A liquid cooling plate and its preparation method
By optimizing the flow channel structure and processing technology of the liquid cooling plate, the problems of high flow resistance, uneven flow distribution and high manufacturing difficulty were solved, thus achieving efficient heat exchange and improved reliability of the liquid cooling plate.
Patent Information
- Application Number
- CN202611338004.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-31
- Publication Date
- 2026-11-17
AI Technical Summary
Existing liquid cooling plates suffer from problems such as high flow resistance, uneven flow distribution, insufficient structural strength, and high manufacturing difficulty in their flow channel design, which affect their heat exchange performance and reliability.
A liquid-cooled plate structure was designed, comprising a liquid inlet transition zone, a first heat exchange zone, an intermediate connecting zone, and a liquid outlet transition zone connected in sequence. Multiple supporting turbulence columns and flow guide ribs were set up, and the smoothness of the flow channel and the welding quality were ensured by precision machining and vacuum brazing technology.
It improves the smoothness of flow, uniformity of heat exchange, structural pressure resistance and manufacturing reliability of liquid cooling plates, reduces flow resistance and pumping energy consumption, and enhances airtightness and long-term pressure resistance.
Smart Images

Figure CN123124289A_ABST
Abstract
Description
Technical Field
[0001] This application relates to a liquid cooling plate and its preparation method, belonging to the field of liquid cooling heat dissipation technology. Background Technology
[0002] Liquid cooling plates rely on the circulation of a cooling medium within internal channels to remove heat from heat-generating components. They are widely used in data center servers, new energy vehicle power batteries, energy storage devices, and high-power electronic devices. As the power density of electronic devices continues to increase, liquid cooling plates, in addition to excellent heat exchange capabilities, must also consider flow resistance, structural strength, airtightness, and long-term reliability. Due to limitations imposed by the installation location and the layout of surrounding components, the structure of liquid cooling plates can cause contraction and expansion of the flow cross-section during the cooling medium's flow, resulting in sudden changes in flow velocity, flow separation, and pressure loss, thus leading to uneven flow distribution across different heat exchange zones.
[0003] To improve the pressure resistance of large-area thin-walled liquid cooling plates, internal support ribs or columns are typically installed. However, these support structures occupy the effective flow area of the flow channel and obstruct the cooling medium. A small number of support structures makes it difficult to effectively suppress plate bulging or warping; a large number of support structures increases flow resistance.
[0004] In addition, the aforementioned liquid cooling plates also present significant manufacturing challenges. Errors in plate forming and processing can easily lead to inaccurate alignment of the flow channels and support structures between the two plates; uneven assembly gaps or brazing filler metal distribution can easily cause incomplete welding of support connection points, discontinuous outer welds, brazing filler metal intrusion into the flow channels, and deformation of the plates after welding, affecting the flow performance, airtightness, and long-term pressure resistance reliability of the liquid cooling plates. Summary of the Invention
[0005] The purpose of this invention is to provide a liquid cooling plate and its preparation method that can take into account the smooth flow of the flow channel, uniform heat exchange, low flow resistance, structural pressure resistance and manufacturability.
[0006] To achieve the above objectives, the technical solution adopted by the present invention is as follows: According to one aspect of this application, a liquid cooling plate is provided, including a first plate and a second plate disposed in a relatively sealed manner, wherein a liquid cooling channel is formed between the first plate and the second plate; One edge of the liquid cooling plate is recessed inward to form a clearance section. The liquid cooling channel includes a liquid inlet transition area, a first heat exchange area, an intermediate connecting area, a second heat exchange area, and a liquid outlet transition area connected in sequence. The first heat exchange area and the second heat exchange area are located on both sides of the clearance section. The intermediate connecting area extends along the periphery of the clearance section and connects the first heat exchange area and the second heat exchange area. Multiple spaced-apart support and turbulence-disrupting columns are respectively provided in the first heat exchange zone, the intermediate connecting zone, and the two ends of the support and turbulence-disrupting columns are respectively connected to the first plate and the second plate.
[0007] Optionally, at least one guide rib is provided in both the liquid inlet transition zone and the liquid outlet transition zone. The guide rib is distributed along the length direction of the liquid cooling plate, and the two sides of the guide rib are respectively connected to the first plate and the second plate.
[0008] Optionally, the cross-section of the supporting turbulence column is cylindrical, frustum-shaped, elliptical cylindrical, or waist-shaped.
[0009] Optionally, the widths of both the first heat exchange zone and the second heat exchange zone are greater than the width of the intermediate connecting zone.
[0010] Optionally, the width of the liquid inlet transition zone is smaller than the width of the first heat exchange zone, and the width of the liquid outlet transition zone is smaller than the width of the second heat exchange zone.
[0011] According to another aspect of this application, a method for preparing a liquid cooling plate is provided, comprising the following steps: (1) The stainless steel sheet is uncoiled and leveled. The flatness of the stainless steel sheet after leveling is not greater than 0.1mm. (2) Stamping is performed on the leveled stainless steel sheet to form a first blank and a second blank, and a flow channel preform is formed by stamping on at least one of the first blank and the second blank. (3) Grind the first and second slabs so that the flatness of the surfaces to be welded is not greater than 0.01 mm, the surface roughness Ra is not greater than 0.4 μm, and the thickness tolerance is not greater than ±0.01 mm; (4) The pre-formed part of the flow channel is precision machined to form a liquid cooling flow channel. The surface roughness Ra of the liquid cooling flow channel is not greater than 0.8μm and the dimensional tolerance is not greater than ±0.025mm. (5) Apply brazing filler metal to the areas to be welded on the first and second slabs, position and assemble the first and second slabs, and seal the liquid cooling channel between the first and second slabs to obtain the assembly to be welded. (6) Place the components to be soldered in a 1×10 -3 ~5×10 -3 Vacuum brazing was performed at Pa, with a brazing temperature of 1050–1120℃ and a holding time of 5–15 min. The plate was then cooled in the furnace to obtain a liquid-cooled plate.
[0012] Optionally, the stainless steel sheet is SUS304 stainless steel or SUS316 stainless steel.
[0013] Optionally, in step (1), the thickness of the stainless steel sheet is 0.5 to 2.5 mm.
[0014] Optionally, in step (2), the stamping speed is 18 to 23 times / min, the single stamping time is 2 to 4 seconds, and the stamping pressure is 180 to 220 tons.
[0015] Optionally, in step (2), the depth of the preformed flow channel is 0.3 to 1.2 mm.
[0016] Optionally, in step (3), the first slab and the second slab are double-sided ground by a double-sided grinding machine, using an alumina grinding slurry with an average particle size of 4 to 6 μm as the grinding medium, the grinding disc speed is 45 to 55 r / min, the grinding pressure is 0.04 to 0.06 MPa, and the grinding time is 8 to 12 min.
[0017] Optionally, in step (4), the spindle speed for finishing is 10000 to 15000 r / min.
[0018] Optionally, in step (4), the feed rate is 250-350 mm / min.
[0019] Optionally, in step (4), the depth of a single cut is 0.08 to 0.12 mm.
[0020] Optionally, in step (5), the solder coating thickness is 0.05 to 0.15 mm.
[0021] Optionally, in step (5), the brazing filler metal is a nickel-based brazing filler metal, a copper-based brazing filler metal, or an iron-based brazing filler metal.
[0022] Optionally, step (6) includes a preheating step before brazing: the preheating temperature is 600-800℃, the heating rate is 10-15℃ / min, and the holding time is 3-8min.
[0023] Optionally, in step (6), the cooling rate for temperatures above 600°C during furnace cooling is 5 to 10°C / min.
[0024] In this application, "room temperature" refers to 20–30°C.
[0025] The beneficial effects of this application include, but are not limited to: 1. This application sets up a liquid inlet transition zone, a first heat exchange zone, an intermediate connecting zone, a second heat exchange zone, and a liquid outlet transition zone in sequence, so that the liquid cooling flow channel bypasses the avoidance part; the guide ribs in the liquid inlet transition zone and the liquid outlet transition zone can guide the cooling medium to split and merge, and the supporting turbulence column can disturb the cooling medium and destroy the flow boundary layer, thereby improving the flow distribution and heat exchange uniformity of each heat exchange zone, and reducing local stagnation and heat dissipation hot spots.
[0026] 2. In this application, the two ends of the multiple supporting baffle columns are respectively connected to the first plate and the second plate, which can shorten the unsupported span of the plate and suppress the bulging, warping or vibration of the liquid cooling plate under internal pressure. At the same time, the space for the flow of cooling medium is reserved between adjacent supporting baffle columns, which can improve the structural strength and pressure resistance reliability of the liquid cooling plate while avoiding excessive obstruction of the liquid cooling channel by the continuous supporting structure, thereby reducing the pressure loss and pumping energy consumption during the flow of cooling medium.
[0027] 3. This application sequentially forms the slab blank and liquid cooling channels of the liquid cooling plate through uncoiling and leveling, stamping pre-forming, grinding, and finishing. Uncoiling and leveling can control the initial deformation of the sheet metal; stamping pre-forming improves forming efficiency and reduces the amount of material removed during finishing; grinding can control the flatness, surface roughness, and thickness tolerance of the surface to be welded, and reduce residual stress, stamping springback, and warping caused by local burrs; finishing further ensures the dimensional accuracy and surface quality of the liquid cooling channels, thereby balancing production efficiency, channel forming accuracy, and the flow stability of the cooling medium.
[0028] 4. This application controls the flatness and surface roughness of the surfaces to be welded, and performs positioning assembly after quantitatively applying brazing filler metal to the welding areas of the first and second slabs. This results in a uniform and stable brazing gap between the two slabs, which is beneficial for the brazing filler metal to be uniformly wetted, spread and filled under capillary action. This reduces problems such as local accumulation, loss, incomplete welding and intrusion into the liquid cooling channels, improves the continuity and density of the brazed joint, and reduces the risk of leakage or blockage of the liquid cooling plate.
[0029] 5. This application utilizes a high-vacuum environment for brazing, which inhibits oxidation of the stainless steel sheet and brazing filler metal, and removes residual gases and volatile substances from the brazing gap. The preheating stage controls the heating rate to ensure uniform heating of the components to be welded and allows the organic components in the brazing paste to gradually volatilize, reducing porosity and spatter. The brazing holding stage allows the brazing filler metal to fully melt and continuously fill the welding gap under capillary action, reducing incomplete welding defects. The cooling stage controls the cooling rate to reduce temperature gradients, shrinkage differences, and residual thermal stress, lowering the risk of warping, cracking, and interface peeling of the liquid-cooled plate, thereby improving the dimensional accuracy, airtightness, and long-term pressure resistance reliability of the liquid-cooled plate. Attached Figure Description
[0030] The accompanying drawings, which are included to provide a further understanding of this application and form part of this application, illustrate exemplary embodiments and are used to explain this application, but do not constitute an undue limitation of this application. In the drawings: Figure 1 This is a schematic diagram of the liquid cooling plate involved in the embodiments of this application.
[0031] Figure 2This is a schematic diagram of the structure of the first plate body involved in the embodiments of this application.
[0032] Figure 3 This is a schematic diagram of the structure of the second plate involved in the embodiments of this application.
[0033] List of components and reference numerals: 1. First plate, 2. Second plate, 3. Clearance section, 4. Liquid inlet transition zone, 5. First heat exchange zone, 6. Intermediate connecting zone, 7. Second heat exchange zone, 8. Liquid outlet transition zone, 9. Supporting turbulence column, 10. Guide rib. Detailed Implementation
[0034] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.
[0035] Unless otherwise specified in the examples, the procedures shall be performed under standard conditions or conditions recommended by the manufacturer. Raw materials or instruments whose manufacturers are not specified are all commercially available products.
[0036] Considering that liquid-cooled plates with clearance structures are prone to local velocity abrupt changes, flow separation, and pressure loss during the flow of cooling medium due to changes in the flow cross-section, and that large-area thin-walled plates are prone to bulging, warping, or local vibration under the pressure of the cooling medium, this application provides a liquid-cooled plate. This liquid-cooled plate, by providing an intermediate connecting area 6 extending along the periphery of the clearance portion 3, allows the cooling medium to bypass the clearance portion 3 and flow between the two heat exchange areas. Simultaneously, by providing multiple spaced-apart support and flow-disrupting columns 9 within the liquid-cooled flow channel, sufficient effective flow area is maintained while improving the pressure resistance of the liquid-cooled plate, thus balancing its heat exchange performance and flow resistance performance.
[0037] like Figures 1 to 3 As shown, the liquid cooling plate in this embodiment includes a first plate 1 and a second plate 2 disposed opposite to each other. The first plate 1 and the second plate 2 are adapted in shape and size, and are sealed together after being stacked, forming a liquid cooling channel for the flow of cooling medium between the first plate 1 and the second plate 2.
[0038] Optionally, the liquid cooling channel can be formed by at least one of the first plate 1 and the second plate 2 being recessed in a direction away from the other plate. When the first plate 1 and the second plate 2 are stacked together, the corresponding recessed areas together with the opposing plates form the liquid cooling channel. In other embodiments, the first plate 1 and the second plate 2 may also each form a corresponding recessed area, and the two recessed areas together form the liquid cooling channel.
[0039] like Figure 1 As shown, one edge of the liquid cooling plate is recessed into the liquid cooling plate to form a clearance portion 3. The clearance portion 3 is used to avoid connectors, mounting components or other peripheral parts on the equipment to be cooled, so that the liquid cooling plate can adapt to the limited installation space. The first plate 1 and the second plate 2 can be provided with corresponding clearance notches. After the first plate 1 and the second plate 2 are stacked, the two clearance notches together constitute the clearance portion 3.
[0040] The liquid cooling channel includes an inlet transition zone 4, a first heat exchange zone 5, an intermediate connecting zone 6, a second heat exchange zone 7, and an outlet transition zone 8, which are sequentially connected along the flow direction of the cooling medium. The first heat exchange zone 5 and the second heat exchange zone 7 are located on opposite sides of the clearance portion 3 along the length of the liquid cooling plate, respectively. The intermediate connecting zone 6 extends along the periphery of the clearance portion 3 and connects the first heat exchange zone 5 and the second heat exchange zone 7. The channel sidewall adjacent to the intermediate connecting zone 6 and the clearance portion 3 can extend along the contour of the clearance portion 3, thereby shortening the flow path of the cooling medium when bypassing the clearance portion 3 while meeting structural clearance requirements.
[0041] In this embodiment, the widths of both the first heat exchange zone 5 and the second heat exchange zone 7 are greater than the width of the intermediate connecting zone 6, creating a variable cross-section flow channel that contracts from the first heat exchange zone 5 towards the intermediate connecting zone 6 and expands from the intermediate connecting zone 6 towards the second heat exchange zone 7. The first heat exchange zone 5 and the second heat exchange zone 7 have large heat exchange areas, capable of covering the main heat-generating areas of the component to be cooled; the intermediate connecting zone 6 has a relatively small width, allowing it to bypass the clearance portion 3 and reduce the installation space occupied by the liquid cooling plate near the clearance portion 3.
[0042] Optionally, a smooth arc-shaped boundary is used to connect the first heat exchange zone 5 and the intermediate connecting zone 6, as well as the intermediate connecting zone 6 and the second heat exchange zone 7, in order to reduce flow separation and local pressure loss caused by changes in the flow channel width, so that the cooling medium can flow smoothly from the first heat exchange zone 5 into the intermediate connecting zone 6, and from the intermediate connecting zone 6 into the second heat exchange zone 7.
[0043] like Figure 2As shown, multiple spaced-apart support and turbulence-disrupting columns 9 are respectively arranged in the first heat exchange zone 5, the intermediate connecting zone 6, and the second heat exchange zone 7. The support and turbulence-disrupting columns 9 extend along the thickness direction of the liquid cooling plate, and their two ends are connected to the first plate 1 and the second plate 2 respectively, thereby forming multiple discrete internal support points between the first plate 1 and the second plate 2.
[0044] When the cooling medium inside the liquid-cooled flow channel has a certain pressure, multiple supporting baffle columns 9 can share the pressure on the first plate 1 and the second plate 2, reducing the unsupported span of the two plates, suppressing bulging, warping, or local vibration of the first plate 1 and the second plate 2, and improving the structural strength and pressure resistance of the liquid-cooled plate. The supporting baffle columns 9 adopt a discrete structure with interval distribution, which can avoid excessive obstruction of the liquid-cooled flow channel by the continuous support structure, retain sufficient effective flow area, thereby reducing pressure loss and pumping energy consumption during the flow of the cooling medium, and ensuring that the cooling medium flows smoothly through each heat exchange area.
[0045] Multiple supporting baffle columns 9 can also divert and turbulent the cooling medium flowing around them. When the cooling medium flows through the supporting baffle columns 9, the flow direction changes locally, which disturbs the fluid boundary layer in the liquid cooling channel. This facilitates heat exchange between the cooling medium and the first plate 1 and the second plate 2, and reduces the possibility of large-area low-speed regions appearing in the liquid cooling channel.
[0046] In this embodiment, the supporting baffle columns 9 in the first heat exchange zone 5 and the second heat exchange zone 7 can be arranged in multiple rows and columns, respectively. Adjacent rows of supporting baffle columns 9 can be aligned or staggered. When arranged in a staggered manner, the cooling medium can form a tortuous flow path between adjacent supporting baffle columns 9, thereby enhancing the disturbance to the cooling medium; when arranged in a straight line, the flow resistance generated by the supporting baffle columns 9 can be reduced. The specific arrangement of the supporting baffle columns 9 can be selected according to the heat exchange requirements and the allowable flow resistance.
[0047] The supporting baffle columns 9 within the intermediate connecting zone 6 can be arranged at intervals along the extension direction of the intermediate connecting zone 6. Since the width of the intermediate connecting zone 6 is smaller than the width of the first heat exchange zone 5 and the second heat exchange zone 7, the number of supporting baffle columns 9 arranged along the width direction of the liquid cooling plate within the intermediate connecting zone 6 can be less than that of the first heat exchange zone 5 and the second heat exchange zone 7, so as to avoid the supporting baffle columns 9 occupying too much of the effective flow area of the intermediate connecting zone 6.
[0048] Optionally, the spacing of the support turbulence columns 9 near the connection between the first heat exchange zone 5 and the intermediate connecting zone 6, and the connection between the intermediate connecting zone 6 and the second heat exchange zone 7, can be appropriately increased to form a flow transition space, so that the cooling medium has a certain flow adjustment space when the flow cross section contracts or expands, thereby reducing the local pressure loss caused by the superposition of the obstruction effect of the support turbulence columns 9 and the change of the flow channel cross section.
[0049] The supporting baffle column 9 can be cylindrical, frustum-shaped, elliptical cylindrical, or waist-shaped. When a cylindrical or frustum-shaped structure is used, the supporting baffle column 9 has no sharp edges in its circumference, which helps to reduce the local resistance generated when the cooling medium flows through the supporting baffle column 9. When an elliptical cylindrical or waist-shaped structure is used, its length direction can be consistent with the main flow direction of the cooling medium to guide the cooling medium and reduce the low-speed region formed on the back flow side.
[0050] The supporting baffle column 9 can be integrally formed with the first plate 1, with one end of the supporting baffle column 9 away from the first plate 1 connected to the second plate 2; alternatively, the supporting baffle column 9 can be integrally formed with the second plate 2, with one end of the supporting baffle column 9 away from the second plate 2 connected to the first plate 1. In other embodiments, the supporting baffle column 9 can also be disposed as an independent component between the first plate 1 and the second plate 2, as long as both ends of it can be reliably connected to the first plate 1 and the second plate 2 respectively.
[0051] In this embodiment, the width of the liquid inlet transition zone 4 is smaller than the width of the first heat exchange zone 5. The liquid inlet transition zone 4 extends from the liquid inlet side of the liquid cooling plate towards the first heat exchange zone 5, allowing the cooling medium to enter the relatively wide first heat exchange zone 5 from a relatively narrow inlet channel. Preferably, the liquid inlet transition zone 4 gradually widens along the flow direction of the cooling medium to reduce flow separation caused by the sudden expansion of the flow cross-section when the cooling medium enters the first heat exchange zone 5.
[0052] At least one guide rib 10 is provided in the liquid inlet transition zone 4. The guide rib 10 extends along the length of the liquid cooling plate, and the two opposite sides of the guide rib 10 along the thickness direction of the liquid cooling plate are respectively connected to the first plate 1 and the second plate 2. The guide rib 10 can not only provide auxiliary support for the first plate 1 and the second plate 2, but also divide the cooling medium entering the liquid inlet transition zone 4 into at least two fluid streams, guiding the cooling medium to flow to different positions in the first heat exchange zone 5, thereby improving the flow distribution at the inlet of the first heat exchange zone 5.
[0053] In this embodiment, the width of the liquid outlet transition zone 8 is smaller than the width of the second heat exchange zone 7. The liquid outlet transition zone 8 gradually narrows along the flow direction of the cooling medium, which is used to gradually collect and discharge the relatively dispersed cooling medium in the second heat exchange zone 7 to the liquid cooling plate, thereby reducing the flow impact generated when the cooling medium enters the liquid outlet transition zone 8 from the second heat exchange zone 7.
[0054] At least one guide rib 10 is also provided in the liquid outlet transition zone 8. The guide rib 10 in the liquid outlet transition zone 8 extends along the length direction of the liquid cooling plate, and its two opposite sides along the thickness direction of the liquid cooling plate are respectively connected to the first plate 1 and the second plate 2. The guide rib 10 can separate and guide the cooling medium at different positions in the second heat exchange zone 7 to the liquid outlet side, reducing the mutual impact, eddy currents and pressure loss generated when multiple cooling media converge in the liquid outlet transition zone 8.
[0055] The guide ribs 10 in the liquid inlet transition zone 4 and the liquid outlet transition zone 8 can be integrally formed with the first plate 1 or the second plate 2, or they can be connected as independent components between the first plate 1 and the second plate 2. The ends of the guide ribs 10 along the length of the liquid cooling plate are preferably arc-shaped or tapered to reduce the local resistance generated when the cooling medium flows through the ends of the guide ribs 10.
[0056] Through the aforementioned liquid-cooled flow channel structure, the first heat exchange zone 5 and the second heat exchange zone 7 can respectively cover the areas to be cooled on both sides of the clearance section 3, while the intermediate connecting zone 6 maintains the connection between the two heat exchange zones while meeting the clearance requirements. Multiple spaced supporting turbulence columns 9 improve the pressure resistance of the liquid-cooled plate and enhance the turbulence of the cooling medium. The guide ribs 10 in the liquid inlet transition zone 4 and the liquid outlet transition zone 8 improve the flow distribution of the cooling medium when it enters and exits the heat exchange zone, thereby enabling the liquid-cooled plate to take into account installation adaptability, heat exchange uniformity, smooth flow, and structural reliability.
[0057] Example 1 This embodiment provides a method for preparing a liquid-cooled plate, including the following steps: (1) A 1.5mm thick SUS304 stainless steel coil is fed into a leveling machine for uncoiling and leveling, and then cut into 200mm×200mm plates. The flatness of the plates is not greater than 0.1mm. (2) The leveled stainless steel sheet is stamped at a stamping speed of 20 times / min, a single stamping time of 3s, and a stamping pressure of 200 tons to form a first blank and a second blank. A flow channel preform with a depth of 1.0mm is formed on the first blank, and the second blank is a cover plate used to close the flow channel preform. (3) Place the first and second slabs in a double-sided grinding machine, use alumina grinding fluid with an average particle size of 5μm as the grinding medium, the grinding disc speed is 50r / min, the grinding pressure is 0.05MPa, the grinding time is 10min, then clean the slabs with deionized water and dry them. After testing, the flatness of the surface to be welded is not greater than 0.01mm, the surface roughness Ra is not greater than 0.4μm, and the thickness tolerance of the slabs is not greater than ±0.01mm. (4) The first blank after grinding is assembled on the vacuum chuck of the CNC machining center and the pre-forming part of the flow channel is precision machined. The spindle speed is 12000r / min, the feed speed is 300mm / min, the single cutting depth is 0.1mm, and the liquid cooling flow channel is formed. The surface roughness Ra of the liquid cooling flow channel is not greater than 0.8μm, and the dimensional tolerance of the width and depth is not greater than ±0.025 mm. (5) Apply BNi-2 type nickel-based brazing paste evenly to the areas to be welded on the first and second slabs. The wet film thickness of the nickel-based brazing paste is 0.10 mm, so that the liquid cooling channel is closed between the first and second slabs to obtain the component to be welded. (6) Place the components to be soldered in a vacuum of 3×10 -3 In a brazing furnace with a pressure of Pa, the temperature is increased to 700°C at a heating rate of 12°C / min and held for 5 minutes. Then, the temperature is increased to 1080°C and held for 10 minutes. After that, the temperature is cooled to 600°C at a cooling rate of 8°C / min and then allowed to cool naturally to room temperature before the liquid cooling plate is removed.
[0058] Example 2 This embodiment provides a method for preparing a liquid-cooled plate, including the following steps: (1) A 1.0mm thick SUS304 stainless steel coil is fed into a leveling machine for uncoiling and leveling, and then cut into 200mm×200mm plates. The flatness of the plates is not greater than 0.1mm. (2) The leveled stainless steel sheet is stamped at a stamping speed of 18 times / min, a single stamping time of 3.3s, and a stamping pressure of 180 tons to form a first slab and a second slab. A flow channel preform with a depth of 0.5mm is formed on the first slab, and the second slab is a cover plate used to close the flow channel preform. (3) The first and second slabs were placed in a double-sided grinding machine. Alumina grinding fluid with an average particle size of 4μm was used as the grinding medium. The grinding disc speed was 45r / min, the grinding pressure was 0.04MPa, and the grinding time was 8min. Then the slabs were cleaned with deionized water and dried. After testing, the flatness of the surface to be welded was not greater than 0.01mm, the surface roughness Ra was not greater than 0.4μm, and the thickness tolerance of the slabs was not greater than ±0.01mm. (4) The first blank after grinding is assembled on the vacuum chuck of the CNC machining center and the pre-forming part of the flow channel is precision machined. The spindle speed is 10000r / min, the feed rate is 250mm / min, the single cutting depth is 0.08mm, and the liquid cooling flow channel is formed. The surface roughness Ra of the liquid cooling flow channel is not greater than 0.8μm, and the dimensional tolerance of the width and depth is not greater than ±0.025mm. (5) Apply BNi-2 type nickel-based brazing paste evenly to the areas to be welded on the first and second slabs. The wet film thickness of the nickel-based brazing paste is 0.05 mm. Position and assemble the first and second slabs so that the liquid cooling channel is closed between the first and second slabs to obtain the assembly to be welded. (6) Place the components to be soldered in a vacuum of 1×10⁻⁶. -3 In the brazing furnace of Pa, the temperature is increased to 600°C at a heating rate of 10°C / min and held for 3 minutes. Then, the temperature is increased to 1050°C and held for 5 minutes. After that, the temperature is cooled to 600°C at a cooling rate of 5°C / min and then allowed to cool naturally to room temperature before the liquid cooling plate is removed.
[0059] Example 3 This embodiment provides a method for preparing a liquid-cooled plate, including the following steps: (1) A 2.5mm thick SUS316 stainless steel coil is fed into a leveling machine for uncoiling and leveling, and then cut into 200mm×200mm plates. The flatness of the plates is not greater than 0.1mm. (2) The leveled stainless steel sheet is stamped at a stamping speed of 23 times / min, a single stamping time of 2.6s, and a stamping pressure of 220 tons to form a first slab and a second slab. A flow channel preform with a depth of 1.2mm is formed on the first slab and the second slab respectively. The flow channel preform on the first slab corresponds to the flow channel preform on the second slab. (3) The first and second slabs were placed in a double-sided grinding machine. Alumina grinding fluid with an average particle size of 6 μm was used as the grinding medium. The grinding disc speed was 55 r / min, the grinding pressure was 0.06 MPa, and the grinding time was 12 min. Then the slabs were cleaned with deionized water and dried. After testing, the flatness of the surface to be welded was not greater than 0.01 mm, the surface roughness Ra was not greater than 0.4 μm, and the thickness tolerance of the slabs was not greater than ±0.01 mm. (4) The first and second blanks after grinding are respectively mounted on the vacuum chuck of the CNC machining center. The pre-formed flow channel on the first and second blanks is precision machined. The spindle speed is 15000r / min, the feed rate is 350mm / min, and the single cutting depth is 0.12mm. The pre-formed flow channel on the first and second blanks together form a liquid cooling flow channel. The surface roughness Ra of the liquid cooling flow channel is not greater than 0.8μm, and the dimensional tolerance of the width and depth is not greater than ±0.025mm. (5) Apply BNi-2 type nickel-based brazing paste evenly to the areas to be welded on the first and second slabs. The wet film thickness of the nickel-based brazing paste is 0.15 mm. The flow channel preform on the first slab and the flow channel preform on the second slab are positioned opposite each other and connected to each other to form a liquid cooling flow channel, thus obtaining the component to be welded. (6) Place the components to be soldered in a vacuum of 5×10 -3 In the Pa brazing furnace, the temperature is increased to 800°C at a heating rate of 15°C / min and held for 8 minutes. Then, the temperature is increased to 1120°C and held for 15 minutes. After that, the temperature is cooled to 600°C at a cooling rate of 10°C / min and then allowed to cool naturally to room temperature before the liquid cooling plate is removed.
[0060] Example 4 The difference from Example 1 is that step (6) is: The components to be soldered are placed in a vacuum of 3×10⁻⁶. -3 In a brazing furnace with a temperature of Pa, the temperature is increased to 1080°C at a heating rate of 12°C / min and held for 10 min. After holding, the temperature is reduced to 600°C at a cooling rate of 8°C / min and allowed to cool naturally to room temperature before the liquid cooling plate is removed.
[0061] Example 5 The difference from Example 1 is that step (6) is: The components to be soldered are placed in a vacuum of 3×10⁻⁶. -3 In a brazing furnace with a temperature of Pa, the temperature is increased to 700°C at a heating rate of 12°C / min and held for 5 minutes. Then, the temperature is increased to 1080°C and held for 10 minutes. After the process is completed, the plate is allowed to cool naturally to room temperature and then removed.
[0062] Comparative Example 1 The difference from Example 1 is that the vacuum degree of vacuum brazing in step (6) is 1×10 -1 Pa.
[0063] Comparative Example 2 The difference from Example 1 is that step (1) is: A 1.5mm thick SUS304 stainless steel coil was cut into 200mm×200mm sheets. The flatness of the sheets was measured to be 0.4mm.
[0064] Comparative Example 3 The difference from Example 1 is that step (3) is: The first and second slabs were ground using a single-sided abrasive belt, then the slabs were cleaned with deionized water and dried. After testing, the flatness of the surface to be welded was 0.04 mm, the surface roughness Ra was 0.7 μm, and the thickness tolerance of the slabs was ±0.035 mm.
[0065] Test case The liquid cooling plates prepared in Examples 1-5 and Comparative Examples 1-3 were subjected to performance tests, and the test methods are as follows: 1. Post-weld flatness test After brazing, the liquid cooling plate was left to stand at room temperature for 24 hours, then placed on a granite platform. The height of the plate surface was collected using a coordinate measuring machine with a grid of 20mm×20mm. The height difference between the highest and lowest points was used as the flatness of the liquid cooling plate after welding. Each liquid cooling plate was measured 3 times and the average value was taken.
[0066] 2. Brazing defect area ratio test Industrial digital X-ray imaging equipment was used to inspect all areas of the liquid cooling plate to be welded, and images were obtained under the same tube voltage, tube current and exposure time. Image analysis software was used to identify areas of porosity, incomplete welding and weld discontinuity interruption, and the brazing defect area rate was calculated as the percentage of the defect projection area to the total projection area of the area to be welded. Two liquid cooling plates were randomly selected from each group for ultrasonic C-scan verification.
[0067] 3. Direct pressure airtightness test Seal the liquid outlet of the liquid-cooled plate and introduce 250 kPa compressed air through the inlet. After the pressure stabilizes, maintain the pressure for 5 minutes and record the pressure difference before and after the pressure maintenance. A pressure drop of no more than 50 Pa is considered as passing the direct pressure airtightness test. The pressure drops listed in Table 1 are the average values of 5 liquid-cooled plates in each group.
[0068] 4. Helium mass spectrometry leak detection test The liquid-cooled plate was placed in a helium pressurization device and held at 0.8 MPa helium pressure for 30 minutes. It was then transferred to the vacuum leak detection chamber of a helium mass spectrometer leak detector to measure the helium leakage rate. The helium leakage rate was no higher than 1 × 10⁻⁶. -7 Pa·m 3 / s is considered acceptable; the helium leakage rate listed in Table 1 is the average value of 5 liquid cooling plates in each group.
[0069] 5. Pressure resistance test Deionized water was injected into the liquid cooling plate and the air was purged. The pressure was increased to 1.5 MPa at 0.1 MPa / s, and the pressure was maintained for 30 minutes before being released. If there was no leakage, bulging, or cracking during the pressure holding period, and the permanent deformation after pressure release was no more than 0.10 mm, the pressure resistance was deemed qualified.
[0070] 6. Air tightness test after temperature cycling The liquid-cooled plate, which passed the initial helium mass spectrometry leak detection, was subjected to 200 temperature cycles between -20°C and 85°C, with the high-temperature end and the low-temperature end held at each temperature for 30 minutes, and the temperature transition time not exceeding 5 minutes. After the cycles were completed and the plate was allowed to return to room temperature, the helium mass spectrometry leak detection method described above was repeated; the helium leakage rate was still not higher than 1×10⁻⁶. -7Pa·m 3 / s is determined to be qualified.
[0071] The test results are shown in Table 1 for details.
[0072] Table 1 Test results of Examples 1 to 5 and Comparative Examples 1 to 3
[0073] As can be seen from Table 1, the preparation method of the liquid cooling plate in the present application is dedicated to filler metal filling, weld seam densification and thermal stress control, reduces the risks of warpage, pores, incomplete welding and interface damage of the liquid cooling plate, and gives consideration to the dimensional accuracy, weld seam compactness, air tightness and long-term pressure resistance reliability of the liquid cooling plate.
[0074] The foregoing descriptions are merely embodiments of the present application, and the protection scope of the present application is not limited by these specific embodiments, but is defined by the claims of the present application. For those skilled in the art, the present application may have various modifications and variations. Any modifications, equivalent substitutions, improvements and the like made within the technical idea and principle of the present application shall all fall within the protection scope of the present application.
Claims
1. A liquid-cooled plate, characterized in that, It includes a first plate and a second plate that are relatively sealed together, with a liquid cooling channel formed between the first plate and the second plate; One edge of the liquid cooling plate is recessed inward to form a clearance section. The liquid cooling channel includes a liquid inlet transition area, a first heat exchange area, an intermediate connecting area, a second heat exchange area, and a liquid outlet transition area connected in sequence. The first heat exchange area and the second heat exchange area are located on both sides of the clearance section. The intermediate connecting area extends along the periphery of the clearance section and connects the first heat exchange area and the second heat exchange area. Multiple spaced-apart support and turbulence-disrupting columns are respectively provided in the first heat exchange zone, the intermediate connecting zone, and the two ends of the support and turbulence-disrupting columns are respectively connected to the first plate and the second plate.
2. The liquid cooling plate according to claim 1, characterized in that, At least one flow guide rib is provided in both the liquid inlet transition zone and the liquid outlet transition zone. The flow guide rib is distributed along the length direction of the liquid cooling plate, and the two sides of the flow guide rib are respectively connected to the first plate and the second plate.
3. The liquid cooling plate according to claim 1, characterized in that, The cross-section of the supporting turbulence column is cylindrical, frustum-shaped, elliptical cylindrical, or waist-shaped.
4. The liquid cooling plate according to claim 1, characterized in that, The widths of both the first and second heat exchange zones are greater than the width of the intermediate connecting zone.
5. The liquid cooling plate according to claim 1, characterized in that, The width of the liquid inlet transition zone is smaller than the width of the first heat exchange zone, and the width of the liquid outlet transition zone is smaller than the width of the second heat exchange zone.
6. A method for preparing a liquid-cooled plate, characterized in that, Includes the following steps: (1) The stainless steel sheet is uncoiled and leveled. The flatness of the stainless steel sheet after leveling is not greater than 0.1mm. (2) Stamping is performed on the leveled stainless steel sheet to form a first blank and a second blank, and a flow channel preform is formed by stamping on at least one of the first blank and the second blank. (3) Grind the first and second slabs so that the flatness of the surfaces to be welded is not greater than 0.01 mm, the surface roughness Ra is not greater than 0.4 μm, and the thickness tolerance is not greater than ±0.01 mm; (4) The pre-formed part of the flow channel is precision machined to form a liquid cooling flow channel. The surface roughness Ra of the liquid cooling flow channel is not greater than 0.8μm and the dimensional tolerance is not greater than ±0.025mm. (5) Apply brazing filler metal to the areas to be welded on the first and second slabs, position and assemble the first and second slabs, and seal the liquid cooling channel between the first and second slabs to obtain the assembly to be welded. (6) Place the components to be soldered in a 1×10⁻³~5×10⁻³ area. -3 Vacuum brazing was performed at Pa, with a brazing temperature of 1050–1120℃ and a holding time of 5–15 min. The plate was then cooled in the furnace to obtain a liquid-cooled plate.
7. The method for preparing a liquid-cooled plate according to claim 6, characterized in that, In step (2), the stamping speed is 18-23 times / min, the single stamping time is 2-4s, and the stamping pressure is 180-220 tons.
8. The method for preparing a liquid-cooled plate according to claim 6, characterized in that, In step (4), the spindle speed for finishing is 10000-15000 r / min.
9. The method for preparing a liquid-cooled plate according to claim 6, characterized in that, In step (6), a preheating step is also included before brazing: the preheating temperature is 600-800℃, the heating rate is 10-15℃ / min, and the holding time is 3-8min.
10. The method for preparing a liquid-cooled plate according to claim 6, characterized in that, In step (6), the cooling rate for temperatures above 600°C during furnace cooling is 5 to 10°C / min.