A high-adhesion, high-flexibility PVDF porous lithium battery separator coating and its preparation method

Through the synergistic effect of aqueous PVDF emulsion with demulsifiers, organic solvents, dispersants and pH adjusters, a three-dimensional network porous structure is formed, which solves the problems of high adhesion, non-clogging, high flexibility and ultra-long cycle life of lithium battery separator coatings, making it suitable for industrial production.

CN123121084APending Publication Date: 2026-11-17HUIZHOU XURAN NEW ENERGY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611413241.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-11
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing lithium battery separator coatings struggle to simultaneously achieve high bonding strength, non-clogging pores, high flexibility, and ultra-long cycle life. In particular, aqueous PVDF coatings suffer from problems such as decreased bonding strength, uneven pore distribution, and brittleness after the addition of inorganic fillers.

Method used

By employing the synergistic effect of water-based PVDF emulsion with demulsifiers, organic solvents, dispersants, and pH adjusters, a three-dimensional network porous structure is formed through controllable micro-demulsification. Combined with a three-stage low-temperature gradient drying process, this ensures that the coating possesses high bonding strength, low air permeability, and excellent resistance to long-term cyclic brittle fracture without the presence of inorganic fillers.

Benefits of technology

It achieves high bonding strength (dry peel strength 22-32 N/m, wet peel strength 11-17 N/m), excellent ion transport performance (air permeability increase of only 5-10 s/100cc) and ultra-long cycle stability (capacity retention rate ≥80% after 2000 cycles), making it suitable for industrial mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention relates to the field of lithium battery separator technology, and more particularly to a high-adhesion, high-flexibility PVDF porous lithium battery separator coating and its preparation method. The high-adhesion, high-flexibility PVDF porous lithium battery separator coating is a three-dimensional network porous structure covering the surface of the separator base membrane, formed by controlled micro-demulsification and drying of an aqueous coating slurry. The aqueous coating slurry comprises the following components: 40-60% aqueous PVDF emulsion, 0.05-1.0% demulsifier, 0.5-3.0% organic solvent, 0.2-0.8% dispersant, 0.5-2.0% alcohol ester film-forming aid, with deionized water to make up the balance, and a pH adjuster to 4.5-6.0. Through precise process parameters and a three-stage low-temperature gradual drying process, a lithium battery separator coating is prepared, exhibiting high adhesion strength, excellent ion transport performance, and ultra-long cycle stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of lithium battery separator technology, and in particular to a high-adhesion, high-flexibility PVDF porous lithium battery separator coating and its preparation method. Background Technology

[0002] Lithium-ion battery separators are crucial components for isolating the positive and negative electrodes, preventing short circuits, and allowing lithium ions to pass through. Simple polyolefin (PE / PP) separators are no longer sufficient to meet the requirements. Currently, there is a lack of effective adhesion between the polyolefin separator and the electrode, leading to interface separation and affecting battery performance and lifespan. Coating the separator surface with a PVDF coating can provide good adhesion and electrochemical stability. However, solvent-based PVDF coatings suffer from problems such as high pollution and high cost. Aqueous PVDF coatings have become a focus of industry development, but significant pain points still exist.

[0003] Firstly, the method of adding inorganic fillers: Commercial water-based PVDF coatings often use a composite formula of "PVDF emulsion + inorganic fillers such as fumed silica / alumina," utilizing the gaps between the filler particles to construct ion transport channels. However, this method has obvious drawbacks: the inert filler dilutes the continuous PVDF phase, leading to a significant decrease in the adhesion strength between the coating and the electrode, making it prone to powder shedding and detachment; the nanofiller is prone to agglomeration, causing uneven channel distribution and affecting the uniform transport of lithium ions; and the detached particles pose a risk of causing micro-short circuits. Patent CN104752659A discloses a composite coating scheme of PVDF and ceramic particles, but the adhesion strength is inversely proportional to the amount of filler added, making it impossible to simultaneously achieve high adhesion and porosity.

[0004] Secondly, the pure PVDF emulsion solution: While significantly improving bonding strength without adding inorganic fillers, it faces two major challenges: First, during the drying process of the PVDF emulsion, latex particles easily fuse on a large scale to form a dense film, leading to pore blockage and a sharp increase in battery internal resistance. Second, after long-term immersion in the electrolyte, PVDF undergoes swelling and recrystallization, causing the coating to gradually become brittle and delaminate under cyclic stress, resulting in a precipitous decrease in cycle life. Patent CN104130647A achieves "complete demulsification" of the PVDF emulsion to form a porous coating through heating and salting. However, the demulsified PVDF particles are merely physically stacked, lacking sufficient cohesive strength, and still pose a risk of particle detachment during long cycles, while not solving the coating brittleness problem.

[0005] Other attempts at existing technologies also have some shortcomings: for example, although adding small molecule plasticizers can improve flexibility, they are easily extracted and dissolved by the electrolyte, which reduces the toughening effect and introduces impurities, affecting battery safety; and the route of using solvents such as NMP to dissolve PVDF returns to the solvent-based system, which has no advantage in terms of environmental protection and cost, and has a high risk of solvent residue and dense pore blockage.

[0006] In summary, current technologies lack a solution for water-based PVDF membrane coatings that can simultaneously achieve "high adhesion, non-clogging, and high flexibility." There is an urgent need to develop new technologies to meet the stringent requirements of high-end batteries for long cycle life. Summary of the Invention

[0007] To achieve the desired effects of high adhesion strength, non-clogging, high flexibility, ultra-long cycle life, and absence of inorganic fillers in lithium battery separator coatings, making them suitable for industrial mass production, this invention provides a high-adhesion, high-flexibility PVDF porous lithium battery separator coating and its preparation method.

[0008] In a first aspect, this application provides a highly adhesive and flexible PVDF porous lithium battery separator coating, employing the following technical solution: A highly adhesive and flexible PVDF porous lithium battery separator coating is formed by a three-dimensional network porous structure covering the surface of the separator base film after controllable micro-demulsification and drying of an aqueous coating slurry. The aqueous coating slurry comprises, by mass percentage, the following components: 40-60% aqueous PVDF emulsion, 0.05-1.0% demulsifier, 0.5-3.0% organic solvent, 0.2-0.8% dispersant, 0.5-2.0% alcohol ester film-forming aid, and deionized water to make up the balance. The pH value is adjusted to 4.5-6.0 using a pH adjuster. The organic solvent is composed of two or more of the following: propylene glycol methyl ether, propylene glycol methyl ether acetate, dipropylene glycol methyl ether, ethylene glycol butyl ether, NMP, and DMAC. The dispersant is composed of a polycarboxylate dispersant and a polyacrylic acid dispersant in a mass ratio of 1:(0.3-1.5); The pH adjuster is any one of dilute acetic acid, citric acid, and dilute hydrochloric acid; The aqueous coating slurry does not contain fumed silica, fumed alumina, or inorganic nanofillers.

[0009] Through the above technical solution, the aqueous PVDF emulsion constitutes the main body of the coating, providing basic adhesion; the pH adjuster and demulsifier work synergistically to precisely control the emulsion to a weakly thixotropic micro-demulsification intermediate state through a dual mechanism of protonation and salting out, forming a continuous three-dimensional network porous framework that balances high adhesion and ion transport; the organic solvents, in combination of two or more, only partially swell and plasticize the particle fusion connection points, achieving synergistic toughening without complete demulsification and pore blockage; the polycarboxylate and polyacrylic acid dispersants are combined to form a dual mechanism of "electrostatic repulsion + steric hindrance" protection, ensuring uniform and stable slurry throughout the micro-demulsification process; and alcohol ester film-forming aids improve coating continuity and base film adhesion. The synergistic effect of each component enables the coating to simultaneously possess high adhesion strength, low air permeability increase, and excellent resistance to long-term cyclic brittle fracture, without any inorganic fillers.

[0010] Preferably, the demulsifier is a compound of sodium chloride and sodium citrate in a mass ratio of 1:(0.5-2).

[0011] Through the above technical solution, sodium chloride and sodium citrate are combined to form a synergistic demulsification system of "driving force + buffer". Sodium chloride, as a neutral strong electrolyte, compresses the electric double layer on the surface of PVDF latex particles through the salting-out effect, reducing electrostatic repulsion and providing the core driving force for micro-demulsification. Sodium citrate, as a weak acid salt, forms a buffer reaction against the acidic microenvironment after hydrolysis, preventing local pH drops from causing uncontrolled demulsification. The two, one "attacking" and the other "defending", make the demulsification process stable and controllable, allowing latex particles to fuse uniformly and to a limited extent, precisely stopping at the weakly thixotropic micro-demulsification intermediate state, avoiding complete demulsification or insufficient demulsification, and laying the foundation for the subsequent formation of a continuous three-dimensional network porous structure.

[0012] Preferably, the solid content of the aqueous PVDF emulsion is 40-50%, and the average particle size of the latex particles is 100-300 nm.

[0013] Preferably, the pH adjuster is dilute acetic acid, which adjusts the pH of the system to 5-5.5.

[0014] Preferably, the organic solvent is composed of propylene glycol methyl ether acetate and ethylene glycol butyl ether in a mass ratio of 1:(0.2-1).

[0015] The above technical solution employs a combination of propylene glycol methyl ether acetate (PMA) and ethylene glycol butyl ether (BCS) to form a toughening mechanism of "penetration-carrying + synergistic swelling". BCS has low surface tension and strong wetting and penetration properties, allowing it to quickly wet the surface of PVDF particles and carry PMA to the deep layers of the three-dimensional network connection points; PMA has moderate swelling capacity, plasticizing and toughening the connection points. The synergistic effect of both achieves efficient toughening without damaging the porous framework at low addition levels.

[0016] Preferably, the dispersant is composed of sodium polycarboxylate and sodium polyacrylate in a mass ratio of 1:(0.5-1).

[0017] The above technical solution employs a combination of sodium polycarboxylate and sodium polyacrylate to form a dual-mechanism protection of "electrostatic repulsion + steric hindrance". Sodium polycarboxylate provides strong electrostatic repulsion, while sodium polyacrylate continuously exerts steric hindrance in the acidic micro-demulsification environment, preventing excessive aggregation of latex particles due to weakened electrostatic charge, thus ensuring uniform and stable slurry throughout the micro-demulsification process, without flocculation or stratification.

[0018] Preferably, the alcohol ester film-forming aid is either dodecyl alcohol ester or ethylene glycol butyl ether acetate.

[0019] Preferably, the pore size distribution of the three-dimensional mesh porous structure is 30-80 nm, and the porosity is 35-45%.

[0020] Secondly, this application provides a method for preparing a highly adhesive and flexible PVDF porous lithium battery separator coating, comprising the following steps: S1. After mixing deionized water and dispersant evenly, add aqueous PVDF emulsion to prepare the basic slurry; S2. Heat the basic slurry prepared in step S1 to 25-35℃, add pH adjuster dropwise at a rate of 2-5mL / min under stirring conditions of 800-1000r / min, then add demulsifier in batches, and continue stirring for 30-40min until the slurry is free of flocculation and does not separate into layers. S3. Add organic solvent dropwise to the slurry obtained in step S2 at a rate of 1-3 mL / min, and continue stirring for 20-30 min; S4. Add alcohol ester film-forming aid, mix evenly, add deionized water to make up the balance, let stand to degas, and obtain water-based coating slurry; S5. Apply the aqueous coating slurry obtained in step S4 to the surface of the separator base membrane, and dry it using a three-stage low-temperature gradient drying process to obtain a high-adhesion, high-flexibility PVDF porous lithium battery separator coating.

[0021] Preferably, the aqueous coating slurry in step S5 is applied to one or both sides of the diaphragm base membrane; the coating method is either microgravure coating or comma blade coating, the coating speed is 50-80 m / min, and the coating thickness is 1-3 μm.

[0022] Preferably, step S5 adopts a three-stage low-temperature gradual drying process: drying in the first temperature zone of 40-50℃, the second temperature zone of 55-65℃, and the third temperature zone of 70-80℃, with a total drying time of 3-5 minutes.

[0023] The above technical solution, through precise process parameters and a three-stage low-temperature gradual drying process, ensures controllable micro-demulsification and pore structure shaping. In S2, a gentle temperature of 25-35℃ and a high-speed stirring rate of 800-1000 r / min are matched to ensure rapid and uniform dispersion of the pH adjuster and demulsifier, preventing uncontrolled demulsification caused by excessively high local concentrations. In S3, the organic solvent is added slowly to ensure uniform toughening without damaging the three-dimensional framework. S5 employs a three-stage low-temperature gradual drying process, progressively removing free water and capillary water by gradually increasing the temperature, avoiding strong capillary forces that could collapse the pores due to high-temperature flash evaporation. Finally, the thermal fixation of particle connection points and pore structure shaping are completed in the third temperature zone.

[0024] In summary, this application has the following beneficial effects: 1. The high-adhesion and high-flexibility PVDF porous lithium battery separator coating prepared in this application has high adhesion strength (dry peel strength 22-32N / m, wet peel strength 11-17N / m), excellent ion transport performance (air permeability increase of only 5-10s / 100cc) and ultra-long cycle stability (capacity retention rate ≥80% after 2000 cycles), which breaks through the technical problem that existing aqueous PVDF coatings cannot simultaneously achieve "high adhesion - non-clogging - high flexibility".

[0025] 2. The preparation method of the high-adhesion and high-flexibility PVDF porous lithium battery separator coating of this application is simple to operate and has mild conditions. The demulsification temperature of 25-35℃ and the coating speed of 50-80m / min can be directly adapted to existing industrial separator coating production lines. The three-stage low-temperature gradient drying process effectively shapes the pore structure and avoids the pore blockage problem caused by high-temperature drying. The process window is wide and the controllability is strong, which has good industrial promotion value. Detailed Implementation

[0026] The technical solutions of this application are further illustrated by specific embodiments below. These specific embodiments do not represent a limitation on the scope of protection of this application. Any non-essential modifications and adjustments made by others based on the concept of this application still fall within the scope of protection of this application.

[0027] Unless otherwise specified, the test methods shown in the following examples are conventional methods. All reagents and materials shown are commercially available products; wherein: Aqueous PVDF emulsion: Arkema (Changshu) Specialty Materials Co., Ltd., Kynar® Aquatec® series, solid content 45%, average particle size 200nm; Sodium polycarboxylate dispersant: Sanopco Co., Ltd., Model: SN-5040, Solid content 40%, Anionic type; Sodium polyacrylate dispersant: Commercially available industrial grade PAAS, solid content 45%, molecular weight 3000-5000; PE porous membrane: Shanghai Enjie New Material Technology Co., Ltd.; Model: ND12, thickness 12μm.

[0028] Propylene glycol methyl ether acetate (PMA); ethylene glycol butyl ether (BCS); N-methylpyrrolidone (NMP); dipropylene glycol methyl ether (DPM) The present application will be further described in detail below with reference to embodiments and comparative examples. Example

[0029] Example 1 A method for preparing a highly adhesive and flexible PVDF porous lithium battery separator coating is provided, comprising the following steps: S1. Mix 200g of deionized water with the dispersant and stir evenly, then add the aqueous PVDF emulsion to prepare the basic slurry; S2. Heat the basic slurry prepared in step S1 to 30°C, add pH adjuster dropwise at a rate of 3 mL / min under stirring conditions of 900 r / min, then add demulsifier in batches, and continue stirring for 30 min to achieve controllable micro-demulsification until the slurry is weakly thixotropic and has no flocculation or stratification. S3. Add organic solvent dropwise to the slurry obtained in step S2 at a rate of 2 mL / min, and continue stirring for 25 min; S4. Add alcohol ester film-forming aid, mix evenly, add deionized water to make up the balance, let stand to degas, and obtain water-based coating slurry; S5. The aqueous coating slurry obtained in step S4 is applied to one side of the separator base membrane using a micro-gravure coating at a speed of 60 m / min and a coating thickness of 2 μm. A three-stage low-temperature gradient drying process is adopted, with the first temperature zone at 40°C, the second temperature zone at 60°C, and the third temperature zone at 80°C for drying. The total drying time is 4 min, thus obtaining a high-adhesion and high-flexibility PVDF porous lithium battery separator coating.

[0030] The pH adjuster is dilute acetic acid (10wt%), which adjusts the pH of the system to 5.0.

[0031] The base membrane of the diaphragm is a PE porous diaphragm ND12.

[0032] The composition and dosage of the aqueous coating slurry are shown in Table 1.

[0033]

[0034] Example 2 The difference from Example 1 is that the composition and dosage of the aqueous coating slurry are shown in Table 1; the pH adjuster is dilute acetic acid (concentration 10wt%), which adjusts the pH of the system to 5.5.

[0035] Example 3 The difference from Example 1 is that the composition and dosage of the aqueous coating slurry are shown in Table 1; the pH adjuster is dilute acetic acid (concentration 8wt%), which adjusts the pH of the system to 5.0.

[0036] Example 4 The difference from Example 1 is as follows: the composition and dosage of the aqueous coating slurry are shown in Table 1; in step S2 of the preparation method, the base slurry prepared in step S1 is heated to 25°C, and a pH adjuster is added dropwise at a rate of 2 mL / min under stirring at 1000 r / min, followed by the addition of demulsifier in batches, and stirring is continued for 30 min until the slurry is free of flocculation and stratification; in step S3, an organic solvent is added dropwise to the slurry obtained in step S2 at a rate of 1 mL / min, and stirring is continued for 30 min; in step S5, the aqueous coating slurry obtained in step S4 is coated onto the surface of the diaphragm base membrane using a comma-shaped doctor blade at a coating speed of 50 m / min, and the coating thickness is 1 μm; a three-stage low-temperature gradient drying process is adopted: drying at 40°C in the first temperature zone, 55°C in the second temperature zone, and 70°C in the third temperature zone, with a total drying time of 5 min.

[0037] Example 5 The difference from Example 1 is as follows: the composition and dosage of the aqueous coating slurry are shown in Table 1; in step S2 of the preparation method, the base slurry prepared in step S1 is heated to 35°C, and a pH adjuster is added dropwise at a rate of 5 mL / min under stirring at 800 r / min, followed by the addition of demulsifier in batches, and stirring is continued for 40 min until the slurry is free of flocculation and does not separate; in step S3, an organic solvent is added dropwise to the slurry obtained in step S2 at a rate of 3 mL / min, and stirring is continued for 20 min; in step S5, the aqueous coating slurry obtained in step S4 is coated onto the surface of the diaphragm base membrane using a comma-shaped doctor blade at a coating speed of 80 m / min, and the coating thickness is 1 μm; a three-stage low-temperature gradient drying process is adopted: drying at 50°C in the first temperature zone, 65°C in the second temperature zone, and 80°C in the third temperature zone, with a total drying time of 3 min.

[0038] Comparative Example Comparative Example 1 The difference from Example 1 is that the aqueous coating slurry does not contain any demulsifiers (sodium chloride and sodium citrate are both 0g), and the pH is adjusted to 5.0 only by a pH adjuster.

[0039] Comparative Example 2 The difference from Example 1 is that the demulsifier in the aqueous coating slurry uses only sodium chloride (5g) and does not contain sodium citrate.

[0040] Comparative Example 3 The difference from Example 1 is that no organic solvent is added to the composition of the aqueous coating slurry (the amount of organic solvent is 0g).

[0041] Comparative Example 4 The difference from Example 1 is that the dispersant used in the aqueous coating slurry is only sodium polycarboxylate (5g), without the addition of sodium polyacrylate.

[0042] Comparative Example 5 The difference from Example 1 is that the preparation conditions are changed as follows: the stirring speed in S2 is reduced to 400 r / min; the temperature of the system in S2 is increased to 50°C; and S5 is dried in a single-stage high-temperature process, directly at 100°C for 4 min.

[0043] Performance testing Slurry condition observation: Visually observe whether the slurry exhibits weak thixotropy, flocculation, or stratification; Heat shrinkage rate: The heat shrinkage rate of the diaphragm under the condition of 150℃ / 1h (average value of MD / TD). Air permeability increase: Gurley air permeability tester to measure the difference in air permeability before and after base film coating; Dry peel strength: After hot pressing the separator and the positive electrode at 85℃ and 1MPa, a 180° peel test is performed. Wet peel strength: After hot pressing, the sample is immersed in electrolyte for 24 hours and then peeled at 180°. Capacity retention rate after 500 cycles, 1000 cycles, and 2000 cycles: NCM523 / graphite soft-pack battery, 1C charge / discharge, 2.8-4.2V; Leakage current: Measured when the battery is fully charged and stationary.

[0044] The products prepared by Examples 1-5 and Comparative Examples 1-5 were subjected to the above performance tests, and the test results are shown in Tables 2 and 3.

[0045]

[0046]

[0047] As shown in Tables 2 and 3, the performance test results of the slurries in Examples 1-5 all exhibited ideal conditions of weak thixotropy, no flocculation, and no stratification. This indicates that within the formulation range and process conditions defined in the claims, pH / salt synergistic micro-demulsification can precisely remain in the intermediate state without excessive aggregation or insufficient demulsification. The air permeability increased by 5-10 s / 100cc, with all increases ≤10 s. The gradient relationship between the smallest increase (5 s) in Example 2 and the largest increase (10 s) in Example 3 verifies that a PVDF emulsion dosage of 40%-60% is a reasonable balance range between "adhesion and air permeability". In terms of adhesion performance, the dry peel strength of 22-32 N / m and the wet peel strength of 11-17 N / m are significantly better than the comparative examples, and the wet peel strength decrease is controllable, proving that the continuous structure of the particle "fusion neck" in the three-dimensional network endows the coating with the ability to maintain good interfacial adhesion after immersion in electrolyte. In terms of cycle performance, the capacity retention rate after 2000 cycles for Examples 1-5 was ≥80%, with Example 1 showing the best retention rate (83%). Example 2, even at the lower limit, still achieved 80%, indicating that the synergistic toughening mechanism provides sufficient protection even under boundary conditions of component dosage. Regarding safety, the heat shrinkage rate was ≤0.7% (far lower than the conventional 3%-5% for polyolefin separators), and the leakage current was ≤24μA, demonstrating that the three-dimensional network of the coating forms an effective thermally stable framework for the base film without localized insulation defects. Overall trends show that the median formulation achieved the optimal balance between air permeability, adhesion, and cycle stability.

[0048] Comparative Example 1: The slurry exhibited "no thickening and strong fluidity," a fundamental difference from the weak thixotropy of Example 1. This indicates that simply adjusting the pH to 5.0 is insufficient to initiate micro-demulsification, and the latex particles remained independently dispersed. After coating and drying, a discrete particle accumulation rather than a continuous three-dimensional network structure was formed, resulting in an increase in air permeability of up to 45 s / 100 cc. The dry peel strength was only 12 N / m, and the wet peel strength was as low as 5 N / m. The capacity retention rate after 2000 cycles was only 40%, a decrease of 43 percentage points compared to Example 1, making it the most severely degraded among all comparative examples. This comparative example demonstrates that demulsifiers are a necessary condition for initiating micro-demulsification. Simply relying on pH adjustment cannot push the PVDF emulsion to a "partially fused" intermediate state; the synergistic effect of pH adjusters and demulsifiers is inseparable.

[0049] Comparative Example 2: Slight flocculation in the slurry is an early sign of uncontrolled micro-demulsification. The lack of a buffering reaction from sodium citrate and the unrestrained salting-out effect of sodium chloride led to localized H+ flocculation in the dripping area. +High concentrations of sodium chloride and sodium citrate exacerbate the salting-out effect, leading to excessive particle aggregation and flocculation, while demulsification is insufficient in areas far from the dripping point. This uneven structure increases air permeability to 25 s / 100cc, reduces dry peel strength to 15 N / m, raises heat shrinkage to 1.2%, and results in a 2000-cycle retention rate of only 48%. This comparative example demonstrates that the "driving + buffering" combination of sodium chloride and sodium citrate is key to achieving uniform micro-demulsification; the buffering effect of sodium citrate is irreplaceable, and a single salting-out agent cannot precisely control the demulsification depth.

[0050] Comparative Example 3: The air permeability increase was only 10s / 100cc, and the 500-cycle retention rate was 93%, only 4 percentage points different from Example 1. However, the real difference became apparent sharply in the later stages of long-term cycling: it dropped to 78% after 1000 cycles and to 58% after 2000 cycles, showing a "cliff-like" decline. The key difference lies in the wet peel strength, which was only 8N / m, a 47% decrease compared to Example 1. This indicates that the three-dimensional network connections without organic solvent toughening were the first to develop and propagate microcracks under electrolyte immersion and repeated stress, and the coating's progression from brittle fracture to delamination was a gradual cumulative process. This comparative example best demonstrates the creativity of "synergistic toughening": the role of organic solvents is not to improve initial performance, but to endow the coating with fatigue resistance during long-term service. This "delayed failure prevention" effect is extremely difficult to predict from the initial performance of the formulation.

[0051] Comparative Example 4: The slurry exhibited a slight tendency to stratify, indicating that the dispersion and protection ability of sodium polycarboxylate alone was significantly insufficient in an acidic environment of pH 5.0. Its dispersion mechanism relies on the electrostatic repulsion of carboxylate groups, but under weakly acidic conditions, some carboxylate groups are protonated, resulting in a decrease in charge density. The lack of a steric barrier from sodium polyacrylate led to localized over-fusion of latex particles, resulting in a non-uniform structure in the coating, characterized by dense spots and weakly connected regions. This manifested as an increase in air permeability of 18 s / 100cc, a wet peel strength of only 7 N / m, and a 2000-cycle retention rate of 52%. This comparative example demonstrates that the combination of sodium polycarboxylate and sodium polyacrylate forms a dual-mechanism protective network of "electrostatic repulsion + steric hindrance," and that a single dispersant has a clear pH-dependent functional blind spot in an acidic micro-demulsification environment.

[0052] Comparative Example 5: Low-speed stirring prevents uniform dispersion of the additives, resulting in excessively high local concentrations; high temperature accelerates the collision and fusion of latex particles, self-accelerating the demulsification process; high-temperature rapid drying generates strong capillary forces that collapse the unformed network, leading to a denser porous structure. Large flocculations directly appear in the slurry, with an increase in air permeability of 35s / 100cc, and a wet peel strength of only 5N / m (a 67% decrease compared to Example 1, the largest decrease), with a retention rate of only 45% after 2000 cycles. This comparative example demonstrates that the stirring speed, temperature, and drying process specified in this invention are not arbitrary choices, but rather establish a precise match with the micro-demulsification kinetics and pore-forming mechanism. Exceeding any one of these conditions is sufficient to trigger uncontrolled micro-demulsification and coating structure collapse.

[0053] The above experimental results show that the high-adhesion, high-flexibility PVDF porous lithium battery separator coating prepared in this application exhibits an ideal slurry state with weak thixotropy, no flocculation, and no stratification in all examples. The air permeability increase is only 5-10 s / 100cc, the dry peel strength is 22-32 N / m, the wet peel strength is 11-17 N / m, the capacity retention rate after 2000 cycles is ≥80%, the thermal shrinkage rate is ≤0.7%, and the leakage current is ≤24 μA. Through the core technical concept of "pH / salt synergistic controllable micro-demulsification to construct a continuous three-dimensional porous framework" and "critical low-volume compounding with organic solvent synergistic toughening", as well as the supporting methods of "dual-mechanism protection with compounded dispersants" and "three-stage low-temperature gradient drying to shape the pores", the comprehensive performance of high adhesion, non-clogging, high flexibility, and ultra-long cycle life is simultaneously achieved in water-based pure PVDF coatings.

[0054] This specific embodiment is merely an explanation of the present invention and is not intended to limit the invention. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but as long as they are within the scope of the present invention, they are protected by patent law.

Claims

1. A highly adhesive and flexible PVDF porous lithium battery separator coating, characterized in that, It is a three-dimensional network porous structure that covers the surface of the diaphragm base membrane, formed by controlled micro-demulsification and drying of the coating water-based slurry. The aqueous coating slurry comprises, by mass percentage, the following components: 40-60% aqueous PVDF emulsion, 0.05-1.0% demulsifier, 0.5-3.0% organic solvent, 0.2-0.8% dispersant, 0.5-2.0% alcohol ester film-forming aid, and deionized water to make up the balance. The pH value is adjusted to 4.5-6.0 using a pH adjuster. The organic solvent is composed of two or more of the following: propylene glycol methyl ether, propylene glycol methyl ether acetate, dipropylene glycol methyl ether, ethylene glycol butyl ether, NMP, and DMAC. The dispersant is composed of a polycarboxylate dispersant and a polyacrylic acid dispersant in a mass ratio of 1:(0.3-1.5); The pH adjuster is any one of dilute acetic acid, citric acid, and dilute hydrochloric acid; The aqueous coating slurry does not contain fumed silica, fumed alumina, or inorganic nanofillers.

2. The high-adhesion, high-flexibility PVDF porous lithium battery separator coating according to claim 1, characterized in that, The demulsifier is a compound of sodium chloride and sodium citrate in a mass ratio of 1:(0.5-2).

3. The high-adhesion, high-flexibility PVDF porous lithium battery separator coating according to claim 1, characterized in that, The aqueous PVDF emulsion has a solid content of 40-50% and an average latex particle size of 100-300 nm.

4. The high-adhesion, high-flexibility PVDF porous lithium battery separator coating according to claim 1, characterized in that, The pH adjuster is dilute acetic acid, which adjusts the pH of the system to 5-5.

5.

5. The high-adhesion, high-flexibility PVDF porous lithium battery separator coating according to claim 1, characterized in that, The organic solvent is composed of propylene glycol methyl ether acetate and ethylene glycol butyl ether in a mass ratio of 1:(0.2-1); the dispersant is composed of sodium polycarboxylate and sodium polyacrylate in a mass ratio of 1:(0.5-1).

6. The high-adhesion, high-flexibility PVDF porous lithium battery separator coating according to claim 1, characterized in that, The film-forming aid is either dodecyl alcohol ester or ethylene glycol butyl ether acetate.

7. The high-adhesion, high-flexibility PVDF porous lithium battery separator coating according to claim 1, characterized in that, The pore size distribution of the three-dimensional mesh porous structure is 30-80 nm, and the porosity is 35-45%.

8. A method for preparing a high-adhesion, high-flexibility PVDF porous lithium battery separator coating as described in any one of claims 1-7, characterized in that, Includes the following steps: S1. After mixing deionized water and dispersant evenly, add aqueous PVDF emulsion to prepare the basic slurry; S2. Heat the basic slurry prepared in step S1 to 25-35℃, add pH adjuster dropwise at a rate of 2-5mL / min under stirring conditions of 800-1000r / min, then add demulsifier in batches, and continue stirring for 30-40min until the slurry is free of flocculation and does not separate into layers. S3. Add organic solvent dropwise to the slurry obtained in step S2 at a rate of 1-3 mL / min, and continue stirring for 20-30 min; S4. Add alcohol ester film-forming aid, mix evenly, add deionized water to make up the balance, let stand to degas, and obtain water-based coating slurry; S5. Apply the aqueous coating slurry obtained in step S4 to the surface of the separator base membrane, and dry it using a three-stage low-temperature gradient drying process to obtain a high-adhesion, high-flexibility PVDF porous lithium battery separator coating.

9. The method for preparing the high-adhesion, high-flexibility PVDF porous lithium battery separator coating according to claim 8, characterized in that, The aqueous coating slurry of step S5 is applied to one or both sides of the diaphragm base membrane; the coating method is either microgravure coating or comma blade coating, the coating speed is 50-80m / min, and the coating thickness is 1-3μm.

10. The method for preparing the high-adhesion, high-flexibility PVDF porous lithium battery separator coating according to claim 8, characterized in that, The step S5 adopts a three-stage low-temperature gradual drying process: the first temperature zone is 40-50℃, the second temperature zone is 55-65℃, and the third temperature zone is 70-80℃ for drying, with a total drying time of 3-5 minutes.

Citation Information

Patent Citations

  • Corrosion-resistant and waterproof coating

    CN104130647A

  • Ceramic diaphragm and its preparation method and use

    CN104752659A