, and research, designed an electrolyte using a cation-anion solvation engineering strategy. This electrolyte can simultaneously address low-temperature ionic conductivity and high-temperature / high-voltage stability. The salt and solvent synergistically minimize Li. + - Solvent binding energy and promotes anion participation of Li + Solvated structures. Specifically, such as Figure 1 As shown, the designed electrolyte may have the following characteristics: (1) solvent and Li + The weak cation-dipole interaction between them is beneficial to Li +(1) Desolvation process; (2) Excellent thermal stability of lithium salt, minimizing the generation of corrosive byproducts; and (3) Anion-involved solvation structure, generating a robust, inorganic-rich CEI to stabilize the cathode (anode) interface stability during high-voltage operation. Therefore, as shown in some exemplary embodiments of this disclosure, the electrolyte can exhibit extremely high ionic conductivity at sub-zero temperatures (0.19 mS cm⁻¹ at -60°C). -1 ) and fluidity (freezing point < -90°C). In some other exemplary embodiments, the electrolyte enables a cathode such as a lithium cobalt oxide (LCO) cathode to maintain 4.6 V (relative to Li / Li) after 400 and 200 cycles. + It exhibits capacity retention of 88.9% and 77.3% at 25°C and 45°C, respectively. In some other exemplary embodiments, the electrolyte enables a positive electrode, such as an LCO positive electrode, to provide 110.1 mAh g⁻¹ at -35°C and 0.33°C, and at -60°C and 0.05°C, respectively. -1 The reversible capacity and 92.6 mAh g -1 The discharge capacity.
[0032] In a first aspect of the invention, an electrolyte for lithium-based batteries is provided. As used herein, the term "lithium-based battery" generally refers to a battery pack or cell that uses lithium chemistry to store or release energy, such as full-cell and half-cell configurations of lithium-ion battery packs / cells and lithium metal battery packs / cells. The electrolyte described herein may comprise a mixture of at least three lithium salts and a carbonate solvent, wherein the at least three lithium salts are selected from the group consisting of lithium tetrafluoroborate (LiBF4), lithium difluorooxalatoborate (LiDFOB), lithium difluorodiooxalatophosphate (LiDFBP), lithium bis(fluorosulfonyl)imide (LiFSI), and lithium bis(trifluoromethanesulfonyl)imide (LiTFSI). In some specific embodiments, the at least three lithium salts may comprise LiBF4, LiDFOB, and LiDFBP. In some exemplary embodiments, the at least three lithium salts may be a ternary lithium salt system, particularly a ternary lithium salt system of LiBF4, LiDFOB, and LiDFBP. While ternary lithium salt systems are believed to offer relatively optimized performance in terms of ionic conductivity, decomposition temperature, and ability to form solid electrolyte interphases, it is not desirable to be bound by theory. It is also believed that, in some other exemplary embodiments, systems having four or more lithium salts can be used to achieve similar performance to ternary lithium salt systems. In some embodiments of ternary lithium salt systems where the at least three lithium salts are LiBF4, LiDFOB, and LiDFBP, LiBF4, LiDFOB, and LiDFBP may each have a molar percentage of at least 10%, provided that the total percentage / proportion of these salts is 100%. In some exemplary embodiments, the molar ratio of lithium tetrafluoroborate (LiBF4), lithium difluorooxalate borate (LiDFOB), and lithium difluorodioxalate phosphate (LiDFBP) may be approximately 4:4:3 (e.g., 3.9:4:3, 3.9:3.9:3, 3.9:4:3.1, 4:4.1:3, 4:4:2.9, 3.9:4.1:2.9, etc.).
[0033] The total concentration of the at least three lithium salts can be from about 0.5 M to about 1.5 M, such as 0.48…0.486…0.49…0.493…0.498…0.5…0.502…0.505…0.51…0.8…0.86…0.9…1…1.04…1.5…1.52 M, etc. In some specific embodiments, the total concentration of the at least three lithium salts can be about 1.1 M, such as 1.06, 1.07, 1.08, 1.09, 1.1, 1.11, 1.12, 1.13, 1.14 M, etc.
[0034] The term "carbonate solvent mixture" generally describes a mixture of carbonates (or organic carbonates or organic carbonates) that is particularly suitable as a solvent in lithium-based batteries. In some specific embodiments, the carbonate solvent mixture may comprise propylene carbonate (PC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), and fluoroethylene carbonate (FEC). Specifically, the volume ratio of propylene carbonate (PC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), and fluoroethylene carbonate (FEC) may be a:b:c:d, where a is about 2-5, b is about 3-5, c is about 1-3, d is about 1-2, and a+b+c+d=1. For example, in some embodiments, the volume ratio may be about 5:3:1:1, 2:5:1:2, 2:5:2:1, 2:3:3:2, etc.
[0035] It is believed that in the typical electrolyte of lithium-based batteries (such as lithium-ion batteries (LIB)), lithium ions (Li... + The electrolyte (or electrolyte-electrolyte) interphase (EEI) associates with solvent molecules, and the electrode-electrolyte (or electrolyte-electrode) phase is primarily derived from solvent decomposition. Not wishing to be bound by theory, the inventors unexpectedly envisioned that the anions of at least three lithium salts of the electrolytes described herein could more preferably associate with Li... + Combining facilitates the process via Li involving anions. + The solvation structure forms an anion-induced EEI. Furthermore, when Li... + When combined with carbonate solvent mixtures as described herein, anions and Li + The electrostatic attraction between them will weaken the interaction between the solvent and Li. + The cation-dipole interaction between them will further reduce the Li + Desolvation energy barrier and enhancement of Li + Interfacial transfer kinetics. Due to the synergistic effect of the lithium salt and carbonate solvent mixture as described herein, the electrolytes described herein are believed to exhibit a variety of favorable electrochemical properties. In one exemplary embodiment, the decomposition voltage of the electrolyte is approximately 4 μA cm⁻¹. -2 (For example, 3.8 μA cm) -2 3.85 μA cm -2 3.9 μA cm -2 3.94 μA cm -2 3.98 μA cm -2 4 μAcm -2 4.01 μA cm -2 4.1 μA cm -2 4.15 μA cm -2The cutoff current density measured by linear sweep voltammetry (LSV) for Li / Li can be approximately 4.43 V (e.g., 4.41 V, 4.42 V, 4.43 V, 4.44 V, 4.45 V, etc.) (relative to Li / Li). + In another exemplary embodiment, the electrolyte can remain in liquid form at temperatures ranging from about -80°C to about 45°C (e.g., -80.5°C to 45°C, -80.5°C to 45.5°C, -80°C to 45.9°C, -81°C to 46°C, -79.9°C to 45°C, -79.5°C to 45°C, -80.5°C to 44.6°C, -79°C to 44.8°C, etc.). In yet another exemplary embodiment, the electrolyte is stable at temperatures below or equal to about 80°C for at least 140 hours (i.e., showing no substantial degradation).
[0036] Optionally or additionally, in some embodiments, the electrolyte may also include additives, particularly additives for the formation of the solid electrolyte intermediate (SEI), selected from the group consisting of vinylene carbonate (VC), 1,3-propanesulfonate lactone (PS), ethylene difluorocarbonate (DFEC), tri-(trimethylsilane)borate (TMSB), methanedisulfonate methylene (MMDS), and tri-(trimethylsilane)phosphate (TMSP), and combinations thereof. Specifically, the additive may constitute 5% or less of the total mass of the electrolyte.
[0037] The electrolytes described herein are particularly suitable for lithium-based batteries (e.g., lithium-ion batteries (LIB)). In a second aspect of the invention, a lithium-based battery is provided, comprising: a cathode (positive electrode) including a cathode active material selected from lithium cobalt oxide (LCO), lithium iron phosphate (LFP), lithium manganese oxide (LMO), lithium manganese iron phosphate (LMFP), nickel-cobalt-manganese nickel-rich material (nickel-rich NCM), nickel-cobalt-aluminum nickel-rich material (nickel-rich NCA), and graphite; an anode (negative electrode); and an electrolyte comprising at least three lithium salts selected from lithium tetrafluoroborate (LiBF4), lithium difluorooxalate borate (LiDFOB), and lithium difluorodioxalate phosphate (LiDFBP), and a carbonate solvent mixture selected from propylene carbonate (PC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), and fluoroethylene carbonate (FEC). In some embodiments, the cathode may comprise a cathode active material of lithium cobalt oxide, and the anode may comprise an anode active material selected from the group consisting of graphite, silicon (such as micron-sized silicon, nano-sized silicon), lithium metal, silicon-carbon composites, and silicon-oxygen (such as silicon dioxide). In some other embodiments, the cathode comprises a cathode active material of graphite, and the anode comprises an anode active material selected from the group consisting of lithium metal, silicon (such as micron-sized silicon, nano-sized silicon), silicon-carbon composites, and silicon-oxygen (such as silicon dioxide). It should be understood that, depending on the materials used for the cathode (positive electrode) and anode (negative electrode), the lithium-based battery described herein can be configured as a half-cell or a full-cell. For example, in embodiments where the lithium-based battery includes an LCO positive electrode (i.e., a positive electrode having an LCO positive electrode active material), the battery pack can be configured as a half-cell by using a lithium metal negative electrode (i.e., a negative electrode having a lithium metal negative electrode active material). On the other hand, a battery having an LCO positive electrode can be configured as a full-cell by using a graphite negative electrode (i.e., a negative electrode having a graphite negative electrode active material). Similarly, in embodiments of lithium-based batteries that include a graphite cathode (i.e., a cathode having a graphite cathode active material), a lithium metal anode can be used to configure the battery pack as a half-cell.
[0038] The cathode described herein may include the cathode active material, conductive carbon, binder, and current collector as described herein. Similarly, the cathode described herein may include the anode active material, conductive carbon, binder, and current collector as described herein. Examples of conductive carbon materials may include Ketjen Black, Super P, Super P-Li, etc. Examples of binder materials may include carboxymethyl cellulose (CMC), sodium carboxymethyl cellulose (CMC-Na), polyacrylic acid (PAA), lithium polyacrylate (PAA-Li), styrene-butadiene rubber (SBR), polyvinylidene fluoride (PVDF), etc. Examples of current collector materials may include copper, aluminum, etc.
[0039] In some exemplary embodiments, the cathode may comprise 70 wt% graphite, 20 wt% Super P, 4 wt% sodium carboxymethyl cellulose (CMC), and 6 wt% styrene-butadiene rubber (SBR). In some other exemplary embodiments, the cathode may comprise 90 wt% LCO, 5 wt% Super P, and 5 wt% polyvinylidene fluoride (PVDF). In some exemplary embodiments, the anode may comprise 94.5 wt% graphite, 2.5 wt% Super P, 1.5 wt% CMC, and 1.5 wt% SBR.
[0040] The mass loads of the cathode and anode can differ. Specifically, the mass load of the cathode can be approximately 6.6 mg cm⁻¹. -2 Such as 6.57 mg cm -2 …6.59 mg cm -2 6.6 mg cm -2 6.61 mg cm -2 …6.63 mg cm -2 The mass loading of the anode can be approximately 2.0 mg cm⁻¹. -2 Approximately 4.0 mg cm -2 Such as 1.85 mg cm -2 …1.9 mg cm -2 …1.99 mgcm -2 …2.0 mg cm -2 …2.2 mg cm -2 …3.85 mg cm -2 3.95 mg cm -2 4.0 mg cm -2 4.05 mg cm -2 4.1 mg cm -2 4.19 mg cm -2 In some implementations where the battery pack is a half-cell, the anode mass load can be reduced to half that of the full cell. For example, the anode mass load can be reduced from 4.0 mg / cm³ in the full cell. -2 Reduced to 2.0 mg cm in half-cell -2 .
[0041] When operated at a temperature of about 45°C (e.g., 43.6°C…44°C…44.8°C…45°C…45.2°C, etc.) and at a voltage of at least 4.6 V, the lithium-based batteries described herein can advantageously have an average coulombic efficiency of at least 99%.
[0042] Not wanting to be bound by theory, the inventors envisioned that the aforementioned unexpected battery pack performance could be attributed to the electrolyte as described herein. As mentioned above, the electrolyte described herein may be particularly advantageous in the formation of the electrode-electrolyte (or electrolyte-electrode) interphase, which can stabilize the surface structures of the negative and positive electrodes. For example, in some specific embodiments, the electrolyte can be arranged to form a cathode (positive electrode)-electrolyte interphase (CEI) on the cathode (positive electrode) at a voltage of about 4.6 V, for stabilizing the interface phase of the positive electrode at said high voltage. The CEI can be uniformly distributed on the surface of the positive electrode and can have a thickness of about 7 nm to about 20 nm, such as 6.9 nm to 20 nm, 6.9 nm to 20.2 nm, 6.88 nm to 20 nm, 6.91 nm to 20 nm, 6.9 nm to 19.9 nm, 6.95 nm to 20 nm, 7 nm to 21 nm, 7.2 nm to 20.1 nm, 7 nm to 20 nm, etc. The CEI may specifically include a concentration gradient of LiF, such that the LiF concentration on the side closer to the positive electrode surface is higher than that on the side farther from the positive electrode surface. In other words, the inner layer of the electrode-electrolyte interphase at the positive electrode surface has a higher LiF concentration than the outer layer. It is not desirable to be bound by theory, but it is believed that a higher LiF concentration closer to the cathode surface will more effectively suppress irreversible interfacial phase transitions / transformations at high voltages (e.g., at 4.6 V). Additionally, in some embodiments, the CEI may also include other inorganic substances, such as PO and BO, which can further enhance the stability of the CEI and help suppress continuous electrolyte decomposition, especially at high temperatures (e.g., at about 45°C or above).
[0043] The invention is described in more detail below by way of examples, but is not limited thereto.
[0044] Example Material The LCO electrode was purchased from WeiMing Co., Ltd., China. Graphite material was purchased from Shenzhen BTR Tech Co., Ltd., China. The basic electrolyte, consisting of 1.0 M LiPF6 in EC / EMC / DMC = 1 / 1 / 1 (by volume), was purchased from DodoChem. PC, EMC, DMC, FEC solvents, and lithium salts LiBF4 and LiDFOB were purchased from DodoChem. Lithium salt LiDFBP was purchased from Changsha T-rock Biochem Co., LTD. The designed electrolyte (i.e., the electrolyte of this work) contained 0.4 M LiBF4, 0.4 M LiDFOB, and 0.3 M LiDFBP in PC / EMC / DMC / FEC = 2 / 3 / 3 / 2 (by volume). In one exemplary embodiment, the cathode (positive electrode) of the half-cell comprises 90 wt% LCO, 5 wt% Super P, and 5 wt% polyvinylidene fluoride (PVDF), while the anode (negative electrode) is lithium metal. In another exemplary embodiment, the positive electrode of the half-cell comprises 70 wt% graphite, 20 wt% Super P, 4 wt% sodium carboxymethyl cellulose (CMC), and 6 wt% styrene-butadiene rubber (SBR), while the negative electrode is lithium metal. The mass loadings of the positive and negative electrodes of the half-cell are 6.6 mg cm⁻¹, respectively. -2 and 2.0 mg cm -2 The mass loadings of the positive and negative electrodes of the full cell were 6.6 and 4.0 mg cm⁻¹, respectively. -2 The negative electrode of the full cell consists of 94.5% by weight graphite, 2.5% by weight Super P, 1.5% by weight CMC and 1.5% by weight SBR.
[0045] Electrochemical Measurement Coin cells were assembled using CR2032 in an argon-filled glove box, with Celgard 2400 (19 mm diameter) as the separator. 80 μl of electrolyte was added to each cell. The assembled coin cells were tested on a NEWARE battery testing system. For long-term cycling performance, the coin cells were tested using constant current charge-discharge profiles with a 10-second rest after each step. Linear sweep voltammetry (LSV) was performed on a Solartron Analytical 1470E electrochemical workstation at a scan rate of 0.5 mV s. -1 The ionic conductivity of different electrolytes was calculated using the Rs impedance at different temperatures using a three-electrode model. The ionic conductivity of the electrolytes was calculated using the following formula:
[0046] Where σ represents the ionic conductivity, Rs is the measured impedance, and a is a constant, obtained by the following formula:
[0047] Where σ' is the ionic conductivity of the base electrolyte at 25°C obtained from the seller, and Rs' is the impedance of the base electrolyte at 25°C. The three electrodes are made of titanium and have an area of 0.785 cm². -2 EIS was performed in the frequency range of 1000 kHz to 0.1 Hz, with an AC signal amplitude of 10 mV. To ensure precise temperature control and thermal balance, the assembled batteries were stored at the target temperature for at least four hours prior to EIS testing.
[0048] Characterization Nuclear magnetic resonance (NMR) spectra were recorded using a Bruker DPX 300 MHz spectrometer. 1 H NMR, 7 Li NMR and 19 FNMR). The morphology and elemental distribution of the samples were studied using scanning electron microscopy (SEM, Zeiss SUPRA-55). TEM samples were prepared using FIB, and HR-TEM was performed using a JEM-100F microscope. The chemical states of selected elements were investigated using X-ray photoelectron spectroscopy (XPS) on a Thermo Scientific Escalab 250Xi spectrometer. In-situ FTIR spectra were recorded using a NICOLET iS50 Frontier-FTIR spectrometer (Thermos Scientific, America).
[0049] DFT calculation and MD simulation All DFT calculations were performed using Gaussian 09 software. Li was calculated based on four different units using density functional theory. + The binding energies with solvents include B3LYP / 6-31+G(d), B3LYP / 6-311++G(d,p), B3LYP / DGDZVPS, and M062X / 6-311++G(d,p). Li + - Solvent binding energy equals Li + - The single-point energy of the solvent compound is subtracted from the corresponding solvent and Li. + The single-point energy of Li was calculated using the B3LYP / 6-311++G(d,p) basis set containing DMSO as an implicit solvent. +Binding energy with anion. Molecular dynamics simulations were performed using a universal force field (UFF) in Materials Studio software. The molecular structure was initially calculated using Gaussian 09 software. Following the energy minimization step, molecular dynamics simulations in the NPT ensemble were performed for 2 ns (1.0 fs time step) at 298 K using a Nose-Hoover cryostat and at 1 atm using Berendsen pressure coupling. Following the energy minimization step, subsequent molecular dynamics simulations in the NVT ensemble were performed for 1 ns (1.0 fs time step) at 298 K using a Nose-Hoover cryostat.
[0050] Example 1 Synergistic pairing of carbonate solvents and lithium salts for wide-temperature, high-voltage electrolytes To optimize the carbonate solvent for a wide-temperature, high-voltage electrolyte, density functional theory (DFT) calculations were performed. It is believed that weaker dipole-cation interactions imply a preference for anion-involved Li... + Solvation structure and fast Li + Desolvation kinetics, which can be inferred from the lower Li-solvent binding energy, are observed. Ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), and fluoroethylene carbonate (FEC) are believed to exhibit desolvation kinetics with Li. + The binding energy is relatively low. Figure 2 Theoretically, this could achieve faster Li + Desolvation kinetics and thus enhanced low-temperature performance.
[0051] To verify the reliability of this result, calculations were performed using three other different basis sets, which are in Li + - The solvent binding energy shows the same distribution trend, indicating the consistency of the calculation results. Figures 3A to 3C Furthermore, the inherent properties of solvents, such as their polarity, are assessed based on electrostatic potential (ESP). max and ESP min A lower value indicates a weaker dipole-cation interaction. Taking this into account, EMC, DMC, and FEC (in...) Figure 4 The triangle inside the image (represented by the triangle) was identified as Li. + The favorable solvents for desolvation are consistent with the results regarding the binding energy of Li-solvents. Furthermore, the lower highest occupied molecular orbital (HOMO) energies of these three solvents indicate enhanced antioxidant properties at higher potentials. Figure 5Therefore, EMC, DMC, and FEC are believed to be suitable primary solvents for electrolytes designed to operate at low temperatures and high voltages. Meanwhile, considering the dissolution of lithium salts and maintaining the ionic conductivity of the electrolyte, it is preferable to include highly polar solvents (in... Figure 4 (shown within the circle) as a co-solvent. Limited by the high freezing point of EC ( Figure 6 Propylene carbonate (PC) was selected as the preferred cosolvent to improve the wide temperature stability of the electrolyte.
[0052] Physical properties of different carbonate solvents, such as Figure 7 As shown. Both EC and PC have high dielectric constants, meaning they possess excellent dissolving capabilities for lithium salts, consistent with their calculated high polarity. Furthermore, low viscosity and low freezing point are believed to be essential for achieving the wide temperature range performance of LIBs. This makes propylene carbonate (PC) a promising alternative to EC as a carbonate solvent to ensure the dissociation of lithium salts, while EMC and DMC are used as co-solvents to reduce the viscosity of the electrolyte. Given its recognized protective properties, FEC is also necessary as a co-solvent. Figure 8 After comprehensively evaluating various indicators, and considering the advantages of wide temperature range performance, high voltage stability, and enhanced ionic conductivity, PC, EMC, DMC, and FEC solvents were selected for the designed electrolyte.
[0053] Considering the stability of lithium salts at high temperatures, LiBF4, LiDFOB, and LiDFBP were selected as the main lithium salts for the designed electrolyte to promote anion-induced CEI formation and electrolyte thermal stability. To verify this selection, DFT calculations and molecular dynamics (MD) simulations were performed. It is believed that in diluted electrolytes, Li... + It typically associates with solvent molecules. The CEI in basic electrolytes mainly originates from solvent decomposition. However, when DFBP... - and DFOB - Anions and Li + The increased HOMO energy upon binding indicates that the designed electrolyte possesses the properties via Li involving anions. + The solvation structure has a high potential to form anion-induced CEI. Figure 9 To further investigate this, MD simulations were performed on the basic electrolyte and the designed electrolyte. For the basic electrolyte, the solvent mainly consists of Li. + First solvation sheath ( Figure 10 In contrast, the designed electrolyte showed involvement of DFOB. - and DFBP - Li + The solvation structure facilitates the formation of anion-induced CEI. Figure 11This change in solvation structure is partly due to the relatively low Li content of the custom solvent. + Solvent binding energy. On the other hand, the stronger cation-anion interaction provided by the selected lithium salt with high thermal stability further promotes the formation of this unique anion-involved solvation structure. Figure 12 ).
[0054] 7 Li nuclear magnetic resonance (NMR) spectroscopy confirmed the modified Li in the designed electrolyte. + Solvation structure ( Figure 13 Compared to the basic electrolyte, the designed electrolyte has... 7 The Li NMR spectrum shifts slightly to lower frequencies, indicating that Li + The increased electron cloud density is primarily due to binding with anions. The preferential oxidation peak observed in the linear sweep voltammetry (LSV) spectrum of the designed electrolyte confirms the anion-induced formation of the CEI. Figure 14 Moreover, using 4 μA cm -2 The cutoff current density was determined, and the designed electrolyte decomposition voltage was 4.43 V (relative to Li / Li). + This is higher than the decomposition voltage of the basic electrolyte (4.22 V, relative to Li / Li). + This demonstrates that the designed carbonate-based electrolyte has higher antioxidant capacity.
[0055] Furthermore, in order to reveal the effect of dipole-cation interactions on Li + The effect of desolvation kinetics on Li was evaluated. + Three different solvation structures ( Figure 15 Initially, when Li + When combined with a highly polar pure solvent (PC), Li + The desolvation energy is the highest, and this energy decreases as weakly polar solvents (FEC / EMC) participate in the solvation structure. Anions and Li + The electrostatic attraction between them weakens the cation-dipole interaction, which in turn reduces the Li... + Desolvation energy barrier and enhancement of Li + Interfacial transfer kinetics. These results indicate the design of weak dipole-cation interactions and Li-related interactions involving anions. + Solvation structure enhances Li + The importance of desolvation kinetics.
[0056] Example 2 Physicochemical properties of electrolytes To investigate the potential application of the designed electrolyte in a wide-temperature lithium-ion battery (LIB), its thermal stability and temperature-dependent ionic conductivity were evaluated. First, due to the high thermal stability of lithium salts, the designed electrolyte exhibited negligible thermal decomposition at high temperatures. In contrast, the base electrolyte with LiPF6 showed significant degradation: after storage at 80 °C for 144 hours, the electrolyte turned brown, and characteristic PF5 and HF were detected. 19 F nuclear magnetic resonance (NMR) peak ( Figure 16 This can be attributed to the severe decomposition of LiPF6 under high-temperature conditions. Simultaneously, in addition to the solvent peak, new peaks appeared in the base electrolyte after long-term high-temperature storage. 1 The characteristic peaks of H NMR indicate the presence of products from the reaction between the carbonate solvent and PF5. Figure 17 These results demonstrate the poor thermal stability of LiPF6-based electrolytes. Conversely, no identifiable decomposition products were observed in the designed electrolyte, indicating its excellent thermal stability and potential for high-temperature applications. Figure 18 ).
[0057] Figure 19 Differential scanning calorimetry (DSC) spectra confirmed that, during heating from -85°C to 30°C, the basic electrolyte showed values at -57.1°C and... An endothermic peak at 20.1 °C indicates a solid-liquid phase transition. Surprisingly, no endothermic peak was observed in the designed electrolyte, indicating that it remains in liquid form over the temperature range of -80 °C to 30 °C. This behavior is believed to be attributed to the prudent choice of solvent blend. Optical photographs of the electrolyte at different temperatures further support this: the base electrolyte solidifies at -60 °C, while the designed electrolyte remains liquid at -90 °C. Figure 20 Due to the extremely low freezing point of the rationally chosen solvent and the moderate lithium salt dissociation capability, the designed electrolyte exhibits excellent ionic conductivity at reduced temperatures. Figure 21 Its high ionic conductivity (in) At 60℃, it is 0.19 mS cm. -1 This indicates its application potential in low-temperature environments.
[0058] Example 3 Electrochemical performance of electrolytes The combination of high thermal stability, excellent low-temperature ionic conductivity, and the ability to form anion-induced CEI is believed to endow the designed electrolyte with high application potential for wide-temperature, high-voltage LIBs. To verify this, the electrochemical performance of both LCO and graphite electrodes was tested. The upper cutoff voltage was 4.6 V (relative to Li / Li). +The LCO cathode, cyclic in both electrolytes, provides approximately 190 mAh g⁻¹ at a current density of 1 C after activation. -1 High reversible capacity. Interestingly, the Li||LCO half-cell using the designed electrolyte achieves excellent long-term cycling stability, retaining 88.9% of its capacity after 400 cycles at 25°C. Figure 22 Furthermore, it exhibits excellent long-term cycling performance and high reproducibility, such as... Figure 23 As shown, all Li||LCO half-cells using electrolytes from different batches exhibited stable long-term cycling performance, with a standard deviation of 4.1% after 200 cycles. In contrast, the LCO electrode in the base electrolyte experienced rapid capacity decay and severe charge / discharge plateau degradation. Figure 24 After 200 cycles, the reversible capacity was only 23.4 mAh g. -1 Furthermore, the Li||LCO half-cell using the designed electrolyte achieves an average coulombic efficiency (CE) of up to 99.4%. Figures 25A to 25C The efficiency of the CE (ce) is higher than that of the base electrolyte (99.03%). The slightly lower CE observed during the initial activation cycle with the designed electrolyte can be attributed to an anion-induced CEI formation process, which rapidly forms a dense CEI on the LCO surface. These results indicate that the CEI formed by the base electrolyte cannot protect the LCO from irreversible phase transitions at high voltages.
[0059] At high temperature (45°C), the LCO in the base electrolyte exhibited poor cycling performance, retaining only 15.5% of its capacity after 200 cycles and showing low fluctuating average CE. This poor performance was mainly due to the unstable CEI formed by the base electrolyte. In contrast, the LCO cathode with the designed electrolyte showed a 77.3% capacity retention after 200 cycles at 45°C, thanks to the superior thermal stability of the designed electrolyte and the formation of anion-induced CEI. Figure 26 It exhibits a stable discharge voltage and a high average CE (conversion rate) of up to 99.35%. Figures 27A to 27C More importantly, the high ionic conductivity of the designed electrolyte below 0°C enables the LCO cathode to provide high capacity at low temperatures. Figure 28 It is worth noting that the base electrolyte provides 198.4, 171.8, 156.4, 142.5, 124.6, 101.0, 62.9, and 0.59 mAh g⁻¹ at 25, 0, -10, -15, -20, -25, -30, and -35 °C, respectively. -1 The reversible capacity indicates the basic electrolyte at... At 35°C, it exhibits almost no activity. Conversely, the designed electrolyte allows the LCO cathode to provide 202.1, 183.6, 171.9, 164.5, 154.1, 141.3, 129.1, and 110.1 mAh g⁻¹ at the same temperature gradient and current density of 0.33 C. -1 The reversible capacity. This is equivalent to in A significantly high capacity retention of 54.5% at 35°C (compared to the capacity at 25°C) clearly demonstrates the wide temperature range advantage of the designed electrolyte. Even at -60°C, at a current density of 0.05 C, the LCO cathode in the designed electrolyte provides 92.6 mAh g⁻¹. -1 High discharge specific capacity ( Figure 29 ).
[0060] like Figure 30 and Figure 31 As shown, the overpotential of Li||LCO half-cells using different electrolytes is the reason for the significant performance differences. The overpotential of the Li||LCO half-cell using the basic electrolyte exceeds 0.7 V at -35°C (relative to Li / Li). + This is approximately three times the overpotential observed with the designed electrolyte. Such a large overpotential is attributed to the extremely low ionic conductivity of the underlying electrolyte at low temperatures and the slow Li₂... + The result of the desolvation process.
[0061] Furthermore, graphite anodes with designed electrolytes also exhibit excellent electrochemical performance. Figure 32 At 25℃ and 45℃, the graphite anode exhibits excellent cycle stability in the designed electrolyte, with negligible capacity decay. Figure 33 Especially in At 10 °C, due to a significant decrease in overpotential, graphite cyclicated in the designed electrolyte exhibited a current density of 212.5 mAh g⁻¹ at 0.2 C. -1 This is approximately three times the capacity exhibited by graphite circulating in the basic electrolyte. Figure 34 These results demonstrate the potential of the designed electrolyte for use in full cells.
[0062] Therefore, the full cell assembled using the designed electrolyte provides 186.6 mAh g⁻¹. -1 It exhibits high specific capacity and excellent cycling stability. Specifically, at 4.6 V (relative to Li / Li + After 500 cycles, the capacity retention rate reached 88.1%. To further demonstrate reproducibility, full cells using different batches of the designed electrolyte were assembled. These full cells all exhibited high capacity retention rates after 250 cycles, with a standard deviation of only 3.8%. Figure 35Furthermore, after two activation cycles, the corresponding CE increased to 99.0% (). Figure 36A and Figure 36B This indicates minimal electrolyte decomposition. This can be attributed to the excellent CEI-forming capability of the designed electrolyte. As mentioned earlier, the LCO cathode will exhibit high energy density at elevated charge cutoff voltages. The cutoff voltage is 4.6 V (relative to Li / Li). + Theoretically, the mass energy density and volumetric energy density of an LCO cathode can reach 885.9 Wh kg. -1 and 3721 Wh L -1 The estimated energy density of the assembled graphite ||LCO full cell, matched with a graphite anode, is 303 Wh / kg. -1 The relevant parameters are summarized in Figure 37 These results highlight the potential application of the designed electrolyte in practical LIBs.
[0063] Example 4 Properties of different CEIs The excellent cycling stability of the LCO cathode at high voltage is believed to be attributed to anion-induced CEI. To confirm this, in-situ Fourier transform infrared spectroscopy (FTIR) was performed. Figures 38A to 38D Ex-situ FTIR spectra of pure EMC, EMC solutions with different lithium salts, and a designed electrolyte are shown. Specifically, at 1063.1 cm⁻¹... -1 The characteristic peak of LiBF4 was observed at 1794.2 cm⁻¹, corresponding to the BF stretching vibration mode, while the peak at 1794.2 cm⁻¹... -1 The characteristic peak of LiDFOB was found at [cm], and designated as a C=O stretching vibration. For LiDFBP, more characteristic peaks appeared, located at 862.1, 915.2, and 1715.3 cm⁻¹. -1 Nearby, representing the stretching vibrations of PF, PO, and C=O, respectively. When charged to 3.5 V (relative to Li / Li... + Five characteristic oxidation peaks appeared, corresponding to DFOB. - (1793.5 cm -1 ) and DFBP - (1716.3 cm -1 ) of the PO bond (863.9 cm) -1 ), PF key (915.5 cm) -1 The decomposition of the C=O bond indicates the DFOB. - and DFBP - Oxidation to form CEI ( Figure 39The subtle differences in characteristic peaks of certain lithium salts in EMC solutions and designed electrolytes are attributed to interactions between components within the electrolyte. Specifically, BF4 - The characteristic peaks of oxidation even appear when charged to 4.6 V (relative to Li / Li). + The presence of BF4 in the designed electrolyte was not observed. - It is difficult for them to participate in the formation of CEI.
[0064] To analyze the morphology and composition of anion-induced CEI, scanning electron microscopy (SEM), high-resolution transmission electron microscopy (HR-TEM), and X-ray photoelectron spectroscopy (XPS) were performed. Due to the enhanced CEI-forming ability, the designed electrolyte exhibited an effective structure of a protective mesophase on the LCO surface after the first two activation cycles, as shown in the SEM images. Figure 40 More specifically, the TEM patterns demonstrate the dense and uniform morphology of the designed electrolyte-induced CEI with a thickness of approximately 7–8 nm. Figure 41 In stark contrast, non-uniform CEI was observed on the surface of LCO cyclic in the basic electrolyte, with thicknesses ranging from a few nanometers to approximately 30 nm.
[0065] XPS data reveals the composition of CEIs formed from different electrolytes. LiF is believed to possess high chemical inertness, which is considered essential for suppressing interfacial degradation of the layered cathode during high-voltage operation. CEIs formed from the designed electrolyte are more enriched in F due to the oxidative decomposition of anions. Figure 42A and Figure 42B Furthermore, the proportion of LiF (located at 685.5 eV) in the CEI formed from the base electrolyte decreases with increasing etching time. Figure 43 and Figure 44 A larger proportion of LiF generated by the designed electrolyte is distributed in the inner layer of the CEI. Figure 45 and Figure 46 This is due to the preferential oxidation of anions. The closer to the LCO surface, the more LiF is present in the internal CEI, making it more effective in suppressing irreversible LCO interfacial phase transitions. The higher proportion of CF bonds on the surface of the LCO cathode cyclic in the designed electrolyte is mainly attributed to the partial exposure of the polyvinylidene fluoride (PVDF) binder caused by the thinner CEI, which can also be supported by the high atomic percentage gradient of Co on the LCO surface. Figure 42A and Figure 42B ).
[0066] Furthermore, the PO and BO substances generated by the designed electrolyte further enhance the stability of CEI and inhibit the continuous decomposition of the electrolyte, especially at high temperatures. Figure 47O1s XPS spectroscopy also confirmed the compactness of the CEI formed by the designed electrolyte. The OM material (~529.5 eV) is believed to be mainly composed of Co-O bonds contributed by LCO particles. On the unetched surface, the observed OM material may be partially generated by dissolved Co ions. Therefore, the relatively high proportion of OM material on the LCO surface cyclic in the base electrolyte indicates that the formed CEI cannot effectively suppress the dissolution of Co ions. Figure 48 and Figure 49 It is noteworthy that the relatively high content of C=O bonds observed on the surface of LCO circulating in the designed electrolyte may originate from a higher proportion of lithium carbonate (Li₂CO₃) in the induced CEI. Figure 50 and Figure 51 This can be achieved through C 1s XPS spectroscopy ( Figure 52A and Figure 52B To verify. Figure 53A and Figure 53B Specific concentration gradients of certain components in different CEI layers are shown. With increasing etching depth, the concentration of inorganic components in the CEI induced by the designed electrolyte is higher than that induced by the electrolyte itself. These inorganic components include LiF, Li₂CO₃, and PF₂ substances, revealing the ability of the designed electrolyte to form an inorganic-rich CEI. These findings enhance the excellent interfacial stability provided by the designed electrolyte under high-voltage operation.
[0067] Example 5 Stability of CEI and protection of LCO interface phase To reveal the stability of different CEIs, HR-TEM and XPS were performed after 200 cycles. Figure 54 As shown, after long-term cycling, the thickness of the designed electrolyte-induced CEI increased to approximately 10-20 nm while maintaining a dense and uniform morphology. However, the CEI formed on the LCO surface in the base electrolyte exhibited significant structural degradation, with visible damage and partial exposure of the underlying LCO particles. This phenomenon is attributed to the higher mechanical strength of the anion-induced CEI, which has more inorganic components, enhancing its stability during long-term cycling. Moreover, the CEI induced by the designed electrolyte exhibited more F and less C, maintaining its compositional characteristics (…). Figure 55A and Figure 55B In the basic electrolyte, after cycling, there is more Co on the LCO surface, exhibiting characteristics such as... Figure 54 The TEM pattern shows partial CEI cracks. These results demonstrate the high morphological and chemical stability of the protective mesophase formed on the LCO surface by the designed electrolyte.
[0068] The protective effect of the designed electrolyte on the LCO interface phase under high voltage was investigated using HR-TEM and in-situ Raman spectroscopy. First, HR-TEM images and corresponding Fast Fourier Transform (FFT) patterns of cyclic LCO particles confirmed the protective effect of the designed electrolyte on the LCO interface structure. Figure 56 After 200 cycles in the base electrolyte, regions exhibiting spinel and rock salt phases with a thickness of approximately 40 nm were observed on the LCO surface. In contrast, LCO particles cycled in the designed electrolyte primarily maintained a layered structure, confirming that anion-induced CEI can effectively inhibit interfacial degradation of LCO under high voltage.
[0069] In-situ Raman spectroscopy is used to monitor the structural evolution of the LCO interface phase during cycling. Figure 57 At the start of charging, both electrolytes exhibited two characteristic peaks for LCO (485 and 595 cm⁻¹). -1 O-Co-O bending (E g ) and Co-O stretching (A 1g The indicator is a layered phase. When the charging voltage reaches 4.6 V (relative to Li / Li), + These peaks disappear when discharged to 3.0 V (relative to Li / Li), indicating a phase transition from the layered phase to the spinel phase in LCO at high voltage. However, when discharged to 3.0 V (relative to Li / Li), the peaks disappear again. + When the LCO circulated in the base electrolyte was in the designed electrolyte, the characteristic peaks of the layered phase could not be reproduced, while the LCO circulated in the designed electrolyte completely reverted to the layered phase. This further confirms the enhanced effect of the designed electrolyte in promoting the reversible phase transition of LCO at high voltages.
[0070] By combining high-temperature stability with enhanced ionic conductivity at low temperatures, the designed electrolyte enables robust high-voltage operation over a wide temperature range. Figure 58 Specifically, mitigating side reactions, including continuous electrolyte decomposition, irreversible interfacial phase transitions in LCO, thermal decomposition of the electrolyte, and unavoidable CEI evolution, significantly enhances the cycle stability of the LCO cathode at high cutoff voltages and high temperatures. These improvements are attributed to the anion-induced dense, protective mesophase with high chemical inertness and uniform morphology, as well as the inherent antioxidant properties and thermal stability of the designed electrolyte. Furthermore, the low overpotential and inherently high ionic conductivity at low temperatures imparted by the designed electrolyte enable the battery pack to exhibit considerable capacity at extremely low temperatures. This demonstrates the significant potential of cation-anion solvation engineering in designing advanced electrolytes that can provide stable and reliable performance under harsh conditions.
[0071] The invention is given by way of example only, and various other modifications and / or alterations may be made to the described embodiments by those skilled in the art without departing from the scope of the invention as specified in the appended claims.
Claims
1. An electrolyte for lithium-based batteries, comprising a mixture of at least three lithium salts and a carbonate solvent, wherein the at least three lithium salts are selected from the group consisting of lithium tetrafluoroborate, lithium difluorooxalate borate, lithium difluorodioxalate phosphate, lithium bis(fluorosulfonyl)imide, and lithium bis(trifluoromethanesulfonyl)imide.
2. The electrolyte of claim 1, wherein the at least three lithium salts comprise lithium tetrafluoroborate, lithium difluorooxalate borate, and lithium difluorodioxalate phosphate.
3. The electrolyte of claim 2, wherein the lithium tetrafluoroborate, the lithium difluorooxalate borate, and the lithium difluorodioxalate phosphate have a molar ratio of 4:4:
3.
4. The electrolyte of claim 1, wherein the at least three lithium salts have a total concentration of 0.5 M to 1.5 M.
5. The electrolyte of claim 4, wherein the at least three lithium salts have a total concentration of 1.1 M.
6. The electrolyte of claim 1, wherein the carbonate solvent mixture comprises propylene carbonate, ethyl methyl carbonate, dimethyl carbonate, and fluoroethylene carbonate.
7. The electrolyte of claim 6, wherein the propylene carbonate, the methyl ethyl carbonate, the dimethyl carbonate and the fluoroethylene carbonate have a volume ratio of a:b:c:d, wherein a is 2-5, b is 3-5, c is 1-3, d is 1-2, and a+b+c+d=1.
8. The electrolyte of claim 1, further comprising additives selected from the group consisting of vinylene carbonate, 1,3-propanesulfonate lactone, difluoroethylene carbonate, tri-(trimethylsilane)borate, methanedisulfonate, and tri-(trimethylsilane)phosphate, and combinations thereof.
9. The electrolyte of claim 8, wherein the mass of the additive is 5% or less of the total mass of the electrolyte.
10. The electrolyte of claim 1, wherein the electrolyte has a decomposition voltage of 4.43 V (vs. Li / Li + ) under measurement by linear sweep voltammetry with a cutoff current density of 4 μA cm -2 .
11. The electrolyte of claim 1, wherein it remains in liquid form at a temperature of -80°C to 45°C.
12. The electrolyte of claim 1, wherein it is stable at 80°C or below for at least 140 hours.
13. A lithium-based battery, comprising: The cathode includes a cathode active material selected from the group consisting of lithium cobalt oxide, lithium iron phosphate, lithium manganese oxide, lithium manganese iron phosphate, nickel-cobalt-manganese-rich materials, nickel-cobalt-aluminum-rich materials, and graphite. Anode; and The electrolyte comprises at least three lithium salts selected from lithium tetrafluoroborate, lithium difluorooxalate borate and lithium difluorodioxalate phosphate, and a carbonate solvent mixture selected from the group consisting of propylene carbonate, ethyl methyl carbonate, dimethyl carbonate and fluoroethylene carbonate.
14. The lithium-based battery of claim 13, wherein the cathode comprises a cathode active material of lithium cobalt oxide, and the anode comprises an anode active material selected from the group consisting of graphite, silicon, lithium metal, silicon-carbon composites, and silicon dioxide.
15. The lithium-based battery of claim 13, wherein the cathode comprises a graphite cathode active material, and the anode comprises an anode active material selected from the group consisting of lithium metal, silicon, silicon-carbon composites, and silicon dioxide.
16. The lithium-based battery of claim 13, wherein the mass loading of the cathode is 6.6 mg cm⁻¹. -2 .
17. The lithium-based battery of claim 13, wherein the mass loading of the anode is 2.0 mg cm⁻¹. -2 Up to 4.0 mgcm -2 .
18. The lithium-based battery of claim 13, wherein the average coulombic efficiency of the lithium-based battery is at least 99% when operating at a voltage of at least 4.6 V and a temperature of 45°C.
19. The lithium-based battery of claim 13, wherein the electrolyte is arranged to form a cathode-electrolyte interphase on the cathode at a voltage of 4.6 V to stabilize the interface phase of the cathode at the high voltage.
20. The lithium-based battery of claim 19, wherein the cathode-electrolyte interphase is uniformly distributed on the cathode surface and has a thickness of 7 nm to 20 nm.
21. The lithium-based battery of claim 20, wherein the cathode-electrolyte intermediate phase comprises LiF with a concentration gradient, such that the LiF concentration on the side closer to the cathode surface is higher than the LiF concentration on the side farther from the cathode surface.