A corrosion-resistant and flame-retardant aluminum alloy casing for lithium-ion batteries, its preparation method and application
By depositing an Al2O3 layer and a polymer layer on the surface of the aluminum alloy casing of lithium-ion batteries, the problems of fluoride ion corrosion and electrolyte leakage were solved, thereby improving the safety and corrosion resistance of lithium-ion batteries.
Patent Information
- Application Number
- CN202611263325.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-19
- Publication Date
- 2026-11-17
AI Technical Summary
The safety hazards caused by fluoride corrosion and electrolyte leakage in the aluminum alloy casing of lithium-ion batteries are difficult to solve effectively with existing technologies, leading to risks such as battery spontaneous combustion and explosion.
An Al2O3 layer and a polymer layer are deposited on the surface of an aluminum alloy substrate. The polymer layer is formed by the cross-linking reaction of polyethylene glycol methyl ether methacrylate and triallyl isocyanurate, forming a composite layer structure that blocks the penetration of corrosive components and inhibits side reactions.
It significantly improves the safety performance, fluorine corrosion resistance, and flame retardant protection of lithium-ion batteries, reduces the risk of spontaneous combustion after electrolyte leakage, and maintains the mechanical properties of the aluminum alloy casing.
Smart Images

Figure CN123121008A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of lithium-ion battery casing manufacturing technology, specifically to a corrosion-resistant and flame-retardant aluminum alloy casing for lithium-ion batteries, its manufacturing method, and its application. Background Technology
[0002] Lithium-ion batteries are widely used in electric vehicles, portable electronic devices, energy storage systems, and other fields due to their advantages such as high energy density, long cycle life, and no memory effect. As a crucial component of lithium-ion batteries, the casing not only needs to possess good mechanical properties to support the battery structure and withstand external impacts, but also needs excellent corrosion resistance to prevent safety hazards caused by electrolyte leakage or external environmental corrosion.
[0003] Aluminum alloys have become the mainstream material for lithium-ion battery casings due to their low density, high specific strength, good machinability, and relatively low cost. However, lithium-ion battery electrolytes typically contain fluorinated electrolytes such as lithium hexafluorophosphate, which generate fluoride ions (F₂O₃) during battery charging and discharging. - Fluoride ions are highly corrosive and readily react with aluminum alloys, leading to pitting and intergranular corrosion on the casing surface. As corrosion intensifies, the casing thickness gradually decreases, reducing its mechanical support capacity and potentially causing electrolyte leakage, which can then trigger serious safety incidents such as battery short circuits, fires, or even explosions.
[0004] Furthermore, when lithium-ion batteries are overcharged, the electrolyte inside the battery may decompose, generating gas and high temperatures, increasing internal pressure, and potentially causing the battery to swell or even spontaneously combust or explode. When lithium-ion batteries are subjected to severe impacts, the electrolyte may leak into the battery, reacting with the electrode materials to generate gas, further increasing internal pressure and potentially triggering spontaneous combustion. Summary of the Invention
[0005] To improve the safety performance of lithium-ion batteries, this invention provides a corrosion-resistant and flame-retardant aluminum alloy casing for lithium-ion batteries and its preparation method. This aluminum alloy casing not only resists fluorine corrosion but also prevents the penetration of corrosive components and inhibits side reactions between the electrolyte and aluminum metal. The composite layer structure synergistically achieves flame-retardant protection, significantly improving the battery's safety performance.
[0006] Specifically, in order to achieve the above objectives, the present invention adopts the following technical solution: A lithium-ion battery aluminum alloy casing comprises an aluminum alloy substrate, an Al2O3 layer deposited on the surface of the aluminum alloy substrate, and a polymer layer deposited on the surface of the Al2O3 layer facing away from the aluminum alloy substrate; the thickness of the Al2O3 layer is 5~15μm; the polymer layer is obtained by crosslinking polyethylene glycol methyl ether methacrylate with triallyl isocyanurate, and the thickness of the polymer layer is 3~8μm.
[0007] In a preferred embodiment, the aluminum alloy matrix is 6061 aluminum alloy or 7075 aluminum alloy.
[0008] The method for preparing the aluminum alloy casing of the lithium-ion battery includes the following steps: S1. Cut the aluminum alloy substrate into shell blanks of a preset size, and perform degreasing, pickling, water washing and drying treatments in sequence; S2. The shell blank after the pretreatment in step S1 is subjected to oxygen plasma treatment to form a dense Al2O3 layer on the surface of the shell blank; the treatment gas is a mixture of oxygen and argon, and the oxygen accounts for 30% to 60% of the volume of the mixture. S3. The product obtained in step S2 is stamped at room temperature to form a battery casing; the battery casing is then cleaned and dried. S4. The polymerization reaction solution is coated onto the surface of the Al2O3 layer on the inner surface of the battery casing, pre-baked, and then irradiated with ultraviolet light to cause the polymerization reaction solution to undergo a cross-linking reaction to obtain a polymer layer; the polymerization reaction solution contains polyethylene glycol methyl ether methacrylate and triallyl isocyanurate in a mass ratio of (3~5):1. S5. Heat the product obtained in step S4 to solidify the polymer layer, and then cool it to room temperature in the furnace to obtain the aluminum alloy casing for the lithium-ion battery.
[0009] In a preferred embodiment, in step S1, degreasing is performed using a 5wt%~10wt% sodium hydroxide aqueous solution, and the shell blank is immersed at 50℃~60℃ for 10~15 minutes.
[0010] In a preferred embodiment, in step S1, the pickling process involves immersing the degreased shell blank in a nitric acid aqueous solution with a volume percentage of 10% to 15% for 3 to 5 minutes at room temperature.
[0011] In the preferred embodiment, the drying conditions in step S1 are: drying at 80℃~100℃ for 1~2 hours.
[0012] In the preferred embodiment, the conditions for oxygen plasma treatment in step S2 are: controlling the pressure in the reaction chamber ≤ 10. - 3Pa; after introducing the mixed gas, adjust the pressure of the mixed gas to 10~50Pa, adjust the radio frequency power to 200~500W, the processing temperature to 200℃~400℃, and the processing time to 10~30min.
[0013] In the preferred embodiment, the cleaning in step S3 is performed by ultrasonic cleaning with anhydrous ethanol, and the drying is carried out at 60℃~80℃.
[0014] In a preferred embodiment, the polymerization reaction solution in step S4 contains an initiator, the mass of which accounts for 1% to 3% of the total mass of the polyethylene glycol methyl ether methacrylate and the triallyl isocyanurate.
[0015] In a further preferred embodiment, the initiator is azobisisobutyronitrile (AIBN).
[0016] In a preferred embodiment, the solid content in the polymerization reaction solution in step S4 is 20wt%~40wt%.
[0017] In a preferred embodiment, the coating thickness of the polymerization reaction liquid on the surface of the Al2O3 layer in step S4 is 5~10 μm.
[0018] In the preferred embodiment, the pre-baking temperature in step S4 is 60℃~80℃, and the time is 5~10min; In the preferred embodiment, the wavelength of the ultraviolet light in step S4 is 254~365nm, the power of the ultraviolet light source is 100~300W, and the ultraviolet light irradiation time is 3~10min.
[0019] In the preferred embodiment, the curing temperature in step S5 is 100℃~120℃, and the time is 20~40min.
[0020] Compared with the prior art, the technical solution of the present invention has the following beneficial effects: (1) The lithium-ion battery aluminum alloy shell provided by the present invention has an aluminum oxide layer and a polymer layer on an aluminum alloy substrate, and the outermost polymer protective layer has an isocyanurate ring structure. When the lithium-ion battery leaks electrolyte, the ring structure can quickly capture the active lithium and HF acidic components in the electrolyte, passivate the corrosive active substances, and suppress the occurrence of battery spontaneous combustion reaction from the source, so as to realize active safety control after electrolyte leakage.
[0021] (2) The aluminum oxide layer in the lithium-ion battery aluminum alloy casing provided by this invention has a dense structure and is firmly bonded to the aluminum alloy substrate (critical load ≥ 20 N). The polymer layer has a stable molecular structure and good resistance to fluoride ions. The dual protection of the aluminum alloy substrate by the aluminum oxide layer and the polymer layer results in no significant corrosion of the battery casing after immersion in a simulated electrolyte environment for 1000 hours. The corrosion rate is reduced by more than 55% compared to the aluminum alloy casing prepared by the anodizing method. Therefore, the battery casing prepared using this aluminum alloy casing material has both fluoride corrosion resistance and the ability to rapidly reduce electrolyte activity, which can significantly improve the safety performance of lithium-ion batteries.
[0022] (3) The oxygen plasma treatment and ultraviolet light irradiation polymerization reaction liquid used in the method of preparing aluminum alloy shell for lithium-ion battery of the present invention are carried out at a low temperature, which will not have an adverse effect on the mechanical properties of the aluminum alloy matrix. The tensile strength of the shell material after molding is ≥300MPa and the elongation is ≥7%, which meets the mechanical support and processing requirements of lithium-ion battery shell.
[0023] (4) The polymer reaction solution for preparing the polymer layer in this invention is simple to prepare, and the coating and ultraviolet light polymerization process is mature and controllable. The thickness of the polymer layer can be precisely controlled by adjusting the monomer ratio and irradiation parameters. It has good compatibility with existing aluminum alloy shell processing production lines and is suitable for large-scale mass production. Attached Figure Description
[0024] Figure 1 This is a polarization curve diagram of the aluminum alloy casing of the lithium-ion battery in Embodiment 1 of the present invention; Figure 2 This is a polarization curve diagram of the aluminum alloy casing of the lithium-ion battery in Embodiment 2 of the present invention; Figure 3 This is a polarization curve diagram of the aluminum alloy casing of the lithium-ion battery in Embodiment 3 of the present invention; Figure 4 The polarization curve of the aluminum alloy casing of the lithium-ion battery in Comparative Example 1 of this invention is shown. Figure 5 The polarization curve of the aluminum alloy casing of the lithium-ion battery in Comparative Example 2 of this invention is shown. Figure 6 This is a polarization curve of the aluminum alloy casing of the lithium-ion battery in Comparative Example 3 of the present invention. Detailed Implementation
[0025] The following description, in conjunction with embodiments, clearly and completely describes the technical solutions of this application, so that those skilled in the art can fully understand this application. Obviously, the described embodiments are merely some preferred embodiments of this application, and not all embodiments. Any equivalent modifications or substitutions made by those skilled in the art to the following embodiments without creative effort are within the protection scope of this application.
[0026] The 6061 aluminum alloy used in the following examples is composed of the following elements by mass percentage: Si 0.4%-0.8%, Fe≤0.7%, Cu 0.15%-0.4%, Mn≤0.15%, Mg 0.8%-1.2%, Cr 0.04%-0.35%, Zn≤0.25%, Ti≤0.15%, with the balance being Al. The 7075 aluminum alloy used is composed of the following elements by mass percentage: Si≤0.4%, Fe≤0.5%, Cu 1.2%-2.0%, Mn≤0.3%, Mg 2.1%-2.9%, Cr 0.18%-0.28%, Zn 5.1%-6.1%, Ti≤0.2%, with the balance being Al.
[0027] Example 1 A method for preparing a corrosion-resistant and flame-retardant aluminum alloy casing for lithium-ion batteries includes the following steps: S1. Pretreatment of Aluminum Alloy Substrate: Cut 6061 aluminum alloy into shell blanks of 100mm×100mm×2mm, immerse them in a 5wt% sodium hydroxide aqueous solution at 50℃ for 15 minutes. After removal, rinse with deionized water until the washing solution is neutral. Then immerse in a 10% (v / v) nitric acid aqueous solution at room temperature for 5 minutes, remove and rinse with deionized water until the pH of the washing solution is 7, and then dry at 80℃ for 2 hours.
[0028] S2. Oxygen Plasma Treatment: Place the pretreated shell blank from step S1 into the reaction chamber of the plasma oxidation device, and evacuate to 10°C. -3 Pa, introduce a mixture of oxygen and argon (oxygen volume accounts for 30% of the total volume of the mixture), and adjust the pressure to 10 Pa. Start the plasma generator with a radio frequency power of 200 W, a processing temperature of 200 °C, and a processing time of 30 min to form an Al2O3 layer with a thickness of 5 μm on the surface of the aluminum alloy substrate.
[0029] S3. Stamping: The aluminum alloy substrate with an Al2O3 layer deposited on its surface in step S2 is placed in a stamping die and stamped at room temperature to prepare a cubic battery casing. After stamping, the surface of the casing is ultrasonically cleaned with anhydrous ethanol for 5 minutes to remove residual lubricating oil from the stamping process, and then dried at 60°C for 10 minutes.
[0030] S4. Preparation of the polymer layer: The pre-prepared polymerization reaction solution is uniformly coated onto the surface of the Al2O3 layer on the inner surface of the shell, with a coating thickness of 5μm, and pre-baked at 60℃ for 10min; then, the polymerization reaction solution is irradiated with ultraviolet light of wavelength 254nm, with a power of 100W and an irradiation time of 10min, forming a polymer layer with a thickness of 3μm on the surface of the Al2O3 layer. The polymerization reaction solution is prepared as follows: PEGMA (polyethylene glycol methyl ether methacrylate) and triallyl isocyanurate are mixed uniformly at a mass ratio of 3:1, and 1% of the total mass of the two initiators azobisisobutyronitrile is added, followed by dilution with anhydrous ethanol to adjust the monomer solid content in the polymerization reaction solution to 20wt%.
[0031] S5. Polymer layer curing: The product obtained in step S4 is placed at 100°C for curing for 40 minutes, and then cooled to room temperature in the furnace to obtain a lithium-ion battery aluminum alloy shell with a 5μm thick Al2O3 layer deposited on the surface of the 6061 aluminum alloy substrate and a 3μm thick polymer layer deposited on the surface of the Al2O3 layer.
[0032] Example 2 A method for preparing a corrosion-resistant and flame-retardant aluminum alloy casing for lithium-ion batteries includes the following steps: S1. Pretreatment of Aluminum Alloy Substrate: Cut 7075 aluminum alloy into shell blanks of 100mm×100mm×2mm, immerse them in an 8wt% sodium hydroxide aqueous solution at 55℃ for 12min. After removal, rinse with deionized water until the washing solution is neutral. Then immerse in a 12% (v / v) nitric acid aqueous solution at room temperature for 4min, remove and rinse with deionized water until the pH of the washing solution is 7, and then dry at 90℃ for 1.5h.
[0033] S2. Oxygen Plasma Treatment: The pretreated shell blank from step S1 is placed into the reaction chamber of the plasma oxidation device, and a vacuum of 5 × 10⁻⁶ is drawn. -4 Pa, a mixture of oxygen and argon gas (oxygen volume accounts for 45% of the total volume of the mixture) is introduced, and the pressure is adjusted to 30 Pa. The plasma generator is started, with a radio frequency power of 350 W, a processing temperature of 300 °C, and a processing time of 20 min, forming an Al2O3 layer with a thickness of 10 μm on the surface of the aluminum alloy substrate.
[0034] S3. Stamping: The aluminum alloy substrate with an Al2O3 layer deposited on its surface in step S2 is placed in a stamping die and stamped at room temperature to prepare a cubic battery casing. After stamping, the surface of the casing is ultrasonically cleaned with anhydrous ethanol for 5 minutes to remove residual lubricating oil from the stamping process, and then dried at 70°C for 10 minutes.
[0035] S4. Preparation of the polymer layer: The pre-prepared polymerization reaction solution is uniformly coated onto the surface of the Al2O3 layer on the inner surface of the shell, with a coating thickness of 8μm, and pre-baked at 70℃ for 8min; then, the polymerization reaction solution is irradiated with ultraviolet light of wavelength 313nm, with a power of 200W and an irradiation time of 6min, forming a polymer layer with a thickness of 5μm on the surface of the Al2O3 layer. The polymerization reaction solution is prepared as follows: PEGMA (polyethylene glycol methyl ether methacrylate) and triallyl isocyanurate are mixed uniformly at a mass ratio of 4:1, and 2% of the total mass of the two initiators, azobisisobutyronitrile, is added. Then, anhydrous ethanol is added for dilution, adjusting the monomer solid content in the polymerization reaction solution to 30wt%.
[0036] S5. Polymer layer curing: The product obtained in step S4 is cured at 110°C for 30 minutes, and then cooled to room temperature in the furnace to obtain a lithium-ion battery aluminum alloy shell with a 10μm thick Al2O3 layer deposited on the surface of the 7075 aluminum alloy substrate and a 5μm thick polymer layer deposited on the surface of the Al2O3 layer.
[0037] Example 3 A method for preparing a corrosion-resistant and flame-retardant aluminum alloy casing for lithium-ion batteries includes the following steps: S1. Pretreatment of Aluminum Alloy Substrate: Cut 6061 aluminum alloy into shell blanks of 100mm×100mm×2mm, immerse them in a 10wt% sodium hydroxide aqueous solution at 60℃ for 10min. After removal, rinse with deionized water until the washing solution is neutral. Then immerse in a 15% (v / v) nitric acid aqueous solution at room temperature for 3min, remove and rinse with deionized water until the pH of the washing solution is 7, and then dry at 100℃ for 1h.
[0038] S2. Oxygen plasma treatment: The pretreated shell blank from step S1 is placed into the reaction chamber of the plasma oxidation device, and the vacuum is evacuated to 1×10⁻⁶. -4 Pa, a mixture of oxygen and argon gas (oxygen volume accounts for 60% of the total volume of the mixture) is introduced, and the pressure is adjusted to 50 Pa. The plasma generator is started, with a radio frequency power of 500 W, a processing temperature of 400 °C, and a processing time of 10 min, forming an Al2O3 layer with a thickness of 15 μm on the surface of the aluminum alloy substrate.
[0039] S3. Stamping: The aluminum alloy substrate with an Al2O3 layer deposited on its surface in step S2 is placed in a stamping die and stamped at room temperature to prepare a cubic battery casing. After stamping, the surface of the casing is ultrasonically cleaned with anhydrous ethanol for 5 minutes to remove residual lubricating oil from the stamping process, and then dried at 80°C for 10 minutes.
[0040] S4. Preparation of the polymer layer: The pre-prepared polymerization reaction solution is uniformly coated onto the surface of the Al2O3 layer on the inner surface of the shell, with a coating thickness of 10 μm, and pre-baked at 80℃ for 5 min; then, the polymerization reaction solution is irradiated with ultraviolet light of wavelength 365 nm, with a power of 300 W and an irradiation time of 3 min, forming a polymer layer with a thickness of 8 μm on the surface of the Al2O3 layer. The polymerization reaction solution is prepared as follows: PEGMA (polyethylene glycol methyl ether methacrylate) and triallyl isocyanurate are mixed uniformly at a mass ratio of 5:1, and 1% of the total mass of the two initiators, azobisisobutyronitrile, is added, followed by dilution with anhydrous ethanol to adjust the monomer solid content in the polymerization reaction solution to 40 wt%.
[0041] S5. Polymer layer curing: The product obtained in step S4 is cured at 120°C for 20 minutes, and then cooled to room temperature in the furnace to obtain a lithium-ion battery aluminum alloy shell with a 15μm thick Al2O3 layer deposited on the surface of the 6061 aluminum alloy substrate and an 8μm thick polymer layer deposited on the surface of the Al2O3 layer.
[0042] Comparative Example 1 A method for preparing a corrosion-resistant and flame-retardant aluminum alloy casing for lithium-ion batteries includes the following steps: P1. Pretreatment of Aluminum Alloy Substrate: Cut 6061 aluminum alloy into shell blanks of 100mm×100mm×2mm, immerse them in a 10wt% sodium hydroxide aqueous solution at 60℃ for 10min. After removal, rinse with deionized water until the washing solution is neutral. Then immerse in a 15% (v / v) nitric acid aqueous solution at room temperature for 3min, remove and rinse with deionized water until the pH of the washing solution is 7, and then dry at 100℃ for 1h.
[0043] P2. Anodizing Treatment: The pretreated aluminum alloy substrate from step P1 is used as the anode, and a stainless steel plate is used as the cathode, both placed in an electrolytic cell. The electrolyte is a 150 g / L sulfuric acid aqueous solution, and the electrolyte temperature is controlled at (20 ± 1)℃. A DC regulated power supply is used, with a constant current density of 2 A / dm³. 2 The oxidation treatment time is 50 minutes. Compressed air is used for stirring during the treatment to ensure uniform electrolyte temperature and concentration. After the treatment, the billet is taken out and immediately rinsed three times with deionized water, then placed in deionized water at 60°C for 15 minutes for sealing treatment. After taking it out, it is dried at 100°C for 1 hour to form a porous anodic aluminum oxide layer with a thickness of about 15 μm on the surface of the aluminum alloy substrate.
[0044] P3. Stamping: The aluminum alloy substrate with an anodized aluminum layer deposited on its surface in step P2 is placed in a stamping die and stamped at room temperature to prepare a cubic battery casing. After stamping, the surface of the casing is ultrasonically cleaned with anhydrous ethanol for 5 minutes to remove residual lubricating oil from the stamping process, and then dried at 80°C for 10 minutes.
[0045] P4. Preparation of the polymer layer: The pre-prepared polymerization reaction solution is uniformly coated onto the anodic aluminum oxide layer on the inner surface of the shell, with a coating thickness of 10 μm, and pre-baked at 80℃ for 5 min; then, the polymerization reaction solution is irradiated with ultraviolet light at a wavelength of 365 nm, with a power of 300 W and an irradiation time of 3 min, forming a polymer layer with a thickness of 8 μm on the surface of the anodic aluminum oxide layer. The polymerization reaction solution is prepared as follows: PEGMA (polyethylene glycol methyl ether methacrylate) and triallyl isocyanurate are mixed uniformly at a mass ratio of 5:1, and 1% of the total mass of the two initiators, azobisisobutyronitrile, is added, followed by dilution with anhydrous ethanol to adjust the monomer solid content in the polymerization reaction solution to 40 wt%.
[0046] P5. Polymer layer curing: The product obtained in step P4 is cured at 120°C for 20 minutes, and then cooled to room temperature in the furnace to obtain a lithium-ion battery aluminum alloy shell with an anodic aluminum oxide layer and a polymer layer deposited on the surface of a 6061 aluminum alloy substrate.
[0047] In this comparative example, anodizing was used instead of plasma oxidation to prepare the aluminum alloy casing for lithium-ion batteries. The alumina layer obtained by anodizing has a typical nanoscale porous structure (pore size approximately 10-50 nm), with pores penetrating the oxide layer. During subsequent coating with the polymerization reaction solution, although the liquid precursor could partially penetrate the pores, the monomers inside the pores were not fully cross-linked due to limited light exposure during UV polymerization, and micropores remained inside the pores after solvent evaporation. Therefore, the density, critical load of interlayer bonding, and fluorine corrosion resistance of the sample obtained in this comparative example were all lower than those of the example using oxygen plasma oxidation. Specific performance comparison data are shown in Table 1.
[0048] Comparative Example 2 A method for preparing a corrosion-resistant and flame-retardant aluminum alloy casing for lithium-ion batteries includes the following steps: Q1. Pretreatment of Aluminum Alloy Substrate: Cut 6061 aluminum alloy into shell blanks of 100mm×100mm×2mm, immerse them in a 10wt% sodium hydroxide aqueous solution at 60℃ for 10min. After removal, rinse with deionized water until the washing solution is neutral. Then immerse in a 15% (v / v) nitric acid aqueous solution at room temperature for 3min, remove and rinse with deionized water until the pH of the washing solution is 7, and then dry at 100℃ for 1h.
[0049] Q2. Oxygen plasma treatment: Place the pretreated shell blank from step Q1 into the reaction chamber of the plasma oxidation device and evacuate to 1×10⁻⁶. -4 Pa, a mixture of oxygen and argon gas (oxygen volume accounts for 60% of the total volume of the mixture) is introduced, and the pressure is adjusted to 50 Pa. The plasma generator is started, with a radio frequency power of 500 W, a processing temperature of 400 °C, and a processing time of 10 min, forming an Al2O3 layer with a thickness of 15 μm on the surface of the aluminum alloy substrate.
[0050] Q3. Stamping: The aluminum alloy substrate with an Al2O3 layer deposited on its surface in step Q2 is placed in a stamping die and stamped at room temperature to prepare a cubic battery casing. After stamping, the surface of the casing is ultrasonically cleaned with anhydrous ethanol for 5 minutes to remove residual lubricating oil from the stamping process, and then dried at 80°C for 10 minutes.
[0051] Q4. Physical Mix Coating (Non-Crosslinking Coating): PEGMA (polyethylene glycol methyl ether methacrylate) and triallyl isocyanurate are mixed uniformly at a mass ratio of 5:1. Anhydrous ethanol is added to adjust the solid content to 40wt%, and the mixture is stirred until completely dissolved to obtain a physically mixed coating solution. This physically mixed coating solution is uniformly coated onto the Al2O3 layer on the inner surface of the shell to a thickness of 10μm. It is then placed in an 80℃ oven for 20min to remove the solvent, forming a physically mixed coating with a thickness of approximately 8μm on the Al2O3 layer surface. No photoinitiator is added during this process, and no ultraviolet light irradiation is performed. No chemical crosslinking reaction occurs between PEGMA and triallyl isocyanurate; the coating exists in a physically mixed state.
[0052] Q5. Drying treatment: The product obtained in step Q4 is placed at 120℃ and dried for 20 minutes, and then cooled to room temperature in the furnace to obtain a lithium-ion battery aluminum alloy shell with a 15μm thick Al2O3 layer deposited on the surface of the 6061 aluminum alloy substrate and a physical mixed coating deposited on the surface of the Al2O3 layer.
[0053] In this comparative example, PEGMA and triallyl isocyanurate were only physically mixed, without undergoing a chemical cross-linking reaction initiated by ultraviolet light, resulting in a lack of a three-dimensional network structure within the coating. During immersion in the electrolyte, the PEGMA molecular chains in this physically mixed coating may dissolve or swell, and small TAIC (triallyl isocyanurate) molecules may also migrate and precipitate, leading to coating structure damage and interfacial bonding failure. Therefore, the fluorine corrosion resistance and long-term stability of the aluminum alloy shell obtained in this comparative example are significantly lower than those in the examples. Specific performance comparison data are shown in Table 1.
[0054] Comparative Example 3 A method for preparing a corrosion-resistant and flame-retardant aluminum alloy casing for lithium-ion batteries includes the following steps: R1. Pretreatment of Aluminum Alloy Substrate: Cut 6061 aluminum alloy into shell blanks of 100mm×100mm×2mm, immerse them in a 10wt% sodium hydroxide aqueous solution at 60℃ for 10min. After removal, rinse with deionized water until the washing solution is neutral. Then immerse in a 15% (v / v) nitric acid aqueous solution at room temperature for 3min, remove and rinse with deionized water until the pH of the washing solution is 7, and then dry at 100℃ for 1h.
[0055] R2, Oxygen Plasma Treatment: The pretreated shell blank from step R1 is placed into the reaction chamber of the plasma oxidation device, and the vacuum is evacuated to 1×10⁻⁶. -4 Pa, a mixture of oxygen and argon gas (oxygen volume accounts for 60% of the total volume of the mixture) is introduced, and the pressure is adjusted to 50 Pa. The plasma generator is started, with a radio frequency power of 500 W, a processing temperature of 400 °C, and a processing time of 10 min, forming an Al2O3 layer with a thickness of 15 μm on the surface of the aluminum alloy substrate.
[0056] R3. Stamping: The aluminum alloy substrate with an Al2O3 layer deposited on its surface in step R2 is placed in a stamping die and stamped at room temperature to prepare a cubic battery casing. After stamping, the surface of the casing is ultrasonically cleaned with anhydrous ethanol for 5 minutes to remove residual lubricating oil from the stamping process, and then dried at 80°C for 10 minutes.
[0057] R4. Preparation of Conventional Flame-Retardant Coating: By weight, the conventional flame-retardant coating consists of 40 parts waterborne epoxy emulsion (Jiangsu Fuqisen New Material Technology Co., Ltd.), 25 parts ammonium polyphosphate (Shanghai Maclean Biochemical Technology Co., Ltd.), 15 parts pentaerythritol (Shanghai Maclean Biochemical Technology Co., Ltd.), 15 parts melamine (Shanghai Maclean Biochemical Technology Co., Ltd.), 2 parts dispersant (ammonium polyacrylate, Shanghai Maclean Biochemical Technology Co., Ltd.), 1 part defoamer (polyether-modified silicone defoamer, BYK Chemie, Germany), and 2 parts deionized water. The components are mixed and stirred evenly to obtain the flame-retardant coating. The flame-retardant coating is uniformly coated onto the Al2O3 layer on the inner surface of the shell, with a coating thickness of 200 μm. It is pre-baked at 80°C for 30 min, then cured at 150°C for 60 min, forming a conventional intumescent flame-retardant coating with a thickness of approximately 150 μm on the surface of the Al2O3 layer.
[0058] R5. Cooling treatment: The product obtained in step R4 is naturally cooled to room temperature to obtain a lithium-ion battery aluminum alloy shell with a 15μm thick Al2O3 layer deposited on the surface of the 6061 aluminum alloy substrate and a conventional flame-retardant coating deposited on the surface of the Al2O3 layer.
[0059] This comparative example uses a conventional intumescent flame-retardant coating (ammonium polyphosphate / pentaerythritol / melamine system). While this coating exhibits good flame-retardant properties and can expand to form a carbonized layer at high temperatures to insulate against heat, its thickness is relatively large (approximately 150 μm), significantly greater than the thickness of the polymer layer in the embodiments of this invention (3-8 μm). The high content of inorganic fillers such as ammonium polyphosphate in the coating results in low coating density, high brittleness, and poor adhesion to the alumina layer and aluminum alloy substrate. Furthermore, conventional flame-retardant coatings pose a risk of component leaching during long-term immersion in the electrolyte, affecting the corrosion resistance and interfacial stability of the shell material. Therefore, the fluorine corrosion resistance of the aluminum alloy shell prepared in this comparative example is significantly lower than that of the embodiments of this invention. Specific performance comparison data are shown in Table 1.
[0060] Product performance testing The performance of the lithium-ion battery aluminum alloy casings prepared in Examples 1-3 and Comparative Examples 1-3 was tested, and the test results are shown in Table 1.
[0061] 1. Density detection of Al2O3 layer in aluminum alloy shell material of lithium-ion battery: The method of image analysis is performed in accordance with the current guiding technical document GB / Z 45463-2025 "Determination of porosity of thermal spray coating".
[0062] 2. Vickers hardness test of Al2O3 layer of aluminum alloy shell material for lithium-ion battery: The test shall be conducted in accordance with the provisions of GB / T 4340.1-2024 "Metallic materials Vickers hardness test - Part 1: Test method".
[0063] 3. Testing of interlayer bonding strength between the aluminum alloy substrate and the Al2O3 layer in the aluminum alloy shell material of lithium-ion batteries: The test shall be conducted in accordance with the scratch test method specified in GB / T 30707-2014 "Test Method for Bond Strength of Fine Ceramic Coatings - Scratch Method".
[0064] 4. Lithium-ion battery casing fluorine corrosion rate test: Electrolyte preparation: Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) were mixed in a volume ratio of 3:4:3 to dissolve lithium hexafluorophosphate and prepare a 1 mol / L LiPF6 basic electrolyte; anhydrous HF mother liquor was added to make the HF concentration in the electrolyte reach 50 ppm. Potentiodynamic polarization tests were performed using a three-electrode system at (25±2)℃. The lithium-ion battery casing was used as the working electrode (only the modified outer surface was exposed), a platinum sheet as the counter electrode, and a saturated calomel electrode (SCE) as the reference electrode. The scanning potential range was -1.2V to 0.6V (vs. SCE), and the scanning rate was 0.5 mV / s. The self-corrosion current density was obtained by fitting the polarization curve using the Tafel linear extrapolation method; the equivalent corrosion rate calculation formula for aluminum alloy was obtained according to Faraday's law: corrosion rate = 0.01086 × i, where 0.01086 is in mm·cm. 2 ·a -1 ·μA -1 i represents the corrosion current density, in μA·cm. -2 The obtained values represent equivalent uniform corrosion rates, used for lateral comparison of fluorine corrosion resistance among samples. Polarization curves are shown below. Figures 1-6 As shown.
[0065] 5. Tensile strength test of lithium-ion battery casing: The test shall be conducted in accordance with the provisions of GB / T 228.1-2021 "Metallic materials - Tensile testing - Part 1: Test method at room temperature".
[0066] 6. Lithium-ion battery casing elongation test: The test shall be conducted in accordance with the provisions of GB / T 228.1-2021 "Metallic materials - Tensile testing - Part 1: Test method at room temperature".
[0067] 7. Lithium-ion battery immersion corrosion test: The lithium-ion battery casing was immersed in a corrosive medium for 1000 hours at (25±2)℃. Corrosive medium preparation: Ethylene carbonate, ethyl methyl carbonate, and dimethyl carbonate were mixed in a volume ratio of 3:4:3 to dissolve lithium hexafluorophosphate, obtaining a 1 mol / L LiPF6 basic electrolyte. A trace amount of anhydrous hydrofluoric acid mother liquor was added to achieve a HF concentration of 50 ppm in the electrolyte. The mixture was sealed and allowed to stand to simulate electrolyte leakage corrosion conditions.
[0068] 8. Detection of spontaneous combustion after electrolyte leakage: A laboratory simulation test was conducted in a 25℃ explosion-proof test chamber. Micro-perforations were pre-fabricated in the test casing to simulate corrosion damage. A 1mol / L LiPF6 carbonate electrolyte containing 50ppm HF was introduced and maintained at a slight positive pressure to allow continuous electrolyte leakage. After the leaked electrolyte wetted the battery casing, the temperature was increased to 180℃ at a rate of 2℃ / min, and continuous observation was conducted for 2 minutes. A stable open flame lasting longer than 1 second was considered spontaneous combustion; smoke, instantaneous sparks, or short-term flashover were not considered spontaneous combustion.
[0069] Table 1 Performance test results of aluminum alloy casing for lithium-ion batteries
[0070] Because the medium used in the fluorine corrosion resistance test contains hydrofluoric acid, which is a highly corrosive simulated environment, the overall corrosion rate benchmark is higher than that of a conventional neutral, fluorine-free system. As shown in Table 1, the lithium-ion battery aluminum alloy casing prepared using the method of this invention exhibits excellent fluorine corrosion resistance, preventing spontaneous combustion reactions caused by electrolyte leakage and significantly improving the safety of lithium-ion batteries.
[0071] The measured potentiodynamic polarization curves were fitted using Tafel fitting, and the self-corrosion current density was obtained by extrapolating and intersecting the anode and cathode branches. From Figures 1-6 It can be seen that the corrosion current of the aluminum alloy shell in Example 1 is 81.6 μA / cm. 2 The corrosion current of the aluminum alloy casing in Example 2 was 63.6 μA / cm. 2 The corrosion current of the aluminum alloy casing in Example 3 was 52.8 μA / cm. 2 The corrosion current of the aluminum alloy casing in Comparative Example 1 was 1.9 × 10⁻⁶. 2 μA / cm 2 The corrosion current of the aluminum alloy casing in Comparative Example 2 was 3.24 × 10⁻⁶. 2 μA / cm 2 The corrosion current of the aluminum alloy casing in Comparative Example 3 was 8 × 10⁻⁶. 2 μA / cm 2 The higher the corrosion current value, the worse the corrosion resistance of the aluminum alloy shell; therefore, the aluminum alloy shell prepared in Example 3 of the present invention has the best corrosion resistance; the corrosion resistance of the aluminum alloy shells prepared in Comparative Examples 1 to 3 is significantly lower than that of the examples of the present invention.
[0072] The embodiments described above are merely preferred embodiments of this application and are not intended to limit the scope of protection of this application. Various modifications and variations can be made to this application by anyone skilled in the art. Any simple equivalent changes and modifications made based on the scope of protection claimed in this application and the content of the specification should be included within the scope of protection of this application.
Claims
1. An aluminum alloy casing for a lithium-ion battery, characterized in that, It consists of an aluminum alloy substrate, an Al2O3 layer deposited on the surface of the aluminum alloy substrate, and a polymer layer deposited on the surface of the Al2O3 layer facing away from the aluminum alloy substrate; the thickness of the Al2O3 layer is 5~15μm; the polymer layer is obtained by crosslinking polyethylene glycol methyl ether methacrylate and triallyl isocyanurate, and the thickness of the polymer layer is 3~8μm.
2. The lithium-ion battery aluminum alloy casing according to claim 1, characterized in that, The aluminum alloy matrix is 6061 aluminum alloy or 7075 aluminum alloy.
3. The method for preparing the aluminum alloy casing of a lithium-ion battery according to claim 1 or 2, characterized in that, Includes the following steps: S1. Cut the aluminum alloy substrate into shell blanks of a preset size, and perform degreasing, pickling, water washing and drying treatments in sequence; S2. The shell blank after the pretreatment in step S1 is subjected to oxygen plasma treatment to form a dense Al2O3 layer on the surface of the shell blank; the treatment gas is a mixture of oxygen and argon, and the oxygen accounts for 30% to 60% of the volume of the mixture. S3. The product obtained in step S2 is stamped at room temperature to form a battery casing; the battery casing is then cleaned and dried. S4. The polymerization reaction solution is coated onto the surface of the Al2O3 layer on the inner surface of the battery casing, pre-baked, and then irradiated with ultraviolet light to cause the polymerization reaction solution to undergo a cross-linking reaction to obtain a polymer layer; the polymerization reaction solution contains polyethylene glycol methyl ether methacrylate and triallyl isocyanurate in a mass ratio of (3~5):
1. S5. Heat the product obtained in step S4 to solidify the polymer layer, and then cool it to room temperature in the furnace to obtain the aluminum alloy casing for the lithium-ion battery.
4. The preparation method according to claim 3, characterized in that, In step S1, degreasing is performed using a 5wt%~10wt% sodium hydroxide aqueous solution, and the shell blank is immersed at 50℃~60℃ for 10~15 minutes. Or / and, in step S1, the pickling is performed by immersing the degreased shell blank in a nitric acid aqueous solution with a volume percentage of 10%~15% for 3~5 minutes at room temperature.
5. The preparation method according to claim 3, characterized in that, The drying conditions in step S1 are: drying at 80℃~100℃ for 1~2 hours; Or / and, in step S5, the curing temperature is 100℃~120℃ and the time is 20~40min.
6. The preparation method according to claim 3, characterized in that, The conditions for oxygen plasma treatment in step S2 are: controlling the pressure in the reaction chamber ≤ 10. -3 Pa; after introducing the mixed gas, adjust the pressure of the mixed gas to 10~50Pa, adjust the radio frequency power to 200~500W, the processing temperature to 200℃~400℃, and the processing time to 10~30min.
7. The preparation method according to claim 3, characterized in that, The polymerization reaction solution in step S4 contains an initiator, the mass of which accounts for 1% to 3% of the total mass of the polyethylene glycol methyl ether methacrylate and the triallyl isocyanurate.
8. The preparation method according to claim 3, characterized in that, The solid content in the polymerization reaction solution in step S4 is 20wt%~40wt%; Or / and, the coating thickness of the polymerization reaction liquid on the surface of the Al2O3 layer in step S4 is 5~10μm.
9. The preparation method according to claim 3, characterized in that, In step S4, the pre-baking temperature is 60℃~80℃ and the time is 5~10min; Or / and, in step S4, the wavelength of the ultraviolet light is 254~365nm, the power of the ultraviolet light source is 100~300W, and the ultraviolet light irradiation time is 3~10min.
10. The application of the aluminum alloy casing for lithium-ion batteries according to claim 1 or 2 in the preparation of lithium-ion batteries.