A thermally expandable microsphere and a composite separator containing it, and a secondary battery

By using core-shell structured ceramic-coated thermally expanding microspheres on lithium battery separators, the problems of poor electrolyte stability of coatings and easy damage to the shell of thermally expanding microspheres are solved. This enables rapid response and active thermal shutdown at high temperatures, reduces the risk of battery thermal runaway, and improves the durability and safety of the separator.

CN123121073APending Publication Date: 2026-11-17WUHAN INSTITUTES OF ADVANCED TECHNOLOGY CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611331153.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-31
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing lithium battery separator coatings have poor electrolyte stability, the thermal expansion microsphere shells are easily damaged, thermal response is hysteretic and passive protection is limited, posing a risk of thermal runaway.

Method used

The core-shell structure of the thermally expandable microspheres consists of an outer ceramic layer, an inner polymer resin layer, and a core material that is a foaming agent. By preparing ceramic-coated thermally expandable microspheres and coating them onto a base film, a semi-dense porous structure is formed, achieving both active expansion and passive heat resistance protection.

Benefits of technology

It improves the electrolyte resistance and mechanical strength of the separator, quickly blocks the contact between the positive and negative electrodes in thermal runaway scenarios, reduces the risk of battery thermal runaway, and extends service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123121073A_ABST
    Figure CN123121073A_ABST
Patent Text Reader

Abstract

This invention relates to the field of battery technology, and particularly to a thermally expandable microsphere and a composite separator and secondary battery containing the same. The thermally expandable microsphere provided by this invention has an outer shell material of ceramic, an inner shell material of polymer resin, and a core material of a foaming agent. The preparation method of the thermally expandable microsphere includes the following steps: preparing primary thermally expandable microspheres with a core material of a foaming agent and a shell material of polymer resin; adding ceramic precursor raw materials to an ethanol-water solution to obtain a ceramic precursor dispersion, heating and stirring, adding a pH adjuster to adjust the pH to 4-5, aging to obtain a transparent, precipitate-free ceramic nanosol; adding the primary thermally expandable microspheres to the ceramic nanosol, stirring and dispersing to allow colloidal particles to adsorb onto the surface of the microspheres; after adsorption, centrifuging at low speed to collect the microsphere precipitate, then heating for condensation and solidification, washing and drying to obtain ceramic-coated thermally expandable microspheres.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of battery technology, and in particular to a thermally expandable microsphere and a composite separator and a secondary battery containing the same. Background Technology

[0002] Conventional lithium-ion battery separators are primarily single-layer porous PP / PE membranes, placed between the positive and negative electrodes to provide insulation and ion transport. Existing technologies employ a composite structure of "base film + coating layer" to improve the separator's thermal stability. Ceramic coating is the most widely used technique, utilizing the high heat resistance of ceramic materials to delay thermal shrinkage and melting of the separator at high temperatures, thereby reducing the risk of thermal runaway and internal short circuits. For example, patent CN119695396A discloses a modified lithium-ion battery separator, its preparation method, and its application, which involves mixing ceramic particles, microcapsules, binders, and dispersants to form a ceramic coating, which is then loaded onto a polyolefin base film.

[0003] However, the existing technology has the following defects: (1) poor electrolyte stability of the coating: the functional layer (such as polymer layer, ceramic coating) is prone to swelling and aging when immersed in electrolyte for a long time. Especially under long-term cycling or high temperature environment, the coating is prone to peeling off and foaming agent leakage; (2) the outer shell of the thermal expansion microsphere is a linear low cross-linked thermoplastic resin with large molecular chain gaps. The electrolyte carbonate solvent can penetrate into the resin through the principle of like dissolves like. At the same time, the electrolyte hydrolysis produces HF hydrofluoric acid, which continuously destroys the resin of the expansion microsphere shell. Long-term cycling and After high-temperature storage, the microsphere shell cracks and the internal foaming agent leaks and fails; (3) The passive protection effect is limited: relying on the passive heat resistance of materials such as ceramics, the battery still has a high risk of thermal runaway under thermal abuse conditions due to the limited amount of ceramic materials used in the limited membrane thickness; (4) The thermal response is slow and the pores are not completely closed: the existing composite membrane has a slow thermal response speed, the membrane pores melt and close, and the mechanical strength is insufficient after the pores are closed, which easily leads to problems such as membrane breakage and thermal shrinkage. It cannot fundamentally block the contact between the positive and negative electrodes, and there is still a risk of short circuit and thermal runaway.

[0004] Based on the above analysis, it is very important to provide thermal expansion microspheres with good stability and whose wall material will not be damaged by electrolyte for use in battery separators. Summary of the Invention

[0005] This invention provides a thermally expandable microsphere to solve the problem that the shell material of existing thermally expandable microspheres is easily damaged in related technologies.

[0006] In a first aspect, the present invention provides a thermally expandable microsphere, wherein the outer shell material of the thermally expandable microsphere is a ceramic layer, the inner shell material is a polymer resin, and the core material is a foaming agent.

[0007] In some embodiments, the ceramic layer is selected from any one of alumina ceramic, spinel ceramic, and alumina-zirconia ceramic.

[0008] In some embodiments, the polymer resin is selected from materials with a glass transition temperature of less than 110°C, and the polymer resin is obtained by copolymerization of acrylonitrile, methacrylic acid, methyl methacrylate, and butyl acrylate in a mass ratio of 18:1.5:12:2-20:2:15:5 under the action of a crosslinking agent.

[0009] In some embodiments, the crosslinking agent is selected from any one of butanediol dimethacrylate, neopentyl glycol dimethacrylate, and polyethylene glycol dimethacrylate.

[0010] In some embodiments, the foaming agent is selected from C5-C7 alkanes or cycloalkanes.

[0011] In some preferred embodiments, the foaming agent is selected from any one of n-pentane, isopentane, n-hexane, cyclohexane, 2-methylpentane, 3-methylpentane, and n-heptane.

[0012] In some embodiments, the amount of the foaming agent is 5-8 times the sum of the mass of the mixture of acrylonitrile, methacrylic acid, methyl methacrylate, and butyl acrylate.

[0013] Secondly, the present invention provides a method for preparing the above-mentioned thermally expandable microspheres, comprising the following steps: Step S101: Prepare primary thermal expansion microspheres with a core material of foaming agent and a shell material of polymer resin; Step S102: Add the ceramic precursor raw material to an 80% ethanol aqueous solution to obtain a ceramic precursor dispersion with a solid content of 2wt%-12wt%. Hydrolyze it in a water bath at 40℃-60℃ with constant temperature stirring at 300 r / min for 1.5h-3h. Add a pH adjuster to adjust the pH to 4-5 and age for 2h to obtain a transparent ceramic nanosol without precipitation. In step S103, the primary thermally expanded microspheres from step S101 are added to the ceramic nanosol and stirred and dispersed at 150-200 r / min for 30 min. The ceramic nanocolloidal particles are uniformly deposited on the surface of the microspheres by electrostatic adsorption, hydrogen bonding and van der Waals forces to complete the physical adsorption coating. Then, the mixture is heated to 60-80℃ and stirred for 2-6 h. The adsorbed ceramic colloidal particles form a ceramic gel solid film through surface hydroxyl dehydration and condensation. After the reaction is completed, the microsphere precipitate is collected by centrifugation at 3000 r / min for 5 min, heated for condensation and solidification, washed repeatedly with anhydrous ethanol 2-3 times, and dried to obtain ceramic-coated thermally expanded microspheres.

[0014] In some embodiments, in step S102, the pH adjuster is selected from oxalic acid or acetic acid.

[0015] In some embodiments, in step S103, the mass ratio of the primary thermally expanded microspheres to the ceramic nanosol is 1:4-6.

[0016] In some embodiments, the ceramic precursor raw material is selected from one or more of aluminum isopropoxide, aluminum nitrate, and butyl zirconate, which, after hydrolysis, form alumina, alumina-zirconia, and magnesium aluminum spinel ceramic phases respectively.

[0017] In some embodiments, the drying conditions in step S103 are: vacuum degree ≤ -0.08 MPa, temperature 60-70℃, and time 8-12h.

[0018] In some embodiments, the total thickness of the outer and inner shells of the ceramic-coated thermal expansion microspheres is 0.3-5.0 μm.

[0019] In some embodiments, the preparation process of the primary thermal expansion microspheres is as follows: polyvinyl alcohol, silica sol, sodium nitrite, and sodium chloride are added to water and mixed evenly to obtain an aqueous phase; resin monomers, foaming agents, crosslinking agents, benzoyl peroxide, and divinylbenzene are mixed evenly and added to the aqueous phase, emulsified to obtain an oil-in-water emulsion, and heated to react at 60-80°C; after the reaction is completed, the mixture is centrifuged, washed, and dried to obtain the primary thermal expansion microspheres.

[0020] In some embodiments, the resin monomer is a mixture of acrylonitrile, methacrylic acid, methyl methacrylate, and butyl acrylate.

[0021] Thirdly, the present invention provides a composite membrane comprising the above-mentioned ceramic-coated thermally expanding microspheres, wherein the composite membrane further comprises a binder and a dispersant.

[0022] Fourthly, the present invention also provides a method for preparing the above-mentioned composite membrane, comprising the following steps: Step S201: Mix ceramic-coated thermal expansion microspheres, binder, dispersant and water, add to a disperser and disperse evenly to obtain a coating with a solid content of 30%-50%. Step S202: Using a slit coating process, the coating is evenly applied to one or both sides of the base film at a coating speed of 1-3 m / min. After drying at 80-120℃, the film is rolled up and slit to obtain the composite separator.

[0023] In some embodiments, the adhesive is selected from PVDF or PMMA.

[0024] In some embodiments, the dispersant is selected from polyvinylpyrrolidone or acrylic / polyether polymers.

[0025] In some embodiments, the mass ratio of ceramic-coated thermal expansion microspheres, PVDF binder, and dispersant is 42:5:1-45:7:1.

[0026] In some embodiments, the base membrane is selected as a PP membrane or a PE membrane with a porosity of 35%–50%.

[0027] Fifthly, the present invention also provides a secondary battery, wherein the separator of the secondary battery is the aforementioned composite separator.

[0028] This invention introduces ceramic-coated core-shell thermally expandable microspheres into the separator. The outer shell is a ceramic layer, the middle layer is a thermoplastic polymer, and the interior encapsulates low-boiling-point liquid alkanes, forming a stable microcapsule structure. At the microscopic level, it is a semi-dense porous structure formed by the accumulation of nanoparticles with a porosity of 10%-20%. This achieves excellent pressure resistance and electrolyte resistance within the normal operating temperature range. In thermal runaway scenarios, when the temperature reaches the glass transition point of the shell, the outer shell softens, the internal liquid alkanes rapidly vaporize, the internal pressure increases, and the volume expands sharply, directly blocking the contact between the positive and negative electrodes and cutting off the lithium-ion channel, thereby improving the battery's resistance to thermal runaway and reducing the risk of fire and explosion.

[0029] The process of membrane change at different temperatures in this invention is as follows: At room temperature (25–60℃): the ceramic thermal expansion microspheres maintain their original particle size (5–30μm), the membrane porosity is 30%–45%, the impedance is low, and the ion conduction is normal; At medium temperatures (90–110℃): the ceramic thermal expansion microspheres soften their shells and vaporize their cores, rapidly expanding (50–100 times) to fill and completely close the pores, blocking lithium-ion conduction and achieving thermal shutdown. High temperature (120–170℃): The ceramic layer and core shell structure work together to suppress shrinkage, retard flame and prevent the spread of thermal runaway.

[0030] The beneficial effects of the technical solution provided by this invention include: 1. This invention employs a core-shell composite microsphere structure with a core material as the foaming agent and a shell material consisting of polymer resin and a ceramic layer from the inside out. The ceramic layer is directly coated on the surface of the microsphere, giving the microsphere its own ceramic protective framework. This not only does not restrict the expansion of the microsphere but also leverages the heat resistance and corrosion resistance advantages of ceramics. Under thermal abuse conditions, the ceramic-coated thermally expanding microspheres can achieve rapid response and active expansion, sealing the pores of the separator, thickening the separator, and forming a stable physical barrier layer that blocks ion conduction and isolates the positive and negative electrode contacts. At the same time, the ceramic layer can delay heat conduction and inhibit oxygen diffusion from the positive electrode, achieving a dual synergy of active thermal shutdown and passive heat resistance protection, effectively suppressing battery thermal runaway. 2. The ceramic coating layer is chemically inert, which can effectively block the corrosion of thermally expanding microspheres by electrolytes, HF and other corrosive media, avoid microsphere swelling, aging and foaming agent leakage, and extend the service life of microspheres. At the same time, the ceramic layer improves the mechanical strength and wear resistance of microspheres, avoids microsphere damage during the cell manufacturing process, and improves the process adaptability and long-term durability of the separator. Attached Figure Description

[0031] To more clearly illustrate the technical solutions in the embodiments of the present invention, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0032] Figure 1 This is a schematic diagram of the structure of the ceramic-coated thermal expansion microspheres prepared in Example 1 of the present invention.

[0033] Figure 2 This is a schematic diagram of the structure of the diaphragm prepared in Example 1 of the present invention.

[0034] Figure 3 This is a microscope image of the ceramic-coated thermally expanding microspheres prepared in Example 1 of the present invention. Detailed Implementation

[0035] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0036] This invention provides a thermally expandable microsphere that solves the problem of easy damage to the shell material of existing thermally expandable microspheres.

[0037] Example 1: 300g deionized water, 0.1g polyvinyl alcohol, 20g silica sol, 0.01g sodium nitrite, and 100g sodium chloride were mixed and stirred evenly to obtain a Pickering emulsion aqueous phase. 180g isopentane, 18g acrylonitrile, 1.5g methacrylic acid, 12g methyl methacrylate, 2g butyl acrylate, 6g butanediol dimethacrylate, 4g benzoyl peroxide, and 1.8g divinylbenzene were mixed evenly to form an oil phase. This oil phase was added to the aqueous phase, and the mixture was homogenized and emulsified at high speed for 15 minutes to obtain an oil-in-water emulsion. This emulsion was transferred to a pressure-resistant reactor, and high-purity nitrogen was introduced to replace the air, maintaining a nitrogen atmosphere of 0.6MPa. The reactor was then sealed and pressurized at 65℃ for 8 hours. After the reaction, the pressure was released and the mixture was cooled, centrifuged, washed with deionized water, and dried to obtain primary thermally expanded microspheres. 22.4 g of aluminum isopropoxide was added to 778 g of 80% ethanol aqueous solution to obtain an alumina precursor dispersion with a solid content of 2.8 wt%. The dispersion was hydrolyzed in a 50°C water bath with constant temperature stirring at 300 r / min for 2 h. Oxalic acid was added to adjust the pH to 4, and the mixture was aged for 2 h to obtain a transparent ceramic nanosol without precipitate. 200g of the prepared primary thermally expanded microspheres were added to 800g of ceramic nanosol and dispersed by stirring at 150r / min for 30min. The mixture was then heated to 65℃ and stirred for 2h. After the reaction, the microsphere precipitate was collected by centrifugation at 3000r / min for 5min, heated to 60℃ for polycondensation and solidification, washed repeatedly with anhydrous ethanol 2-3 times, and dried in a vacuum drying oven at 70℃ for 12h under vacuum conditions ≤-0.08MPa to obtain ceramic-coated thermally expanded microspheres with a shell thickness of 0.3μm. A schematic diagram of the ceramic-coated thermally expanded microspheres is shown below. Figure 1 , Figure 1 In the diagram, 21 represents the foaming agent, 22 represents the polymer resin, and 23 represents the ceramic layer.

[0038] 340g of ceramic-coated thermally expandable microspheres, 52g of PVDF binder, 8g of polyvinylpyrrolidone, and 600g of water were mixed and added to a disperser, then dispersed evenly to obtain a coating with a solid content of 40%. A slot coating process was used to evenly coat the coating onto one or both sides of a PE film at a coating speed of 2m / min. The film was then dried at 90℃, wound up, and slit to obtain the composite separator. A schematic diagram of the composite separator is shown below. Figure 2 , Figure 2 In the diagram, 1 represents the base film, and 2 represents ceramic-coated thermally expanding microspheres.

[0039] Microscopic image of the ceramic-coated thermally expanding microspheres prepared in Example 1 is shown below. Figure 3 .

[0040] Example 2: 300g deionized water, 0.1g polyvinyl alcohol, 20g silica sol, 0.01g sodium nitrite, and 100g sodium chloride were mixed and stirred evenly to obtain a Pickering emulsion aqueous phase. 235.2g isopentane, 20g acrylonitrile, 1.8g methacrylic acid, 14.4g methyl methacrylate, 3g butyl acrylate, 6g butanediol dimethacrylate, 4g benzoyl peroxide, and 1.8g divinylbenzene were mixed evenly to form an oil phase. This oil phase was added to the aqueous phase and homogenized at high speed for 15 minutes to obtain an oil-in-water emulsion. This emulsion was transferred to a pressure-resistant reactor, and high-purity nitrogen was introduced to replace the air, maintaining a nitrogen atmosphere of 0.6MPa. The reactor was then heated under closed pressure at 65℃ for 8 hours. After the reaction, the pressure was released and the mixture was cooled, centrifuged, washed with deionized water, and dried to obtain primary thermally expanded microspheres. Aluminum nitrate and magnesium nitrate were mixed and compounded in a molar ratio of Al:Mg=2:1 to obtain a composite precursor. 42g of the composite precursor was weighed and added to 758g of an 80% ethanol aqueous solution to obtain a spinel precursor dispersion with a solid content of 5.25wt%. The mixture was hydrolyzed in a 45℃ water bath with constant temperature stirring at 300 r / min for 2h. Oxalic acid was added to adjust the pH to 4, and the mixture was aged for 2h to obtain a transparent ceramic nanosol without precipitate. 200g of the prepared primary thermal expansion microspheres were added to 800g of ceramic nanosol and dispersed by stirring at 150r / min for 30min. Then, the mixture was heated to 80℃ and stirred for 2h. After the reaction was completed, the microsphere precipitate was collected by centrifugation at 3000r / min for 5min. The precipitate was then heated to 60℃ for polycondensation and solidification. The microspheres were washed repeatedly with anhydrous ethanol 2-3 times and dried in a vacuum drying oven at 65℃ with a vacuum degree ≤-0.08 MPa for 8h to obtain ceramic-coated thermal expansion microspheres with a shell thickness of 0.6μm.

[0041] 258g of ceramic-coated thermal expansion microspheres, 36g of PVDF binder, 6g of polyvinylpyrrolidone, and 700g of water were mixed and added to a disperser and dispersed evenly to obtain a coating with a solid content of 30%. The coating was then uniformly coated on one or both sides of a PP base film using a slot coating process at a coating speed of 3m / min. After drying at 100℃, the film was wound up and slit to obtain a composite diaphragm.

[0042] Example 3: 300g deionized water, 0.1g polyvinyl alcohol, 20g silica sol, 0.01g sodium nitrite, and 100g sodium chloride were mixed and stirred evenly to obtain a Pickering emulsion aqueous phase. 210g n-hexane, 20g acrylonitrile, 2g methacrylic acid, 15g methyl methacrylate, 5g butyl acrylate, 6g butanediol dimethacrylate, 4g benzoyl peroxide, and 2.0g divinylbenzene were mixed evenly to form an oil phase. This oil phase was added to the aqueous phase and homogenized at high speed for 15 minutes to obtain an oil-in-water emulsion. This emulsion was transferred to a pressure-resistant reactor, and high-purity nitrogen was introduced to replace the air, maintaining a nitrogen atmosphere of 0.6MPa. The reactor was then heated under closed pressure at 65℃ for 8 hours. After the reaction, the pressure was released and the mixture was cooled, centrifuged, washed with deionized water, and dried to obtain primary thermally expanded microspheres. Aluminum nitrate and butyl zirconate were mixed and compounded in a molar ratio of Al:Zr=6:1 to obtain a composite precursor. 48g of the composite precursor was weighed and added to 752g of ethanol aqueous solution with a volume concentration of 80% to obtain an alumina-zirconia precursor dispersion with a solid content of 6wt%. The dispersion was hydrolyzed in a 60℃ water bath with constant temperature stirring at 300 r / min for 2h. Oxalic acid was added to adjust the pH to 4, and the mixture was aged for 2h to obtain a transparent ceramic nanosol without precipitate. 200g of the prepared primary thermal expansion microspheres were added to 800g of ceramic nanosol and dispersed by stirring at 200r / min for 30min. Then, the mixture was heated to 80℃ and stirred for 3h. After the reaction was completed, the microsphere precipitate was collected by centrifugation at 3000r / min for 5min. The precipitate was then heated to 60℃ for polycondensation and solidification. The microspheres were washed repeatedly with anhydrous ethanol 2-3 times and dried in a vacuum drying oven at 60℃ for 8h under a vacuum of ≤-0.08 MPa to obtain ceramic-coated thermal expansion microspheres with a shell thickness of 1.2μm.

[0043] 425g of ceramic-coated thermal expansion microspheres, 65g of PVDF binder, 10g of polyvinylpyrrolidone, and 500g of water were mixed and added to a disperser and dispersed evenly to obtain a coating with a solid content of 50%. The coating was then uniformly coated on one or both sides of the base film using a slot coating process at a coating speed of 3m / min. After drying at 90℃, the film was wound up and slit to obtain the composite diaphragm.

[0044] Example 4: 300g deionized water, 0.1g polyvinyl alcohol, 20g silica sol, 0.01g sodium nitrite, and 100g sodium chloride were mixed and stirred evenly to obtain a Pickering emulsion aqueous phase. 180g isopentane, 18g acrylonitrile, 1.5g methacrylic acid, 12g methyl methacrylate, 2g butyl acrylate, 6g butanediol dimethacrylate, 4g benzoyl peroxide, and 1.8g divinylbenzene were mixed evenly to form an oil phase. This oil phase was added to the aqueous phase, and the mixture was homogenized and emulsified at high speed for 15 minutes to obtain an oil-in-water emulsion. This emulsion was transferred to a pressure-resistant reactor, and high-purity nitrogen was introduced to replace the air, maintaining a nitrogen atmosphere of 0.6MPa. The reactor was then sealed and pressurized at 65℃ for 8 hours. After the reaction, the pressure was released and the mixture was cooled, centrifuged, washed with deionized water, and dried to obtain primary thermally expanded microspheres. 32g of aluminum isopropoxide raw material was added to 768g of ethanol aqueous solution with a volume concentration of 80% to obtain an alumina precursor dispersion with a solid content of 4wt%. The dispersion was hydrolyzed in a 55℃ water bath with constant temperature stirring at 300 r / min for 2h. Oxalic acid was added to adjust the pH to 4, and the mixture was aged for 2h to obtain a transparent ceramic nanosol without precipitation. 200g of the prepared primary thermal expansion microspheres were added to 850g of ceramic nanosol and dispersed by stirring at 150r / min for 30min. Then, the mixture was heated to 65℃ and stirred for 3h. After the reaction was completed, the microsphere precipitate was collected by centrifugation at 3000r / min for 5min. The precipitate was then heated to 60℃ for polycondensation and solidification. The microspheres were washed repeatedly with anhydrous ethanol 2-3 times and dried in a vacuum drying oven at 70℃ for 9h under a vacuum of ≤-0.08 MPa to obtain ceramic-coated thermal expansion microspheres with a shell thickness of 0.9μm.

[0045] 261g of ceramic-coated thermal expansion microspheres, 33g of PMMA binder, 6g of polyvinylpyrrolidone, and 700g of water were mixed and added to a disperser and dispersed evenly to obtain a coating with a solid content of 30%. The coating was then uniformly coated on one or both sides of the base film using a slot coating process at a coating speed of 2m / min. After drying at 95℃, the film was wound up and slit to obtain the composite diaphragm.

[0046] Example 5: 300g deionized water, 0.1g polyvinyl alcohol, 20g silica sol, 0.01g sodium nitrite, and 100g sodium chloride were mixed and stirred evenly to obtain a Pickering emulsion aqueous phase. 180g isopentane, 18g acrylonitrile, 1.5g methacrylic acid, 12g methyl methacrylate, 2g butyl acrylate, 6g butanediol dimethacrylate, 4g benzoyl peroxide, and 1.8g divinylbenzene were mixed evenly to form an oil phase. This oil phase was added to the aqueous phase, and the mixture was homogenized and emulsified at high speed for 15 minutes to obtain an oil-in-water emulsion. This emulsion was transferred to a pressure-resistant reactor, and high-purity nitrogen was introduced to replace the air, maintaining a nitrogen atmosphere of 0.6MPa. The reactor was then sealed and pressurized at 65℃ for 8 hours. After the reaction, the pressure was released and the mixture was cooled, centrifuged, washed with deionized water, and dried to obtain primary thermally expanded microspheres. Aluminum nitrate and magnesium nitrate were mixed and compounded in a molar ratio of Al:Mg=2:1 to obtain a composite precursor. 48g of the composite precursor was weighed and added to 752g of an 80% ethanol aqueous solution to obtain a spinel precursor dispersion with a solid content of 6wt%. The mixture was hydrolyzed in a 50℃ water bath with constant temperature stirring at 300 r / min for 2h. Oxalic acid was added to adjust the pH to 4, and the mixture was aged for 2h to obtain a transparent ceramic nanosol without precipitate. 200g of the prepared primary thermal expansion microspheres were added to 800g of ceramic nanosol and dispersed by stirring at 200r / min for 30min. Then, the mixture was heated to 60℃ and stirred for 3h. After the reaction was completed, the microsphere precipitate was collected by centrifugation at 3000r / min for 5min. The precipitate was then heated to 60℃ for polycondensation and solidification. The microspheres were washed repeatedly with anhydrous ethanol 2-3 times and dried in a vacuum drying oven at 65℃ for 12h under vacuum conditions ≤-0.08 MPa to obtain ceramic-coated thermal expansion microspheres with a shell thickness of 1.5μm.

[0047] 420g of ceramic-coated thermal expansion microspheres, 70g of PVDF binder, 10g of polyvinylpyrrolidone, and 500g of water were mixed and added to a disperser and dispersed evenly to obtain a coating with a solid content of 50%. The coating was then uniformly coated on one or both sides of the base film using a slot coating process at a coating speed of 1m / min. After drying at 90℃, the film was wound up and slit to obtain the composite diaphragm.

[0048] Comparative Example 1: The difference between Comparative Example 1 and Example 1 is that primary thermally expanded microspheres were used in the preparation of the diaphragm, while the rest of the process was basically the same as in Example 1.

[0049] Comparative Example 2: The difference between Comparative Example 2 and Example 1 is as follows: The process of preparing the diaphragm is as follows: 170g of primary thermal expansion microspheres, 170g of alumina ceramic, 52g of PVDF binder, 8g of dispersant and 600g of water are mixed and added to a disperser and dispersed evenly to obtain a coating with a solid content of 40%; a slit coating process is used to evenly coat the coating on one or both sides of the base film at a coating speed of 2m / min, and then dried at 90°C, wound up and cut to obtain the composite diaphragm.

[0050] Comparative Example 3: The only difference between Comparative Example 3 and Example 1 is that the mass of aluminum isopropoxide used is 9g; the rest of the process is basically the same as in Example 1.

[0051] Comparative Example 4: The only difference between Comparative Example 4 and Example 1 is that the membrane preparation process is as follows: 340g of alumina ceramic, 52g of PVDF binder, 8g of dispersant and 600g of water are mixed and added to a disperser and dispersed evenly to obtain a coating with a solid content of 40%; a slit coating process is used to evenly coat the coating on one or both sides of the PE film at a coating speed of 2m / min, and then dried at 90°C, wound up and cut to obtain the composite membrane.

[0052] Comparative Example 5: The only difference between Comparative Example 5 and Example 1 is that the process of preparing ceramic-coated thermal expansion microspheres is as follows: 200g of the prepared primary thermal expansion microspheres are added to 800g of ceramic nanosol, stirred and dispersed at 300r / min for 30min, then heated to 65℃ and stirred for 3h. After the reaction is completed, the microspheres are centrifuged at 3000r / min for 5min, washed repeatedly with anhydrous ethanol 2-3 times, and dried in a vacuum drying oven at 70℃ for 12h with a vacuum degree ≤-0.08MPa to obtain ceramic-coated thermal expansion microspheres.

[0053] The separators prepared in Examples 1-5 and Comparative Examples 1-5 were applied to lithium-ion batteries. The battery assembly process was as follows: positive electrode → separator → negative electrode → stacking / winding → encapsulation → electrolyte injection → formation → capacity testing, resulting in a lithium-ion battery (capacity 5Ah). NCM811 was used as the positive electrode material, graphite as the negative electrode material, and conventional LiPF6 electrolyte. The battery underwent thermal abuse performance testing (thermal chamber test: 130±2℃, 30min), and the results are shown in Table 1.

[0054] Table 1: Thermal abuse performance test results of batteries from Examples 1-5 and Comparative Examples 1-5 ; As can be seen from the results of Examples 1-5 and Comparative Example 1 in Table 1, the battery without ceramics experienced thermal runaway and fire after 22 minutes. The inventors analyzed that this was because the bare microspheres had no continuous inorganic barrier layer, and the electrolyte continuously corroded the microspheres, leading to microsphere failure after long cycles.

[0055] As can be seen from the results of Examples 1-5 and Comparative Example 2 in Table 1, the battery obtained by physically mixing thermally expanded microspheres and ceramic layers experienced thermal runaway and fire within 28 minutes. The inventors analyzed that this was because the ceramic and microspheres were independently dispersed, and there was no continuous ceramic protective layer to wrap the individual microspheres. The electrolyte hydrolysis produced HF that continuously corroded the microspheres. After long-term cycling, a large number of microspheres were damaged, the foaming agent leaked and became inactive, and thermal runaway occurred during the thermal abuse test.

[0056] As can be seen from the results of Examples 1-5 and Comparative Example 3 in Table 1, the battery obtained by reducing the amount of ceramic layer showed a near-runaway phenomenon during the thermal abuse performance test. The inventors analyzed that this was because the ceramic coating layer was incomplete and the thickness was insufficient, the protective barrier was not complete, the microspheres were easily corroded by the electrolyte at high temperature, the separator partially melted during the test, and the battery was close to thermal runaway.

[0057] As can be seen from the results of Examples 1-5 and Comparative Example 4 in Table 1, the battery obtained by adding only ceramic exhibits severe thermal runaway. The inventors analyzed that this is because relying solely on the passive heat resistance of ceramic without actively expanding to seal the pore structure of the separator, the high-temperature electrode contact cannot be isolated, resulting in violent gas production and smoke emission, leading to severe thermal runaway.

[0058] As can be seen from the results of Examples 1-5 and Comparative Example 5 in Table 1, the batteries prepared after increasing the rotation speed exhibited a small amount of electrolyte leakage. The inventors analyzed that this was because after increasing the rotation speed, the high-speed shearing destroyed the ceramic nanocolloid particles adsorbed on the surface of the microspheres. The ceramic layer was only physically loosely attached and did not form a continuous and dense inorganic film. There were a large number of micropore defects, poor adhesion, and a significant decrease in electrolyte barrier performance. The high-temperature storage capacity decayed significantly, and thermal abuse resulted in local bulging and a small amount of electrolyte leakage.

[0059] In embodiments 1-5 of this invention, a continuous and dense ceramic shell is grown in situ on the surface of thermally expandable microspheres. The dense inorganic ceramic isolates the electrolyte from HF corrosion, significantly reducing high-temperature storage capacity decay and improving long-cycle stability. At the same time, the thickness of the ceramic shell is controlled within the range of 0.3 to 1.5 μm, which not only completely protects the internal microspheres from being eroded and rendered ineffective by the electrolyte, but also does not rigidly restrict the expansion of the microspheres. During thermal abuse, the microspheres expand rapidly to block the membrane pores and physically separate the positive and negative electrodes, resulting in only slight bulging or no bulging, no leakage, no fire, low high-temperature storage decay, and excellent long-cycle stability.

[0060] In the description of this specification, the references to terms such as "one embodiment / mode," "some embodiments / modes," "example," "specific example," or "some examples," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment / mode or example is included in at least one embodiment / mode or example of the present invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment / mode or example. Moreover, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments / modes or examples. Furthermore, without contradiction, those skilled in the art can combine and integrate the different embodiments / modes or examples described in this specification, as well as the features of different embodiments / modes or examples.

[0061] It should be noted that in this invention, relational terms such as "first" and "second" are used merely to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Without further limitations, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes said element. In this invention, "a plurality of" means at least two, such as two, three, etc., unless otherwise expressly specified.

[0062] The above description is merely a specific embodiment of the present invention, enabling those skilled in the art to understand or implement the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the present invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features claimed herein.

Claims

1. A thermally expandable microsphere, characterized in that, The outer shell of the thermally expanding microspheres is a ceramic layer, the inner shell is a polymer resin, and the core is a foaming agent.

2. The thermally expanding microspheres according to claim 1, characterized in that, The ceramic layer is selected from any one of alumina ceramic, spinel ceramic, and alumina-zirconia ceramic.

3. The thermally expanding microspheres according to claim 1, characterized in that, The polymer resin is obtained by copolymerizing acrylonitrile, methacrylic acid, methyl methacrylate, and butyl acrylate under the action of a crosslinking agent.

4. The thermally expanding microspheres according to claim 1, characterized in that, The foaming agent is selected from C5-C7 alkanes or cycloalkanes.

5. A method for preparing thermally expandable microspheres, characterized in that, Includes the following steps: S101, Preparation of primary thermal expansion microspheres with foaming agent as core material and polymer resin as shell material; S102, ceramic precursor raw materials are added to an ethanol aqueous solution to obtain a ceramic precursor dispersion, which is heated and stirred, and a pH adjuster is added to adjust the pH to 4-5. After aging, a transparent ceramic nanosol without precipitate is obtained. S103, the primary thermal expansion microspheres from step S101 are added to the ceramic nanosol, stirred and dispersed, then heated and stirred. After the reaction is complete, the microspheres are centrifuged, washed and dried to obtain ceramic-coated thermal expansion microspheres.

6. The method for preparing thermally expandable microspheres according to claim 5, characterized in that, In step S103, the drying conditions are: vacuum degree ≤ -0.08 MPa, temperature 60-70℃, and time 8-12h.

7. The method for preparing thermally expandable microspheres according to claim 5, characterized in that, The total thickness of the outer and inner shells of the ceramic-coated thermal expansion microspheres is 0.3-5.0 μm.

8. The method for preparing thermally expandable microspheres according to claim 5, characterized in that, In step S101, the preparation process of the primary thermal expansion microspheres is as follows: polyvinyl alcohol, silica sol, sodium nitrite, and sodium chloride are added to water and mixed evenly to obtain an aqueous phase; resin monomer, foaming agent, crosslinking agent, benzoyl peroxide, and divinylbenzene are mixed evenly and added to the aqueous phase, emulsified to obtain an oil-in-water emulsion, and heated to react at 60-80℃; after the reaction is completed, the mixture is centrifuged, washed, and dried to obtain the primary thermal expansion microspheres.

9. A composite diaphragm, characterized in that, At least one side of the composite diaphragm is coated with ceramic-coated thermally expandable microspheres as described in any one of claims 1-4 or ceramic-coated thermally expandable microspheres prepared by the preparation method described in any one of claims 5-8.

10. A secondary battery, characterized in that, Includes the composite diaphragm as described in claim 9.