A long-cycle electrolyte, its preparation method and application

By using a dual-solvent system of α- or ortho-substituted epoxy ether T1 and branched ethylene glycol dialkyl ether T2, the problems of electrolyte oxidation and interfacial film instability in negative electrode-less sodium-ion batteries under high voltage were solved, achieving long cycle life and high-efficiency electrochemical performance.

CN123120875APending Publication Date: 2026-11-17ZHEJIANG ZHIYUAN NAKE ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611628360.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing sodium-ion battery electrolytes without negative electrodes are prone to oxidation and decomposition under high pressure, and have poor interfacial film stability, resulting in shortened battery cycle life and failing to meet long-cycle requirements.

Method used

A weak solvation system was constructed using α- or ortho-substituted epoxy ether T1 and branched ethylene glycol dialkyl ether T2 as solvents. The α-hydrogen was protected by steric hindrance, which inhibited ring-opening polymerization and promoted the formation of inorganic SEI film, thus achieving high-pressure stability.

Benefits of technology

It significantly improves the high-voltage cycle stability and electrochemical performance of anode-free sodium-ion batteries, enhances capacity retention, strengthens interfacial film stability, and reduces interfacial impedance accumulation.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This application discloses a long-cycle electrolyte and its preparation method and application, belonging to the field of sodium-ion battery and electrolyte technology. It includes a solvent and a sodium salt. The solvent includes epoxy ether T1 and ethylene glycol dialkyl ether T2. Through the synergistic design of epoxy ether T1 and ethylene glycol dialkyl ether T2, this application addresses the pain points of traditional ether electrolytes such as easy oxidation under high pressure, easy ring opening of cyclic ethers, and poor stability of the negative electrode interface from multiple dimensions, including steric hindrance protection of α hydrogen, inhibition of cyclic ether ring-opening polymerization, regulation of sodium ion solvation sheath layer, construction of inorganic-dominated stable SEI film, and high-voltage positive electrode interface passivation. This significantly improves the high-voltage long-cycle performance of negative electrode-free sodium-ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of sodium-ion battery and electrolyte technology, and particularly relates to a long-cycle electrolyte, its preparation method and application. Background Technology

[0002] Electrodeless sodium-ion batteries abandon traditional negative electrode active materials, relying on in-situ deposition of metallic sodium on the current collector surface to perform the negative electrode function. This significantly simplifies the cell structure and reduces material costs, while fully leveraging the specific capacity advantages of layered oxides and polyanion cathodes, making it an important technological route for long-term, large-scale energy storage. Long cycle life is the core bottleneck restricting the industrialization of electrodeless sodium-ion batteries. This system lacks a buffer layer of negative electrode active material; metallic sodium directly nucleates and grows on the current collector surface. The sodium deposition-stripping process is highly sensitive to the molecular structure of the electrolyte solvent. Not only do layered oxides experience transition metal dissolution and lattice degradation under high voltage, but polyanion cathodes also continuously undergo interfacial side reactions with cycling. Once the electrolyte's oxidation resistance is insufficient and the mechanical stability of the negative electrode SEI film is poor, repeated breakage and repair of the interfacial film, continuous consumption of active sodium, and continuous deterioration of coulombic efficiency lead to irreversible and rapid capacity decay. Therefore, for long-cycle, anode-free sodium-ion batteries, the electrolyte needs to withstand the high-voltage oxidation environment on the positive electrode side and be able to regulate the solvation behavior of sodium ions. A stable SEI film with low impedance and high inorganic component ratio is constructed on the sodium metal anode to reduce the loss of active sodium.

[0003] Ether solvents, with their moderate viscosity, high ionic conductivity, and good intrinsic compatibility with metallic sodium, are an important research direction for electrolytes in anode-less sodium-ion batteries. Ordinary linear ether molecules contain a large number of α-hydrogen sites, making them easily oxidized on the surface of the high-voltage positive electrode, causing continuous solvent decomposition and gas generation. While unsubstituted cyclic ethers have a cyclic structure that facilitates solvation control, the ether oxygen on the ring is easily attacked by Lewis acids evolved from the positive electrode, resulting in ring-opening polymerization side reactions and generating a large number of low-molecular-weight byproducts that continuously damage the electrode interface. Both linear and unmodified cyclic ethers are mostly strong solvation systems, with solvent molecules entering the sodium ion solvation sheath in large quantities and preferentially decomposing on the negative electrode surface to generate an SEI film with a high proportion of organic components and poor mechanical strength. This type of interfacial film lacks toughness and is prone to cracking under sodium deposition volume stress, requiring continuous consumption of electrolyte and active sodium for repair, directly compressing the battery's long cycle life.

[0004] To address the shortcomings of ether-based electrolytes, existing technologies typically employ high salt concentrations and the addition of functional additives. While high-salt systems can reconstruct the solvated sheath to some extent, they introduce practical problems such as a sharp increase in electrolyte viscosity, poor wettability, and a significant rise in raw material costs. Furthermore, film-forming additives are continuously consumed during cycling, making it difficult to support long-term cycling conditions of thousands of cycles. Some studies have directly combined cyclic ethers with linear ethers, but without substituting or modifying the cyclic and linear ether molecules, they cannot inhibit the ring-opening polymerization of cyclic ethers, nor can they protect the α-hydrogen in the molecule through steric hindrance, still failing to simultaneously meet the dual requirements of high-voltage oxidation resistance and stable film formation at the negative electrode. If only cyclic ethers are used, the electrolyte viscosity is too high, resulting in significant ion migration resistance; if only linear ethers are used, it is difficult to achieve a weak solvation effect, failing to induce preferential reduction of anions to form an inorganic-dominated SEI film.

[0005] Furthermore, to achieve a long-cycle, anode-free sodium battery electrolyte, relying solely on a single solvent is insufficient. Simultaneous molecular substitution modification of cyclic ethers and chain ethers is necessary. For cyclic epoxy ethers, substituents need to be introduced to provide steric hindrance, protecting the ether oxygen atom on the ring from Lewis acid attack and inhibiting ring-opening, while also reducing easily oxidized α-hydrogen sites. For chain ether components, branched structures need to be introduced to shield α-hydrogen sites through steric hindrance, while simultaneously working in conjunction with the modified epoxy ether to construct a weakly solvated solvent environment, promoting the preferential reduction of sodium salt anions and building an inorganic-based SEI film. Without this synergistic molecular structural modification, simply mixing existing commercial ether solvents is insufficient to simultaneously address a series of issues, including cyclic ether ring-opening, high-pressure oxidation of ether molecules, excessively high organic content in the anode SEI, and continuous consumption of active sodium.

[0006] In summary, existing ether electrolytes generally suffer from the following shortcomings: cyclic ethers are prone to ring-opening polymerization, α-hydrogen in ether molecules are easily oxidized under high pressure, the proportion of organic components in the negative electrode SEI is high, and the active sodium is severely depleted during long cycles. They are difficult to adapt to both layered oxide and polyanion cathodes at the same time, and cannot meet the industrial application requirements for long-cycle sodium-ion batteries without negative electrodes. Summary of the Invention

[0007] To address the aforementioned deficiencies, the first objective of this application is to provide a long-cycle electrolyte employing an α- or ortho-substituted epoxy ether T1 and a branched ethylene glycol dialkyl ether T2. Due to the reduced number of α-hydrogens, the steric hindrance effect further protects the α-hydrogens from oxidation, resulting in strong antioxidant properties. This electrolyte is suitable for high-voltage systems. This weakly solvated system induces the reduction of anions at the negative electrode to form an inorganic-dominated SEI film, which can significantly improve the long-cycle performance of a negative electrode-less sodium battery.

[0008] To achieve the above-mentioned objectives, this application adopts the following technical solution: A long-cycle electrolyte includes a solvent and a sodium salt. The solvent includes an epoxy ether T1 and a ethylene glycol dialkyl ether T2. The epoxy ether T1 is selected from at least one of 2,4-dimethyl-1,3-dioxolane, 2-methyltetrahydrofuran, and 2-(trifluoromethyl)-1,3-dioxolane. The ethylene glycol dialkyl ether T2 is selected from one or a combination of two of 1,2-diethoxypropane and propylene glycol dimethyl ether.

[0009] Further settings are as follows: When ethylene glycol dialkyl ether T2 is a combination of 1,2-diethoxypropane and propylene glycol dimethyl ether, the mass ratio of 1,2-diethoxypropane to propylene glycol dimethyl ether is 1:1.

[0010] The mass ratio of epoxy ether T1 to ethylene glycol dialkyl ether T2 is 1:9-2:1, preferably 1:2-2:1.

[0011] The sodium salt is selected from at least one of NaPF6, NaClO4, NaBF4, NaODFB, NaFSI, and NaTFSI.

[0012] The concentration of sodium salt is 0.6–2.0 mol / L.

[0013] The mechanism of action of this application is as follows: Research has revealed that ordinary chain ether and cyclic ether electrolyte molecules contain a large amount of α-hydrogen, which is extremely prone to oxidative degradation on the surface of the high-voltage positive electrode under high-voltage conditions. Cyclic ethers are also prone to ring-opening polymerization under the action of Lewis acids, which can trigger continuous side reactions and cell gas generation. At the same time, conventional strong solvation ether systems are prone to forming an SEI film with a high proportion of organic components and poor stability on the sodium metal negative electrode. The interface is repeatedly damaged and rebuilt, which seriously restricts the high-voltage long cycle life of negative electrode-less sodium-ion batteries.

[0014] To address the aforementioned issues, this application constructs a dual-solvent weak solvation electrolyte system consisting of "epoxy ether T1 + ethylene glycol dialkyl ether T2", wherein: (1) The epoxy ether T1 of this application has methyl, ethyl, ethoxy or fluoromethyl substituents; methyl, ethyl or fluoromethyl substituents bring significant steric hindrance effect, which can protect the oxygen atom on the ring from the attack of Lewis acid on the positive electrode surface while realizing weak solvation and inhibiting the ring-opening polymerization side reaction of epoxy ether; ethoxy substituents can provide additional coordination sites, further enhance the dissociation ability of sodium salt and ensure the ion conduction performance of electrolyte.

[0015] (2) The branched ethylene glycol dialkyl ether T2 can form a solvation sheath with sodium ions with moderate strength, taking into account both weak solvation characteristics and the stability of the solvation sheath structure; the α-position / ortho-position substitution of epoxy ether T1 and the branched structure of ethylene glycol dialkyl ether T2 together reduce the number of α hydrogens in the molecule, and rely on steric hindrance to shield the α hydrogen sites, reducing its reactivity under high pressure oxidation, so that the dual solvent system has excellent antioxidant capacity.

[0016] (3) The present application is a weak solvation solvent system. The proportion of free solvent molecules in the sodium ion solvation sheath is reduced, which preferentially drives the anions in the electrolyte to undergo reduction and decomposition on the sodium metal anode surface, inducing the formation of an inorganic component-dominated, dense and stable SEI film. Fluoromethyl substitution can further increase the proportion of fluorine-containing inorganic species (NaF) at the interface, enhance the mechanical strength and ion conductivity of the SEI film, inhibit repeated SEI rupture and regeneration, slow down sodium dendrite growth, and reduce the accumulation of interfacial impedance.

[0017] On the high-voltage positive electrode side, T1 and T2 work together to construct a stable positive electrode interface passivation film, which prevents the electrolyte from directly contacting the high-voltage positive electrode, inhibits solvent oxidation and decomposition, dissolution of positive electrode transition metal and destruction of crystal structure, and alleviates the gas generation problem under high voltage. On the side without negative electrode current collector, the weak solvation system regulates the desolvation behavior of sodium ions and guides uniform sodium metal deposition and stripping.

[0018] This application addresses the pain points of traditional ether electrolytes, such as easy oxidation under high voltage, easy ring-opening of cyclic ethers, and poor stability of the negative electrode interface, through the synergistic design of epoxy ether T1 and ethylene glycol dialkyl ether T2. These issues are addressed from multiple dimensions, including steric hindrance protection of α-hydrogen, inhibition of cyclic ether ring-opening polymerization, regulation of sodium ion solvation sheath layer, construction of inorganic-dominated stable SEI film, and high-voltage positive electrode interface passivation. This significantly improves the high-voltage long-cycle performance of negative electrode-free sodium-ion batteries.

[0019] The second aspect of this application is to provide a method for preparing a long-cycle electrolyte, comprising the following steps: in an argon atmosphere glove box with a water content of <10ppm, dissolving sodium salt in a mixed solvent of epoxy ether T1 and ethylene glycol dialkyl ether T2, stirring until completely dissolved, to obtain a long-cycle electrolyte.

[0020] The third objective of this application is to provide an application of a long-cycle electrolyte in a negative electrode-free sodium-ion battery, wherein the positive electrode material of the negative electrode-free sodium-ion battery is a layered oxide positive electrode material or a polyanion-based positive electrode material.

[0021] The negative electrode-free sodium-ion battery includes a positive electrode, a negative electrode current collector, an electrolyte, and a separator.

[0022] The electrolyte is the aforementioned long-cycle electrolyte.

[0023] The layered oxide cathode material is selected from at least one of the following compounds: NaCoO2, NaMnO2, NaNiO2, NaCrO2, NaNi 0.5 Mn 0.5 O2, NaNi 0.5 Ti 0.5 O2, NaFe 0.5 Mn 0.5 O2, NaCu 0.5 Fe 0.5 O2, NaNi 0.33 Fe 0.33 Mn 0.33 O2, NaNi 0.33 Co 0.33 Mn 0.33 O2.

[0024] The polyanionic cathode material is selected from at least one of the following compounds: Na2FeP2O7, Na2MnP2O7, Na4Fe3(PO4)2P2O7; Na2Fe2(SO4)3, Na2Fe2(PO4)(SO4)2, Na4Fe3(PO4)2P2O7.

[0025] The diaphragm is selected from any one of polyethylene monolayer membrane (PE), polypropylene monolayer membrane (PP), multilayer microporous membrane composed of PP and PE, cellulose nonwoven fabric, polyvinylidene fluoride porous membrane, polyimide electrospun porous membrane, and glass fiber diaphragm, preferably glass fiber diaphragm.

[0026] The negative electrode current collector is made of aluminum foil or copper foil, and a conductive coating is coated on the surface of the negative electrode current collector. The conductive coating is at least one of graphene, carbon nanotubes or hard carbon, and the coating thickness is 1 to 5 μm.

[0027] Compared with existing technical solutions, this application has the following advantages: (1) The long-cycle electrolyte for a negative electrode-free sodium-ion battery disclosed in this application adopts a dual-solvent weak solvation synergistic system composed of "α-position / ortho-position substituted epoxy ether T1 + branched ethylene glycol dialkyl ether T2", which breaks through the technical bottlenecks of ordinary cyclic ethers being prone to Lewis acid-induced ring-opening polymerization and conventional ether solvent α-hydrogen being easily oxidized by high voltage. This application selects epoxy ether T1 with methyl, ethyl, ethoxy, and fluoromethyl substitution. Relying on the steric hindrance effect brought by the substituent groups, on the one hand, it protects the oxygen atoms on the epoxy ring from Lewis acid attack on the positive electrode surface and inhibits the side reaction of cyclic ether ring-opening polymerization. On the other hand, it reduces the number of oxidizable α-hydrogens and improves the molecular antioxidant capacity. Among them, the ethoxy substitution can also provide additional coordination sites, improve the sodium salt dissociation level, and ensure the ion conduction of the electrolyte. By combining it with branched ethylene glycol dialkyl ether T2, a sodium ion solvation sheath layer of moderate strength can be formed, further reducing the α-hydrogen sites in the system. The steric hindrance of the branched chain inhibits α-hydroxylation, optimizes the sodium ion desolvation energy barrier, and reduces the interfacial charge transfer impedance. This overcomes the inherent contradictions of traditional ether electrolytes, such as "cyclic ethers are prone to ring opening, easy oxidation and degradation under high pressure, and high organic content and poor stability of the negative electrode SEI".

[0028] The weakly solvated dual-solvent electrolyte of this application achieves long-term stability at both the positive and negative electrode interfaces under high-voltage conditions: the synergistic system of "epoxy ether T1 + ethylene glycol dialkyl ether T2" can construct dense and stable passivation interface films on the high-voltage positive electrode surface and the sodium metal deposition side, respectively. On the positive electrode side, the passivation film effectively prevents direct contact between the electrolyte and the high-voltage layered oxide positive electrode active material, inhibiting solvent oxidation decomposition, transition metal dissolution, positive electrode lattice destruction, and cell gas generation under high-voltage conditions, maintaining the structural integrity of the positive electrode during high-voltage cycling. On the side without sodium metal in the negative electrode, the weak solvation effect promotes the preferential reduction and decomposition of sodium salt anions, inducing the formation of an inorganic-dominated SEI film; fluoromethyl substitution can further increase the proportion of fluorine-containing inorganic components such as NaF at the interface, improve the mechanical strength of the SEI film, inhibit repeated rupture and regeneration of the interface film, alleviate sodium dendrite growth, reduce the continuous accumulation of interface impedance, and significantly improve the high-voltage cycling stability of the battery.

[0029] (2) The electrolyte of this application, when applied to a negative electrode-free sodium-ion battery, exhibits excellent high-voltage, long-cycle electrochemical performance: The electrolyte is combined with layered oxides (NaNi) 0.33 Fe 0.33 Mn 0.33 An O2-based sodium-ion battery without a negative electrode, after 800 cycles at 25°C with a cutoff voltage of 4.0V, retains >80% of its capacity; it also incorporates polyanion (NaNi) compounds. 0.33 Fe 0.33 Mn 0.33An O2-based sodium-ion battery without a negative electrode exhibits a capacity retention of >80% after 1500 cycles at 25°C with a cutoff voltage of 3.6V. This electrolyte effectively suppresses problems such as ring-opening of cyclic ethers under high voltage, continuous oxidative decomposition of the electrolyte, collapse of the positive electrode structure, and interfacial film loss during long cycles. It overcomes the shortcomings of traditional cyclic / linear ether electrolytes, such as rapid capacity decay after increasing the cutoff voltage, large fluctuations in coulombic efficiency, and instability of the interfacial phase during long cycles, ensuring the electrochemical reversibility of the battery under high voltage conditions. Furthermore, this electrolyte also demonstrates good compatibility with polyanionic positive electrode materials, meeting the cycling requirements of different positive electrode systems.

[0030] (3) The electrolyte formulation of this application is simple and controllable, the raw materials are highly versatile, and it has good industrial adaptability: The solvent is obtained by compounding substituted epoxy ether T1 and branched ethylene glycol dialkyl ether T2. The sodium salt is a commercially available sodium salt, eliminating the need for large amounts of additional functional additives. The dual-solvent compound system maintains good ionic conductivity and membrane wetting ability of the electrolyte. This electrolyte exhibits good compatibility with layered oxides, mainstream sodium battery cathode materials of polyanionic type, various membranes, and negative electrode current collectors with carbon-based conductive coatings. The preparation process only requires dissolving the sodium salt in the mixed solvent and stirring in an inert glove box with low water content. The process is simple, compatible with existing battery cell mass production systems, has low implementation costs, and has good engineering and industrialization promotion value. Detailed Implementation

[0031] The technical solutions of this application will be further described in detail below with reference to specific embodiments. It should be understood that the following embodiments are merely illustrative and explanatory of this application, and should not be construed as limiting the scope of protection of this application. All technologies implemented based on the above content of this application are covered within the scope of protection intended by this application.

[0032] Unless otherwise stated, the raw materials and reagents used in the following examples are commercially available products or can be prepared by known methods.

[0033] The epoxy ether T1 used in the examples is as follows: Solvent T1-A: 2,4-Dimethyl-1,3-dioxolane (CAS: 3390-12-3). Solvent T1-B: 2-Methyltetrahydrofuran (2-Me-THF, CAS: 96-47-9); Solvent T1-C: 2-(trifluoromethyl)-1,3-dioxolane (CAS: 2344-09-4). Meanwhile, an unsubstituted epoxy ether: 1,3-dioxolane was used as a control example: Comparative epoxy ether: 1,3-dioxolane (CAS: 646-06-0). The ethylene glycol dialkyl ether T2 used in the examples is as follows: Solvent T2-A: 1,2-diethoxypropane (CAS: 10221-57-5); Solvent T2-B: Propylene glycol dimethyl ether (DMP, CAS: 7778-85-0); Diethylene glycol dimethyl ether was used as a control example. Compare with straight-chain ethers: diethylene glycol dimethyl ether (DEGDME, CAS: 111-96-6).

[0034] Example 1

[0035] A long-cycle electrolyte comprising a sodium salt and a mixed solvent.

[0036] Mixed solvent: Solvent T1-A (2,4-dimethyl-1,3-dioxolane) + Solvent T2-A (1,2-diethoxypropane); the mass ratio of T1-A to T2-A is 1:2.

[0037] Sodium salt: Common sodium salt NaPF6 and NaTFSI are used in combination. The total concentration of sodium salt is 1.2 mol / L, of which NaPF6 is 0.84 mol / L and NaTFSI is 0.36 mol / L.

[0038] Preparation method: In an argon glove box with a water content of <10ppm, fully dried NaPF6 and NaTFSI are added sequentially to the above mixed solvent, and the mixture is continuously magnetically stirred for 4-8 hours until the solid is completely dissolved and the system is homogeneous and transparent, thus obtaining a long-cycle electrolyte.

[0039] To investigate the effect of different sodium salt combinations on electrolyte performance, Examples 2-6 were set up.

[0040] Example 2

[0041] The preparation method is the same as in Example 1, except that NaTFSI in the sodium salt is replaced with NaClO4, and the total concentration of sodium salt is maintained at 1.2 mol / L, of which: NaPF6 0.84 mol / L + NaClO4 0.36 mol / L.

[0042] Example 3

[0043] The preparation method is the same as in Example 1, except that NaTFSI in the sodium salt is replaced with NaFSI, and the total concentration of sodium salt is maintained at 1.2 mol / L, of which: NaPF6 0.84 mol / L + NaFSI 0.36 mol / L.

[0044] Example 4

[0045] The preparation method is the same as in Example 1, except that a single sodium salt, NaTFSI, is used, and the total concentration of sodium salt is maintained at 1.2 mol / L, i.e., NaTFSI 1.2 mol / L.

[0046] Example 5

[0047] The preparation method is the same as in Example 1, except that the common sodium salt component NaPF6 is replaced with NaBF4, and the total sodium salt concentration is maintained at 1.2 mol / L, of which: NaBF4 0.84 mol / L + NaTFSI 0.36 mol / L.

[0048] Example 6

[0049] The preparation method is the same as in Example 1, except that the common sodium salt component NaPF6 is replaced with NaODFB, and the total sodium salt concentration is maintained at 1.2 mol / L, of which: NaODFB 0.1 mol / L + NaFSI 1.1 mol / L.

[0050] To investigate the effect of different solvent ratios on electrolyte performance, Examples 7-10 were set up.

[0051] Example 7

[0052] The preparation method is the same as in Example 1, except that: epoxy ether T1 is replaced with solvent T1-B (2-methyltetrahydrofuran); the mass ratio of T1-B to T2-A is 1:2.

[0053] Example 8

[0054] The preparation method is the same as in Example 1, except that: the epoxy ether T1 is replaced with solvent T1-C (2-(trifluoromethyl)-1,3-dioxolane); the mass ratio of T1-C to T2-A is 1:2.

[0055] Example 9

[0056] The preparation method is the same as in Example 1, except that: the epoxy ether is T1-A, and the ethylene glycol dialkyl ether T2 is replaced with a combination of "T2-A + T2-B" (1,2-diethoxypropane + propylene glycol dimethyl ether), wherein: the mass ratio of T1-A to (T2-A + T2-B) is 2:1, and the mass ratio of 1,2-diethoxypropane (T2-A) to propylene glycol dimethyl ether (T2-B) is 1:1.

[0057] Example 10 The preparation method is the same as in Example 1, except that: T1-A is used for epoxy ether and T2-A is used for ethylene glycol dialkyl ether; the mass ratio of T1-A to T2-A is 1:9.

[0058] To investigate the effect of sodium salt concentration on electrolyte performance, Examples 11-12 were set up.

[0059] Example 11 The preparation method is the same as in Example 1, except that the total concentration of sodium salt is adjusted to 0.8 mol / L, of which: NaPF6 0.56 mol / L + NaTFSI 0.24 mol / L.

[0060] Example 12 The preparation method is the same as in Example 1, except that the total concentration of sodium salt is adjusted to 1.6 mol / L, of which: NaPF6 1.12 mol / L + NaTFSI 0.48 mol / L.

[0061] Comparative Example 1 The preparation method is the same as in Example 1, except that the substituted epoxy ether T1-A is replaced with the unsubstituted epoxy ether: 1,3-dioxolane.

[0062] Mixed solvent: 1,3-dioxolane + T2-A; the mass ratio of 1,3-dioxolane to T2-A is 1:2; Sodium salt: NaPF6 0.84mol / L + NaTFSI 0.36mol / L, total sodium salt concentration 1.2mol / L.

[0063] Comparative Example 2 The preparation method is the same as in Example 1, except that ethylene glycol dialkyl ether T2-A is replaced with an unsubstituted straight-chain ether: diethylene glycol dimethyl ether DEGDME.

[0064] Mixed solvent: T1-A + diethylene glycol dimethyl ether; the mass ratio of T1-A to diethylene glycol dimethyl ether is 1:2; Sodium salt: NaPF6 0.84mol / L + NaTFSI 0.36mol / L, total sodium salt concentration 1.2mol / L.

[0065] Comparative Example 3 The preparation method is the same as in Example 1, except that the solvent system of "epoxy ether T1 + ethylene glycol dialkyl ether T2" of this application is not used.

[0066] Mixed solvent: 1,3-dioxolane + diethylene glycol dimethyl ether; the mass ratio of 1,3-dioxolane to diethylene glycol dimethyl ether is 1:2; Sodium salt: NaPF6 0.84mol / L + NaTFSI 0.36mol / L, total sodium salt concentration 1.2mol / L.

[0067] Comparative Example 4 The preparation method is the same as in Example 1, except that the mass ratio of epoxy ether T1 and ethylene glycol dialkyl ether T2 is adjusted.

[0068] Mixed solvent: T1-A + T2-A; the mass ratio of T1-A to T2-A is 1:10.

[0069] Sodium salt: NaPF6 0.84mol / L + NaTFSI 0.36mol / L, total sodium salt concentration 1.2mol / L.

[0070] Comparative Example 5 The preparation method is the same as in Example 1, except that only T1-A single solvent is used, and ethylene glycol dialkyl ether T2 is not added.

[0071] Solvent: T1-A.

[0072] Sodium salt: NaPF6 0.84mol / L + NaTFSI 0.36mol / L, total sodium salt concentration 1.2mol / L.

[0073] Application Examples

[0074] The electrolytes prepared in the aforementioned examples and comparative examples were applied to non-negative electrode sodium-ion batteries (NFPP and NFM batteries) to test their electrochemical performance.

[0075] A negative electrode-free sodium-ion battery includes a positive electrode, a negative electrode current collector, a separator, and an electrolyte.

[0076] Positive electrode preparation: The positive electrode active material is selected from NFPP (Na4Fe3(PO4)2P2O7) or NFM (NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3O2), the positive electrode active material, conductive carbon black (SP), and polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 92:5:3, and an appropriate amount of N-methylpyrrolidone (NMP) is added and stirred thoroughly until the slurry is uniform; the mixed slurry is uniformly coated on the surface of the aluminum foil current collector, and then dried, rolled and compacted, and cut into sheets to obtain NFPP and NFM positive electrode sheets.

[0077] Negative electrode current collector: Copper foil with a 2μm carbon-based conductive layer on its surface is used as the negative electrode current collector.

[0078] Separator: Glass fiber diaphragm is selected.

[0079] Electrolyte: The electrolyte prepared in the aforementioned examples and comparative examples is used.

[0080] Battery assembly: The positive electrode, separator, and negative electrode current collector are stacked and aligned in sequence to obtain a bare cell; the bare cell is packaged in an aluminum-plastic film bag to complete the dry cell preparation, and then the electrolyte is injected into the dry cell to complete the heat sealing; after going through the electrolyte full wetting, small current activation formation, and cell shaping processes in sequence, a negative electrode-free sodium-ion battery is finally obtained.

[0081] Performance testing: The Blue Battery testing system was used, and the test environment temperature was set to 25℃ according to the experimental requirements. The voltage range of NFPP batteries was 2.0V-3.6V, and the voltage range of NFM batteries was 2.0V-4.0V.

[0082] NFPP battery cycle performance test At 25°C, the NFM system sodium-ion battery without a negative electrode was charged to 3.6V with a constant current of 0.1C and then discharged to 2.0V with a constant current of 0.1C. This charge-discharge cycle was repeated twice to activate the cell. After activation, the cell was continuously cycled for 1500 times using a charge-discharge regime of charging to 3.6V with a constant current of 1C and discharging to 2.0V with a constant current of 1C. The discharge capacity during the cycle was recorded, and the battery capacity retention rate after the cycle was calculated.

[0083] NFM Battery Cycling Performance Test At 25°C, the NFM system sodium-ion battery without a negative electrode was charged to 4.0V with a constant current of 0.1C and then discharged to 2.0V with a constant current of 0.1C. This charge-discharge cycle was repeated twice to activate the cell. After activation, the cell was continuously cycled for 800 times using a charge-discharge regime of 1C constant current to 4.0V and 1C constant current to 2.0V. The discharge capacity during the cycle was recorded, and the battery capacity retention rate after the cycle was calculated.

[0084] (3) Battery internal resistance test DC pulse internal resistance tests were performed on NFPP and NFM sodium-ion batteries at 25℃ and 50% SOC. The batteries were allowed to stand until the open-circuit voltage stabilized, and a 1C constant current discharge pulse was applied for 10 seconds. The open-circuit voltage before the pulse and the terminal voltage at the end of the pulse were collected. The DC internal resistance was calculated based on the voltage difference and the pulse current.

[0085] The formula for calculating battery capacity retention rate is as follows: Capacity retention rate = Discharge capacity for the corresponding number of cycles / First stable cycle discharge capacity after activation × 100%.

[0086] The test results are shown in Table 1.

[0087] Table 1 .

[0088] The test results in the table above show that: (1) Examples 1-12 of this application use a dual-solvent weak solvation electrolyte system of “substituted epoxy ether T1 + ethylene glycol dialkyl ether T2”. Under the two negative electrode-free sodium-ion battery systems of NFPP polyanion and NFM high-voltage layered oxide, it has higher capacity retention and lower battery internal resistance. The electrochemical performance is significantly better than that of each comparative example group. The NFPP battery has a capacity retention of >80% after 1500 cycles at 25℃ and the NFM battery has a capacity retention of >80% after 800 cycles at -4.0V at 25℃.

[0089] Comparative Example 1 used an unsubstituted epoxy ether 1,3-dioxolane to replace the substituted epoxy ether T1 in this application. Although paired with the branched ether T2 in this application and a qualified sodium salt system, the unsubstituted epoxy ether lacked the steric hindrance protection provided by alkyl / fluorine substitution. The oxygen atoms on the ring were susceptible to Lewis acid attack on the cathode surface, resulting in ring-opening polymerization side reactions and continuous electrolyte decomposition and gas production. The NFPP battery in this group had a capacity retention of only 62.3% after 1500 cycles at 25°C, and the NFM battery had a capacity retention of only 58.6% after 800 cycles at 25°C and -4.0V. The internal resistance of the battery increased significantly, proving that the α-position / ortho-position substituted epoxy ether T1 is a necessary component to suppress ring-opening of the ether and achieve high-voltage stability.

[0090] Comparative Example 2 uses the epoxy ether T1-A as described in this application, but replaces the branched T2-A with a common straight-chain ether: diethylene glycol dimethyl ether (DEGDME). Straight-chain ether molecules have a large number of α-hydrogens and lack the steric hindrance shielding provided by branches, making them prone to oxidative degradation under high voltage conditions, and the interfacial passivation film is easily damaged. The NFPP battery in this group retained only 67.5% of its capacity after 1500 cycles at 25°C, and the NFM battery retained only 64.1% of its capacity after 800 cycles at 25°C and -4.0V. This indicates that the branched structure of the branched ethylene glycol dialkyl ether T2 plays a crucial role in improving the system's antioxidant capacity.

[0091] Comparative Example 3 uses both unsubstituted epoxy ether and ordinary straight-chain ether, without using the "epoxy ether T1 + ethylene glycol dialkyl ether T2" dual solvent system of this application. It cannot suppress the ring opening of epoxy ether, and lacks the steric protection of α-H by the branched structure. The electrolyte undergoes ring opening and oxidative decomposition on the high-voltage positive electrode side at the same time, which is one of the poor performance groups. The NFPP battery has a capacity retention rate of only 53.8% after 1500 cycles at 25℃, and the NFM battery has a capacity retention rate of only 49.2% after 800 cycles at 25℃ and -4.0V. This directly verifies the important significance of the synergistic effect of the "epoxy ether T1 + ethylene glycol dialkyl ether T2" dual solvent system.

[0092] In Comparative Example 4, the mass ratio of epoxy ether T1 to ethylene glycol dialkyl ether T2 was 1:10. The proportion of epoxy ether component was too low, resulting in insufficient weak solvation effect and inability to effectively control the sodium ion solvation sheath layer. The anion reduction film formation effect was weakened, the positive and negative electrode interface protection effect decreased, and the high-voltage cycling performance was significantly deteriorated. This proves that the ratio of the two solvents needs to be controlled within the range specified in this application.

[0093] Comparative Example 5 used only the single solvent T1-A, which replaced epoxy ether, without adding ethylene glycol dialkyl ether T2. The solvent system viscosity was too high, the solvation structure was uncontrollable, and it was impossible to form a solvent sheath of moderate strength. The proportion of organic components in the SEI membrane increased and the stability deteriorated. The NFPP battery had a capacity retention rate of only 58.2% after 1500 cycles at 25°C, and the NFM battery had a capacity retention rate of only 54.7% after 800 cycles at 25°C and -4.0V. This shows that ethylene glycol dialkyl ether T2 is indispensable, and only a dual solvent combination can achieve the technical effect of balancing weak solvation and solvent sheath stability.

[0094] (2) By adjusting the combination of electron-rich sodium salts, the selection of epoxy ether T1 and ethylene glycol dialkyl ether T2, the ratio of the two solvents, and the total concentration of sodium salts, the degree of sodium salt dissociation in the electrolyte, the sodium ion solvation sheath, the interfacial film formation characteristics, and the high-voltage long-cycle performance of the negative electrode-free sodium-ion battery can be precisely controlled. Within the formulation parameters specified in this application, both NFPP and NFM cathode systems can achieve excellent long-cycle performance.

[0095] As can be seen from Examples 1-6, NaTFSI, NaClO4, and NaFSI can all be used as electron-rich sodium salts. They can be combined with ordinary sodium salts or used alone to construct the weak solvation system of this application. Among them, the single NaTFSI system (Example 4) has excellent comprehensive performance. The high proportion of electron-rich anions is more conducive to preferential reduction and decomposition, thus constructing an inorganic-dominated SEI film.

[0096] As can be seen from the comparison with Examples 1 and 7-8, the epoxy ethers T1 with different substitutions can all be adapted to this electrolyte system; among them, the fluorine-substituted T1-C (Example 8) can further increase the interfacial fluorine source, increase the proportion of NaF inorganic components, and achieve the lowest battery internal resistance and the best cycle performance; the alkyl-substituted T1-A and T1-B can also meet the performance indicators, proving that the various substituted solvents under the general formula of epoxy ethers in this application have universality.

[0097] As can be seen from Examples 1 and 9-10, adjusting the T1 / T2 ratio still allows the electrolyte to meet the performance indicators of this application. When the mass ratio of T1 / T2 is adjusted to the lower limit of 1:9, the performance drops slightly but still meets the standard, demonstrating the rationality of the ratio range setting in this application.

[0098] As can be seen from Examples 1 and 11-12, the total sodium salt concentration can operate normally within the preferred range of 0.8-1.6 mol / L. When the concentration is too low (0.8 mol / L), there are insufficient ion carriers, the internal resistance of the battery increases, and the cycle performance decreases slightly. When the concentration is increased to 1.6 mol / L, the viscosity of the system increases, the resistance to ion transport increases, and the overall performance is slightly lower than that of the 1.2 mol / L reference formulation.

[0099] Summarize: This application's long-cycle electrolyte relies on a dual-solvent weak solvation synergistic mechanism of "α-position / ortho-position substituted epoxy ether T1 + branched substituted ethylene glycol dialkyl ether T2". It utilizes the steric hindrance of the substituent groups to inhibit the ring-opening polymerization of the epoxy ether and shields the α-hydrogen sites to reduce high-voltage oxidation activity. The weak solvation effect promotes preferential reduction of anions, constructing an inorganic-dominated stable SEI film. This achieves interface protection on both the high-voltage positive electrode and the sodium-free negative electrode sides, solving the industry pain points of traditional ether electrolytes: easy ring-opening of cyclic ethers, easy oxidation under high voltage, and poor stability due to high organic content in the negative electrode SEI. The optimal embodiment 8 achieves an 87.6% capacity retention rate for NFPP batteries after 1500 cycles at 25℃ and an 85.9% capacity retention rate for NFM batteries after 800 cycles at 25℃-4.0V. The batteries exhibit low internal resistance and no significant capacity drop during long-cycle operation. The raw materials in this application are commercially available solvents, the formulation is simple, and the preparation process is compatible with existing cell manufacturing processes, possessing good engineering application and industrialization promotion value.

Claims

1. A long-cycle electrolyte, characterized in that: The mixture includes a solvent and a sodium salt. The solvent includes an epoxy ether T1 and a ethylene glycol dialkyl ether T2. The epoxy ether T1 is selected from at least one of 2,4-dimethyl-1,3-dioxolane, 2-methyltetrahydrofuran, and 2-(trifluoromethyl)-1,3-dioxolane. The ethylene glycol dialkyl ether T2 is selected from one or a combination of two of 1,2-diethoxypropane and propylene glycol dimethyl ether.

2. The long-cycle electrolyte according to claim 1, characterized in that: When ethylene glycol dialkyl ether T2 is a combination of 1,2-diethoxypropane and propylene glycol dimethyl ether, the mass ratio of 1,2-diethoxypropane to propylene glycol dimethyl ether is 1:

1.

3. The long-cycle electrolyte according to claim 1, characterized in that: The mass ratio of the epoxy ether T1 to the ethylene glycol dialkyl ether T2 is 1:9-2:

1.

4. The long-cycle electrolyte according to claim 3, characterized in that: The mass ratio of the epoxy ether T1 to the ethylene glycol dialkyl ether T2 is 1:2-2:

1.

5. The long-cycle electrolyte according to claim 1, characterized in that: The sodium salt is selected from at least one of NaPF6, NaClO4, NaBF4, NaODFB, NaFSI, and NaTFSI.

6. The long-cycle electrolyte according to claim 1, characterized in that: The concentration of sodium salt is 0.6–2.0 mol / L.

7. A method for preparing the long-cycle electrolyte according to claim 1, comprising the following steps: In an argon atmosphere glove box with a water content of <10ppm, sodium salt is dissolved in a mixed solvent of epoxy ether T1 and ethylene glycol dialkyl ether T2 and stirred until completely dissolved to obtain a long-cycle electrolyte.

8. The application of the long-cycle electrolyte of claim 1 in a negative electrode-free sodium-ion battery.