A separator for rechargeable lithium batteries and a rechargeable lithium battery including the separator.

By using nanofiber separators, which are composed of polyimide resin and meta-aramid resin, the problems of insufficient stability and mechanical strength of existing lithium battery separators at high temperatures are solved, and high energy density and high capacity rechargeable lithium battery performance are achieved.

CN123121072APending Publication Date: 2026-11-17SAMSUNG SDI CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610615128.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2026-04-23
Filing Date
2026-05-07
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing rechargeable lithium battery separators lack stability and mechanical strength at high temperatures, making it difficult to meet the demands for high energy density and high capacity.

Method used

Nanofiber membranes are used, with nanofibers composed of polyimide resin and meta-aramid resin, which are prepared by electrospinning to form single-layer or multi-layer structures, including core-shell nanofibers, thereby optimizing porosity and mechanical strength.

Benefits of technology

It improves the heat resistance, mechanical strength and thermal stability of the separator, enhances lithium-ion conductivity and air permeability, and meets the requirements of high energy density and high capacity rechargeable lithium batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123121072A_ABST
    Figure CN123121072A_ABST
Patent Text Reader

Abstract

A separator for a rechargeable lithium battery and a rechargeable lithium battery including the separator are provided. The separator comprises nanofibers, wherein the nanofibers comprise polyimide resin and meta-aramid resin, and the content of meta-aramid resin is greater than about 1 wt% and less than about 8 wt% based on 100 wt% of the separator.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] A separator for a rechargeable lithium battery and a rechargeable lithium battery including the separator are disclosed. Background Technology

[0002] With the increasing prevalence of battery-powered electronic devices (such as mobile phones, laptops, and electric vehicles), the demand for rechargeable batteries with high energy density and high capacity is growing. Therefore, improving the performance of rechargeable lithium batteries can be beneficial.

[0003] A rechargeable lithium battery includes a positive electrode and a negative electrode, both containing active materials capable of inserting and deintercalating lithium ions, as well as an electrolyte solution, and generates electrical energy through oxidation and reduction reactions during the insertion / deintercalation of lithium ions at the positive and negative electrodes. Summary of the Invention

[0004] Some example embodiments include separators for rechargeable lithium batteries with desired or improved heat resistance and mechanical strength, as well as optimal, desired or improved porosity.

[0005] Some example embodiments include rechargeable lithium batteries that have desired or improved thermal stability and charge / discharge characteristics by including the separator.

[0006] Some example embodiments include a separator for a rechargeable lithium battery, and the separator includes nanofibers, wherein the nanofibers include polyimide resin and meta-aramid resin, and the content of meta-aramid resin is greater than about 1 wt% and less than about 8 wt% based on 100 wt% of the separator.

[0007] Some example embodiments include a separator for a rechargeable lithium battery, and the separator includes a plurality of nanofiber layers comprising nanofibers, wherein the nanofiber layers comprise a polyimide resin, and at least one of the plurality of nanofiber layers further comprises a meta-aramid resin.

[0008] Some example embodiments include a separator for a rechargeable lithium battery, and the separator includes nanofibers having a core-shell structure, the core-shell structure including a core and a shell located on the surface of the core, the core and shell each independently comprising one of a polyimide resin, a meta-aramid resin, and a mixture of a polyimide resin and a meta-aramid resin, the core and shell comprising different resins.

[0009] Some example embodiments include a rechargeable lithium battery that includes a positive electrode, a negative electrode, and a separator located between the positive and negative electrodes.

[0010] The separator for rechargeable lithium batteries according to some example embodiments has desired or improved heat resistance and mechanical strength, and can exhibit optimal, desired or improved porosity.

[0011] According to some example embodiments, the rechargeable lithium battery includes the separator and has desired or improved thermal stability and charge / discharge characteristics. Attached Figure Description

[0012] Figures 1 to 6 This is a schematic diagram illustrating a separator for a rechargeable lithium battery according to some example embodiments.

[0013] Figure 7 This is a schematic diagram of an electrospinning apparatus for manufacturing multilayer separators for rechargeable lithium batteries.

[0014] Figures 8 to 11 This is a schematic diagram illustrating a rechargeable lithium battery according to some example embodiments. Detailed Implementation

[0015] Example embodiments are described in detail below. However, these embodiments are merely examples, and this disclosure is not limited thereto; rather, it is defined by the scope of the claims.

[0016] As used herein, unless otherwise specifically defined, it is understood that when an element such as a layer, film, region, or substrate is referred to as being “on” another element, the element may be directly on the other element or there may be an intervening element between them.

[0017] As used herein, unless otherwise specifically defined, singular expressions may also include plural expressions. Furthermore, unless otherwise stated, “A or B” may mean “including A, including B, or including both A and B”.

[0018] As used herein, “combination of them” can refer to mixtures of components, laminates, complexes, copolymers, alloys, blends, reaction products, etc.

[0019] As used herein, “thickness” can be measured, for example, with a micrometer or by means of a photograph taken with an optical microscope (such as a scanning electron microscope).

[0020] For example, in this specification, the thickness of the separator or nanofiber layer can be measured by observing a cross-section of a lithium secondary battery or separator using a scanning electron microscope (SEM). In this case, SEM images magnified 1000x to 10000x can be obtained from a region representing the overall cross-sectional thickness of the separator or nanofiber layer. The start and end points for measuring the thickness can be set based on the outermost boundary of the separator or nanofiber layer. As an example, a first virtual tangent line can be drawn on one surface of the separator or nanofiber layer, passing through the vertex of the most convex nanofiber, and the direction perpendicular to the first virtual tangent line can be defined as the thickness measurement direction. The start point can be defined as the outermost convex of the nanofiber located on the first virtual tangent line, and the end point can be defined as the outermost convex of a second virtual tangent line parallel to the first virtual tangent line and contacting another surface opposite to the first surface. The shortest distance between the start and end points set in this way can be determined as the thickness of the separator or nanofiber layer. Measurements can be repeated at 10 or more different points, and the arithmetic mean of the obtained values ​​can be determined as the final thickness.

[0021] Alternatively, in this specification, a micrometer can be used to measure the thickness of the diaphragm or nanofiber layer. In this case, a digital micrometer (MDH-25MC, Mitutoyo Corporation) can be used to measure the thickness of the diaphragm or nanofiber layer itself. Measurements can be repeated at 10 or more different points, and the arithmetic mean of the obtained values ​​can be determined as the final thickness.

[0022] As used herein, the content of components in the diaphragm can be measured using inductively coupled plasma optical emission spectrometry (ICP-OES) or scanning electron microscopy-energy dispersive spectroscopy (SEM-EDS), or can be predicted by the amount of polymer added to the electrospinning solution.

[0023] When the terms “about” or “substantially” are used in conjunction with numerical values ​​in this specification, it is intended that the relevant numerical value includes a tolerance of ±10% around the stated value. When a range is specified, the range includes all values ​​within that range, such as increments of 0.1%.

[0024] Separator for rechargeable lithium batteries In the following text, refer to Figures 1 to 6 A detailed description of a separator for a rechargeable lithium battery according to an example embodiment.

[0025] Figures 1 to 6 This is a schematic diagram illustrating a separator for a rechargeable lithium battery according to some example embodiments.

[0026] Reference Figure 1According to some example embodiments, the separator 30A for a rechargeable lithium battery includes nanofibers, wherein the nanofibers include polyimide resin and meta-aramid resin.

[0027] Polyimide resins can be or include heat-resistant polymers and can be prepared by thermal imidization of a precursor (polyamic acid).

[0028] Because polyimide resins possess desired or improved heat resistance and high-temperature stability, separators for rechargeable lithium batteries incorporating polyimide resins can be stable at high temperatures without shrinkage, compared to conventional polyolefin separators. Furthermore, polyamic acid is soluble in solvents, and its viscosity can be easily controlled, which can be advantageous for electrospinning processes.

[0029] In polyimide resins, polyimides can be obtained by imidizing polyamic acid synthesized from dianhydrides and diamines through a condensation reaction.

[0030] Examples of dianhydrides may include, but are not limited to, at least one of the following: pyromellitic dianhydride (PMDA), 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA), 4,4'-(hexafluoroisopropylidene)diphthalic dianhydride (6FDA), 3,3',4,4'-benzophenone tetracarboxylic dianhydride (BTDA), 1,4,5,8-naphthalenetetracarboxylic dianhydride (NTCDA), 1,2,4,5-cyclohexanetetracarboxylic dianhydride (HPMDA), oxydiphthalic dianhydride (ODPA), benzophenone tetracarboxylic dianhydride, biphenyltetracarboxylic dianhydride, or terphenyltetracarboxylic dianhydride (TPDA).

[0031] Examples of diamines may include, but are not limited to, arylamines (wherein the aryl group may be C6 to C20 aryl), such as, at least one of, diaminodiphenyl ether (ODA), m-phenylenediamine (MDA), m-phenylenediamine (mPDA), p-phenylenediamine (pPDA), 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP), 1,3-bis(3-aminophenoxy)benzene (APB), 3,3'-diaminobenzidine (DAB), or 4,4'-diaminodiphenyl sulfone (DDS).

[0032] For example, based on a 100 wt% separator, the polyimide resin content can be in the range of about 90 wt% to about 99 wt%, for example, about 92 wt% to about 99 wt%, about 93 wt% to about 99 wt%, or about 93 wt% to about 97 wt%. Within the above range, separators with desired or improved mechanical strength and heat resistance can be achieved.

[0033] For example, the weight-average molecular weight (M) of polyimide resins wThe electrospinning strength can be in the range of about 100,000 g / mol to about 300,000 g / mol, for example, about 200,000 g / mol to about 250,000 g / mol. Within the above range, diaphragms with desired or improved electrospinning properties can be achieved.

[0034] Meta-aromatic polyamide resin is an aromatic polyamide with desired or improved heat resistance and chemical stability. Therefore, it is a polymer that is generally stable even at high temperatures greater than or equal to about 400°C, has desired or improved self-extinguishing properties, and is also durable.

[0035] Meta-aromatic polyamide resins can be or include polymers containing amide bonds generated by the reaction between an amino group of an aromatic diamine and an acyl chloride group of a diacyl chloride.

[0036] Examples of aromatic diamines may include, but are not limited to, m-phenylenediamine, 3,3'-diaminodiphenylmethane, 3,4'-diaminodiphenyl ether, and bis(3-aminophenyl) sulfone. Examples of diacyl chlorides may include, but are not limited to, isophthaloyl chloride, terephthaloyl chloride, and 4,4'-oxobenzoyl chloride.

[0037] For example, based on 100 mol% of a meta-aromatic polyamide resin, the amide bond content can be in the range of about 70 mol% to about 90 mol%, for example, about 80 mol% to about 90 mol% or about 85 mol% to about 90 mol%. If the above numerical range is met (when the above numerical range is met), a meta-aromatic polyamide resin with desired or improved heat resistance and durability can be achieved.

[0038] By including an optimal, desired, or improved amount of meta-aromatic polyamide resin together with the polyimide resin, the diaphragm according to some example embodiments has improved or excellent durability and heat resistance.

[0039] For example, the weight-average molecular weight (M) of meta-aromatic polyamide resins w The values ​​can be in the range of about 30,000 g / mol to about 300,000 g / mol, for example about 50,000 g / mol to about 200,000 g / mol, about 80,000 g / mol to about 150,000 g / mol, or about 80,000 g / mol to about 120,000 g / mol. If this numerical range is met (when this numerical range is met), a membrane with uniformly formed nanofibers having desired or improved mechanical strength can be achieved.

[0040] For example, based on a 100 wt% separator, the content of meta-aramid resin can be greater than about 1 wt% and less than about 8 wt%, and can be, for example, greater than about 2 wt% and less than about 8 wt%, in the range of about 2 wt% to about 7 wt%, or about 3 wt% to about 7 wt%. If the above ranges are met (when the above ranges are met), a separator for rechargeable lithium batteries with desired or improved tensile strength and elongation, desired or improved mechanical strength, and optimal, desired or improved porosity can be achieved.

[0041] The diaphragm 30A may be or include a single-layer electrospun diaphragm, which is manufactured by electrospinning an electrospun solution prepared from a mixed polyamic acid and meta-aramid electrospun solution using a nozzle assembly.

[0042] Electrospinning is a process that uses a high-voltage electric field to spray a polymer solution into fine nanofibers. When separators for rechargeable lithium batteries are manufactured using electrospinning, separators with a uniform nanofiber network can be achieved, ensuring optimal, desired, or improved porosity. This results in improved ionic conductivity and permeability, as well as superior heat resistance and mechanical strength compared to existing separators.

[0043] Therefore, the separator for a rechargeable lithium battery according to some example embodiments includes nanofibers, which include polyimide resin and meta-aramid resin.

[0044] Within the framework of this invention, the term "nanofiber" refers to any fiber with an average diameter in the range of 1 nm to 1000 nm.

[0045] For example, the average diameter of nanofibers can be in the range of about 10 nm to about 200 nm, such as about 10 nm to about 150 nm, about 50 nm to about 150 nm, or about 50 nm to about 100 nm.

[0046] If the above numerical range is met (when the above numerical range is met), a membrane with desired or improved mechanical strength and porosity can be achieved.

[0047] The diameter of a nanofiber can refer to the widest diameter among the diameters of the fibers measured based on a cross-section of a single nanofiber, and can be measured in a direction perpendicular to the longitudinal direction of the nanofiber.

[0048] The average diameter of the nanofibers can be calculated by randomly measuring the cross-sectional diameter of about 20 fibers in a scanning electron microscope (SEM) image of the membrane surface and then calculating the arithmetic mean of the cross-sectional diameters of the 20 fibers.

[0049] For example, the thickness of the membrane can be in the range of about 1 μm to about 30 μm, such as about 1 μm to about 25 μm, about 1 μm to about 20 μm, about 5 μm to about 20 μm, or about 5 μm to about 15 μm. If this numerical range is met (when this numerical range is met), ultrathin membranes can be designed, and membranes with desired or improved durability, porosity, and heat resistance can be achieved.

[0050] The separators 30B, 30C, and 30C' for rechargeable lithium batteries according to some example embodiments are described in detail below. Since the contents concerning polyimide resins and meta-aramid resins, as well as the contents concerning the average diameter of nanofibers, are the same as those described above, their descriptions are omitted, and only the remaining contents are described below.

[0051] Figures 2 to 4 This is a schematic diagram illustrating a separator 30B for a rechargeable lithium battery according to some example embodiments.

[0052] According to some example embodiments, the separator 30B for a rechargeable lithium battery includes a plurality of nanofiber layers comprising nanofibers, wherein the plurality of nanofiber layers comprise a polyimide resin, and at least one of the plurality of nanofiber layers further comprises a meta-aramid resin.

[0053] For example, in a diaphragm, nanofiber layers may be included in two or more layers (e.g., three or more layers).

[0054] Reference Figures 2 to 4 The separator 30B for a rechargeable lithium battery includes: a first nanofiber layer 31; a second nanofiber layer 32 on the first nanofiber layer 31; and a third nanofiber layer 33 on the second nanofiber layer 32. The first nanofiber layer 31, the second nanofiber layer 32, and the third nanofiber layer 33 comprise polyimide resin, and at least one of the first nanofiber layer 31, the second nanofiber layer 32, and the third nanofiber layer 33 may further comprise meta-aramid resin.

[0055] The diaphragm 30B may be or include a multilayer electrospun diaphragm manufactured by electrospun electrospinning electrospinning solutions of the same or different compositions using multiple supply devices (multiple nozzle groups).

[0056] Reference Figure 2 The first nanofiber layer 31, the second nanofiber layer 32, and the third nanofiber layer 33 may comprise polyimide resin and meta-aromatic polyamide resin. For example, the components of the first nanofiber layer 31, the second nanofiber layer 32, and the third nanofiber layer 33, and the amount of each component, may be the same or different.

[0057] Reference Figure 3 The first nanofiber layer 31 and the third nanofiber layer 33 comprise polyimide resin and meta-aromatic polyamide resin, and the second nanofiber layer 32 may comprise polyimide resin. For example, the components and the amount of each component in the first nanofiber layer 31 and the third nanofiber layer 33 may be the same or different.

[0058] Reference Figure 4 The first nanofiber layer 31 and the third nanofiber layer 33 may include polyimide resin, and the second nanofiber layer 32 may include polyimide resin and meta-aromatic polyamide resin.

[0059] According to some example embodiments, the separator 30B for a rechargeable lithium battery may consist of or include multiple layers of separators, and each layer may consist of or include only polyimide resin, or may consist of or include optimal, desired, or improved amounts of polyimide resin and meta-aramid resin, such that the heat resistance, flexibility, and mechanical strength may be better than in the case of a single-layer separator.

[0060] For example, the nanofiber layer also includes 100 wt% meta-aramid resin, the content of which may be greater than about 1 wt% and less than about 8 wt%, for example, greater than or equal to about 2 wt% and less than about 8 wt%, or in the range of about 2 wt% to about 7 wt% or about 3 wt% to about 7 wt%.

[0061] For example, based on 100 wt% of membrane 30B, the content of meta-aromatic polyamide resin can be greater than or equal to about 0.5 wt% and less than about 8 wt%, for example, greater than or equal to about 1 wt% and less than about 8 wt%, greater than or equal to about 2 wt% and less than about 8 wt%, in the range of about 2 wt% to about 7 wt% or about 3 wt% to about 7 wt%.

[0062] For example, based on 100 wt% of diaphragm 30B, the content of polyimide resin can be in the range of about 90 wt% to about 99 wt%, for example about 92 wt% to about 99 wt%, about 93 wt% to about 99 wt%, or about 93 wt% to about 97 wt%.

[0063] When the meta-aramid resin in the multilayer separator 30B is included in the above-mentioned numerical range, a three-layer separator for rechargeable lithium batteries with desired or improved tensile strength and elongation, desired or improved mechanical strength, and optimal, desired or improved porosity can be achieved.

[0064] For example, the thickness of the nanofiber layer can be in the range of about 0.5 μm to about 30 μm, such as about 0.5 μm to about 15 μm, about 1 μm to about 30 μm, about 1 μm to about 25 μm, about 1 μm to about 20 μm, about 5 μm to about 20 μm, or about 5 μm to about 15 μm.

[0065] For example, the thickness of the diaphragm 30B can be in the range of about 1 μm to about 50 μm, such as about 3 μm to about 50 μm, about 5 μm to about 40 μm, about 5 μm to about 30 μm or about 5 μm to about 20 μm.

[0066] If the above numerical range is met (when the above numerical range is met), ultrathin membranes can be designed, and membranes with desired or improved durability, porosity, and heat resistance can be achieved.

[0067] Figure 5 and Figure 6 This is a schematic diagram illustrating separators 30C, 30C' for rechargeable lithium batteries according to some example embodiments.

[0068] Reference Figure 5 The rechargeable lithium battery separator 30C is a separator comprising nanofibers having a core-shell structure comprising a core a and a shell b on the surface of the core a, wherein the core a and the shell b each independently comprise one of a polyimide resin, a meta-aromatic polyamide resin, and a mixture of a polyimide resin and a meta-aromatic polyamide resin, and the core and the shell comprise different resins.

[0069] Reference Figure 6 The separator 30C' for rechargeable lithium batteries may include two or more nanofiber layers comprising nanofibers having a core-shell structure, and may include, for example, three or more nanofiber layers.

[0070] Reference Figure 6 The diaphragm 30C' may include: a first nanofiber layer 31'; a second nanofiber layer 32' on the first nanofiber layer 31'; and a third nanofiber layer 33' on the second nanofiber layer 32'. The first nanofiber layer 31', the second nanofiber layer 32', and the third nanofiber layer 33' may include nanofibers having the core-shell structure described above.

[0071] According to some example embodiments, the diaphragm (not shown in the figure) includes nanofiber layers comprising nanofibers, wherein multiple nanofiber layers comprise polyimide resins, and at least one of the multiple nanofiber layers comprises nanofibers having a core-shell structure comprising a core and a shell on the surface of the core, wherein the core and shell each independently comprise one of a polyimide resin, a meta-aromatic polyamide resin, and a mixture of a polyimide resin and a meta-aromatic polyamide resin, the core and shell comprising different resins.

[0072] For example, based on 100 wt% of membrane 30C, 30C', the content of meta-aromatic polyamide resin can be greater than about 1 wt% and less than about 8 wt%, and can be, for example, greater than about 2 wt% and less than about 8 wt%, in the range of about 2 wt% to about 7 wt% or about 3 wt% to about 7 wt%.

[0073] For example, based on 100 wt% of membrane 30C, 30C', the content of polyimide resin can be in the range of about 90 wt% to about 99 wt%, for example about 92 wt% to about 99 wt%, about 93 wt% to about 99 wt%, or about 93 wt% to about 97 wt%.

[0074] If the above range is met (when the above range is met), a separator for rechargeable lithium batteries with desired or improved tensile strength and elongation, desired or improved mechanical strength, and optimal, desired or improved porosity can be achieved.

[0075] For example, the average diameter of the nanofibers forming the core-shell structure in membranes 30C and 30C' can be in the range of about 10 nm to about 200 nm, for example, about 10 nm to about 150 nm, about 50 nm to about 150 nm, or about 50 nm to about 100 nm. If the above numerical range is met (when the above numerical range is met), a membrane with desired or improved mechanical strength and porosity can be achieved.

[0076] For example, the thickness of the monolayer diaphragm 30C can be in the range of about 1 μm to about 30 μm, such as about 1 μm to about 25 μm, about 1 μm to about 20 μm, about 5 μm to about 20 μm, or about 5 μm to about 15 μm.

[0077] For example, the thickness of the multilayer diaphragm 30C' can be in the range of about 1 μm to about 50 μm, for example about 5 μm to about 40 μm, about 5 μm to about 30 μm, or about 5 μm to about 20 μm.

[0078] When the above numerical ranges are met, ultra-thin membranes can be designed, and membranes with desired or improved durability, porosity, and heat resistance can be achieved.

[0079] For example, the tensile strength (MD) of the diaphragm can be in the range of about 50 MPa to about 300 MPa, such as about 50 MPa to about 200 MPa, about 50 MPa to about 100 MPa, or about 60 MPa to about 100 MPa.

[0080] For example, the elongation (MD) of the diaphragm can be in the range of about 5% to about 15%, such as about 6% to about 13% or about 7% to about 12%.

[0081] For example, the porosity of the membrane can be in the range of about 20% to about 65%, such as about 30% to about 65%, about 40% to about 65%, or about 45% to about 65%.

[0082] If the tensile strength, elongation, and porosity of the separator meet the above-mentioned numerical ranges (when the tensile strength, elongation, and porosity of the separator meet the above-mentioned numerical ranges), then a separator for rechargeable lithium batteries with desired or improved mechanical properties can be achieved.

[0083] For example, the tensile strength and elongation of the diaphragm can be measured using a universal testing machine (UTM) according to ASTM D882 standard. Tensile strength can be calculated by applying a tensile load to the diaphragm at a stretching rate of 100 mm / min and measuring the maximum load until the diaphragm breaks, then dividing that maximum load value by the initial cross-sectional area of ​​the sample. Elongation can be measured by stretching the diaphragm at a rate of 500 mm / min and calculating the rate at which the diaphragm breaks.

[0084] For example, the porosity (%) of the membrane can be measured by mercury porosimetry or gas adsorption (BET analysis).

[0085] For example, diaphragms 30A, 30B, 30C, and 30C' may also include a heat-resistant polymer, which may include at least one of the following polymers, copolymers thereof, or combinations thereof: polypropylene (PP), polyester, polyamide, polyetherimide (PEI), polyetheretherketone (PEEK), poly(p-phenylene terephthalamide) (PPTA), polysulfone (PSF), polyethersulfone (PES), polyphenylene sulfide (PPS), polyamide-imide (PAI), polyacrylonitrile (PAN), polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP), polycarbonate (PC), polyvinyl chloride (PVC), polyvinylidene chloride, polyethylene glycol derivatives, polyoxides, polyvinyl acetate, polystyrene (PS), and polyvinylpyrrolidone (PVP). The heat-resistant polymer is a non-aqueous polymer, which may be desirable for forming fibers by electrospinning.

[0086] For example, based on 100 wt% of membranes 30A, 30B, 30C, 30C', the content of heat-resistant polymer can be in the range of about 0 wt% to about 10 wt%, for example about 0 wt% to about 8 wt%, or about 0 wt% to about 5 wt%.

[0087] Method for manufacturing a separator for rechargeable lithium batteries A method for manufacturing a separator for a rechargeable lithium battery according to some example embodiments includes: (1) mixing polyamic acid, meta-aramid resin and solvent to prepare an electrospinning solution; (2) electrospinning the electrospinning solution onto a release film to form a coating layer; (3) heat-treating the coating layer at a temperature in the range of about 200°C to about 500°C to form a separator; and (4) removing (peeling off) the release film from the separator.

[0088] The separator manufactured by this manufacturing method may be or include a separator 30A for rechargeable lithium batteries having the above-described single-layer structure.

[0089] The electrospinning solution can be prepared by mixing polyamic acid, meta-aromatic polyamide resin and solvent, and optionally by further including the heat-resistant polymer as described above.

[0090] For example, the solvent may include at least one of dimethylacetamide, N-methylpyrrolidone, dimethylformamide, dimethyl sulfoxide, acetone, or combinations thereof.

[0091] For example, based on the sum of 100 wt% of the amount of polyamic acid and meta-aromatic polyamide resin, the content of polyamic acid can be in the range of about 90 wt% to about 99 wt%, for example about 92 wt% to about 99 wt%, about 93 wt% to about 99 wt%, or about 93 wt% to about 97 wt%.

[0092] For example, based on the sum of 100 wt% of the amount of polyamic acid and the amount of meta-aromatic polyamide resin, the content of meta-aromatic polyamide resin can be greater than about 1 wt% and less than about 8 wt%, and can be, for example, greater than about 2 wt% and less than about 8 wt%, in the range of about 2 wt% to about 7 wt% or about 3 wt% to about 7 wt%.

[0093] When the above numerical ranges are met, a separator for rechargeable lithium batteries can be manufactured with desired or improved tensile strength and elongation, desired or improved mechanical strength, and optimal, desired or improved porosity.

[0094] Next, the electrospinning solution prepared above can be electrospinned onto the release film to form a coating layer.

[0095] For example, the release film may include at least one of aluminum foil, copper foil, SUS, polyethylene terephthalate (PET), polypropylene (PP), polyethylene (PE), polycarbonate (PC), polyvinyl chloride (PVC), or combinations thereof.

[0096] Electrospinning can be performed as follows: a supply device (nozzle assembly) consisting of tips with aperture sizes ranging from about 15G (gauge) to about 30G is positioned with a collection roller at a predetermined or desired interval, an electrospinning solution is added to the tips, the target substrate is positioned on the collection roller, and then a voltage ranging from about 35kV to about 100kV is applied to the tips.

[0097] The number of tips can be adjusted as needed based on the type and amount of polymer included in the electrospinning solution, and can be in the range of, for example, 1 to 1000.

[0098] The predetermined or desired distance between the supply device (nozzle assembly) and the target material can be in the range of approximately 10 cm to approximately 20 cm.

[0099] If the aperture size of the tip is in the range of about 25G to about 30G (when the aperture size of the tip is in the range of about 25G to about 30G), then it is suitable because a coating layer of the desired shape can be formed.

[0100] According to the electrospinning process, a polymer solution is spun and stretched into a fiber shape, and then spun onto a target substrate in the form of nanofibers to form a coating layer. To explain in more detail, the electrospinning solution is suspended in droplets due to surface tension at its tip. When a voltage is applied, charges accumulate on the surface of the electrospinning solution droplets, and repulsive forces occur between these charges. Therefore, the repulsive force between the charges points in the opposite direction to the surface tension of the solution. When a critical voltage is reached, a conical Taylor cone is formed, and a polymer jet is emitted from the tip of the Taylor cone. Through multiaxial stretching in the agitation zone, the nanofibers are collected on a collecting roller in the form of a nonwoven fabric to form the coating layer.

[0101] At this point, the electrospinning process can be carried out under conditions of temperature ranging from approximately 20°C to approximately 30°C and relative humidity ranging from approximately 0% to approximately 60%. If the electrospinning process is carried out under the aforementioned temperature and relative humidity conditions, it is advantageous to maintain a constant fiber thickness while spinning.

[0102] Furthermore, the speed of the collecting roller can be adjusted to allow the coating layer to be formed to a suitable or desired thickness, and can be, for example, in the range of about 50 mpm to about 300 mpm. Additionally, the flow rate of the electrospinning solution discharged from the tip can be adjusted to be discharged at a rate in the range of about 150 μL / min to about 100 mL / min, for example, about 1 mL / min to about 100 mL / min.

[0103] Furthermore, the tip air can be adjusted as needed to minimize interference between tips and achieve uniform electrospinning. Tip air adjustment can be performed by flowing compressed air at a pressure ranging from about 0.01 MPa to about 0.5 MPa.

[0104] For example, the electrospinning process can be performed two or more times.

[0105] Since nanofibers are formed through electrospinning, the resulting nanofibers can possess a three-dimensional network structure. Because the coating layer is formed via electrospinning, the solvent can easily evaporate, thus better suppressing springback that causes electrode damage, which is advantageous.

[0106] Next, the coating layer formed by electrospinning can be heat-treated at a temperature ranging from about 200°C to about 500°C to form a diaphragm. Through heat treatment, the polyamic acid included in the coating layer can be thermally imidized to produce a polyimide resin.

[0107] For example, the heat treatment temperature can be in the range of about 200°C to about 500°C, for example, about 300°C to about 500°C, about 200°C to about 400°C, or about 300°C to about 400°C. If the above numerical range is met (when the above numerical range is met), a diaphragm with desired or improved mechanical strength and porosity can be achieved without deforming the diaphragm.

[0108] After the separator is formed, further rolling can be performed. The rolling process can be carried out at a temperature ranging from about 25°C to about 110°C. If further rolling is performed (when further rolling is performed), the separator can be compressed to shorten the Li ion migration path, which can have the advantage of facilitating lithium ion movement during charging and discharging.

[0109] Next, the release film can be removed (peeled) from the manufactured separator to produce a separator for rechargeable lithium batteries in the form of a self-standing membrane.

[0110] According to some example embodiments, a method for manufacturing a separator for a rechargeable lithium battery includes: (1) preparing a first electrospinning solution comprising polyamic acid and a first solvent and a second electrospinning solution comprising polyamic acid, meta-aramid resin and a second solvent; (2) alternately electrospinning the first electrospinning solution and the second electrospinning solution onto a release film to form a coating layer; (3) heat-treating the coating layer at a temperature in the range of about 200°C to about 500°C to form a separator; and (4) removing the release film from the separator.

[0111] The separator manufactured by this manufacturing method may be or include a separator 30B for rechargeable lithium batteries having the above-described multilayer structure.

[0112] A first electrospinning solution can be prepared by mixing polyamic acid and a first solvent, and a second electrospinning solution can be prepared by mixing polyamic acid, meta-aromatic polyamide resin, and a second solvent. Alternatively, the first and second electrospinning solutions can be prepared by further comprising the heat-resistant polymer as described above.

[0113] The first solvent and the second solvent may include at least one of dimethylacetamide, N-methylpyrrolidone, dimethylformamide, dimethyl sulfoxide, acetone, or combinations thereof.

[0114] For example, based on the sum of 100 wt% of the amount of polyamic acid and meta-aromatic polyamide resin in the second electrospinning solution, the content of polyamic acid can be in the range of about 90 wt% to about 99 wt%, for example about 92 wt% to about 99 wt%, about 93 wt% to about 99 wt%, or about 93 wt% to about 97 wt%.

[0115] For example, based on the sum of 100 wt% of the amount of polyamic acid and meta-aromatic polyamide resin in the second electrospinning solution, the content of meta-aromatic polyamide resin can be greater than about 1 wt% and less than about 8 wt%, for example, greater than or equal to about 2 wt% and less than about 8 wt%, in the range of about 2 wt% to about 7 wt% or about 3 wt% to about 7 wt%.

[0116] If the above numerical range is met (when the above numerical range is met), a separator for rechargeable lithium batteries can be manufactured with desired or improved tensile strength and elongation, desired or improved mechanical strength, and optimal, desired or improved porosity.

[0117] Next, electrospinning of the first electrospinning solution and the second electrospinning solution prepared above are alternately performed on the release film to form a coating layer.

[0118] Figure 7This is a schematic diagram illustrating an electrospinning apparatus used to manufacture multilayer separators for rechargeable lithium batteries. Figure 7 In the example shown, the electrospinning apparatus includes three supply devices, but depending on the desired number of diaphragm layers, it may include more than three supply devices.

[0119] Reference Figure 7 The electrospinning apparatus may include a first supply device 1, a second supply device 2, and a third supply device 3 arranged sequentially along the direction of travel, and each of the first supply device 1, the second supply device 2, and the third supply device 3 may include a tip ranging from one to about 1,000, the tip having an aperture size ranging from about 15G to about 30G.

[0120] The electrospinning apparatus may also include collecting rollers arranged at a given interval at the lower part of the supply device and release films placed on the collecting rollers.

[0121] The first electrospinning solution or the second electrospinning solution can be filled into the first supply device 1, the second supply device 2 and the third supply device 3.

[0122] Furthermore, when the first electrospinning solution or the second electrospinning solution filled in the first supply device 1, the second supply device 2 and the third supply device 3 are alternately electrospinned on the release film in the direction of travel of the electrospinning device, a coating layer with a multilayer structure can be manufactured.

[0123] Since the conditions for other electrospinning processes are the same as those described above, detailed descriptions of them are omitted here.

[0124] Next, methods for manufacturing the diaphragm may include: heat-treating the coating layer at a temperature in the range of about 200°C to about 500°C to form the diaphragm; and removing the release film from the diaphragm. Since these processes are described identically to those described above, detailed descriptions thereof are omitted here.

[0125] According to some example embodiments, a method for manufacturing a separator for a rechargeable lithium battery includes: (1) preparing a first electrospinning solution comprising polyamic acid and a first solvent, a second electrospinning solution comprising polyamic acid, meta-aramid resin and a second solvent, and a third electrospinning solution comprising meta-aramid resin and a third solvent; (2) electrospinning two of the first electrospinning solution, the second electrospinning solution and the third electrospinning solution onto a release film using coaxial double tips to form a coating layer; (3) heat-treating the coating layer at a temperature in the range of about 200°C to about 500°C to form a separator; and (4) removing the release film from the separator.

[0126] The separator manufactured by the above manufacturing method may be or include separators 30C, 30C' for rechargeable lithium batteries having a single-layer or multi-layer structure containing the above core-shell structure.

[0127] A first electrospinning solution can be prepared by mixing polyamic acid and a first solvent; a second electrospinning solution can be prepared by mixing polyamic acid, meta-aromatic polyamide resin, and a second solvent; and a third electrospinning solution can be prepared by mixing meta-aromatic polyamide resin and a third solvent.

[0128] In addition, the first electrospinning solution, the second electrospinning solution, and the third electrospinning solution can optionally be prepared by further including the heat-resistant polymer as described above.

[0129] The first solvent, the second solvent, and the third solvent may include at least one of dimethylacetamide, N-methylpyrrolidone, dimethylformamide, dimethyl sulfoxide, acetone, or combinations thereof.

[0130] For example, based on the sum of 100 wt% of the amount of polyamic acid and meta-aromatic polyamide resin included in two of the first, second, and third electrospinning solutions, the content of meta-aromatic polyamide resin can be greater than about 1 wt% and less than about 8 wt%, for example, greater than or equal to about 2 wt% and less than about 8 wt%, in the range of about 2 wt% to about 7 wt% or about 3 wt% to about 7 wt%.

[0131] For example, based on the sum of 100 wt% of the amount of polyamic acid and meta-aromatic polyamide resin included in two types of electrospinning solutions, namely the first electrospinning solution, the second electrospinning solution, and the third electrospinning solution, the amount of polyamic acid may be in the range of about 90 wt% to about 99 wt%, for example, about 92 wt% to about 99 wt%, about 93 wt% to about 99 wt%, or about 93 wt% to about 97 wt%.

[0132] If the above range is met (when the above range is met), a separator for rechargeable lithium batteries with desired or improved tensile strength and elongation, desired or improved mechanical strength, and optimal, desired or improved porosity can be achieved.

[0133] Next, two of the first, second, and third electrospinning solutions can be electrospinned onto the release film using coaxial dual tips to form a coating layer.

[0134] For example, the process can be performed using coaxial double tips, which can consist of an inner tip and an outer tip, or include both an inner tip and an outer tip, with the outer tips arranged around the inner tip based on the same central axis. The electrospinning solution injected into the inner tip can form a core-shell structure after electrospinning, and the electrospinning solution injected into the outer tip can form a shell structure after electrospinning.

[0135] For example, one of the first, second, and third electrospinning solutions can be injected into the outer tip, and other electrospinning solutions can be injected into the inner tip. For example, the electrospinning solutions injected into the outer tip and the electrospinning solutions injected into the inner tip can be different from each other.

[0136] As an example, a first electrospinning solution can be injected into the inner tip, and a third electrospinning solution can be injected into the outer tip.

[0137] If electrospinning is performed using a coaxial double tip comprising an inner tip filled with a first electrospinning solution and an outer tip filled with a third electrospinning solution (when electrospinning is performed using a coaxial double tip comprising an inner tip filled with a first electrospinning solution and an outer tip filled with a third electrospinning solution), a membrane having a core-shell structure comprising a core containing a polyimide resin and a shell disposed on the surface of the core and comprising a meta-aramid resin can be manufactured.

[0138] As another example, it can be used according to the above-mentioned principles. Figure 7 The electrospinning apparatus manufactures a diaphragm 30C' comprising two or more layers of nanofibers containing nanofibers with a core-shell structure.

[0139] At this time, the tips included in the first supply device 1, the second supply device 2 and the third supply device 3 can be the aforementioned coaxial double tips.

[0140] When using an electrospinning device, it is possible to manufacture products such as... Figure 6 The membrane 30C' shown is a rechargeable lithium battery in which the core-shell structure is stacked in multiple layers.

[0141] Since the conditions for other electrospinning processes are the same as those described above, a detailed description of them is omitted here.

[0142] Next, methods for manufacturing the diaphragm may include: heat-treating the coating layer at a temperature in the range of about 200°C to about 500°C to form the diaphragm; and removing the release film from the diaphragm. Since these processes are described identically to those described above, detailed descriptions thereof are omitted here.

[0143] Rechargeable lithium batteries Some example embodiments include a rechargeable lithium battery comprising a positive electrode, a negative electrode, and a separator between the positive and negative electrodes.

[0144] Because rechargeable lithium batteries include the aforementioned separator, they have desired or improved thermal stability and desired or improved charge / discharge characteristics.

[0145] Rechargeable lithium batteries can be classified according to their shape, such as cylindrical, prismatic, pouch-shaped, and coin-shaped. Figures 8 to 11 This is a schematic diagram illustrating a rechargeable lithium battery according to some example embodiments. Figure 8 A cylindrical battery is shown. Figure 9 A square battery is shown. Figure 10 and Figure 11 A pouch-type battery is shown. (See reference.) Figures 8 to 11 The rechargeable lithium battery 100 includes an electrode assembly 40 and a housing 50. The electrode assembly 40 has a separator 30 between a positive electrode 10 and a negative electrode 20, and the electrode assembly 40 is housed within the housing 50. The positive electrode 10, the negative electrode 20, and the separator 30 may be impregnated with an electrolyte solution (not shown). Figure 8 As shown, the rechargeable lithium battery 100 may include a sealing member 60 of the sealed housing 50. Figure 9 In this context, the rechargeable lithium battery 100 may include a positive electrode lead connector 11, a positive electrode terminal 12 connected to the positive electrode lead connector 11, a negative electrode lead connector 21, and a negative electrode terminal 22 connected to the negative electrode lead connector 21. For example... Figure 10 and Figure 11 As shown, the rechargeable lithium battery 100 may include Figure 11 The electrode terminals 70 shown in the figure or Figure 10 The positive electrode terminal 71 and negative electrode terminal 72 shown in the figure form an electrical path for guiding the current formed in the electrode assembly 40 to the outside of the rechargeable lithium battery 100.

[0146] The rechargeable lithium batteries according to some example embodiments can be used in, for example, automobiles, mobile phones and / or various types of electrical devices, but this disclosure is not limited thereto.

[0147] The remaining components of a rechargeable lithium battery, excluding the separator, are described in detail below.

[0148] positive electrode The positive electrode for a rechargeable lithium battery may include a current collector and a layer of positive electrode active material formed on the current collector. The positive electrode active material layer includes positive electrode active material and may also include a binder and / or a conductive material.

[0149] For example, the positive electrode may also include additives that can constitute a sacrificial positive electrode.

[0150] As the positive electrode active material, compounds capable of intercalating and deintercalating lithium (lithium-intercalating compounds) can be used. For example, one or more composite oxides of lithium with metals (such as or including at least one of cobalt, manganese, nickel and combinations thereof) can be used.

[0151] The composite oxide can be or includes lithium transition metal composite oxides, and examples of such composite oxides can include at least one of lithium nickel oxides, lithium cobalt oxides, lithium manganese oxides, lithium iron phosphate compounds, cobalt-free lithium nickel manganese oxides, or combinations thereof.

[0152] As an example, a compound represented by any of the following chemical formulas can be used. Li a A 1-b X b O 2-c D c (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05); Li a Mn 2-b X b O 4-c D c (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05); Li a Ni 1-b-c Co b X c O 2-α D α (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<α<2); Li a Ni 1-b- c Mn b X c O 2-α D α (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<α<2); Li a Ni b Co c L 1 d G e O2 (0.90≤a≤1.8, 0≤b≤0.9, 0≤c≤0.5, 0≤d≤0.5, 0≤e≤0.1); Li a NiG b O2 (0.90≤a≤1.8, 0.001≤b≤0.1); Li a CoG bO2 (0.90≤a≤1.8, 0.001≤b≤0.1); Li a Mn 1-b G b O2 (0.90≤a≤1.8, 0.001≤b≤0.1); Li a Mn2G b O4 (0.90≤a≤1.8, 0.001≤b≤0.1); Li a Mn 1-g G g PO4 (0.90≤a≤1.8, 0≤g≤0.5); Li (3-f) Fe2(PO4)3 (0≤f≤2); Li a FePO4 (0.90≤a≤1.8).

[0153] In the above chemical formula, A is or includes at least one of Ni, Co, Mn, or combinations thereof; X is or includes at least one of Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, rare earth elements, or combinations thereof; D is or includes at least one of O, F, S, P, or combinations thereof; G is or includes at least one of Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, or combinations thereof; and L 1 It is or includes at least one of Mn, Al, or combinations thereof.

[0154] For example, the positive electrode active material can be or includes a high-nickel positive electrode active material, in which, based on 100 mol% of the metals other than lithium in the lithium transition metal composite oxide, the nickel content is greater than or equal to about 80 mol%, greater than or equal to about 85 mol%, greater than or equal to about 90 mol%, greater than or equal to about 91 mol%, or greater than or equal to about 94 mol% and less than or equal to about 99 mol%. High-nickel positive electrode active materials can achieve high capacity and can be applied to high-capacity, high-density rechargeable lithium batteries.

[0155] Based on a 100wt% positive electrode active material layer, the amount of positive electrode active material can be in the range of about 90wt% to about 99.5wt%, and based on a 100wt% positive electrode active material layer, the amount of each of the binder and conductive material can be independently in the range of about 0.5wt% to about 5wt%.

[0156] The binder causes the positive electrode active material particles to adhere to each other and to adhere the positive electrode active material to the current collector. Examples of binders may include at least one of, but are not limited to, polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers including ethylene oxide, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, (meth)acrylated styrene-butadiene rubber, epoxy resin, (meth)acrylate resin, polyester resin, nylon, etc.

[0157] Conductive materials impart conductivity to electrodes and can be used in batteries as any material that does not cause adverse chemical changes and conducts electrons. Examples of conductive materials may include: carbon-based materials, such as at least one of natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fibers, carbon nanofibers, and carbon nanotubes; metallic materials, including at least one of copper, nickel, aluminum, silver, etc., in the form of metal powder or metal fibers; conductive polymers, such as polyphenylene derivatives; or mixtures thereof.

[0158] Al can be used for current collectors, but current collectors are not limited to this.

[0159] negative electrode The negative electrode for a rechargeable lithium battery includes a current collector and a layer of negative electrode active material on the current collector. The negative electrode active material layer may include negative electrode active material, and may also include a binder and / or a conductive material.

[0160] The negative electrode active material may include at least one of the following: materials that can reversibly insert / deintercalate lithium ions, lithium metal, lithium metal alloys, materials capable of doping / dedoping lithium, or transition metal oxides.

[0161] Materials that can reversibly insert / deintercalate lithium ions can include carbon-based negative electrode active materials, such as crystalline carbon, amorphous carbon, or combinations thereof. Crystalline carbon can be graphite, such as amorphous, flake, sheet, spherical, or fibrous natural or artificial graphite, and amorphous carbon can be or include at least one of soft carbon, hard carbon, mesophase pitch carbonization products, calcined coke, etc.

[0162] Lithium metal alloys include alloys of lithium and metals (including at least one of Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, and Sn).

[0163] Materials capable of doping / dedoping lithium can be, or include, Si-based or Sn-based negative electrode active materials. Si-based negative electrode active materials can include silicon, silicon-carbon composites, and SiO₂.x (0<x≤2), a Si-Q alloy (wherein Q is or includes at least one of an alkali metal, an alkaline earth metal, a Group 13 element, a Group 14 element (other than Si), a Group 15 element, a Group 16 element, a transition metal, a rare earth element, and combinations thereof), or at least one of combinations thereof. The Sn-based negative electrode active material may be or include at least one of Sn, SnO₂, a Sn-based alloy, or combinations thereof.

[0164] The silicon-carbon composite may be or include a composite of silicon and amorphous carbon. According to some example embodiments, the silicon-carbon composite may be in the form of silicon particles and amorphous carbon coated on surfaces of the silicon particles. For example, the silicon-carbon composite may include secondary particles (core) assembled from silicon primary particles and an amorphous carbon coating layer (shell) on surfaces of the secondary particles. Amorphous carbon may also be present between the silicon primary particles, for example, the silicon primary particles may be coated with amorphous carbon. The secondary particles may be dispersed in an amorphous carbon matrix.

[0165] The silicon-carbon composite may further include crystalline carbon. For example, the silicon-carbon composite may include a core containing crystalline carbon and silicon particles, and an amorphous carbon coating layer on a surface of the core. The Si-based negative electrode active material or the Sn-based negative electrode active material may be mixed with a carbon-based negative electrode active material.

[0166] For example, the negative electrode active material layer may include the negative electrode active material in a range of about 90 wt% to about 99 wt%, a binder in a range of about 0.5 wt% to about 5 wt%, and a conductive material in a range of about 0 wt% to about 5 wt%.

[0167] The binder adheres the negative electrode active material particles to each other, and adheres the negative electrode active material to the current collector. The binder may include a non-aqueous binder, an aqueous binder, a dry binder, or a combination thereof.

[0168] The non-aqueous binder may include at least one of polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene propylene copolymer, polystyrene, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamide-imide, polyimide, or combinations thereof.

[0169] The aqueous binder may be or include at least one of styrene-butadiene rubber, (meth)acrylated styrene-butadiene rubber, (meth)acrylonitrile-butadiene rubber, (meth)acrylic rubber, butyl rubber, fluororubber, polyethylene oxide, polyvinylpyrrolidone, polyepichlorohydrin, polyphosphazene, poly(meth)acrylonitrile, ethylene propylene diene copolymer, polyvinylpyridine, chlorosulfonated polyethylene, latex, polyester resin, (meth)acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol, and combinations thereof.

[0170] When an aqueous binder is used as the negative electrode binder, it may further include a cellulose compound capable of imparting viscosity. The cellulose compound may include at least one of carboxymethyl cellulose, hydroxypropyl methyl cellulose, methyl cellulose, or an alkali metal salt thereof. The alkali metal may include at least one of Na, K, or Li.

[0171] The dry adhesive may be or include a polymeric material capable of being fibrous, and may be or include at least one of, for example, polytetrafluoroethylene, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyethylene oxide, or combinations thereof.

[0172] Conductive materials are included to provide electrode conductivity, and any electrically conductive material can be used as a conductive material unless it causes an adverse chemical change. Examples of conductive materials include: carbon-based materials, such as at least one of natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, carbon nanofiber, carbon nanotube, etc.; metallic materials such as metal powders or metal fibers, including at least one of copper, nickel, aluminum, silver, etc.; conductive polymers, such as polyphenylene derivatives; or mixtures thereof.

[0173] The negative electrode current collector may include at least one of copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, polymer substrate coated with a conductive metal, and combinations thereof.

[0174] Electrolyte solution Electrolyte solutions used in rechargeable lithium batteries include non-aqueous organic solvents and lithium salts.

[0175] Non-aqueous organic solvents constitute the medium for transporting ions that participate in the electrochemical reactions of the battery.

[0176] Non-aqueous organic solvents may be or include at least one of carbonate solvents, ester solvents, ether solvents, ketone solvents, alcohol solvents, aprotic solvents, or combinations thereof.

[0177] Carbonate solvents may include at least one of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), methyl ethyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), and butyl carbonate (BC). Esters may include at least one of methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, decanolactone, mevalonolactone, valproic acid lactone, caprolactone, etc. Ether solvents may include at least one of dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, dimethoxyethane, 2-methyltetrahydrofuran, 2,5-dimethyltetrahydrofuran, tetrahydrofuran, etc. Furthermore, ketone solvents may include cyclohexanone, etc. Alcohol solvents may include ethanol, isopropanol, etc. Aprotic solvents may include at least one of the following: nitriles, such as R-CN (wherein R is a C2 to C20 straight-chain, branched or cyclic hydrocarbon group, and may include double bonds, aromatic rings or ether groups, etc.); amides, such as dimethylformamide; dioxolane, such as 1,3-dioxolane, 1,4-dioxolane, etc.; sulfolane, etc.

[0178] Non-aqueous organic solvents can be used alone or in mixtures of two or more types of solvents.

[0179] If a carbonate solvent is used (when using a carbonate solvent), cyclic carbonates and chain carbonates can be mixed together, and cyclic carbonates and chain carbonates can be mixed in a volume ratio ranging from about 1:1 to about 1:9.

[0180] Lithium salts dissolved in organic solvents supply lithium ions in batteries, enabling basic operation of rechargeable lithium batteries and improving lithium ion transport between the positive and negative electrodes. Examples of lithium salts include LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiAlO2, LiAlCl4, LiPO2F2, LiCl, LiI, LiN(SO2C2F5)2, Li(FSO2)2N (lithium bis(fluorosulfonyl)imide; LiFSI), LiC4F9SO3, LiN(C x F 2x+1 SO2)(C y F 2y+1 At least one of the following: (SO2) (where x and y are integers in the range of 1 to 20), lithium trifluoromethane sulfonate, lithium tetrafluoroethane sulfonate, lithium difluorobis(oxalate)phosphate (LiDFBOP), lithium difluoro(oxalate)borate (LiDFOB), and lithium bis(oxalate)borate (LiBOB).

[0181] Examples and comparative examples of this disclosure are described below. However, these examples should not in any sense be construed as limiting the scope of the disclosure.

[0182] Example: (1) Single-layer diaphragm Example 1-1 By mixing polyamic acid and meta-aromatic polyamide resin (M w The electrospinning solution was prepared using a solvent of polyamic acid (100,000 g / mol) and dimethylacetamide. At this point, based on the sum of 100 wt% of the amounts of polyamic acid and meta-aromatic polyamide resin, the content of polyamic acid was 97 wt% and the content of meta-aromatic polyamide resin was 3 wt%.

[0183] Subsequently, the electrospinning solution is electrospinned on the release film to form a coating layer. Electrospinning is performed under the following conditions.

[0184] Electrospinning was performed at 26°C and 50% relative humidity by positioning a nozzle assembly consisting of 52 tips with a 25G orifice size at 15cm intervals with a collecting roller, adding electrospinning solution to the tips, and applying a voltage of 40kV to 50kV. The collecting roller was set to a speed of 50mpm to 300mpm, and the electrospinning solution was adjusted to discharge from the tips at a solid content of 150μL / min. Electrospinning was also performed by introducing compressed air at a pressure of 0.1MPa.

[0185] The coating is then heat-treated at 400°C to form a diaphragm, from which the release film is removed to obtain a diaphragm (thickness = 7.4 μm) according to Example 1-1.

[0186] The final membrane comprises nanofibers (average diameter = 100 nm) and, based on 100 wt% of the membrane, comprises 97 wt% polyimide resin (PI) and 3 wt% meta-aramid resin (MA).

[0187] Examples 1-2 to 1-3 and Comparative Examples 1-1 to 1-4 Except for adjusting the mixing amounts of polyamic acid and meta-aromatic polyamide to prepare an electrospinning solution with the composition shown in Table 1 below, the membrane was manufactured in essentially the same manner as in Example 1-1.

[0188] (2) 3-layer diaphragm Example 2-1 In addition to filling the electrospinning solution of Example 1-1 into the solution according to... Figure 7In each of the first, second, and third supply devices of the electrospinning apparatus, electrospinning is then performed on the release film under the same electrospinning conditions as in Example 1-1, in a manner substantially the same as in Example 1-1, to manufacture a diaphragm with a 3-layer structure.

[0189] Example 2-2 In addition to using the electrospinning solution of Example 1-2, a membrane with a 3-layer structure is manufactured in essentially the same manner as in Example 2-1.

[0190] Example 2-3 In addition to using the electrospinning solution of Examples 1-3, a membrane with a 3-layer structure is manufactured in essentially the same manner as in Example 2-1.

[0191] Example 2-6 The first electrospinning solution was prepared by mixing polyamic acid and dimethylacetamide solvent, and by mixing polyamic acid and meta-aromatic polyamide resin (M... w The second electrospinning solution was prepared using a solvent of polyamic acid (100,000 g / mol) and dimethylacetamide. At this point, based on the sum of 100 wt% of the amount of polyamic acid and meta-aromatic polyamide resin in the second electrospinning solution, the content of polyamic acid was 97 wt% and the content of meta-aromatic polyamide resin was 3 wt%.

[0192] Subsequently, the second electrospinning solution was filled into Figure 7 The electrospinning apparatus shown includes a first supply device and a third supply device, and the first electrospinning solution is filled in... Figure 7 In the second supply device of the electrospinning apparatus shown.

[0193] Next, except that electrospinning is performed on the release film under the same electrospinning conditions as in Example 1-1, a separator with a 3-layer structure is manufactured in essentially the same manner as in Example 2-1.

[0194] In the three-layer membranes of Examples 2-6, each layer has the composition shown in Table 3 below.

[0195] Examples 2-7 and 2-8 Except for adjusting the mixing amounts of polyamic acid and meta-aromatic polyamide to prepare a second electrospinning solution having the composition shown in Table 3 below, the membrane was manufactured in essentially the same manner as in Examples 2-6.

[0196] Example 2-9 The diaphragm is manufactured in substantially the same manner as in Examples 2-6, except that the first electrospinning solution is filled into the first and third supply devices of the electrospinning apparatus and the second electrospinning solution is filled into the second supply device of the electrospinning apparatus.

[0197] Examples 2-10 and 2-11 Except for adjusting the mixing amounts of polyamic acid and meta-aromatic polyamide to prepare a second electrospinning solution having the composition shown in Table 3 below, the membrane was manufactured in essentially the same manner as in Examples 2-9. (3) Core-shell septum Example 3-1 The first electrospinning solution was prepared by mixing polyamic acid and dimethylacetamide solvent, and by mixing meta-aromatic polyamide resin (M... w The third electrospinning solution was prepared using a solvent of 100,000 g / mol and dimethylacetamide.

[0198] At this point, based on the sum of 100 wt% of the amount of polyamic acid and meta-aromatic polyamide resin included in the first and third electrospinning solutions, the content of polyamic acid is 97 wt%, and the content of meta-aromatic polyamide resin is 3 wt%.

[0199] Next, the diaphragm is manufactured in essentially the same manner as in Example 1-1, except that electrospinning is performed using a coaxial double tip consisting of an inner tip and an outer tip arranged around the inner tip based on the same central axis.

[0200] Specifically, the inner tip is filled with a first electrospinning solution, and the outer tip is filled with a third electrospinning solution.

[0201] The final membrane is fabricated comprising nanofibers (average diameter = 100 nm) and the nanofibers are fabricated in the form of a core-shell structure, in which the core comprises a polyimide resin (PI) and the shell is disposed on the surface of the core and comprises a meta-aromatic polyamide resin (MA).

[0202] Based on a 100wt% separator, it comprises 97wt% polyimide resin (PI) and 3wt% meta-aromatic polyamide resin (MA).

[0203] Example 3-2 Besides using according to Figure 7In addition to electrospinning using the first, second, and third supply devices of the electrospinning apparatus, a diaphragm with a three-layer structure is manufactured in substantially the same manner as in Example 3-1 by using a supply device including coaxial double tips, as in Example 3-1.

[0204] Evaluation example: Evaluation Example 1: Evaluation of Tensile Strength and Elongation The tensile strength and elongation of the diaphragms were evaluated based on the example and comparative examples.

[0205] For example, each diaphragm sample (10 mm wide and 500 mm long) was measured using a universal testing machine (UTM).

[0206] For each sample, a tensile load was applied to the sample at a tensile rate of 100 mm / min, the maximum load until the sample was destroyed was measured, and the tensile strength (MPa) was calculated by dividing the maximum load value by the initial cross-sectional area of ​​the sample.

[0207] In addition, for each sample, the elongation was measured at a speed of 100 mm / min.

[0208] The results are shown in Tables 1 through 4 below.

[0209] Evaluation Example 2: Porosity Evaluation The porosity of the membranes according to the example and comparative examples was measured by gas adsorption method (Brunauer-Emmett-Teller (BET) analysis) and is shown in Tables 1 to 4 below.

[0210] Table 1:

[0211] Table 2:

[0212] Table 3:

[0213] Table 4:

[0214] Referring to Table 1 above, Examples 1-1 to 1-3 meet the optimal, desired, or improved porosity, while also possessing desired or improved tensile strength and elongation. Meanwhile, Comparative Example 1-1 does not contain meta-aromatic polyamide resin, therefore its durability is lower than that of the examples, and its tensile strength and elongation are also lower. Furthermore, Comparative Example 1-2 does not contain polyimide resin, therefore its tensile strength is lower than that of the examples. Additionally, Comparative Example 1-3 includes a considerably small amount of meta-aromatic polyamide resin, resulting in lower tensile strength and considerably higher porosity compared to the examples. Furthermore, Comparative Example 1-4 includes a large amount of meta-aromatic polyamide resin, resulting in lower tensile strength compared to the examples.

[0215] Referring to Table 2 above, the multilayer membranes of Examples 2-1 to 2-3 have desired or improved tensile strength and elongation, while the porosity meets the optimal, desired or improved range.

[0216] Referring to Table 3 above, Examples 2-6 to 2-11 all exhibit tensile strength greater than or equal to 80 MPa, elongation greater than or equal to 8%, and porosity within the optimal, desired, or improved range.

[0217] Referring to Table 4 above, Examples 3-1 and 3-2 both meet the optimal, desired, or improved porosity, and have the desired or improved tensile strength and elongation.

[0218] While this disclosure has been described in conjunction with what are now considered to be exemplary embodiments, it will be understood that the disclosure is not limited to the disclosed exemplary embodiments, but rather is intended to cover various modifications and equivalent arrangements included within the spirit and scope of the appended claims.

[0219] Description of reference numerals in the attached figures: 100: Rechargeable lithium battery; 10: Positive electrode 11: Positive electrode lead connector 12: Positive electrode terminal 20: Negative electrode 21: Negative electrode lead connector 22: Negative electrode terminals 30, 30A, 30B, 30C, 30C': Diaphragm a: Core b: Shell 31, 31': First nanofiber layer; 32, 32': Second nanofiber layer 33, 33': Third nanofiber layer 1: First supply device 2: Second supply device; 3: Third supply device 40: Electrode assembly; 50: Housing 60: Sealing component; 70: Electrode terminal piece 71: Positive electrode connector; 72: Negative electrode connector.

Claims

1. A separator for a rechargeable lithium battery, the separator comprising: Nanofibers, wherein the nanofibers comprise polyimide resin and meta-aramid resin, and Based on 100 wt% of the diaphragm, the content of meta-aromatic polyamide resin is greater than 1 wt% and less than 8 wt%.

2. The diaphragm according to claim 1, wherein, Based on 100 wt% of the diaphragm, the content of meta-aromatic polyamide resin is in the range of 3 wt% to 7 wt%.

3. The diaphragm according to claim 1, wherein, The weight-average molecular weight of meta-aromatic polyamide resins ranges from 30,000 g / mol to 300,000 g / mol.

4. The diaphragm according to claim 1, wherein, The average diameter of the nanofibers is in the range of 10 nm to 200 nm.

5. The diaphragm according to claim 1, wherein, The thickness of the diaphragm is in the range of 1 μm to 30 μm.

6. A separator for a rechargeable lithium battery, the separator comprising a plurality of nanofiber layers including nanofibers, wherein: The plurality of nanofiber layers comprise polyimide resin, and At least one of the plurality of nanofiber layers further comprises a meta-aramid resin.

7. The diaphragm according to claim 6, wherein, The 100wt% composition also includes a nanofiber layer of meta-aromatic polyamide resin, wherein the content of meta-aromatic polyamide resin is greater than 1wt% and less than 8wt%.

8. The diaphragm according to claim 6, wherein, Based on 100 wt% of the diaphragm, the content of meta-aromatic polyamide resin is greater than or equal to 0.5 wt% and less than 8 wt%.

9. The diaphragm according to claim 6, wherein, The weight-average molecular weight of meta-aromatic polyamide resins ranges from 30,000 g / mol to 300,000 g / mol.

10. The diaphragm according to claim 6, wherein, The average diameter of the nanofibers is in the range of 10 nm to 200 nm.

11. The diaphragm according to claim 6, wherein, The thickness of the nanofiber layer is in the range of 0.5 μm to 15 μm.

12. The diaphragm according to claim 6, wherein, The thickness of the diaphragm is in the range of 1 μm to 50 μm.

13. A separator for a rechargeable lithium battery, the separator comprising: Nanofibers having a core-shell structure, the core-shell structure comprising a core and a shell located on the surface of the core. The core and the shell each independently comprise one of polyimide resin, meta-aromatic polyamide resin, and a mixture of polyimide resin and meta-aromatic polyamide resin. The core and the shell comprise different resins.

14. The diaphragm according to claim 13, wherein, Based on 100 wt% of the diaphragm, the content of meta-aromatic polyamide resin is greater than 1 wt% and less than 8 wt%.

15. The diaphragm according to claim 13, wherein, The weight-average molecular weight of meta-aromatic polyamide resins ranges from 30,000 g / mol to 300,000 g / mol.

16. The diaphragm according to claim 13, wherein, The average diameter of the nanofibers is in the range of 10 nm to 200 nm.

17. The diaphragm according to claim 13, wherein, The thickness of the diaphragm is in the range of 1 μm to 50 μm.

18. The diaphragm according to claim 13, wherein, The membrane comprises two or more nanofiber layers, the nanofiber layers comprising nanofibers having a core-shell structure.

19. The diaphragm according to any one of claims 1 to 18, wherein, The tensile strength of the diaphragm is in the range of 50 MPa to 300 MPa.

20. The diaphragm according to any one of claims 1 to 18, wherein, The elongation of the diaphragm is in the range of 5% to 15%.

21. The diaphragm according to any one of claims 1 to 18, wherein, The porosity of the diaphragm is in the range of 20% to 65%.

22. A rechargeable lithium battery, said rechargeable lithium battery comprising: Positive electrode; negative electrode; as well as The diaphragm according to any one of claims 1 to 21 is located between the positive electrode and the negative electrode.