A method for preparing a glass cofferdam

By using screen printing technology and composite paste formulation, combined with silane coupling agent and gas-phase SiO2 dispersion rheology aid, the complexity and thermal stress problems of traditional photoresist processes in CMOS image sensor wafer-level packaging have been solved, achieving efficient and low-cost glass dam fabrication suitable for large-size wafer-level packaging.

CN123124470APending Publication Date: 2026-11-17HUATIAN TECHNOLOGY (KUNSHAN) ELECTRONICS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611402264.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-10
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Traditional photoresist processes in CMOS image sensor wafer-level packaging suffer from complex processes, expensive equipment, low material utilization, and thermal stress problems caused by differences in thermal expansion coefficients, making it difficult to meet the requirements of high reliability industrialization.

Method used

By employing screen printing technology and composite paste formulation, combined with silane coupling agent and gas-phase SiO2 dispersion rheology modifier, a high-precision and firmly bonded glass dam is formed through segmented sintering, which simplifies the process, improves material utilization, and reduces costs.

Benefits of technology

It achieves low-cost, high-efficiency, and high-reliability glass dam fabrication, suitable for large-size wafer-level packaging, improving mass production yield and overcoming the shortcomings of traditional photoresist processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124470A_ABST
    Figure CN123124470A_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing a glass cofferdam, comprising the following steps: providing a glass substrate; preparing a composite cofferdam slurry, wherein the composite cofferdam slurry contains inorganic powder, an organic carrier, and a compound additive system composed of a silane coupling agent and a gas-phase SiO2 dispersion rheology modifier; providing a screen printing plate with a cofferdam pattern; transferring the composite cofferdam slurry onto the surface of the glass substrate by screen printing to form a wet film pattern of the cofferdam; and sintering the wet film pattern of the cofferdam to form a solid cofferdam. This invention achieves low-cost, high-efficiency, and high-reliability glass cofferdam preparation through synergistic innovation in screen printing technology, composite slurry formulation, and the entire process, and has good prospects for industrial application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of semiconductor packaging technology, and specifically relates to a method for preparing a glass dam for wafer-level packaging of CMOS image sensors. Background Technology

[0002] CMOS image sensors (CIS) are widely used in consumer electronics imaging, security monitoring, and medical endoscopes due to their advantages such as low power consumption, high integration, and high-speed readout. Currently, in wafer-level packaging (WLP) of CMOS image sensors, a transparent cover glass is typically bonded to the top of the sensor wafer. A precise dam structure needs to be formed between the two to seal the cavity and ensure stable operation of the image sensor during subsequent manufacturing processes and use.

[0003] Traditional cofferdam fabrication processes often employ a photoresist route, which involves sequentially spinning, exposing, and developing the glass surface to form a cofferdam pattern. While this process can achieve high pattern accuracy, it suffers from the following drawbacks: (1) The process is complex and the equipment is expensive, resulting in high manufacturing costs; (2) During the spin coating process, most of the photoresist is thrown off the substrate, and the material utilization rate is usually less than 60%, resulting in significant waste and making it unsuitable for large-size wafer-level packaging; (3) There is a significant difference in the coefficient of thermal expansion (CTE) between the organic photoresist material and the silicon substrate and glass cover, which can easily generate thermal stress in subsequent processes and reliability tests, leading to delamination of the cofferdam interface and sealing failure.

[0004] To overcome these shortcomings, some attempts have been made to combine screen printing with glass paste to replace traditional photoresist damming solutions. However, this approach still faces several technical obstacles in its industrialization process: poor paste uniformity, resulting in uneven dam edges and pinhole breaks after printing; insufficient adhesion between the paste and the glass substrate, leading to cracking and detachment after sintering; and the tendency for air bubbles and pinholes to remain inside the dam during the sintering process. These problems are interconnected, and improvements in a single step are insufficient to fundamentally solve them, meaning that glass paste damming technology still cannot meet the high reliability requirements of wafer-level packaging for industrialization.

[0005] Therefore, there is an urgent need to develop an innovative method for fabricating glass dams to meet the increasingly stringent packaging requirements of CMOS image sensors. Summary of the Invention

[0006] To address the aforementioned technical problems, the present invention aims to provide a method for preparing glass cofferdams. Through collaborative innovation in screen printing technology, composite slurry formulation, and the entire process, the present invention achieves low-cost, high-efficiency, and high-reliability preparation of glass cofferdams, demonstrating promising prospects for industrial application.

[0007] To achieve the above-mentioned technical objectives and effects, the present invention is implemented through the following technical solution: A method for preparing a glass cofferdam includes the following steps: Provide glass substrate; A composite cofferdam slurry is prepared, wherein the composite cofferdam slurry contains inorganic powder, organic carrier, and a compound additive system composed of silane coupling agent and gas-phase SiO2 dispersion rheology aid; A screen printing plate with a cofferdam pattern is provided, and the composite cofferdam slurry is transferred to the surface of the glass substrate by screen printing to form a cofferdam wet film pattern; The wet film pattern of the cofferdam is sintered to form a solid cofferdam.

[0008] Furthermore, in the composite cofferdam slurry, the amount of silane coupling agent added is 0.5-3 wt% of the mass of the organic carrier, and the amount of gaseous SiO2 dispersion rheology modifier added is 1-3 wt% of the mass of the organic carrier.

[0009] Furthermore, the inorganic powder comprises Bi2O3-B2O3-SiO2-Al2O3 series glass powder, and 5-15% by weight of low melting point oxide filler, wherein the low melting point oxide filler is selected from at least one of ZnO and V2O5; the particle size of the glass powder is 2-5μm.

[0010] Furthermore, the composite cofferdam slurry undergoes vacuum degassing and graded filtration treatment before printing.

[0011] Furthermore, the screen printing step is repeated at least twice. After each printing, the screen is pre-dried at 70-90°C for 3-10 minutes until surface dry and then cooled to room temperature before the next printing is performed.

[0012] Furthermore, the sintering is segmented inert atmosphere sintering, including a debinding section, a pre-sintering section, and a densification sintering section performed sequentially; the entire sintering process is carried out under a nitrogen atmosphere.

[0013] Furthermore, the sintering is laser local sintering: the laser wavelength is 808nm or 1064nm, the laser spot scans along the dam pattern, the scanning speed is 5-10mm / s, and the laser power is reduced at the corners of the dam; the printed glass substrate is preheated to 180-200℃, and cooled by nitrogen purging after sintering.

[0014] Furthermore, the laser power is reduced by 10% at the corner of the cofferdam.

[0015] Furthermore, the cofferdam pattern is a double-ring nested structure, including an inner ring pattern and an outer ring pattern, with an annular gap between the inner ring pattern and the outer ring pattern.

[0016] Furthermore, getter slurry is printed and filled in the annular gap, and the getter slurry is cured at low temperature to form a getter material layer.

[0017] The beneficial effects of this invention are as follows: (1) The present invention uses screen printing technology to replace the traditional photolithography process, which can print the dam pattern on the whole glass substrate in one step without the need for lengthy steps such as spin coating, exposure, and development. The process flow is greatly simplified, and the equipment investment and manufacturing cost are significantly reduced. The material utilization rate of screen printing is higher than that of photolithography, avoiding the serious waste problem caused by most of the material being thrown off the substrate during the photoresist spin coating process. It is more economical and environmentally friendly, and is especially suitable for large-scale mass production of large-size wafer-level packaging.

[0018] (2) By adding a compound additive system consisting of silane coupling agent and gaseous SiO2 dispersing rheology modifier to the slurry, the present invention solves the problem of easy agglomeration and sedimentation stratification of glass powder in organic carrier, and improves the storage stability and printing uniformity of slurry. At the same time, the silane coupling agent forms a chemical bridging effect between glass powder and glass substrate, and gaseous SiO2 regulates the rheological properties of slurry and inhibits filler sedimentation. The synergistic effect of the two significantly improves the interfacial bonding strength between the sintering dam and the substrate, and effectively solves the reliability problem of easy cracking and falling off of existing glass slurry dams.

[0019] (3) This invention achieves high-precision molding and strong interface bonding of the cofferdam structure through the synergistic cooperation of screen printing process and composite cofferdam slurry. The inorganic glass cofferdam prepared is resistant to organic solvents and acids and alkalis. It maintains structural integrity in subsequent standard CMOS back-end processes such as photolithography, etching, and redistribution layer fabrication. It does not swell or corrode and is perfectly compatible with wafer-level packaging process, significantly improving mass production yield. Attached Figure Description

[0020] Figure 1 This is a schematic diagram of the cofferdam structure fabricated on a glass substrate according to the present invention.

[0021] Figure 2 This is a CMOS image sensor packaged product containing the cofferdam manufactured according to the present invention.

[0022] In the diagram, 10 represents the glass substrate, and 20 represents the cofferdam. Detailed Implementation

[0023] The technical solutions of the present invention will be clearly and completely described below with reference to specific embodiments. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0024] This invention provides a method for fabricating a glass dam, which is applicable to the fabrication of a covering glass dam in wafer-level packaging of CMOS image sensors.

[0025] Step 1: Pretreatment of the glass substrate A glass substrate is provided, and the glass substrate is cleaned and surface activated before screen printing.

[0026] Preferably, the cleaning process can employ steps such as alkaline washing, deionized water rinsing, and nitrogen air knife drying. Preferably, the surface activation treatment can employ plasma activation cleaning (e.g., plasma corona activation for 60 seconds) to enhance the surface energy and wettability of the glass substrate. After plasma activation cleaning, the interfacial wettability between the subsequent printing paste and the glass substrate is significantly improved, which is beneficial for improving the accuracy of the printed pattern and the interfacial bonding strength.

[0027] Step 1: Prepare composite cofferdam slurry For example, the composite cofferdam slurry contains inorganic powder, organic carrier, and a compound additive system consisting of silane coupling agent and gas-phase SiO2 dispersion rheology modifier.

[0028] Preferably, the inorganic powder comprises Bi2O3-B2O3-SiO2-Al2O3 series lead-free low-melting-point glass powder. Exemplarily, this glass powder can be prepared by: weighing Bi2O3, B2O3, SiO2, and Al2O3 according to a set ratio, uniformly mixing, melting, quenching, ball milling, and filtering through a filter to remove large particles, thereby obtaining glass powder of the desired particle size. Preferably, the glass powder has a particle size of 2-5 μm, a softening point of approximately 480℃, and a coefficient of thermal expansion of approximately 3.8 × 10⁻⁶. -6 / ℃.

[0029] Furthermore, the inorganic powder also contains 5-15% by weight of low-melting-point oxide filler, which is selected from at least one of ZnO and V2O5. By mixing low-melting-point oxide filler into the glass powder, the softening temperature of the glass powder can be effectively reduced, and the overall thermal expansion coefficient of the cofferdam material can be adjusted, enabling it to achieve better thermal matching with the glass substrate and silicon substrate, and buffering the thermal stress generated by thermal shock.

[0030] Preferably, the organic carrier is composed of a resin and a solvent. Exemplarily, the resin may be ethyl cellulose, and the solvent may be terpineol, which can be prepared in a mass ratio of 15:85. The organic carrier is obtained by dissolving ethyl cellulose in terpineol and stirring until completely transparent.

[0031] In this invention, the composite cofferdam slurry also contains a compound additive system composed of a silane coupling agent and a gas-phase SiO2 dispersing rheology modifier. Exemplarily, the amount of the silane coupling agent added can be 0.5-3 wt% of the mass of the organic carrier; the amount of the gas-phase SiO2 dispersing rheology modifier added can be 1-3 wt% of the mass of the organic carrier. The silane coupling agent can form a chemical bridge between the glass powder and the glass substrate, significantly improving the interfacial bonding strength; the gas-phase SiO2 dispersing rheology modifier can adjust the rheological properties of the slurry and inhibit powder sedimentation. The synergistic effect of both effectively solves the problem of easy agglomeration and sedimentation stratification of glass powder in the organic carrier, improving the storage stability and printing uniformity of the slurry.

[0032] The aforementioned inorganic powder is mixed with an organic carrier containing a compounded additive system at a mass ratio of (70-85):(30-15), and then ground multiple times (e.g., 3 times) on a three-roll mill to ensure thorough and uniform dispersion of the components. The composite damming slurry also undergoes vacuum degassing and graded filtration during preparation. For example, the prepared slurry can be vacuum degassed for 30 minutes and then filtered through a 300-mesh filter to eliminate internal air bubbles and agglomerated particles, resulting in a uniform paste-like composite damming slurry, which is then stored at a constant temperature (e.g., 23°C) for later use. This pretreatment of vacuum degassing and graded filtration reduces the risk of printing defects such as pinholes and broken lines from the source.

[0033] Step 3, screen printing A screen printing plate with a cofferdam pattern is provided. For example, a screen of appropriate mesh size can be selected according to the cofferdam design (line width, height, closed or open shape), coated with photosensitive emulsion, and exposed and developed to form a cutout pattern.

[0034] Preferably, the screen printing plate is a stainless steel mesh or a polyurethane mesh with a mesh count of 200-500. For example, a 325-mesh stainless steel mesh can be used. Preferably, the mesh tension is controlled at 25-30 N / cm, for example, 28 N / cm. Preferably, the photosensitive film thickness is 20-40 μm, for example, 30 μm. Preferably, the gap between the screen and the printing plate is 1-2 mm, for example, 1.5 mm.

[0035] The composite cofferdam slurry is transferred to the surface of a pretreated glass substrate by screen printing to form a wet film pattern of the cofferdam. Exemplarily, the squeegee angle can be 40-50° (e.g., 45°) and the printing speed can be 15-25 mm / s (e.g., 20 mm / s).

[0036] Preferably, the screen printing step is repeated at least twice. After each printing, the film is pre-dried at 70-90℃ for 3-10 minutes until surface dry and then cooled to room temperature before the next printing. For example, it can be pre-dried at 80℃ for 5 minutes until surface dry and then cooled to room temperature before the next printing. By stacking multiple layers of printing, the cofferdam height can be flexibly adjusted. Pre-drying each layer at a low temperature until surface dry and then cooling to room temperature before the next layer is printed can effectively avoid the problem of the upper layer of paste washing away the lower layer contour and the problem of interlayer locked air bubbles, thus eliminating interlayer delamination and internal void defects. Preferably, by adjusting the number of repeated printings and the solid content of the paste, the cofferdam height can be precisely controlled within the range of 30-70μm. For example, after three repeated printings, the total wet film thickness can be increased to approximately 95μm.

[0037] Step 4, sintering The wet membrane pattern of the cofferdam is sintered to solidify it into a solid cofferdam, resulting in the following: Figure 1 The glass base 10 shown is equipped with a cofferdam 20.

[0038] In a preferred embodiment of the present invention, the sintering is segmented inert atmosphere sintering. Exemplarily, the segmented inert atmosphere sintering includes a debinding section, a pre-sintering section, and a densification sintering section performed sequentially. Specifically, debinding can be performed first at 140-160℃ with a heating rate of 3-5℃ / min and held for 20-40 min to fully decompose and remove the organic carrier; then, pre-sintering is performed at 430-470℃; finally, densification sintering is performed at 560-590℃ for 10-25 min to completely densify the inorganic powder. The entire sintering process is carried out under a nitrogen inert atmosphere, preferably with an oxygen content <10ppm. The cooling rate is preferably ≤8℃ / min to eliminate defects such as thermal stress cracks. By precisely controlling the temperature, heating rate, holding time, and cooling rate in segments, defects such as pinholes, overheating collapse, and thermal stress cracks can be effectively eliminated.

[0039] In another preferred embodiment of the invention, the sintering is laser localized sintering. Exemplarily, the laser wavelength can be 808nm or 1064nm. The laser spot scans uniformly along the dam pattern at a speed of 5-10mm / s. Preferably, the laser power is reduced by 10% at the corners of the dam to avoid heat concentration at the corners leading to overheating. The printed glass substrate is preheated to 180-200°C and cooled by nitrogen purging after sintering. Laser localized sintering allows for rapid localized heating and densification of the dam, while the main body temperature of the glass substrate remains below 200°C. This method is particularly suitable for wafer-level packaging scenarios where heat-sensitive areas or active areas are already integrated, effectively avoiding glass microcracks and dam cracking caused by laser thermal stress.

[0040] In a preferred embodiment of the present invention, the screen printing plate has a double-ring nested structure for the cofferdam pattern, comprising an inner ring pattern and an outer ring pattern, with an annular gap between the inner and outer ring patterns. Preferably, the width of the annular gap is ≥100μm. This structure makes the printed cofferdam a labyrinthine sealed cofferdam with inner and outer rings, which can disperse thermal stress from thermal shock and reduce the risk of interface delamination and air leakage.

[0041] More preferably, a getter slurry is printed and filled into the annular gap, and the getter slurry is cured at low temperature to form a getter material layer. For example, the getter slurry can be a zeolite-based getter slurry, and the screen used for printing and filling is 40 μm wider than the annular gap width, cured by baking at 80°C. Since the cofferdam sintering is carried out at high temperatures (560-590°C), and the getter will deactivate at high temperatures, the getter slurry needs to be filled and cured at low temperatures after the cofferdam sintering is completed to maintain the activity of the getter. This structure requires external moisture to bypass two glass barriers and be actively absorbed by the getter layer, significantly improving the sealing life.

[0042] In another preferred embodiment of the invention, the screen printing pattern of the cofferdam further includes multiple support column patterns in the inner region surrounded by the outer cofferdam. Preferably, the support columns and the cofferdam are printed and sintered simultaneously using the same paste, and the height tolerance of the support columns is controlled within ±5μm. After printing and sintering, glass support columns are simultaneously formed inside the cavity surrounded by the outer cofferdam, which can prevent the wafer bonding cover from cracking under pressure at a single point.

[0043] In another preferred embodiment of the present invention, the composite damming slurry may further contain light-shielding filler to form a light-shielding dam. Exemplarily, the chip substrate may be a back-illuminated CMOS chip substrate, and the composite damming slurry may be printed on the back side of the chip.

[0044] For example, the glass substrate with a dam structure prepared by the above method can be processed through subsequent processes such as wafer bonding, back-side grinding, etching, spin coating, photolithography, plasma chemical vapor deposition (PECVD), redistribution layer (RDL) fabrication, laser pre-cutting, and chemical solder resist application, and then finally cut to obtain the desired structure. Figure 2 The encapsulated CMOS image sensor product is shown. The cofferdam material of this invention is inorganic glass, which has excellent resistance to organic solvents and acids and alkalis. It maintains structural integrity during the aforementioned back-end processes, without swelling or corrosion, and is perfectly compatible with standard CMOS back-end process flows.

[0045] Example 1: Preparation of a single-layer cofferdam This embodiment provides a specific implementation plan for preparing a single-layer cofferdam using screen printing on glass.

[0046] Glass powder preparation: 70wt% Bi₂O₃, 15wt% B₂O₃, 10wt% SiO₂, and 5wt% Al₂O₃ were weighed, uniformly mixed, melted, quenched, and ball-milled. The mixture was then filtered through an 800-mesh screen to remove large particles, yielding glass powder with an average particle size of 3μm. This glass powder has a softening point of approximately 480℃ and a coefficient of thermal expansion of approximately 3.8 × 10⁻⁶. -6 / ℃.

[0047] Preparation of organic carrier: Ethyl cellulose was dissolved in terpineol at a mass ratio of 15:85 and stirred until completely transparent. 1 wt% of silane coupling agent and 2 wt% of gaseous SiO2 rheology modifier were added and stirred until homogeneous.

[0048] Slurry preparation: Take the above glass powder and add 10wt% of ZnO low-melting-point oxide filler. Mix the inorganic powder with the organic carrier containing the compound additive system at a mass ratio of 80:20. Grind the mixture three times on a three-roll mill to ensure that the components are fully dispersed and uniform. Then, degas the mixture under vacuum for 30 minutes and filter it through a 300-mesh filter to obtain a uniform paste-like composite damming slurry. Store the slurry at a constant temperature of 23℃ for later use.

[0049] Substrate pretreatment: The glass substrate was sequentially washed with alkali, rinsed with deionized water, dried with nitrogen air knife, and then activated by plasma corona treatment for 60 seconds.

[0050] Screen printing: A 325-mesh stainless steel screen is used, with a tension of 28 N / cm, a photosensitive emulsion thickness of 30 μm, and a gap of 1.5 mm between the screen and the screen. The dam pattern on the screen is a rectangular closed loop with a width of 200 μm, and the inner circle size corresponds to the photosensitive area of ​​the chip. The paste is coated onto the screen, the squeegee angle is 45°, and the printing speed is 20 mm / s. The paste is printed onto the pretreated glass substrate surface to form a rectangular dam wet film pattern.

[0051] Sintering: The wet film pattern of the cofferdam is sintered in a segmented inert atmosphere. First, the temperature is raised to 150℃ at a rate of 3-5℃ / min and held for 30 minutes to remove the binder; then, the temperature is raised to 450℃ for pre-sintering; finally, densification sintering is performed at 570-580℃ for 15-20 minutes. The entire process is carried out under a nitrogen atmosphere with an oxygen content <10ppm and a cooling rate ≤8℃ / min. After sintering, a glass cover plate with a solid cofferdam is obtained.

[0052] Example 2: Preparation of a multi-layer printed, superimposed thickened cofferdam This embodiment is similar to Embodiment 1, except that the height of the dam is increased by repeated screen printing to meet the packaging requirements of a larger cavity height.

[0053] The same composite cofferdam slurry, screen printing plate, printing parameters, and glass substrate pretreatment process as in Example 1 were used.

[0054] After the first printing is completed, pre-bake at 80℃ for 5 minutes until surface dry, then remove and cool to room temperature.

[0055] With the screen printing plate unchanged, a second printing is performed to completely cover the original pattern with new paste, followed by pre-baking and cooling under the same conditions.

[0056] Repeat the above printing-pre-baking-cooling steps a total of 3 times, increasing the total wet film thickness to approximately 95 μm.

[0057] Sintering was carried out using the same segmented inert atmosphere sintering method as in Example 1, with the densification holding time extended to 20 minutes to promote interlayer melting and fusion and eliminate interlayer interface defects. After sintering, the total height of the cofferdam reached 85 μm, and the cross-section was dense without delamination or air bubbles.

[0058] Example 3: Preparation of a double-ring nested cofferdam This embodiment provides a cofferdam preparation scheme with a double-ring nested structure, which can further improve the sealing reliability.

[0059] The screen printing pattern is designed as two equidistant concentric rectangular rings, namely an inner ring pattern and an outer ring pattern. The width of the inner ring pattern is 180μm, the width of the outer ring pattern is 180μm, and the annular gap between the two is 100μm.

[0060] Using the same composite cofferdam slurry, substrate pretreatment process, printing parameters and sintering conditions as in Example 1, a double-ring wet film pattern is directly formed in one printing. After sintering, an inner ring cofferdam and an outer ring cofferdam are obtained, thus forming a double-ring nested cofferdam structure.

[0061] After the cofferdam has been sintered and cooled, a zeolite-based getter slurry is printed into the annular gap. The printing screen width is 40 μm smaller than the gap width. After curing at 80°C, a getter material layer is formed. The resulting double-ring nested cofferdam structure allows external water vapor to bypass two glass barriers before entering the cavity, significantly improving the sealing life compared to a single-ring cofferdam structure.

[0062] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from the spirit or essential characteristics of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, it is intended that all variations falling within the meaning and scope of equivalents of the claims be included within the present invention.

[0063] Furthermore, it should be understood that although this specification describes embodiments, not every embodiment contains only one independent technical solution. This narrative style is merely for clarity. Those skilled in the art should consider the specification as a whole, and the technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.

Claims

1. A method for preparing a glass cofferdam, characterized in that, Includes the following steps: Provide glass substrate; A composite cofferdam slurry is prepared, wherein the composite cofferdam slurry contains inorganic powder, organic carrier, and a compound additive system composed of silane coupling agent and gas-phase SiO2 dispersion rheology aid; A screen printing plate with a cofferdam pattern is provided, and the composite cofferdam slurry is transferred to the surface of the glass substrate by screen printing to form a cofferdam wet film pattern; The wet film pattern of the cofferdam is sintered to form a solid cofferdam.

2. The method according to claim 1, characterized in that, In the composite cofferdam slurry, the amount of silane coupling agent added is 0.5-3 wt% of the mass of the organic carrier, and the amount of gaseous SiO2 dispersion rheology modifier added is 1-3 wt% of the mass of the organic carrier.

3. The method according to claim 1, characterized in that, The inorganic powder comprises Bi2O3-Bi2O3-B2O3-SiO2-Al2O3 series glass powder, and 5-15% by weight of low melting point oxide filler, wherein the low melting point oxide filler is selected from at least one of ZnO and V2O5; the particle size of the glass powder is 2-5μm.

4. The method according to claim 1, characterized in that, The composite cofferdam slurry is subjected to vacuum degassing and graded filtration before printing.

5. The method according to claim 1, characterized in that, The screen printing step is repeated at least twice. After each printing, the screen is pre-dried at 70-90°C for 3-10 minutes until surface dry and then cooled to room temperature before the next printing is performed.

6. The method according to claim 1, characterized in that, The sintering is a segmented inert atmosphere sintering, which includes a debinding section, a pre-sintering section and a densification sintering section performed sequentially; the entire sintering process is carried out under a nitrogen atmosphere.

7. The method according to claim 1, characterized in that, The sintering is laser local sintering: the laser wavelength is 808nm or 1064nm, the laser spot scans along the dam pattern, the scanning speed is 5-10mm / s, and the laser power is reduced at the corners of the dam; the printed glass substrate is preheated to 180-200℃, and cooled by nitrogen purging after sintering.

8. The method according to claim 7, characterized in that, The laser power is reduced by 10% at the corner of the cofferdam.

9. The method according to claim 1, characterized in that, The cofferdam pattern is a double-ring nested structure, including an inner ring pattern and an outer ring pattern, with an annular gap between the inner and outer ring patterns.

10. The method according to claim 9, characterized in that, A getter slurry is printed and filled in the annular gap, and the getter slurry is cured at low temperature to form a getter material layer.