A method for preparing lithium-rich manganese-based cathode materials based on waste cathode sheets and the lithium-rich manganese-based cathode materials.

By pretreatment, mixing, ball milling and sintering of waste nickel-cobalt-manganese ternary cathode sheets and lithium manganese oxide cathode sheets, lithium-rich manganese-based cathode materials are formed, which solves the problem of poor electrochemical performance of recycled materials and achieves performance improvement and environmentally friendly process.

CN123120951APending Publication Date: 2026-11-17WELNENG ENVIRONMENTAL TECH (SUZHOU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611314952.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-27
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing technologies, the electrochemical performance of recycled materials obtained by simply mixing and sintering nickel-cobalt-manganese ternary lithium battery cathode waste and lithium manganese oxide cathode waste is poor.

Method used

By pretreating waste nickel-cobalt-manganese ternary cathode sheets and lithium manganese oxide cathode sheets, mixing them and adding lithium, nickel, cobalt and manganese sources, and using organic acids and vanadium-containing modifiers, ball milling, vacuum drying, pre-sintering and main sintering are carried out to form lithium-rich manganese-based cathode materials.

Benefits of technology

Constructing a stable chemical bridging structure reduces the interfacial diffusion barrier, promotes material bonding, and improves electrochemical performance, which aligns with the concepts of green chemistry and sustainable development.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120951A_ABST
    Figure CN123120951A_ABST
Patent Text Reader

Abstract

This application discloses a method for preparing lithium-rich manganese-based cathode materials based on waste cathode sheets, and the lithium-rich manganese-based cathode materials themselves, relating to the technical field of lithium battery regeneration. The method includes the following steps: mixing waste nickel-cobalt-manganese ternary cathode materials and waste lithium manganese oxide cathode materials in a specific ratio, and adding at least one of a lithium source, nickel source, cobalt source, and manganese source to obtain a first mixture; adding organic acid and a vanadium-containing modifier stepwise to the first mixture, followed by ball milling and vacuum drying to obtain a precursor; and sintering the precursor under an oxygen atmosphere to obtain the lithium-rich manganese-based cathode material. This application effectively complexes nickel, cobalt, and manganese ions by ball milling the carboxyl functional groups in the organic acid, constructing a chemical bridging structure between the waste nickel-cobalt-manganese ternary cathode materials and the waste lithium manganese oxide cathode materials, reducing the interfacial diffusion barrier during subsequent high-temperature sintering, and promoting effective bonding between materials; and promoting oxygen vacancy formation through the vanadium-containing modifier during pre-sintering.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the technical field of lithium battery recycling, specifically to a method for preparing lithium-rich manganese-based cathode materials based on waste cathode sheets and the lithium-rich manganese-based cathode materials. Background Technology

[0002] With the rapid development of the energy storage industry, the number of retired lithium-ion batteries has surged. Nickel-cobalt-manganese ternary lithium batteries and lithium manganese oxide batteries, as mainstream cathode materials, are of great significance for resource recycling and environmental protection through recycling and reuse.

[0003] Currently, the recycling of waste cathode materials mainly adopts direct regeneration technology, which involves mixing different types of cathode waste (such as ternary materials and lithium manganese oxide), adding appropriate elements, and then preparing recycled materials through high-temperature sintering to achieve efficient resource utilization. However, simply mixing and sintering nickel-cobalt-manganese ternary lithium battery cathode waste and waste lithium manganese oxide cathode waste results in recycled materials with poor electrochemical performance. Summary of the Invention

[0004] The first aspect of this application provides a method for preparing lithium-rich manganese-based cathode materials based on waste cathode sheets, comprising the following steps: Waste nickel-cobalt-manganese ternary cathode sheets and waste lithium manganese oxide cathode sheets are pretreated to obtain waste nickel-cobalt-manganese ternary cathode materials and waste lithium manganese oxide cathode materials. Waste nickel-cobalt-manganese ternary cathode material and waste lithium manganese oxide cathode material are mixed in proportion, and at least one of lithium source, nickel source, cobalt source and manganese source is added to obtain the first mixture. An organic acid is added to the first mixture for solid dry mixing to obtain a second mixture. A vanadium-containing modifier is added to the second mixture to obtain a third mixture. The third mixture is ball-milled and vacuum-dried to obtain a precursor. The organic acid contains a carboxyl group. The precursor was pre-sintered and main-sintered in an oxygen atmosphere, cooled to room temperature, and then crushed and screened to obtain lithium-rich manganese-based cathode material.

[0005] In some optional embodiments of the first aspect of this application, the vanadium element in the vanadium-containing modifier accounts for 1% to 5% of the total molar amount of nickel, cobalt and manganese elements in the first mixture.

[0006] In some optional embodiments of the first aspect of this application, the vanadium-containing modifier includes ammonium metavanadate.

[0007] In some optional embodiments of the first aspect of this application, the vanadium-containing modifier includes vanadium pentoxide and a reducing agent, wherein the reducing agent is selected from at least one of ammonium oxalate and urea.

[0008] In some optional embodiments of the first aspect of this application, the amount of reducing agent added is 1% to 10% of the mass of the first mixture.

[0009] In some optional embodiments of the first aspect of this application, the amount of organic acid added is 2% to 8% of the mass of the first mixture.

[0010] In some optional embodiments of the first aspect of this application, the amount of organic acid added is 4% to 6% of the mass of the first mixture.

[0011] In some optional embodiments of the first aspect of this application, the organic acid is selected from at least one of oxalic acid, citric acid, malic acid and tartaric acid.

[0012] In some optional embodiments of the first aspect of this application, the third mixture is ball-milled and vacuum-dried, including: Using anhydrous ethanol as the dispersion medium, the third mixture was ball-milled for 2-6 hours with a ball-to-material ratio of (5-10):1 and a ball milling speed of 200-400 r / min. After ball milling, the mixture was vacuum-dried at 45-65℃ for 6-24 hours.

[0013] In some optional embodiments of the first aspect of this application, the precursor is pre-sintered and main sintered in an oxygen atmosphere, including: Under an oxygen atmosphere, the temperature is increased to 400℃~550℃ at a heating rate of 2℃ / min~5℃ / min, and the precursor is held at this temperature for 4h~6h for pre-sintering. Then, the temperature is increased to 850℃~1000℃ at a heating rate of 2℃ / min~5℃ / min, and the temperature is held for 12h~20h for main sintering.

[0014] In some optional embodiments of the first aspect of this application, pretreatment of waste nickel-cobalt-manganese ternary cathode sheets and waste lithium manganese oxide cathode sheets includes: Waste nickel-cobalt-manganese ternary cathode sheets and waste lithium manganese oxide cathode sheets were heat-treated at 400~600℃ for 1h~3h, then crushed and sieved.

[0015] The second aspect provides a lithium-rich manganese-based cathode material, which is prepared by the above-mentioned method for preparing lithium-rich manganese-based cathode materials based on waste cathode sheets.

[0016] Beneficial effects: In the first aspect of this application, waste nickel-cobalt-manganese ternary cathode material and waste lithium manganese oxide cathode material are mixed, and organic acid and vanadium-containing modifier are added. By ball milling, the carboxyl functional groups in the organic acid effectively complex nickel ions, cobalt ions and manganese ions, and a stable chemical bridging structure is constructed between the waste nickel-cobalt-manganese ternary cathode material and the waste lithium manganese oxide cathode material. This effectively reduces the interfacial diffusion barrier during the subsequent high-temperature sintering process and promotes effective bonding between the materials. In the pre-sintering process, the vanadium-containing modifier reacts with lattice oxygen to generate oxygen vacancies. Vanadium ions diffuse into the oxygen vacancies, stabilizing the layered structure of the material. At the same time, an in-situ fast ion conductor Li3VO4 coating layer is generated to improve the performance of the final recycled material.

[0017] The first aspect of this application uses high-temperature solid-state sintering as the core process, adding only a small amount of organic acid and vanadium-containing modifier, avoiding the use of corrosive reagents and avoiding the generation of a large amount of wastewater and waste residue, which is in line with the concepts of green chemistry and sustainable development. Attached Figure Description

[0018] Figure 1 This is the main phase X-ray diffraction pattern of the lithium-rich manganese-based cathode material obtained in Example 1 of this application. Detailed Implementation

[0019] The present application will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only for explaining the present application and are not intended to limit the present application.

[0020] In one embodiment, a method for preparing lithium-rich manganese-based cathode materials based on waste cathode sheets is provided, comprising the following steps: Step 1: Pre-treat the waste nickel-cobalt-manganese ternary cathode sheet and the waste lithium manganese oxide cathode sheet to obtain waste nickel-cobalt-manganese ternary cathode material and waste lithium manganese oxide cathode material. Step 2: Mix waste nickel-cobalt-manganese ternary cathode material and waste lithium manganese oxide cathode material in proportion, and add at least one of lithium source, nickel source, cobalt source and manganese source to obtain the first mixture. Step 3: Add organic acid to the first mixture and perform solid dry mixing to obtain the second mixture. Add vanadium-containing modifier to the second mixture to obtain the third mixture. Ball mill and vacuum dry the third mixture to obtain the precursor. The organic acid contains carboxyl groups. Step 4: The precursor is pre-sintered and main-sintered in an oxygen atmosphere, cooled to room temperature, crushed and screened to obtain lithium-rich manganese-based cathode material.

[0021] In the above technical solution, waste nickel-cobalt-manganese ternary cathode sheets and waste lithium manganese oxide cathode sheets are pretreated to remove binders and conductive agents, as well as metallic impurities such as copper and aluminum, to obtain pure waste nickel-cobalt-manganese ternary cathode materials and waste lithium manganese oxide cathode materials (hereinafter referred to as the two types of waste). The waste nickel-cobalt-manganese ternary cathode materials have high Ni and Co content and low Mn content, while the waste lithium manganese oxide cathode materials have high Mn content. By mixing the two, elemental complementarity can be achieved.

[0022] After mixing the two types of waste materials in a specific ratio, the contents of Li, Ni, Co, and Mn elements were simultaneously measured using inductively coupled plasma optical emission spectrometry (ICP-OES). The stoichiometric ratio of Li in the target lithium-rich manganese-based cathode material was then determined. a Ni x Co y Mn z O2 (a=1.1~1.4, x=0.1~0.3, y=0.05~0.25, z=0.53~0.6), with the addition of the corresponding elements, the first mixture is obtained. For common 111, 523 and 622 type waste ternary materials, in order to reduce the amount of auxiliary materials added, waste nickel-cobalt-manganese ternary cathode materials and waste lithium manganese oxide cathode materials are compounded in a ratio of 1:(0.4~1.2).

[0023] For example, based on the stoichiometry of the target lithium-rich manganese-based cathode material, Li 1.2 Ni 0.13 Co 0.13 Mn 0.54 After designing the mixing ratio of the two waste materials, the molar ratio of Ni, Co, and Mn is made close to 0.13:0.13:0.54. Simultaneously, based on elemental analysis results, Ni sources (such as NiO), Co sources (such as Co3O4), Mn sources (such as MnO2 or Mn2O3), and lithium sources (such as Li2CO3 or LiOH) are added in corresponding stoichiometric ratios. The amount of lithium added is controlled to be 1.0 to 1.05 times the target Li / (Ni+Co+Mn) molar ratio, meaning that the molar amount of Li in the first mixture after supplementation is 1.2 / (0.13+0.13+0.54) times 1.0 to 1.05 times.

[0024] In this embodiment, an organic acid is added to the first mixture for solid dry mixing, so that the first mixture and the organic acid are mixed evenly, and the organic acid is uniformly adhered to the surface of the particles of the first mixture, to obtain the second mixture. A vanadium-containing modifier is added to the second mixture to obtain the third mixture.

[0025] The third mixture is ball-milled. Under mechanical collision, the carboxyl groups in the organic acid coordinate with the transition metal ions on the surface of the waste nickel-cobalt-manganese ternary cathode material particles and waste lithium manganese oxide cathode material particles. Through chelation, a chemical bridge is established between the two different crystal forms of waste particles. The original aged and deactivated layer on the surface of the waste nickel-cobalt-manganese ternary cathode material and waste lithium manganese oxide cathode material is transformed into a transition metal oxalate precursor layer. This reduces the temperature and energy consumption required for the subsequent high-temperature sintering process and effectively shortens the reaction time. At the same time, the carbon dioxide gas released during the decomposition of organic matter in the subsequent sintering generates micro-regional disturbances between particles, further promoting the material exchange and structural fusion of the particle interface.

[0026] After ball milling, the precursor is obtained by vacuum drying and then sintered in an oxygen atmosphere. Pre-sintering and main sintering in an oxygen atmosphere effectively maintain the specific valence states of the transition metals (nickel +2, cobalt +3, and manganese +4). Simultaneously, the lithium in the precursor reacts with a vanadium-containing modifier to form an in-situ lithium vanadium oxide (Li3VO4) coating layer with rapid ion conduction characteristics, thereby improving the electrochemical performance of the lithium-rich manganese-based cathode material. This coating reaction exhibits higher reactivity and better film formation under oxidizing atmosphere conditions.

[0027] In this embodiment, the waste nickel-cobalt-manganese ternary cathode sheet comes from retired nickel-cobalt-manganese ternary lithium batteries, and the waste lithium manganese oxide cathode sheet comes from retired lithium manganese oxide batteries.

[0028] In some optional embodiments of this application, the vanadium element in the vanadium-containing modifier accounts for 1% to 5% of the total molar amount of nickel, cobalt and manganese elements in the first mixture.

[0029] In the above scheme, when the vanadium element in the vanadium-containing modifier accounts for 1% to 5% of the total molar amount of nickel, cobalt, and manganese elements in the first mixture, vanadium doping can effectively combine with lattice oxygen to form VO bonds, inhibiting the irreversible release of lattice oxygen; at the same time, high-valence vanadium... 5+ The charge compensation effect induced by doping can further improve the overall electrochemical performance of the material.

[0030] It should be noted that the total molar amount of nickel, cobalt, and manganese in the first mixture can be calculated as follows: the mass fraction of nickel, cobalt, and manganese in the first mixture is measured using the ICP-OES method, and then the molar amount of nickel, cobalt, and manganese is calculated separately by combining the mass of the first mixture and the molar mass of each element. Finally, the molar amounts of these three elements are added together to obtain the total number of moles.

[0031] In some optional embodiments of this application, the vanadium-containing modifier includes ammonium metavanadate.

[0032] In this embodiment, during the pre-sintering stage, NH4VO3 decomposes to produce NH3 and V2O5. NH3 mildly reduces the surface of the two types of waste particles, and NH3 reacts with the lattice oxygen on the surface of the two types of waste particles to generate oxygen vacancies, promoting V2O5 production. 5+ Effective doping; during the main sintering stage, V₂O₅ liquid-phase fluxing promotes crystal reconstruction, V 5+ It enters the lattice for doping and forms a Li3VO4 coating layer in situ.

[0033] In some optional embodiments of this application, the vanadium-containing modifier includes vanadium pentoxide and a reducing agent, wherein the reducing agent is selected from at least one of ammonium oxalate and urea.

[0034] In this embodiment, ammonium oxalate and urea decompose to produce NH3 during the pre-sintering stage. NH3 gently reduces the surface of the two waste particles, generating oxygen vacancies and promoting V 5+ Effective doping.

[0035] In some optional embodiments of this application, the vanadium-containing modifier includes ammonium metavanadate, vanadium pentoxide, and a reducing agent.

[0036] In some optional embodiments of this application, the amount of reducing agent added is 1% to 10% of the mass of the first mixture.

[0037] In the above scheme, the amount of reducing agent added is 1% to 10% of the mass of the first mixture. An appropriate amount of reducing agent can ensure sufficient oxygen vacancies, which is beneficial for the stable structure of vanadium doping. If the reducing agent is excessive, it will lead to over-reduction of the material and structural damage.

[0038] In some optional embodiments of this application, the amount of reducing agent added is 2% to 5% of the mass of the first mixture.

[0039] In some optional embodiments of this application, the organic acid is selected from at least one of oxalic acid, citric acid, malic acid and tartaric acid.

[0040] In this embodiment, oxalic acid, citric acid, malic acid and tartaric acid all contain multiple carboxyl groups, which can effectively coordinate with transition metal ions in waste nickel-cobalt-manganese ternary cathode materials and waste lithium manganese oxide cathode materials, and no foreign impurities are introduced during the entire reaction process.

[0041] In some optional embodiments of this application, the amount of organic acid added is 2% to 8% of the mass of the first mixture.

[0042] In the above scheme, the amount of organic acid added is 2% to 8% of the mass of the first mixture. By controlling the amount of organic acid added within this range, impurities on the material surface can be effectively removed through etching and complexation. At the same time, the organic acid can coordinate with the transition metal ions dissolved from the two wastes, promoting the co-complexation of the two wastes and thus constructing a stable chemical bridging structure.

[0043] In some optional embodiments of this application, the amount of organic acid added is 4% to 6% of the mass of the first mixture.

[0044] In some optional embodiments of this application, the third mixture is ball-milled and vacuum-dried, including: Using anhydrous ethanol as the dispersion medium, the third mixture was ball-milled for 2-6 hours with a ball-to-material ratio of (5-10):1 and a ball milling speed of 200-400 r / min. After ball milling, the mixture was vacuum-dried at 45-65℃ for 6-24 hours.

[0045] During ball milling, numerous fresh interfaces and lattice defects form on the surfaces of the two types of waste particles. The carboxyl functional groups in the organic acid effectively complex nickel, cobalt, and manganese ions, constructing a stable chemical bridging structure between the two waste materials. This chemical bridging effectively reduces the interfacial diffusion barrier during subsequent high-temperature sintering, promoting effective bonding between the materials. Simultaneously, the vanadium-containing modifier achieves uniform dispersion during ball milling, providing favorable conditions for subsequent processes.

[0046] In this embodiment, ethanol is used as the dispersion medium to promote uniform dispersion of materials, effectively reduce particle agglomeration, and ensure the coordination effect of organic acids.

[0047] In some optional embodiments of this application, the precursor is pre-sintered and main sintered in an oxygen atmosphere, including: Under an oxygen atmosphere, the temperature is increased to 400℃~550℃ at a heating rate of 2℃ / min~5℃ / min, and the precursor is held at this temperature for 4h~6h for pre-sintering. Then, the temperature is increased to 850℃~1000℃ at a heating rate of 2℃ / min~5℃ / min, and the temperature is held for 12h~20h for main sintering.

[0048] During the pre-sintering stage, NH4VO3 decomposes to produce NH3 and V2O5, or the reducing agent decomposes to produce NH3, while the organic acid is completely decomposed. NH3, acting as a reducing agent, reacts with the lattice oxygen on the surface of both types of waste particles to generate oxygen vacancies. These oxygen vacancies are the source of subsequent V2O5 production. 5+ Preferred sites are occupied. During this process, the lithium salt begins to melt, initially completing lithium compensation and removal of organic impurities.

[0049] During the main sintering stage, driven by high temperature, two types of waste materials, mechanically activated by organic acids, undergo crystal reconstruction and fusion to form a lithium-rich manganese-based matrix phase. V₂O₅ forms a liquid phase at 850℃~950℃, acting as a flux to promote atomic diffusion; V 5+ Lithium diffuses into the bulk phase, replacing some Mn sites and stabilizing the layered structure. Simultaneously, lithium reacts with V₂O₅ to form an in-situ fast-ion conductor, Li₃VO₄, coating layer.

[0050] In some optional embodiments of this application, pretreatment of waste nickel-cobalt-manganese ternary cathode sheets and waste lithium manganese oxide cathode sheets includes: Waste nickel-cobalt-manganese ternary cathode sheets and waste lithium manganese oxide cathode sheets were heat-treated at 400℃~600℃ for 1h~3h, then crushed and sieved.

[0051] In this embodiment, retired nickel-cobalt-manganese ternary lithium batteries and retired lithium manganese oxide batteries are discharged and disassembled to obtain waste nickel-cobalt-manganese ternary cathode sheets and waste lithium manganese oxide cathode sheets. The waste nickel-cobalt-manganese ternary cathode sheets and waste lithium manganese oxide cathode sheets are heat-treated at 400℃~600℃ for 1h~3h to remove the binder PVDF and conductive agent. They are then crushed and sieved to remove metal impurities, resulting in waste nickel-cobalt-manganese ternary cathode materials and waste lithium manganese oxide cathode materials.

[0052] In some other embodiments, waste nickel-cobalt-manganese ternary cathode sheets and waste lithium manganese oxide cathode sheets can be soaked in organic solvents such as NMP, followed by ultrasonic treatment, drying, crushing and sorting to obtain pure waste nickel-cobalt-manganese ternary cathode materials and waste lithium manganese oxide cathode materials.

[0053] In another embodiment, a lithium-rich manganese-based cathode material is provided, which is prepared by the above-described method for preparing lithium-rich manganese-based cathode materials based on waste cathode sheets.

[0054] The present application is further illustrated below with reference to embodiments and comparative examples. Unless otherwise specified, the raw materials, reagents, materials and equipment used in this application are all commercially available products conventionally used in the art.

[0055]

Example 1

[0056] S2. Elemental analysis was performed on waste NCM523 ternary cathode material and waste LiMn2O4 cathode material using ICP-OES. The molar ratio of Li, Ni, Co and Mn in the waste NCM523 ternary cathode material was approximately 1:0.53:0.20:0.27, and the molar ratio of Li:Mn in the waste LiMn2O4 cathode material was approximately 1:1.96.

[0057] Based on the target lithium-rich manganese-based cathode material with the chemical formula Li 1.2 Ni 0.13 Co 0.13 Mn 0.54 O2 was used to calculate and determine the optimal mixing ratio of the two waste materials: waste NCM523 ternary cathode material and waste LiMn2O4 cathode material were mixed at a mass ratio of 1:1. Under this mixing ratio, the molar ratio of Li, Ni, Co, and Mn in the resulting waste was approximately 1.5:0.53:0.20:1.29. Based on the elemental analysis results, Co source Co3O4, manganese source MnO2, and lithium source Li2CO3 were added to the resulting waste to achieve a molar ratio of Li, Ni, Co, and Mn of 1.2:0.13:0.13:0.54, thus obtaining the first mixture.

[0058] S3. Take 100g of the first mixture above, add 5g of oxalic acid (H2C2O4·2H2O), and ball mill and mix for 5 minutes to make the oxalic acid crystals uniformly adhere to the surface of the waste particles to obtain the second mixture. 2.19 g of ammonium metavanadate (NH4VO3) was added to the second mixture, so that the added vanadium element accounted for 2% of the total molar amount of nickel, cobalt and manganese elements in the first mixture, to obtain the third mixture. The third mixture was transferred to a planetary ball mill, and 200 mL of anhydrous ethanol was added as the dispersion medium. Zirconia balls (ball-to-material ratio 8:1) were used to ball mill the mixture at a speed of 300 r / min for 4 h. After ball milling, the material was removed and vacuum dried at 60 °C for 12 h to obtain the precursor.

[0059] S4. Place the precursor in an alumina crucible and put it into a tube furnace. Heat the furnace to 500°C at a rate of 3°C / min and hold it at this temperature for 5 hours under an oxygen atmosphere for pre-sintering. Then, continue heating the furnace to 900°C at a rate of 3°C / min and hold it at this temperature for 15 hours for main sintering. The oxygen flow rate is maintained at 100 mL / min. After sintering, the product is cooled to room temperature in the furnace. The cooled block sintered product is then crushed and passed through a 300-mesh sieve to obtain lithium-rich manganese-based cathode material.

[0060]

Example 2

[0061]

Example 3

[0062]

Example 4

[0063]

Example 5

[0064]

Example 6

[0065]

Example 7

[0066]

Example 8

[0067]

Example 9

[0068]

Example 10

[0069] Comparative Example 1 The only difference between this comparative example and Example 1 is that oxalic acid and ammonium metavanadate are not added in S3; the other steps are the same. S3 is detailed below: S3. Take 100g of the first mixture and ball mill it for 5 minutes to obtain the second mixture; The second mixture was transferred to a planetary ball mill, and 200 mL of anhydrous ethanol was added as a dispersion medium. Zirconia balls (ball-to-material ratio 8:1) were used to ball mill the mixture at a speed of 300 r / min for 4 h. After ball milling, the material was removed and vacuum dried at 60 °C for 12 h to obtain the precursor.

[0070] Comparative Example 2 The only difference between this comparative example and Example 1 is that ammonium metavanadate is not added in step S3; the other steps are the same. Step S3 is as follows: S3. Take 100g of the first mixture above, add 5g of oxalic acid (H2C2O4·2H2O), and ball mill and mix for 5 minutes to make the oxalic acid crystals uniformly adhere to the surface of the waste particles to obtain the second mixture. The second mixture was transferred to a planetary ball mill, and 200 mL of anhydrous ethanol was added as a dispersion medium. Zirconia balls (ball-to-material ratio 8:1) were used to ball mill the mixture at a speed of 300 r / min for 4 h. After ball milling, the material was removed and vacuum dried at 60 °C for 12 h to obtain the precursor.

[0071] Comparative Example 3 The difference between this comparative example and Example 1 is that oxalic acid is not added in step S3; the other steps are the same. Step S3 is as follows: S3. Take 100g of the first mixture above, ball mill and mix for 5 minutes to obtain the second mixture; Ammonium metavanadate (NH4VO3) was added to the second mixture so that the added vanadium element accounted for 2% of the total molar amount of nickel, cobalt and manganese elements in the first mixture, thus obtaining the third mixture. The third mixture was transferred to a planetary ball mill, and 200 mL of anhydrous ethanol was added as the dispersion medium. Zirconia balls (ball-to-material ratio 8:1) were used to ball mill the mixture at a speed of 300 r / min for 4 h. After ball milling, the material was removed and vacuum dried at 60 °C for 12 h to obtain the precursor.

[0072] Comparative Example 4 The only difference between this comparative example and Example 1 is that the main sintering temperature in S4 is adjusted to 1030℃; the other steps are the same. S4 is detailed below: S4. Place the precursor in an alumina crucible and put it into a tube furnace. Heat the furnace to 500°C at a rate of 3°C / min and hold it at this temperature for 5 hours under an oxygen atmosphere for pre-sintering. Then, continue heating the furnace to 1030°C at a rate of 3°C / min and hold it at this temperature for 15 hours for main sintering. The oxygen flow rate is maintained at 100 mL / min. After sintering, the product is cooled to room temperature in the furnace. The cooled block sintered product is then crushed and passed through a 300-mesh sieve to obtain lithium-rich manganese-based cathode material.

[0073] The parameters and conditions of each embodiment and comparative example are summarized in Table 1.

[0074] Table 1

[0075] [Performance Testing] Electrochemical performance testing: The obtained lithium-rich manganese-based cathode material was mixed with conductive carbon black and PVDF binder at a mass ratio of 8:1:1, coated onto aluminum foil to form a cathode sheet, and a lithium metal sheet was used as the counter electrode. CR2032 coin cells were assembled in an argon-filled glove box. The electrolyte was 1M LiPF6 dissolved in EC / DMC / EMC (volume ratio 1:1:1), and the separator was Celgard 2500. Charge-discharge tests were conducted within a voltage window of 2.0~4.8V. The initial discharge specific capacity and initial coulombic efficiency at 0.1C were tested, and the capacity retention after 200 cycles at 1C at 25℃ was tested. The test results are shown in Table 2.

[0076] Table 2

[0077] As shown in Table 2, the initial discharge specific capacity of Examples 1 to 10 ranged from 273.7 mAh / g to 276.3 mAh / g, the initial coulombic efficiency ranged from 84.3% to 87.9%, and the capacity retention after 200 cycles at 1C rate was all above 88%, demonstrating good energy density, interface stability, and cycle life. In contrast, the indicators of Comparative Examples 1 to 4 were all lower than those of the Examples.

[0078] Comparative Example 1 did not use oxalic acid and ammonium metavanadate, Comparative Example 2 used only oxalic acid and not ammonium metavanadate, and Comparative Example 3 used only ammonium metavanadate and not oxalic acid. The data obtained from Comparative Examples 1 to 3 were all inferior to those of Example 1. This indicates that oxalic acid and ammonium metavanadate have a synergistic effect. Oxalic acid assists in the mechanical activation of the two waste materials, and the oxygen vacancies generated by the reduction of NH3 produced by ammonium metavanadate provide more active sites for vanadium doping. The synergistic effect of the two further improves the electrochemical performance of the material.

[0079] Compared to Example 1, Comparative Example 4 also used oxalic acid and ammonium metavanadate, but the main sintering temperature in S4 was adjusted to 1030°C. The excessively high temperature led to increased lithium volatilization, material structure collapse, and a decrease in material performance.

[0080] It should be noted that, in this document, "comprising," "including," or any other variation thereof is intended to cover non-exclusive inclusion, such that a process, method, or article that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, or article.

[0081] The various embodiments in this specification are described in a related manner. The same or similar parts between the various embodiments can be referred to each other. Each embodiment focuses on describing the differences from other embodiments.

[0082] The above description is only a preferred embodiment of this application and is not intended to limit this application. Any modifications, equivalent substitutions, improvements, etc., made within the principles of this application should be included within the scope of protection of this application.

Claims

1. A method for preparing a lithium-rich manganese-based cathode material based on waste positive plate, characterized in that, Includes the following steps: Waste nickel-cobalt-manganese ternary cathode sheets and waste lithium manganese oxide cathode sheets are pretreated to obtain waste nickel-cobalt-manganese ternary cathode materials and waste lithium manganese oxide cathode materials. The waste nickel-cobalt-manganese ternary cathode material and the waste lithium manganese oxide cathode material are mixed in proportion, and at least one of the lithium source, nickel source, cobalt source and manganese source is added to obtain a first mixture. An organic acid is added to the first mixture for solid dry mixing to obtain a second mixture. A vanadium-containing modifier is added to the second mixture to obtain a third mixture. The third mixture is ball-milled and vacuum-dried to obtain a precursor. The organic acid contains a carboxyl group. The precursor was pre-sintered and main-sintered in an oxygen atmosphere, cooled to room temperature, and then crushed and screened to obtain lithium-rich manganese-based cathode material.

2. The method for preparing lithium-rich manganese-based cathode materials based on waste cathode sheets as described in claim 1, characterized in that, The vanadium-containing modifier contains vanadium, which accounts for 1% to 5% of the total molar amount of nickel, cobalt, and manganese in the first mixture.

3. The method for preparing lithium-rich manganese-based cathode materials based on waste cathode sheets as described in claim 2, characterized in that, The vanadium-containing modifier includes ammonium metavanadate.

4. The method for preparing lithium-rich manganese-based cathode materials based on waste cathode sheets as described in any one of claims 1 to 3, characterized in that, The vanadium-containing modifier includes vanadium pentoxide and a reducing agent, wherein the reducing agent is selected from at least one of ammonium oxalate and urea.

5. The method for preparing lithium-rich manganese-based cathode materials based on waste cathode sheets as described in claim 4, characterized in that, The amount of reducing agent added is 1% to 10% of the mass of the first mixture.

6. The method for preparing lithium-rich manganese-based cathode materials based on waste cathode sheets as described in claim 1, characterized in that, The amount of organic acid added is 2% to 8% of the mass of the first mixture; Preferably, the amount of organic acid added is 4% to 6% of the mass of the first mixture; Preferably, the organic acid is selected from at least one of oxalic acid, citric acid, malic acid and tartaric acid.

7. The method for preparing lithium-rich manganese-based cathode materials based on waste cathode sheets as described in claim 1, characterized in that, The process of ball milling and vacuum drying the third mixture includes: Using anhydrous ethanol as the dispersion medium, the third mixture is ball-milled for 2-6 hours at a ball-to-material ratio of (5-10):1 and a ball-milling speed of 200-400 r / min. After ball milling, the mixture is vacuum-dried at 45-65°C for 6-24 hours.

8. The method for preparing lithium-rich manganese-based cathode materials based on waste cathode sheets as described in claim 1, characterized in that, The process of pre-sintering and main sintering the precursor in an oxygen atmosphere includes: Under an oxygen atmosphere, the precursor is heated to 400℃~550℃ at a heating rate of 2℃ / min~5℃ / min and held at that temperature for 4h~6h for pre-sintering. Then, the temperature is increased to 850℃~1000℃ at a heating rate of 2℃ / min~5℃ / min and held at that temperature for 12h~20h for main sintering.

9. The method for preparing lithium-rich manganese-based cathode materials based on waste cathode sheets as described in claim 1, characterized in that, The pretreatment of waste nickel-cobalt-manganese ternary cathode sheets and waste lithium manganese oxide cathode sheets includes: The waste nickel-cobalt-manganese ternary cathode sheet and the waste lithium manganese oxide cathode sheet were heat-treated at 400~600℃ for 1h~3h, and then crushed and sieved.

10. A lithium-rich manganese-based cathode material, characterized in that, It is prepared by the method for preparing lithium-rich manganese-based cathode materials based on waste cathode sheets as described in any one of claims 1 to 9.