A separator for rechargeable lithium batteries and a rechargeable lithium battery including the separator.

By using nanofibers of polyimide resin and polyphosphate compounds in rechargeable lithium battery separators and preparing single-layer or multi-layer structures using electrospinning technology, the problems of insufficient stability and mechanical strength of the separators at high temperatures are solved, flame retardant properties and fire extinguishing performance are improved, and the electrochemical performance of lithium batteries is enhanced.

CN123121071APending Publication Date: 2026-11-17SAMSUNG SDI CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610605340.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2026-04-23
Filing Date
2026-05-06
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The separators of existing rechargeable lithium batteries lack stability and mechanical strength at high temperatures, and their flame-retardant properties and fire-extinguishing performance need to be improved.

Method used

The membrane incorporates nanofibers, which are composed of polyimide resin and polyphosphate compounds and are prepared by electrospinning to form single-layer or multi-layer structures, including core-shell structures, to improve the membrane's heat resistance, mechanical strength and flame retardant properties.

Benefits of technology

It improves the stability and mechanical strength of the diaphragm at high temperatures, has good flame retardant properties and fire extinguishing performance, and improves the charging/discharging characteristics of lithium batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123121071A_ABST
    Figure CN123121071A_ABST
Patent Text Reader

Abstract

A separator for a rechargeable lithium battery and a rechargeable lithium battery including the separator are disclosed. The separator comprises nanofibers. The nanofibers comprise a polyimide resin and a polyphosphate compound, and the polyphosphate compound is included in an amount greater than about 20 wt% and less than about 75 wt% based on 100 wt% of the separator.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] A separator for a rechargeable lithium battery and a rechargeable lithium battery including the separator are disclosed. Background Technology

[0002] With the increasing prevalence of battery-powered electronic devices (such as mobile phones, laptops, and electric vehicles), the demand for rechargeable batteries with high energy density and high capacity is growing. Therefore, improving the performance of rechargeable lithium batteries can be beneficial.

[0003] A rechargeable lithium battery includes a positive electrode and a negative electrode containing active materials capable of intercalating and deintercalating lithium ions, as well as an electrolyte, and generates electrical energy through oxidation and reduction reactions when lithium ions are intercalated / deintercalated at the positive and negative electrodes. Summary of the Invention

[0004] Some example embodiments include a separator for rechargeable lithium batteries having desired or improved heat resistance and mechanical strength, as well as desired or improved flame retardant and fire extinguishing properties.

[0005] Some example embodiments include a rechargeable lithium battery that has desired or improved thermal stability and charge / discharge characteristics by including a separator.

[0006] Some example embodiments include a separator for a rechargeable lithium-ion battery, the separator comprising nanofibers, wherein the nanofibers comprise: a polyimide resin; and a polyphosphate compound. Based on 100 wt% of the separator, the polyphosphate compound comprises in an amount greater than about 20 wt% and less than about 75 wt%.

[0007] Another example embodiment includes a separator for a rechargeable lithium-ion battery, the separator comprising a plurality of nanofiber layers comprising nanofibers. The nanofiber layers comprise a polyimide resin, and at least one of the plurality of nanofiber layers further comprises a polyphosphate compound.

[0008] Some example embodiments include a separator for a rechargeable lithium battery comprising nanofibers having a core-shell structure, the core-shell structure comprising a core and a shell on the surface of the core, wherein the core and shell each independently comprise at least one of a polyimide resin, a polyphosphate compound, and a mixture of a polyimide resin and a polyphosphate compound, and the core and shell comprise different compounds.

[0009] Some example embodiments include a rechargeable lithium battery comprising: a positive electrode; a negative electrode; and a separator between the positive and negative electrodes.

[0010] The separator for rechargeable lithium batteries according to some example embodiments may have desired or improved heat resistance and mechanical strength, and may exhibit desired or improved flame retardant and fire extinguishing properties.

[0011] According to some example embodiments, the rechargeable lithium battery includes a separator and has desired or improved thermal stability and charge / discharge characteristics. Attached Figure Description

[0012] Figures 1 to 6 This is a schematic diagram illustrating a separator for a rechargeable lithium battery according to some example embodiments.

[0013] Figure 7 This is a schematic diagram of an electrospinning apparatus for manufacturing multilayer separators for rechargeable lithium batteries.

[0014] Figures 8 to 11 This is a schematic diagram illustrating a rechargeable lithium battery according to some example embodiments. Detailed Implementation

[0015] Example embodiments are described in detail below. However, these embodiments are merely examples, and this disclosure is not limited thereto; rather, it is defined by the scope of the claims.

[0016] As used herein, unless otherwise specifically defined, it is understood that when an element such as a layer, film, region, or substrate is referred to as being “on” another element, the element may be directly on the other element or there may be an intervening element between them.

[0017] As used herein, unless otherwise specifically defined, singular expressions may also include plural expressions. Additionally, unless otherwise stated, “A or B” may mean “including A, including B, or including both A and B”.

[0018] As used herein, “combination of them” can refer to mixtures of components, laminates, complexes, copolymers, alloys, blends, reaction products, etc.

[0019] As used herein, “thickness” can be measured, for example, with a micrometer or by means of a photograph taken with an optical microscope, such as a scanning electron microscope (SEM).

[0020] For example, in this specification, the thickness of the separator or nanofiber layer can be measured using a scanning electron microscope (SEM) by observing a cross-section of a lithium secondary battery or separator. In this case, an SEM image with a magnification of 1000× to 10000× can be obtained by using a region representing the overall cross-sectional thickness of the separator or nanofiber layer. The start and end points for measuring the thickness can be set based on the outermost boundary of the separator or nanofiber layer. As an example, a first virtual tangent line can be drawn through the vertex of the most convex nanofiber on one surface of the separator or nanofiber layer, and the direction perpendicular to the first virtual tangent line can be defined as the thickness measurement direction. The start point can be defined as the outermost protrusion of the nanofiber located on the first virtual tangent line, and the end point can be defined as the outermost protrusion on a second virtual tangent line parallel to the first virtual tangent line and contacting the other surface opposite to said one surface. The shortest distance between the start and end points set in this way can be determined as the thickness of the separator or nanofiber layer. Measurements can be repeated at 10 or more different points, and the arithmetic mean of the obtained values ​​can be determined as the final thickness.

[0021] Alternatively, in this specification, the thickness of the diaphragm or nanofiber layer can be measured using a micrometer. In this case, the thickness of the diaphragm or nanofiber layer itself can be measured using a Digimatic Micrometer (MDH-25MC, Mitutoyo Corporation). Measurements can be repeated at 10 or more different points, and the arithmetic mean of the obtained values ​​can be determined as the final thickness.

[0022] As used herein, the amount of components in the diaphragm can be measured using inductively coupled plasma optical emission spectrometry (ICP-OES) or scanning electron microscopy-energy dispersive spectroscopy (SEM-EDS), or can be predicted by the amount of polymer added to the electrospinning solution.

[0023] When the terms “about” or “substantially” are used in conjunction with numerical values ​​in this specification, it is intended that the relevant numerical value includes a tolerance of ±10% around the stated value. When a range is specified, the range includes all values ​​within that range, such as increments of 0.1%.

[0024] Separator for rechargeable lithium batteries In the following text, refer to Figures 1 to 6 A separator for a rechargeable lithium battery according to an embodiment is described in detail.

[0025] Figures 1 to 6 This is a schematic diagram illustrating a separator for a rechargeable lithium battery according to some example embodiments.

[0026] Reference Figure 1According to some example embodiments, the separator 30A for a rechargeable lithium battery includes nanofibers, wherein the nanofibers include polyimide resin (PI) and polyphosphate compounds.

[0027] Polyimide resins can be or include heat-resistant polymers and can be prepared by thermally imidizing a precursor (polyamic acid).

[0028] Because polyimide resins possess desired or improved heat resistance and high-temperature stability, separators for rechargeable lithium batteries incorporating polyimide resins can be stable at high temperatures without shrinkage, compared to conventional polyolefin separators. Furthermore, polyamic acid is soluble in solvents, and its viscosity can be easily controlled, which can be advantageous for electrospinning processes.

[0029] In polyimide resins, polyimides can be obtained by imidizing polyamic acid synthesized by the condensation reaction of dianhydrides and diamines.

[0030] Examples of dianhydrides may include, but are not limited to, at least one of the following: pyromellitic dianhydride (PMDA), 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA), 4,4'-(hexafluoroisopropylidene)diphthalic dianhydride (6FDA), 3,3',4,4'-benzophenone tetracarboxylic dianhydride (BTDA), 1,4,5,8-naphthalenetetracarboxylic dianhydride (NTCDA), 1,2,4,5-cyclohexanetetracarboxylic dianhydride (HPMDA), oxydiphthalic dianhydride (ODPA), benzophenone tetracarboxylic dianhydride (BTDA), biphenyltetracarboxylic dianhydride, or terphenyltetracarboxylic dianhydride (TPDA).

[0031] Examples of diamines may include, but are not limited to, at least one of arylamines (wherein the aryl group may be a C6 to C20 aryl group), such as diaminodiphenyl ether (ODA), methylene diphenyl diamine (MDA), m-phenylenediamine (mPDA), p-phenylenediamine (pPDA), 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP), 1,3-bis(3-aminophenoxy)benzene (APB), 3,3'-diaminobenzidine (DAB), or 4,4'-diaminodiphenyl sulfone (DDS).

[0032] For example, based on 100 wt% of the separator, polyimide resin may be included in an amount ranging from about 25 wt% to about 80 wt% (e.g., about 30 wt% to about 75 wt%, about 40 wt% to about 75 wt%, or about 50 wt% to about 75 wt%). Within the above range, separators with desired or improved mechanical strength and heat resistance can be achieved.

[0033] For example, the weight-average molecular weight (M) of polyimide resins wThe electrospinning strength can be in the range of about 100,000 g / mol to about 300,000 g / mol (e.g., about 200,000 g / mol to about 250,000 g / mol). Within the above range, diaphragms with desired or improved electrospinning properties can be achieved.

[0034] In the context of this application, polyphosphate compounds refer to compounds containing polyphosphate anions, that is, anions that can be formed by at least 2PO4 structural units linked together by shared oxygen atoms to form a linear or cyclic structure.

[0035] Polyphosphate compounds are polymers that include phosphate anions, and when included in a diaphragm, polyphosphate compounds can impart flame-retardant and fire-extinguishing properties to the diaphragm.

[0036] For example, polyphosphate compounds can be prepared by polycondensing phosphates (e.g., ammonium dihydrogen phosphate), and can be decomposed at high temperatures to produce inert gases and form a glassy HPO3 (metaphosphate) film, thereby exhibiting flame-retardant and fire-extinguishing properties.

[0037] In addition, polyphosphate compounds can be used in combination with polyimide resins to provide flexibility to the diaphragm, thereby further improving its mechanical properties.

[0038] For example, polyphosphate compounds may include monovalent organic cations, monovalent metal cations, or combinations thereof.

[0039] Monovalent organic cations can include ammonium cations (N(R)) 1 R 2 R 3 R 4 ) + , where R 1 To R 4 Each is independently hydrogen, deuterium, or at least one of C1 to C6 alkyl groups, and melamine cation (C3N6H7). + ), guanidinium cation ((C(NH2)3) + (or combinations thereof).

[0040] Ammonium cations can be or include, for example, NH4. + or N(CH3)4 + .

[0041] Monovalent metal cations can include Li + Na + K + Or at least one of their combinations.

[0042] For example, polyphosphate compounds may include at least one of ammonium polyphosphate (APP), melamine polyphosphate (MPP), or combinations thereof.

[0043] As an example, polyphosphate compounds may include ammonium polyphosphate, which decomposes at high temperatures to produce inert gases NH3 and H2O and forms a glassy HPO3 film, thereby exhibiting desired or improved flame retardant and fire extinguishing properties.

[0044] According to some example embodiments, by including an optimal amount of polyphosphate compound together with a polyimide resin, a diaphragm with desired or improved flexibility, flame retardant properties, and fire extinguishing properties can be achieved.

[0045] For example, the weight-average molecular weight (M) of polyphosphate compounds w The value can be in the range of about 50,000 g / mol to about 100,000 g / mol (e.g., about 60,000 g / mol to about 100,000 g / mol or about 60,000 g / mol to about 90,000 g / mol). If the above numerical range is met (when the above numerical range is met), a diaphragm with desired or improved mechanical strength, flame retardant properties and fire extinguishing properties can be achieved.

[0046] For example, based on a 100 wt% separator, polyphosphate compounds may be included in an amount greater than about 20 wt% and less than about 75 wt% (e.g., in the range of about 22.5 wt% to about 70 wt%, about 25 wt% to about 65 wt%, about 25 wt% to about 60 wt%, or about 25 wt% to about 50 wt%). If the above range is satisfied (when the above range is satisfied), a separator for rechargeable lithium batteries with desired or improved heat resistance, desired or improved mechanical strength (such as flexibility), flame retardant properties, and fire extinguishing properties can be achieved.

[0047] The diaphragm 30A may be or include a single-layer electrospun diaphragm manufactured by electrospinning an electrospun solution prepared by mixing polyamic acid and polyphosphate compounds using a nozzle assembly.

[0048] Electrospinning involves using a high-voltage electric field to spray a polymer solution into fine nanofibers. When separators for rechargeable lithium batteries are manufactured using electrospinning, separators with a uniform nanofiber network can be achieved, ensuring high porosity. This improves ionic conductivity and permeability, and provides superior heat resistance and mechanical strength compared to existing separators.

[0049] Therefore, the separator for a rechargeable lithium battery according to some example embodiments includes nanofibers, and the nanofibers include polyimide resins and polyphosphate compounds.

[0050] Within the framework of this invention, the term "nanofiber" refers to any fiber having an average diameter in the range of 1 nm to 1000 nm.

[0051] For example, the average diameter of the nanofibers can be in the range of about 10 nm to about 300 nm (e.g., about 50 nm to about 300 nm, about 50 nm to about 150 nm, about 150 nm to about 250 nm, or about 150 nm to about 200 nm). If the above numerical range is met (when the above numerical range is met), a membrane with desired or improved mechanical strength and porosity can be achieved.

[0052] The diameter of a nanofiber can refer to the widest diameter among the diameters of the fibers measured based on a cross-section of a single nanofiber, and can be measured in a direction perpendicular to the longitudinal direction of the nanofiber.

[0053] The average diameter of the nanofibers can be calculated by randomly measuring the cross-sectional diameter of about 20 fibers in a scanning electron microscope (SEM) image of the membrane surface and then calculating the arithmetic mean of the cross-sectional diameters of the 20 fibers.

[0054] For example, the thickness of the membrane can be in the range of about 1 μm to about 30 μm (e.g., about 5 μm to about 30 μm, about 5 μm to about 25 μm, about 5 μm to about 15 μm, about 8 μm to about 20 μm, or about 8 μm to about 15 μm). If this numerical range is met (when this numerical range is met), ultrathin membranes can be designed, and membranes with desired or improved durability, porosity, and heat resistance can be achieved.

[0055] The following describes in detail separators 30B, 30C, and 30C' for rechargeable lithium batteries according to some example embodiments. Since the descriptions of polyimide resins and polyphosphate compounds, as well as the average diameter of nanofibers, are the same as those described above, their descriptions are omitted, and only the remaining information is described.

[0056] Figures 2 to 4 This is a schematic diagram illustrating a separator 30B for a rechargeable lithium battery according to some example embodiments.

[0057] According to some example embodiments, the separator 30B for a rechargeable lithium battery includes a plurality of nanofiber layers comprising nanofibers, wherein the nanofiber layers comprise a polyimide resin, and at least one of the plurality of nanofiber layers further comprises a polyphosphate compound.

[0058] For example, in a diaphragm, nanofiber layers may be included in two or more layers (e.g., three or more layers).

[0059] Reference Figures 2 to 4 The separator 30B for a rechargeable lithium battery includes: a first nanofiber layer 31; a second nanofiber layer 32 on the first nanofiber layer 31; and a third nanofiber layer 33 on the second nanofiber layer 32. The first nanofiber layer 31, the second nanofiber layer 32, and the third nanofiber layer 33 comprise a polyimide resin, and at least one of the first nanofiber layer 31, the second nanofiber layer 32, and the third nanofiber layer 33 may further comprise a polyphosphate compound.

[0060] The diaphragm 30B may be or include a multilayer electrospun diaphragm manufactured by electrospun electrospinning electrospinning solutions of the same or different compositions using multiple supply devices (nozzle groups).

[0061] Reference Figure 2 The first nanofiber layer 31, the second nanofiber layer 32, and the third nanofiber layer 33 may include polyimide resin and polyphosphate compounds. For example, the components of the first nanofiber layer 31, the second nanofiber layer 32, and the third nanofiber layer 33, and the amount of each component, may be the same or different.

[0062] Reference Figure 3 The first nanofiber layer 31 and the third nanofiber layer 33 comprise polyimide resin and polyphosphate compounds, and the second nanofiber layer 32 may comprise polyimide resin. For example, the components and the amount of each component in the first nanofiber layer 31 and the third nanofiber layer 33 may be the same or different.

[0063] Reference Figure 4 The first nanofiber layer 31 and the third nanofiber layer 33 may include polyimide resin, and the second nanofiber layer 32 may include polyimide resin and polyphosphate compound.

[0064] According to some example embodiments, the separator 30B for a rechargeable lithium battery may consist of or include multiple separators, and each layer may consist of or include a single polyimide resin, or may consist of or include an optimal amount of each polyimide resin and a polyphosphate compound, such that mechanical strength (such as flexibility), flame retardant properties, and fire extinguishing properties are better than in the case of a single-layer separator.

[0065] For example, a nanofiber layer comprising 100 wt% of a polyphosphate compound may include a polyphosphate compound in an amount greater than about 20 wt% and less than about 75 wt% (e.g., in the range of about 22.5 wt% to about 70 wt%, about 25 wt% to about 65 wt%, about 25 wt% to about 60 wt%, or about 25 wt% to about 50 wt%).

[0066] For example, based on 100 wt% of the membrane 30B, polyphosphate compounds may be included in an amount greater than or equal to about 8 wt% and less than about 75 wt% (e.g., in the range of about 15 wt% to about 70 wt%, about 20 wt% to about 70 wt%, or about 25 wt% to about 70 wt%).

[0067] For example, based on 100 wt% of the membrane 30B, polyimide resin may be included in an amount ranging from about 25 wt% to about 95 wt% (e.g., about 25 wt% to about 80 wt%, about 30 wt% to about 75 wt%, about 40 wt% to about 75 wt%, or about 50 wt% to about 75 wt%).

[0068] If polyphosphate compounds are included in the multilayer separator 30B within the above-mentioned numerical range (when polyphosphate compounds are included in the multilayer separator 30B within the above-mentioned numerical range), a multilayer separator for rechargeable lithium batteries with desired or improved mechanical strength, flame retardant properties and fire extinguishing properties can be achieved.

[0069] For example, the thickness of the nanofiber layer can be in the range of about 1 μm to about 30 μm (e.g., about 1 μm to about 20 μm, about 1 μm to about 15 μm, about 1 μm to about 10 μm, about 5 μm to about 15 μm, or about 5 μm to about 10 μm).

[0070] For example, the thickness of the diaphragm 30B can be in the range of about 1 μm to about 50 μm (e.g., about 5 μm to about 40 μm, about 5 μm to about 30 μm, or about 10 μm to about 30 μm).

[0071] If the above numerical range is met (when the above numerical range is met), an ultra-thin diaphragm can be designed, and a diaphragm with desired or improved durability, heat resistance, flame retardant properties and fire extinguishing properties can be achieved.

[0072] Figure 5 and Figure 6 This is a schematic diagram illustrating separators 30C, 30C' for rechargeable lithium batteries according to some example embodiments.

[0073] Reference Figure 5The separator 30C for rechargeable lithium batteries comprises nanofibers as a core-shell structure, the core-shell structure comprising a core a and a shell b on the surface of the core a. Both core a and shell b independently comprise any one of a polyimide resin, a polyphosphate compound, or a mixture of a polyimide resin and a polyphosphate compound. For example, core a and shell b may comprise different compounds.

[0074] Reference Figure 6 The separator 30C' for rechargeable lithium batteries may include two or more stacked nanofiber layers, and may include, for example, three or more nanofiber layers, the nanofiber layers including nanofibers with a core-shell structure.

[0075] Reference Figure 6 The diaphragm 30C' may include: a first nanofiber layer 31'; a second nanofiber layer 32' on the first nanofiber layer 31'; and a third nanofiber layer 33' on the second nanofiber layer 32'. The first nanofiber layer 31', the second nanofiber layer 32', and the third nanofiber layer 33' may include nanofibers having the above-described core-shell structure.

[0076] According to some example embodiments, a separator for a rechargeable lithium-ion battery (not shown in the figures) includes multiple nanofiber layers comprising nanofibers. The nanofiber layers comprise a polyimide resin. At least one of the multiple nanofiber layers comprises nanofibers having a core-shell structure, the core-shell structure comprising a core and a shell on the surface of the core. Both the core and the shell independently comprise any one of a polyimide resin, a polyphosphate compound, and a mixture of a polyimide resin and a polyphosphate compound. The core and the shell may comprise different compounds.

[0077] For example, based on 100 wt% of the membrane 30C, 30C', polyphosphate compounds may be included in an amount greater than about 20 wt% and less than about 75 wt% (e.g., in the range of about 22.5 wt% to about 70 wt%, about 25 wt% to about 65 wt%, about 25 wt% to about 60 wt%, or about 25 wt% to about 50 wt%).

[0078] For example, based on 100 wt% of the separator 30C, 30C', polyimide resin may be included in an amount ranging from about 25 wt% to about 80 wt% (e.g., from about 30 wt% to about 75 wt%, from about 40 wt% to about 75 wt%, or from about 50 wt% to about 75 wt%).

[0079] When the above-mentioned quantity range is met, a separator for rechargeable lithium batteries with desired or improved mechanical strength (such as flexibility) and desired or improved flame retardant and fire extinguishing properties can be achieved.

[0080] For example, the average diameter of the nanofibers forming the core-shell structure in membranes 30C and 30C' can be in the range of about 10 nm to about 300 nm (e.g., about 10 nm to about 200 nm, about 10 nm to about 150 nm, about 50 nm to about 150 nm, or about 50 nm to about 100 nm). If the above numerical range is met (when the above numerical range is met), a membrane with desired or improved mechanical strength and porosity can be achieved.

[0081] For example, the thickness of the monolayer diaphragm 30C can be in the range of about 1 μm to about 30 μm (e.g., about 1 μm to about 20 μm, about 1 μm to about 15 μm, about 1 μm to about 10 μm, about 5 μm to about 15 μm or about 5 μm to about 10 μm).

[0082] For example, the thickness of the multilayer diaphragm 30C' can be in the range of about 1 μm to about 50 μm (e.g., about 5 μm to about 40 μm, about 5 μm to about 30 μm, or about 10 μm to about 30 μm).

[0083] If the above numerical range is met (when the above numerical range is met), ultrathin membranes can be designed, and membranes with desired or improved durability, porosity, and heat resistance can be achieved.

[0084] For example, diaphragms 30A, 30B, 30C, and 30C' may also include heat-resistant polymers, which may include polymers of at least one of the following: polypropylene (PP), polyester, polyamide, polyetherimide (PEI), polyetheretherketone (PEEK), polyphenylene terephthalamide (PTA), polysulfone (PSF), polyethersulfone (PES), polyphenylene sulfide (PPS), polyamide-imide (PAI), polyetherimide (PEI), polyacrylonitrile (PAN), polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP), polycarbonate (PC), polyvinyl chloride (PVC), polyvinylidene chloride, polyethylene glycol derivatives, polyoxides, polyvinyl acetate, polystyrene (PS), polyvinylpyrrolidone (PVP), copolymers thereof, or combinations thereof. The heat-resistant polymer is a non-aqueous polymer, which may be desirable for forming fibers by electrospinning.

[0085] For example, based on 100 wt% of the separators 30A, 30B, 30C, 30C', the heat-resistant polymer may be included in an amount ranging from about 0 wt% to about 10 wt% (e.g., about 0 wt% to about 8 wt% or about 0 wt% to about 5 wt%).

[0086] Method for manufacturing a separator for rechargeable lithium batteries A method for manufacturing a separator for a rechargeable lithium battery according to some example embodiments includes: (1) mixing polyamic acid, a polyphosphate compound and a solvent to prepare an electrospinning solution; (2) electrospinning the electrospinning solution onto a release film to form a coating layer; (3) heat-treating the coating layer at a temperature in the range of about 200°C to about 500°C; and (4) removing (peeling off) the release film from the separator.

[0087] The separator manufactured by this manufacturing method may be or include a separator 30A for rechargeable lithium batteries having the above-described single-layer structure.

[0088] Electrospinning solutions can be prepared by mixing polyamic acid, polyphosphate compounds and solvents, and optionally by further including heat-resistant polymers as described above.

[0089] For example, the solvent may include at least one of dimethylacetamide, N-methylpyrrolidone, dimethylformamide, dimethyl sulfoxide, acetone, or combinations thereof.

[0090] For example, based on the total amount of polyamic acid and polyphosphate compound of 100 wt%, polyamic acid may be included in an amount ranging from about 25 wt% to about 80 wt% (e.g., about 30 wt% to about 75 wt%, about 40 wt% to about 75 wt%, or about 50 wt% to about 75 wt%).

[0091] For example, based on the total amount of polyamic acid and polyphosphate compound being 100 wt%, polyphosphate compound may be included in an amount greater than about 20 wt% and less than about 75 wt% (e.g., in the range of about 22.5 wt% to about 70 wt%, about 25 wt% to about 65 wt%, about 25 wt% to about 60 wt%, or about 25 wt% to about 50 wt%).

[0092] If the above numerical range is met (when the above numerical range is met), a separator for rechargeable lithium batteries can be manufactured with desired or improved mechanical strength (such as flexibility) and desired or improved flame retardant and fire extinguishing properties.

[0093] Next, the electrospinning solution prepared above can be electrospinned onto the release film to form a coating layer.

[0094] For example, the release film may include at least one of aluminum foil, copper foil, SUS, polyethylene terephthalate (PET), polypropylene (PP), polyethylene (PE), polycarbonate (PC), polyvinyl chloride (PVC), or combinations thereof.

[0095] The electrospinning process can be performed by positioning a supply device (nozzle assembly) consisting of tips with aperture sizes ranging from about 15G (gauge) to about 30G at a predetermined or desired interval with a collection roller, adding an electrospinning solution to the tips, positioning the target substrate on the collection roller, and then applying a voltage ranging from about 35kV to about 100kV to the tips.

[0096] The number of tips can be adjusted as needed based on the type and amount of polymer included in the electrospinning solution, and can be in the range of, for example, 1 to 1000.

[0097] The predetermined or desired distance between the supply device (nozzle assembly) and the target material can be in the range of approximately 10 cm to approximately 20 cm.

[0098] If the aperture size of the tip is in the range of about 25G to about 30G (when the aperture size of the tip is in the range of about 25G to about 30G), then the aperture size of the tip is suitable because a coating layer of the desired shape can be formed.

[0099] According to the electrospinning process, a polymer solution is spun and stretched into a fiber shape, and then spun onto a target substrate in the form of nanofibers to form a coating layer. More specifically, the electrospinning solution is suspended in droplets due to surface tension at the tip, and when a voltage is applied, charges accumulate on the surface of the electrospinning solution droplets, and repulsive forces occur between the charges. Therefore, the repulsive force between the charges points in the opposite direction to the surface tension of the solution, and when a critical voltage is reached, a conical Taylor cone is formed, and a polymer jet is emitted from the tip of the Taylor cone. Through multiaxial stretching in the agitation zone, the nanofibers are collected on a collecting roller in the form of a nonwoven fabric to form the coating layer.

[0100] For example, electrospinning can be performed under conditions ranging from about 20°C to about 30°C and from about 0% to about 60% relative humidity. Performing electrospinning under these temperature and relative humidity conditions offers advantages in maintaining a constant fiber thickness.

[0101] Additionally, the speed of the collecting roller can be adjusted to allow the coating layer to be formed to a desired thickness, and can be, for example, in the range of about 50 meters per minute (mpm) to about 300 mpm. Furthermore, the flow rate of the electrospinning solution discharged from the tip can be adjusted to be discharged at a rate in the range of about 150 μL / min to about 100 mL / min (e.g., about 1 mL / min to about 100 mL / min).

[0102] Furthermore, the tip air can be adjusted as needed to reduce or minimize interference between tips and to achieve uniform electrospinning. Tip air adjustment can be performed by flowing compressed air at a pressure ranging from about 0.01 MPa to about 0.5 MPa.

[0103] For example, the electrospinning process can be performed two or more times.

[0104] Since nanofibers are formed through electrospinning, the resulting nanofibers can possess a three-dimensional network structure. Because the coating layer is formed via electrospinning, the solvent can easily evaporate, thus better reducing or suppressing springback that causes electrode damage, which is advantageous.

[0105] Next, the coating layer formed by electrospinning can be heat-treated at a temperature ranging from about 200°C to about 500°C to form a diaphragm. Through heat treatment, the polyamic acid included in the coating layer can be thermally imidized to produce polyimide nanofibers.

[0106] For example, the heat treatment temperature can be in the range of about 200°C to about 500°C (e.g., about 300°C to about 500°C, about 200°C to about 400°C, or about 300°C to about 400°C). When the above numerical range is met, a diaphragm with desired or improved mechanical strength, flame retardant properties, and fire extinguishing properties can be achieved without deforming the diaphragm.

[0107] After the separator is formed, further rolling can be performed. The rolling process can be carried out at a temperature ranging from about 25°C to about 110°C. If further rolling is performed (when further rolling is performed), the separator can be compressed to shorten the Li ion migration path, which can facilitate lithium ion movement during charging and discharging.

[0108] Next, the release film can be removed (peeled) from the manufactured separator to produce a separator for rechargeable lithium batteries in the form of a self-standing membrane.

[0109] According to some example embodiments, a method for manufacturing a separator for a rechargeable lithium battery includes: (1) preparing a first electrospinning solution comprising polyamic acid and a first solvent and a second electrospinning solution comprising a polyphosphate compound and a second solvent; (2) alternately electrospinning the first electrospinning solution and the second electrospinning solution onto a release film to form a coating layer; (3) heat-treating the coating layer at a temperature in the range of about 200°C to about 500°C; and (4) removing (peeling off) the release film from the separator.

[0110] The separator manufactured by this manufacturing method may be or include a separator 30B for rechargeable lithium batteries having the above-described multilayer structure.

[0111] A first electrospinning solution can be prepared by mixing polyamic acid and a first solvent, and a second electrospinning solution can be prepared by mixing polyamic acid, a polyphosphate compound, and a second solvent. Alternatively, the first and second electrospinning solutions can be optionally prepared by further comprising the heat-resistant polymer as described above.

[0112] The first solvent and the second solvent may include at least one of dimethylacetamide, N-methylpyrrolidone, dimethylformamide, dimethyl sulfoxide, acetone, or combinations thereof.

[0113] For example, based on the total amount of polyamic acid and polyphosphate compound in the second electrospinning solution of 100 wt%, polyamic acid may be included in an amount ranging from about 25 wt% to about 80 wt% (e.g., about 30 wt% to about 75 wt%, about 40 wt% to about 75 wt%, or about 50 wt% to about 75 wt%).

[0114] For example, based on a total of 100 wt% of polyamic acid and polyphosphate compound in the second electrospinning solution, the polyphosphate compound can be included in an amount greater than about 20 wt% and less than about 75 wt% (e.g., in the range of about 22.5 wt% to about 70 wt%, about 25 wt% to about 65 wt%, about 25 wt% to about 60 wt%, or about 25 wt% to about 50 wt%). When the above numerical range is met, a separator for rechargeable lithium batteries with desired or improved mechanical strength (such as flexibility) as well as flame retardant and fire extinguishing properties can be manufactured.

[0115] Next, electrospinning of the first electrospinning solution and the second electrospinning solution prepared above are alternately performed on the release film to form a coating layer.

[0116] Figure 7 This is a schematic diagram illustrating an electrospinning apparatus used to manufacture multilayer separators for rechargeable lithium batteries. Figure 7 In the example shown, the electrospinning apparatus includes three supply devices, but depending on the desired number of diaphragm layers, it may include more or fewer than three supply devices.

[0117] Reference Figure 7 The electrospinning apparatus may include a first supply device 1, a second supply device 2, and a third supply device 3 arranged sequentially along the direction of travel, and the first supply device 1, the second supply device 2, and the third supply device 3 may include a tip having an aperture size in the range of 1 to 1000 in the range of about 15G to about 30G.

[0118] The electrospinning apparatus may also include collecting rollers arranged at a given interval at the lower part of the supply device and release films placed on the collecting rollers.

[0119] The first electrospinning solution or the second electrospinning solution can be filled into the first supply device 1, the second supply device 2 and the third supply device 3.

[0120] In addition, when the first electrospinning solution or the second electrospinning solution filled in the first supply device 1, the second supply device 2 and the third supply device 3 are alternately electrospinned on the release film in the direction of travel of the electrospinning device, a coating layer with a multilayer structure can be manufactured.

[0121] Since the conditions for other electrospinning processes are the same as those described above, detailed descriptions of them are omitted here.

[0122] Next, methods for manufacturing the diaphragm may include: heat-treating the coating layer at a temperature in the range of about 200°C to about 500°C to form the diaphragm; and removing the release film from the diaphragm. Since these processes are described identically to those described above, detailed descriptions thereof are omitted here.

[0123] According to some example embodiments, a method for manufacturing a separator for a rechargeable lithium battery includes: (1) preparing a first electrospinning solution comprising polyamic acid and a first solvent, a second electrospinning solution comprising polyamic acid, a polyphosphate compound, and a second solvent, and a third electrospinning solution comprising a polyphosphate compound and a third solvent; (2) electrospinning two of the first, second, and third electrospinning solutions onto a release film using coaxial double tips to form a coating layer; (3) heat-treating the coating layer at a temperature in the range of about 200°C to about 500°C; and (4) removing (peeling off) the release film from the separator.

[0124] The separator manufactured by this manufacturing method may be or include separators 30C and / or 30C' for rechargeable lithium batteries having a single-layer or multi-layer structure including the core-shell structure described above.

[0125] A first electrospinning solution can be prepared by mixing polyamic acid and a first solvent; a second electrospinning solution can be prepared by mixing polyamic acid, a polyphosphate compound, and a second solvent; and a third electrospinning solution can be prepared by mixing a polyphosphate compound and a third solvent.

[0126] Alternatively, the first electrospinning solution, the second electrospinning solution, and the third electrospinning solution may be prepared by further comprising the heat-resistant polymer as described above.

[0127] The first solvent, the second solvent, and the third solvent may include at least one of dimethylacetamide, N-methylpyrrolidone, dimethylformamide, dimethyl sulfoxide, acetone, or combinations thereof.

[0128] For example, based on a total of 100 wt% of the amount of polyamic acid and polyphosphate compound in two of the electrospinning solutions, including the first, second, and third electrospinning solutions, the polyphosphate compound may be included in an amount greater than about 20 wt% and less than about 75 wt%, and may be included in an amount ranging from about 22.5 wt% to about 70 wt%, about 25 wt% to about 65 wt%, about 25 wt% to about 60 wt%, or about 25 wt% to about 50 wt%.

[0129] For example, based on the total amount of polyamic acid and polyphosphate compound in two electrospinning solutions including the first electrospinning solution, the second electrospinning solution, and the third electrospinning solution, which is 100 wt%, polyamic acid may be included in an amount ranging from about 25 wt% to about 80 wt% (e.g., about 30 wt% to about 75 wt%, about 40 wt% to about 75 wt%, or about 50 wt% to about 75 wt%).

[0130] If the above range is met (when the above range is met), a separator for rechargeable lithium batteries with desired or improved mechanical strength (such as flexibility) and desired or improved flame retardant and fire extinguishing properties can be achieved.

[0131] Next, a coating layer can be formed by electrospinning two of the first, second, and third electrospinning solutions onto the release film using coaxial double tips.

[0132] For example, this process can be performed using coaxial double tips, which can consist of or include an inner tip and an outer tip, arranged around an inner needle based on the same central axis. The electrospinning solution injected into the inner tip can form a core-shell structure after electrospinning, and the electrospinning solution injected into the outer tip can form a core-shell structure after electrospinning.

[0133] For example, one of the first, second, and third electrospinning solutions can be injected into the outer tip, and another of the remaining electrospinning solutions can be injected into the inner tip. For example, the electrospinning solutions injected into the outer tip and the electrospinning solutions injected into the inner tip can be different from each other.

[0134] As an example, a first electrospinning solution can be injected into the inner tip, and a third electrospinning solution can be injected into the outer tip.

[0135] If electrospinning is performed using a coaxial double tip comprising an inner tip filled with a first electrospinning solution and an outer tip filled with a third electrospinning solution (when electrospinning is performed using a coaxial double tip comprising an inner tip filled with a first electrospinning solution and an outer tip filled with a third electrospinning solution), a diaphragm comprising a core-shell structure comprising a core containing a polyimide resin and a shell disposed on the surface of the core and comprising a polyphosphate compound.

[0136] As another example, it can be used according to the above-mentioned principles. Figure 7 The electrospinning apparatus manufactures a diaphragm 30C' comprising two or more stacked nanofiber layers, the nanofiber layers including nanofibers with a core-shell structure.

[0137] For example, the tips included in the first supply device 1, the second supply device 2, and the third supply device 3 may be or include the aforementioned coaxial double tips.

[0138] When using an electrospinning device, it is possible to manufacture products such as... Figure 6 The membrane 30C' shown is a rechargeable lithium battery in which the core-shell structure is stacked in multiple layers.

[0139] Since the conditions for other electrospinning processes are the same as those described above, detailed descriptions of them are omitted below.

[0140] Next, methods for manufacturing the diaphragm may include: heat-treating the coating layer at a temperature in the range of about 200°C to about 500°C to form the diaphragm; and removing the release film from the diaphragm. Since these processes are described identically to those described above, detailed descriptions thereof are omitted here.

[0141] Rechargeable lithium batteries Some example embodiments include a rechargeable lithium battery comprising a positive electrode, a negative electrode, and a separator between the positive and negative electrodes.

[0142] Because rechargeable lithium batteries include the aforementioned separator, they have desired or improved thermal stability and desired or improved charge / discharge characteristics.

[0143] Rechargeable lithium batteries can be classified according to their shape, such as cylindrical, prismatic, pouch-shaped, and coin-shaped. Figures 8 to 11 This is a schematic diagram illustrating a rechargeable lithium battery according to some example embodiments. Figure 8 A cylindrical battery is shown. Figure 9 A square battery is shown. Figure 10 and Figure 11 A pouch-type battery is shown. (See reference.) Figures 8 to 11 The rechargeable lithium battery 100 includes an electrode assembly 40 and a housing 50. The electrode assembly 40 has a separator 30 between a positive electrode 10 and a negative electrode 20, and the electrode assembly 40 is housed within the housing 50. The positive electrode 10, the negative electrode 20, and the separator 30 may be impregnated with an electrolyte (not shown). Figure 8 As shown, the rechargeable lithium battery 100 may include a sealing member 60 of the sealed housing 50.

[0144] exist Figure 9 In this context, the rechargeable lithium battery 100 may include a positive electrode lead connector 11, a positive electrode terminal 12 connected to the positive electrode lead connector 11, a negative electrode lead connector 21, and a negative electrode terminal 22 connected to the negative electrode lead connector 21. For example... Figure 10 and Figure 11 As shown, the rechargeable lithium battery 100 may include Figure 11 The electrode terminals 70 shown in the figure or Figure 10 The positive electrode terminal 71 and negative electrode terminal 72 shown in the figure form an electrical path for guiding the current formed in the electrode assembly 40 to the outside of the rechargeable lithium battery 100.

[0145] Rechargeable lithium batteries according to some example embodiments can be used in, for example, automobiles, mobile phones and / or various types of electrical devices, but this disclosure is not limited thereto.

[0146] The remaining components of a rechargeable lithium battery, excluding the separator, are described in detail below.

[0147] positive electrode The positive electrode for a rechargeable lithium battery may include a current collector and a layer of positive electrode active material formed on the current collector. The positive electrode active material layer includes positive electrode active material and may also include a binder and / or a conductive material.

[0148] For example, the positive electrode may also include additives that can constitute a sacrificial positive electrode.

[0149] As the positive electrode active material, compounds capable of intercalating and deintercalating lithium (lithiation intercalation compounds) can be used. For example, one or more composite oxides of lithium with metals (such as or including at least one of cobalt, manganese, nickel and combinations thereof) can be used.

[0150] The composite oxide can be or includes lithium transition metal composite oxides, and examples of such composite oxides can include at least one of lithium nickel oxides, lithium cobalt oxides, lithium manganese oxides, lithium iron phosphate compounds, cobalt-free lithium nickel manganese oxides, or combinations thereof.

[0151] As an example, a compound represented by any of the following chemical formulas can be used. Li a A 1-b X b O 2-c D c (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05); Li a Mn 2-b X b O 4-c D c (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05); Li a Ni 1-b-c Co b X c O 2-α D α (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<α<2); Li a Ni 1-b- c Mn b X c O 2-α D α (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<α<2); Li a Ni b Co c L 1 d G e O2 (0.90≤a≤1.8, 0≤b≤0.9, 0≤c≤0.5, 0≤d≤0.5, 0≤e≤0.1); Li a NiG b O2 (0.90≤a≤1.8, 0.001≤b≤0.1); Li a CoG b O2 (0.90≤a≤1.8, 0.001≤b≤0.1); Li a Mn 1-b G b O2 (0.90≤a≤1.8, 0.001≤b≤0.1); Li a Mn2G b O4 (0.90≤a≤1.8, 0.001≤b≤0.1); Li a Mn1-g G g PO4 (0.90≤a≤1.8, 0≤g≤0.5); Li (3-f) Fe2(PO4)3 (0≤f≤2); Li a FePO4 (0.90≤a≤1.8).

[0152] In the above chemical formula, A is or includes at least one of Ni, Co, Mn, or combinations thereof; X is or includes at least one of Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, rare earth elements, or combinations thereof; D is or includes at least one of O, F, S, P, or combinations thereof; G is or includes at least one of Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, or combinations thereof; and L 1 It is or includes at least one of Mn, Al, or combinations thereof.

[0153] For example, the positive electrode active material can be or includes a high-nickel positive electrode active material, in which, based on 100 mol% of the metals other than lithium in the lithium transition metal composite oxide, the nickel content is greater than or equal to about 80 mol%, greater than or equal to about 85 mol%, greater than or equal to about 90 mol%, greater than or equal to about 91 mol%, or greater than or equal to about 94 mol% and less than or equal to about 99 mol%. High-nickel positive electrode active materials can achieve high capacity and can be applied to high-capacity, high-density rechargeable lithium batteries.

[0154] Based on a 100wt% positive electrode active material layer, the amount of positive electrode active material can be in the range of about 90wt% to about 99.5wt%, and based on a 100wt% positive electrode active material layer, the amount of each of the binder and conductive material can be independently in the range of about 0.5wt% to about 5wt%.

[0155] The binder causes the positive electrode active material particles to adhere to each other and to adhere the positive electrode active material to the current collector. Examples of binders may include at least one of, but are not limited to, polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers including ethylene oxide, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, (meth)acrylated styrene-butadiene rubber, epoxy resin, (meth)acrylate resin, polyester resin, nylon, etc.

[0156] The conductive material can impart conductivity to the electrode, and any material that does not cause adverse chemical changes and conducts electrons can be used in the battery. Examples of the conductive material may include: carbon-based materials, such as at least one of natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, carbon nanofiber and carbon nanotube; metal-based materials, containing at least one of copper, nickel, aluminum, silver and the like, in the form of metal powder or metal fiber; conductive polymers, such as polyphenylene derivatives; or mixtures thereof.

[0157] Al can be used for the current collector, but the current collector is not limited thereto.

[0158] negative electrode A negative electrode for a rechargeable lithium battery includes a current collector and a negative electrode active material layer on the current collector. The negative electrode active material layer may include a negative electrode active material, and may further include a binder and / or a conductive material.

[0159] The negative electrode active material may include at least one of a material capable of reversibly intercalating / deintercalating lithium ions, lithium metal, a lithium metal alloy, a material capable of doping / dedoping lithium, or a transition metal oxide.

[0160] The material capable of reversibly intercalating / deintercalating lithium ions may include a carbon-based negative electrode active material, for example, crystalline carbon, amorphous carbon, or a combination thereof. The crystalline carbon may be graphite, such as amorphous, flake-like, platelet-like, spherical or fibrous natural graphite or artificial graphite, and the amorphous carbon may be or include at least one of soft carbon, hard carbon, mesophase pitch carbonization product, calcined coke and the like.

[0161] The lithium metal alloy includes an alloy of lithium and a metal (including at least one of Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al and Sn).

[0162] The material capable of doping / dedoping lithium may be or include a Si-based negative electrode active material or a Sn-based negative electrode active material. The Si-based negative electrode active material may include silicon, silicon-carbon composite, SiO x (0<x≤2), a Si-Q alloy (where Q is or includes at least one of an alkali metal, an alkaline earth metal, a Group 13 element, a Group 14 element (other than Si), a Group 15 element, a Group 16 element, a transition metal, a rare earth element, and combinations thereof), or at least one of combinations thereof. The Sn-based negative electrode active material may be or include at least one of Sn, SnO₂, a Sn-based alloy, or a combination thereof.

[0163] Silicon-carbon composites can be or include composites of silicon and amorphous carbon. According to some example embodiments, the silicon-carbon composite can be in the form of silicon particles and amorphous carbon coated on the surface of the silicon particles. For example, the silicon-carbon composite can include secondary particles (cores) assembled from primary silicon particles and an amorphous carbon coating (shell) on the surface of the secondary particles. Amorphous carbon can also be present between the primary silicon particles; for example, the primary silicon particles can be coated with amorphous carbon. The secondary particles can be dispersed in an amorphous carbon matrix.

[0164] Silicon-carbon composites may also include crystalline carbon. For example, a silicon-carbon composite may include a core comprising crystalline carbon and silicon particles, and an amorphous carbon coating layer on the surface of the core.

[0165] Si-based or Sn-based negative electrode active materials can be mixed with carbon-based negative electrode active materials.

[0166] For example, the negative electrode active material layer may include a negative electrode active material ranging from about 90 wt% to about 99 wt%, a binder ranging from about 0.5 wt% to about 5 wt%, and a conductive material ranging from about 0 wt% to about 5 wt%.

[0167] The binder causes the negative electrode active material particles to adhere to each other and to adhere the negative electrode active material to the current collector. The binder may include at least one of non-aqueous binders, aqueous binders, dry binders, or combinations thereof.

[0168] Non-aqueous adhesives may include at least one of polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene-propylene copolymer, polystyrene, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamide-imide, polyimide, or combinations thereof.

[0169] The waterborne adhesive may be or include at least one of styrene-butadiene rubber, (meth)acrylated styrene-butadiene rubber, (meth)acrylonitrile-butadiene rubber, (meth)acrylic rubber, butyl rubber, fluororubber, polyethylene oxide, polyvinylpyrrolidone, polyepoxychloropropane, polyphosphazene, poly(meth)acrylonitrile, ethylene propylene diene copolymer, polyvinylpyridine, chlorosulfonated polyethylene, latex, polyester resin, (meth)acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol, and combinations thereof.

[0170] When an aqueous binder is used as the negative electrode binder, it may further include a cellulose compound capable of imparting viscosity. The cellulose compound may include at least one of carboxymethyl cellulose, hydroxypropyl methyl cellulose, methyl cellulose, or an alkali metal salt thereof. The alkali metal may include at least one of Na, K, or Li.

[0171] The dry adhesive may be or include a polymeric material capable of being fibrous, and may be or include at least one of, for example, polytetrafluoroethylene, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyethylene oxide, or combinations thereof.

[0172] Conductive materials are included to provide electrode conductivity, and any electrically conductive material can be used as a conductive material unless it causes an adverse chemical change in the battery. Examples of conductive materials include: carbon-based materials, such as at least one of natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, carbon nanofiber, carbon nanotube, etc.; metallic materials such as metal powders or metal fibers, including at least one of copper, nickel, aluminum, silver, etc.; conductive polymers, such as polyphenylene derivatives; or mixtures thereof.

[0173] The negative electrode current collector may include at least one of copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, polymer substrate coated with a conductive metal, and combinations thereof.

[0174] electrolyte Electrolytes used in rechargeable lithium batteries include non-aqueous organic solvents and lithium salts.

[0175] Non-aqueous organic solvents constitute the medium for transporting ions that participate in the electrochemical reactions of the battery.

[0176] Non-aqueous organic solvents may be or include at least one of carbonate solvents, ester solvents, ether solvents, ketone solvents, alcohol solvents, aprotic solvents, or combinations thereof.

[0177] Carbonate solvents may include at least one of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), methyl ethyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), and butyl carbonate (BC). Esters may include at least one of methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, decanolactone, mevalonolactone, valproic acid lactone, caprolactone, etc. Ether solvents may include at least one of dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, dimethoxyethane, 2-methyltetrahydrofuran, 2,5-dimethyltetrahydrofuran, tetrahydrofuran, etc. Additionally, ketone solvents may include cyclohexanone, etc. Alcohol solvents may include at least one of ethanol and isopropanol. Aprotic solvents may include at least one of the following: nitriles, such as R-CN (wherein R is a C2 to C20 straight-chain, branched or cyclic hydrocarbon group, and may include double bonds, aromatic rings or ether groups, etc.); amides, such as dimethylformamide; dioxolane, such as 1,3-dioxolane, 1,4-dioxolane, etc.; sulfolane, etc.

[0178] Non-aqueous organic solvents can be used alone or in mixtures of two or more types of solvents.

[0179] If a carbonate solvent is used (when using a carbonate solvent), cyclic carbonates and chain carbonates can be mixed together, and cyclic carbonates and chain carbonates can be mixed in a volume ratio ranging from about 1:1 to about 1:9.

[0180] Lithium salts dissolved in organic solvents supply lithium ions in batteries, enabling basic operation of rechargeable lithium batteries and improving lithium ion transport between the positive and negative electrodes. Examples of lithium salts include LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiAlO2, LiAlCl4, LiPO2F2, LiCl, LiI, LiN(SO3C2F5)2, Li(FSO2)2N (lithium bis(fluorosulfonyl)imide; LiFSI), LiC4F9SO3, LiN(C x F 2x+1 SO2)(C y F 2y+1 At least one of the following: (SO2) (where x and y are integers in the range of 1 to 20), lithium trifluoromethane sulfonate, lithium tetrafluoroethane sulfonate, lithium difluorobis(oxalate)phosphate (LiDFBOP), lithium difluoro(oxalate)borate (LiDFOB), and lithium bis(oxalate)borate (LiBOB).

[0181] Examples and comparative examples of this disclosure are described below. However, these examples should not in any sense be construed as limiting the scope of the disclosure.

[0182] Example: (1) Single-layer diaphragm Example 1-1 By using polyamic acid, ammonium polyphosphate (APP, M) w The electrospinning solution was prepared by mixing polyamic acid (90,000 g / mol) and dimethylacetamide solvent. Based on the total amount of polyamic acid and ammonium polyphosphate (100 wt%), polyamic acid was included in 75 wt% and ammonium polyphosphate in 25 wt%.

[0183] Subsequently, the electrospinning solution is electrospinned onto the release film to form a coating layer. Electrospinning is performed under the following conditions.

[0184] Electrospinning was performed at 26°C and 50% relative humidity by positioning a nozzle assembly consisting of 52 tips with a 25G orifice size 15 cm apart from a collecting roller, adding electrospinning solution to the tips, and applying a voltage of 40 kV to 50 kV. The collecting roller was set to a speed of 50 to 300 mpm, and the electrospinning solution was adjusted to discharge from the tips at a solids content of 150 μL / min. Electrospinning was also performed by introducing compressed air at a pressure of 0.1 MPa.

[0185] Subsequently, the coating layer is heat-treated at 400°C to form a diaphragm, from which the release film is removed to obtain a diaphragm (thickness = 10 μm) according to Example 1-1.

[0186] The final membrane comprises nanofibers (average diameter = 200 nm) and, based on 100 wt% of the membrane, comprises 75 wt% polyimide resin (PI) and 25 wt% ammonium polyphosphate (APP).

[0187] Example 1-2 and Comparative Examples 1-1 to 1-5 Except for adjusting the mixing amounts of polyamic acid and ammonium polyphosphate to prepare an electrospinning solution with the composition shown in Table 1 below, the membrane is manufactured in essentially the same manner as in Example 1-1.

[0188] (2) 3-layer diaphragm Example 2-1 In addition to filling the electrospinning solution of Example 1-1 into the solution according to... Figure 7 In the first, second, and third supply devices of the electrospinning apparatus, electrospinning is then performed on the release film under the same electrospinning conditions as in Example 1-1, in addition to electrospinning on the release film in a manner substantially the same as in Example 1-1.

[0189] Example 2-2 Except for using the electrospinning solution of Example 1-2, a membrane with a 3-layer structure is manufactured in essentially the same manner as in Example 2-1.

[0190] Example 2-6 The first electrospinning solution was prepared by mixing polyamic acid and dimethylacetamide solvent, and by mixing polyamic acid and ammonium polyphosphate (M... wThe second electrospinning solution is prepared by mixing polyamic acid (60,000 g / mol) and dimethylacetamide solvent. At this point, based on a total amount of 100 wt% of polyamic acid and ammonium polyphosphate in the second electrospinning solution, polyamic acid comprises 75 wt% and ammonium polyphosphate comprises 25 wt%.

[0191] Subsequently, the second electrospinning solution was filled into Figure 7 The electrospinning apparatus shown includes a first supply device and a third supply device, and the first electrospinning solution is filled in... Figure 7 In the second supply device of the electrospinning apparatus shown.

[0192] Next, except that electrospinning is performed on the release film under the same electrospinning conditions as in Example 1-1, a diaphragm with a 3-layer structure is manufactured in a manner substantially the same as in Example 1-1.

[0193] In the three-layer membranes of Examples 2-6, each layer has the composition shown in Table 3.

[0194] Examples 2-7 and 2-8 Except for adjusting the mixing amounts of polyamic acid and ammonium polyphosphate to prepare a second electrospinning solution having the composition shown in Table 3, the diaphragm is manufactured in essentially the same manner as in Examples 2-6.

[0195] Example 2-9 Except that the first electrospinning solution is filled into the first and third supply devices of the electrospinning apparatus and the second electrospinning solution is filled into the second supply device of the electrospinning apparatus, the diaphragm is manufactured in a manner substantially the same as that in Examples 2-6.

[0196] Examples 2-10 and 2-11 Except for adjusting the mixing amounts of polyamic acid and ammonium polyphosphate to prepare a second electrospinning solution having the composition shown in Table 3 below, the membrane is manufactured in essentially the same manner as in Examples 2-9.

[0197] (3) Core-shell membrane Example 3-1 The first electrospinning solution was prepared by mixing polyamic acid and dimethylacetamide solvent, and by mixing ammonium polyphosphate (M... w The third electrospinning solution was prepared by mixing a solvent of 90,000 g / mol and dimethylacetamide.

[0198] Based on a total of 100 wt% of the amount of polyamic acid and ammonium polyphosphate included in the first and third electrospinning solutions, polyamic acid is included in 75 wt% and ammonium polyphosphate is included in 25 wt%.

[0199] Next, the diaphragm is manufactured in essentially the same manner as in Example 1-1, except that electrospinning is performed using a coaxial double tip consisting of an inner tip and an outer tip (the inner tip and the outer tip are arranged around the inner needle based on the same central axis) instead of the tip used in the electrospinning of Example 1-1.

[0200] Specifically, the inner tip is filled with a first electrospinning solution, and the outer tip is filled with a third electrospinning solution.

[0201] The final membrane produced comprises nanofibers (average diameter = 150 nm) and is fabricated in the form of a core-shell structure, in which the core comprises polyimide resin (PI) and the shell is disposed on the surface of the core and comprises ammonium polyphosphate (APP).

[0202] Based on 100 wt% of the separator, it includes 75 wt% polyimide resin (PI) and 25 wt% ammonium polyphosphate (APP).

[0203] Example 3-2 In addition to using a supply device including coaxial double tips as in Example 3-1, by using according to Figure 7 The electrospinning apparatus uses the first, second, and third supply devices to electrospin in a manner substantially the same as that in Example 3-1 to manufacture a diaphragm with a three-layer structure.

[0204] Example 3-3 Except for adjusting the amounts of polyamic acid and ammonium polyphosphate during the preparation of the electrospinning solution to produce a diaphragm having the composition shown in Table 4 below, the diaphragm is manufactured in essentially the same manner as in Example 3-1.

[0205] Example 3-4 Except for adjusting the amounts of polyamic acid and ammonium polyphosphate during the preparation of the electrospinning solution to produce a diaphragm having the composition shown in Table 4 below, the diaphragm is manufactured in essentially the same manner as in Example 3-2.

[0206] Evaluation example: Evaluation Example 1: Evaluation of tensile strength and elongation The tensile strength and elongation of the diaphragms according to the example and comparative examples were measured using a universal testing machine (UTM) according to ASTM D882, and the results are shown in Tables 1 through 4 below.

[0207] Evaluation Example 2: Evaluation of the thermal exposure characteristics of a single battery cell The separators according to the example and comparative examples are used to manufacture rechargeable lithium battery cells.

[0208] A positive electrode active material slurry was prepared by mixing 96 wt% LiCoO2, 2 wt% Ketjen black, and 2 wt% polyvinylidene fluoride in an N-methylpyrrolidone solvent. The positive electrode active material slurry was coated onto an Al current collector, then dried and compressed to fabricate the positive electrode.

[0209] A negative electrode active material slurry was prepared by mixing 97.5 wt% artificial graphite, 1.0 wt% carboxymethyl cellulose, and 1.5 wt% styrene-butadiene rubber (SBR) in an aqueous solvent. The negative electrode active material slurry was coated onto a copper current collector, then dried and compressed to fabricate the negative electrode.

[0210] Between the manufactured positive and negative electrodes, each of the separators according to the example and comparative example is set, and then an electrolyte prepared by dissolving LiPF6 in a mixed solvent of ethylene carbonate and ethyl methyl carbonate (volume ratio of 50:50) is injected into it to manufacture a rechargeable lithium battery cell.

[0211] Each rechargeable lithium-ion battery cell was fully charged to SOC 100, and then its thermal exposure characteristics were evaluated.

[0212] Each of the rechargeable lithium battery cells was placed in a room and its temperature was increased from room temperature (25°C) to 137°C, 140°C, and 143°C at a rate of 7°C / min, and then maintained at that temperature for 1 hour. The changes in the batteries were then examined.

[0213] While maintaining the temperature, if thermal runaway does not occur (when thermal runaway does not occur), "OK" is given; however, if thermal runaway occurs rapidly when exposed to high temperature (when thermal runaway occurs rapidly when exposed to high temperature), "NG" is given. The results are shown in Tables 1 to 4 below.

[0214] Table 1:

[0215] Table 2:

[0216] Table 3:

[0217] Table 4:

[0218] Referring to Table 1, even when the temperature rises to 143°C, Examples 1-1 and 1-2 do not exhibit thermal runaway. However, Comparative Example 1-1, excluding APP, shows thermal runaway at 140°C, and Comparative Example 1-2, excluding PI, shows thermal runaway from 137°C.

[0219] In addition, comparative examples 1-3, which included less than expected amounts of APP, showed thermal runaway at 143°C, and comparative examples 1-4 and 1-5, which included more than expected amounts of APP, showed thermal runaway at 143°C and 140°C, respectively.

[0220] Furthermore, referring to Table 1, comparative examples 1-2 excluding PI show that the diaphragms exhibit deteriorated tensile strength and elongation compared to the examples. Additionally, comparative examples 1-4 and 1-5 including an excessive amount of APP (beyond the expected amount) show that the diaphragms exhibit deteriorated tensile strength and elongation compared to the examples.

[0221] Referring to Table 2, when a 100 wt% monolayer membrane includes 25 wt% (Example 2-1) and 50 wt% (Example 2-2) of APP, the most desired or improved heat exposure characteristics, as well as the tensile strength and elongation, are achieved.

[0222] Referring to Table 3, Examples 2-6, 2-7, 2-9, and 2-10, which include the desired amount of APP, exhibit the most desired or improved heat exposure properties, as well as the desired or improved tensile strength and elongation.

[0223] On the other hand, Examples 2-8 exhibit slightly deteriorated heat exposure characteristics, and Examples 2-8 and 2-11, which include more APP than expected, show that the diaphragm exhibits slightly deteriorated tensile strength.

[0224] Referring to Table 4, Examples 3-1 to 3-4, which include the desired amount of APP, exhibit the most desired or improved heat exposure properties as well as the desired or improved tensile strength and elongation.

[0225] While this disclosure has been described in conjunction with what are now considered to be exemplary embodiments, it will be understood that the disclosure is not limited to the disclosed embodiments, but rather is intended to cover various modifications and equivalent arrangements included within the spirit and scope of the appended claims.

[0226] Description of reference numerals in the attached figures: 100: Rechargeable lithium battery; 10: Positive electrode 11: Positive electrode lead connector 12: Positive electrode terminal 20: Negative electrode 21: Negative electrode lead connector 22: Negative electrode terminal 30, 30A, 30B, 30C, 30C': Diaphragm a: Core b: Shell 31, 31': First nanofiber layer; 32, 32': Second nanofiber layer 33, 33': Third nanofiber layer 1: First supply device 2: Second supply device; 3: Third supply device 40: Electrode assembly; 50: Housing 60: Sealing component; 70: Electrode terminal piece 71: Positive electrode connector; 72: Negative electrode connector.

Claims

1. A separator for a rechargeable lithium battery, the separator comprising: Nanofibers, wherein the nanofibers comprise polyimide resin and polyphosphate compound; and Based on 100 wt% of the membrane, the polyphosphate compound is included in an amount greater than 20 wt% and less than 75 wt%.

2. The diaphragm according to claim 1, wherein, Based on 100 wt% of the membrane, the polyphosphate compound is included in an amount ranging from 25 wt% to 50 wt%.

3. The diaphragm according to claim 1, wherein: The polyphosphate compound includes at least one of monovalent organic cations, monovalent metal cations, and combinations thereof; The monovalent organic cation includes at least one of ammonium cations, melamine cations, guanidinium cations, and combinations thereof; and The monovalent metal cation includes Li + Na + K + and at least one of their combinations.

4. The diaphragm according to claim 1, wherein, The polyphosphate compounds include at least one of ammonium polyphosphate, melamine polyphosphate, and combinations thereof.

5. The diaphragm according to claim 1, wherein, The average diameter of the nanofibers is in the range of 10 nm to 300 nm.

6. The diaphragm according to claim 1, wherein, The thickness of the diaphragm is in the range of 1 μm to 30 μm.

7. A separator for a rechargeable lithium battery, the separator comprising: The invention comprises multiple nanofiber layers, wherein the multiple nanofiber layers comprise a polyimide resin; and At least one of the plurality of nanofiber layers also includes a polyphosphate compound.

8. The diaphragm according to claim 7, wherein, The nanofiber layer, which includes the polyphosphate compound at 100 wt%, comprises the polyphosphate compound in an amount greater than 20 wt% and less than 75 wt%.

9. The diaphragm according to claim 7, wherein, Based on 100 wt% of the membrane, the polyphosphate compound is included in an amount greater than or equal to 8 wt% and less than 75 wt%.

10. The diaphragm according to claim 7, wherein: The polyphosphate compound includes at least one of monovalent organic cations, monovalent metal cations, and combinations thereof; The monovalent organic cation includes at least one of ammonium cations, melamine cations, guanidinium cations, and combinations thereof; and The monovalent metal cation includes Li + Na + K + and at least one of their combinations.

11. The diaphragm according to claim 7, wherein, The polyphosphate compounds include at least one of ammonium polyphosphate, melamine polyphosphate, and combinations thereof.

12. The diaphragm according to claim 7, wherein, The average diameter of the nanofibers is in the range of 10 nm to 300 nm.

13. The diaphragm according to claim 7, wherein, The thickness of the nanofiber layer is in the range of 1 μm to 30 μm.

14. The diaphragm according to claim 7, wherein, The thickness of the diaphragm is in the range of 1 μm to 50 μm.

15. A separator for a rechargeable lithium battery, the separator comprising: Nanofibers having a core-shell structure, wherein the core-shell structure comprises a core and a shell on the surface of the core; wherein: Both the core and the shell independently comprise at least one of a polyimide resin, a polyphosphate compound, and a mixture of the polyimide resin and the polyphosphate compound; and The core and the shell comprise different compounds.

16. The diaphragm according to claim 15, wherein, Based on 100 wt% of the membrane, the polyphosphate compound is included in an amount greater than 20 wt% and less than 75 wt%.

17. The diaphragm according to claim 15, wherein: The polyphosphate compound includes at least one of monovalent organic cations, monovalent metal cations, and combinations thereof; The monovalent organic cation includes at least one of ammonium cations, melamine cations, guanidinium cations, and combinations thereof; and The monovalent metal cation includes Li + Na + K + and at least one of their combinations.

18. The diaphragm according to claim 15, wherein, The polyphosphate compounds include at least one of ammonium polyphosphate, melamine polyphosphate, and combinations thereof.

19. The diaphragm according to claim 15, wherein, The average diameter of the nanofibers is in the range of 10 nm to 300 nm.

20. The diaphragm according to claim 15, wherein, The thickness of the diaphragm is in the range of 1 μm to 50 μm.

21. The diaphragm according to claim 15, wherein, The membrane comprises two or more stacked nanofiber layers, each nanofiber having the core-shell structure.

22. A rechargeable lithium battery, said rechargeable lithium battery comprising: Positive electrode; negative electrode; as well as The diaphragm according to any one of claims 1 to 21 is located between the positive electrode and the negative electrode.