A method for patterning a battery surface, a patterned silicon wafer, and a back contact battery containing the patterned wafer.

By using a metal mask and ultra-fine atomized spraying method, the cost and accuracy issues of screen-printed photoresist for patterning battery surfaces have been solved, achieving efficient and low-cost battery surface patterning processing and improving battery production efficiency and quality.

CN123124497APending Publication Date: 2026-11-17DAS SOLAR CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611581283.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-13
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the existing technology, screen printing photoresist has problems such as high cost and poor control of film thickness and precision when preparing battery surface patterns, resulting in low electrode forming accuracy and affecting battery conversion efficiency.

Method used

A method using a metal mask and ultra-fine atomization spraying is employed. By covering the silicon wafer surface with a metal mask and performing ultrasonic atomization spraying of ultraviolet photoresist, a protective film layer is formed. Combined with ultraviolet curing and etching processes, this method replaces the traditional screen printing process.

Benefits of technology

It improves the thickness uniformity and dimensional accuracy of the photoresist film, reduces production costs, and enhances battery yield and performance, making it suitable for mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124497A_ABST
    Figure CN123124497A_ABST
Patent Text Reader

Abstract

This application belongs to the field of photovoltaic technology and provides a method for patterning the surface of a battery, a patterned silicon wafer, and a back contact battery containing the pattern. The method uses a metal mask and ultra-fine atomization spraying to prepare a patterned photoresist layer on the doped glass layer of the silicon wafer, followed by ultraviolet curing to form a protective film layer. This formation method improves the thickness uniformity and dimensional accuracy of the protective film layer, and avoids the process defects and high costs associated with screen printing. The resulting high-precision protective film layer can protect the BSG / PSG layer in designated areas during subsequent etching processes and can be easily peeled off after etching. This method is easy to implement and highly efficient, achieving the same production capacity as traditional screen printing. It is particularly suitable for mass production scenarios involving selective etching of the doped glass layer of back contact batteries, effectively reducing production costs and improving battery yield and performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of photovoltaic technology and relates to a method for patterning the surface of a battery, a patterned silicon wafer, and a back contact battery containing the patterned silicon wafer. Background Technology

[0002] In the manufacturing process of N-type back contact (BC) solar cells, boron diffusion on the back side is required to prepare the P-type emitter, and phosphorus diffusion is required to prepare the N-type back field. After the diffusion process, borosilicate glass (BSG) and phosphorus silicate glass (PSG) are formed on the silicon wafer surface. The BSG and PSG layers cannot be directly used to fabricate electrodes; selective wet etching is required to remove the doped glass layer in designated areas, retaining the glass layer in the target areas as a protective layer for subsequent processes. This is a core pre-process for BC solar cell PN junction isolation and electrode formation. Currently, the industry uses screen-printed photoresist as an acid-resistant protective layer for selective etching of the BSG / PSG layers. However, due to the characteristics of screen printing, it inevitably brings inherent problems such as high cost and poor control over film thickness and precision. Summary of the Invention

[0003] In view of the problems existing in the prior art, the purpose of this application is to provide a method for patterning the surface of a battery, a patterned silicon wafer and a back contact battery containing the patterned silicon wafer. This method uses a metal plate mask and ultra-fine atomized spraying to replace screen printing, which can effectively improve the thickness uniformity and dimensional accuracy of the patterned protective film layer formed by photoresist.

[0004] To achieve this objective, the following technical solution is adopted in this application: In a first aspect, some embodiments of this application provide a method for patterning a battery surface, comprising the following steps: A silicon wafer that has undergone boron diffusion or phosphorus diffusion treatment is provided, and the surface of the silicon wafer is covered with a corresponding BSG layer or PSG layer; A metal mask is covered on the BSG layer or PSG layer, the metal mask including a patterned masking area and a cutout area; Ultraviolet photoresist is ultrasonically atomized and sprayed onto the side of the metal mask away from the silicon wafer to form a photoresist layer; The photoresist layer is cured with ultraviolet light, the metal mask is removed, a protective film layer is formed at the position corresponding to the hollow area, and the BSG layer or PSG layer is exposed at the position corresponding to the shielded area. The exposed BSG or PSG layer is removed by etching, and then the protective film layer is removed to obtain a patterned silicon wafer.

[0005] In some embodiments, the method further includes cleaning and preheating the silicon wafer before covering the metal mask.

[0006] In some embodiments, the preheating temperature is 45°C to 55°C.

[0007] In some embodiments, the ultraviolet photoresist is a negative photoresist.

[0008] In some embodiments, the viscosity of the ultraviolet photoresist is 50,000 mPa·s to 200,000 mPa·s.

[0009] In some embodiments, the solid content of the ultraviolet lithography is 30% to 50%.

[0010] In some embodiments, the metal mask is made of stainless steel.

[0011] In some embodiments, the thickness of the metal mask is 0.1 mm to 0.2 mm.

[0012] In some embodiments, the hollowed-out area includes straight through grooves with a line width of 200μm to 400μm and a straightness error of <1μm. The straight through grooves are arranged in parallel at equal intervals along the line width direction to form a pattern.

[0013] In some embodiments, the ultrasonic atomization spraying and the ultraviolet curing are performed under inert gas protection.

[0014] In some embodiments, the ultrasonic frequency of the ultrasonic atomization spray is 50kHz to 100kHz.

[0015] In some embodiments, the size of the microdroplets generated by the ultrasonic atomization spraying is 3μm to 10μm.

[0016] In some embodiments, the ultrasonic atomization spraying speed is 150 mm / s to 300 mm / s.

[0017] In some embodiments, the vertical distance between the ultrasonic atomizing nozzle and the surface of the silicon wafer is 15mm to 25mm, and the atomization column divergence angle is 8° to 15°.

[0018] In some embodiments, the method further includes using a visual closed-loop correction system to control the offset of the ultrasonic atomization spraying to ≤20 μm.

[0019] In some embodiments, the line width of the photoresist layer formed by ultrasonic atomization spraying in the hollowed-out area is ≤10μm, and the thickness uniformity difference is ≤15%.

[0020] In some embodiments, the method further includes pre-baking the photoresist layer before UV curing, wherein the pre-baking temperature is 75°C to 90°C and the time is 5s to 10s.

[0021] In some embodiments, the UV curing uses a single-wavelength UV light source, with the wavelength selected from 355nm to 375nm.

[0022] In some embodiments, the UV curing energy is 8000 mJ / cm². 2 ~12000mJ / cm 2 The curing time is 1s to 5s.

[0023] In some embodiments, the etching process includes immersion in an acidic etchant; the acidic etchant includes a hydrofluoric acid solution with a concentration of 10% to 15%.

[0024] In some embodiments, the method for removing the protective film includes soaking the material in a mixed solution of a 1% to 2.5% alkaline solution and a 3% to 5% hydrogen peroxide solution; the alkaline solution includes a sodium hydroxide solution.

[0025] Secondly, some embodiments of this application provide a patterned silicon wafer, fabricated according to the method described in the first aspect.

[0026] Thirdly, some embodiments of this application provide a back contact battery containing the patterned silicon wafer described in the second aspect.

[0027] Compared with existing technical solutions, this application has at least the following beneficial effects: The method provided in this application employs a metal mask and ultra-fine atomization spraying to prepare a patterned photoresist layer on a silicon wafer with a BSG / PSG doped glass layer on its surface. A protective film layer is then formed through short-time UV curing. Compared to screen printing, the protective photoresist film layer formed by this method effectively improves and controls the thickness uniformity and dimensional accuracy, while avoiding the process defects and high costs associated with screen printing. The resulting high-precision protective film layer can protect the BSG / PSG layer in designated areas during subsequent etching processes and can be easily peeled off after etching, thus forming a high-precision etched pattern on the silicon wafer surface, laying a foundation for the precision of subsequent battery processes. Furthermore, the mask application, ultrasonic atomization spraying, and UV curing processes in this method are easy to implement and operate efficiently. The overall production capacity can reach the same level as traditional screen printing, making it particularly suitable for mass production scenarios involving selective etching of the doped glass layer in back-contact batteries. This effectively reduces production costs and improves battery yield and performance. Attached Figure Description

[0028] Figure 1 This is a schematic diagram of a system apparatus capable of implementing the method for patterning the battery surface provided in the embodiments of this application.

[0029] In the figure, 1-silicon wafer support platform; 2-silicon wafer preheating platform; 3-transfer belt; 4-silicon wafer; 5-metal mask plate; 6-ultrasonic atomizing nozzle; 7-visual correction system; 8-UV lamp plate; 9-UV lamp beads. Detailed Implementation

[0030] The technical solution of this application will be further described below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely to help understand this application and should not be regarded as specific limitations on this application.

[0031] The scope of this application can be defined by lower and upper limits. The selected lower and upper limits define the boundaries of a specific range. The range defined in this way can be defined by the inclusion or exclusion of endpoints. Any endpoint can be independently selected for inclusion or exclusion, and all lower and upper limits can be arbitrarily combined to form new ranges. That is, any lower limit can be combined with any upper limit to form a valid range. For example, if the ranges of 60~120 and 80~110 are listed for specific parameters, it should be understood that the ranges of 60~110 and 80~120 also fall within the scope of this application. In addition, if the minimum range values ​​1 and 2 are listed, and the maximum range values ​​3, 4 and 5 are also listed, then all ranges of 1~3, 1~4, 1~5, 2~3, 2~4 and 2~5 fall within the scope of this application. In this application, the numerical range "a~b" represents a shortened representation of any combination of real numbers between a and b, where a and b are both real numbers. For example, the numerical range "0~5" means that all real numbers between 0 and 5 have been fully listed in this document, and "0~5" is only a shortened representation of this set of numerical combinations. When a parameter is expressed as an integer ≥2, it is equivalent to listing positive integers that meet the requirements, such as 2, 3, 4, 5, 6, 7, 8, 9, 10, etc. When a parameter is expressed as an integer selected from "2~10", it is equivalent to listing any integer among 2, 3, 4, 5, 6, 7, 8, 9, and 10.

[0032] In this application, "at least two combinations" refers to a quantity greater than or equal to 2 unless otherwise specified. For example, "any one or at least two combinations" means any one of the listed items, or a combination of at least two of the listed items formed in a manner that does not conflict and enables the implementation of this application. In this application, unless otherwise specified, the features or solutions corresponding to "and / or" cover any one of two or more related listed items, as well as any and all combinations of the related listed items. The arbitrary and all combinations include any two related listed items, any more related listed items, or a combination of all related listed items. For example, "A and / or B" represents a set consisting of A, B, and combinations of A and B, where "containing A and / or B" can be understood, depending on the context of the statement, as containing A, containing B, or simultaneously containing both A and B. In this application, "optional" means that the corresponding feature, component, step or solution is not necessary, that is, it is selected from either "with" or "without". If there are multiple "optional" limitations in a technical solution, unless otherwise specified and there is no technical conflict or mutual constraint, each "optional" limitation is independent and does not affect the others.

[0033] In this application, technical features or solutions described using open-ended terms such as "comprising" or "including" do not exclude additional non-conflicting elements beyond those listed unless otherwise specified. They are considered to disclose both closed-ended features or solutions consisting solely of the listed elements and open-ended features or solutions that may include additional non-conflicting elements beyond the listed elements. For example, if A includes a1, a2, and a3, unless otherwise specified, this means that A can consist only of a1, a2, and a3, or it can include other non-conflicting elements based on a1, a2, and a3. This corresponds to the disclosure of technical solutions such as "A consists of a1, a2, and a3," "A is selected from a1, a2, and a3," and "A not only includes a1, a2, and a3, but may also include other non-conflicting elements." All embodiments and optional embodiments of this application, unless otherwise specified and without technical conflict, can be combined to form new technical solutions, and such combinations fall within the scope of this application. The term "embodiment" as used in this application means that a specific feature, structure, or characteristic described in connection with an embodiment can be included in at least one embodiment or implementation of this application. The appearance of this phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment mutually exclusive with other embodiments. Those skilled in the art can explicitly and implicitly understand that the embodiments described in this application can be combined with other embodiments that do not conflict with the technology. The ordinal numbers "first," "second," "third," and "fourth," etc., used in this application in the expressions "first aspect," "second aspect," "third aspect," and "fourth aspect," are for descriptive purposes only and should not be construed as indicating or implying relative importance or quantity, nor should they be construed as implicitly specifying the importance or quantity of the indicated technical features. They serve only as a non-exhaustive enumeration and do not constitute a closed limitation on quantity.

[0034] In this application, the order in which the steps are written in the methods described in the various embodiments does not imply a strict execution order. The actual execution order of each step should be determined based on its function and possible internal logic. Unless otherwise specified, all steps in this application can be executed in the order they are written, or in any order that does not conflict with the technology. For example, if the method includes steps (a) and (b), it means that the method may include steps (a) and (b) executed sequentially, or it may include steps (b) and (a) executed sequentially. If the method also includes step (c), then step (c) can be added to the method in any order that does not conflict with the technology, including but not limited to the execution order of steps (a), (b), and (c), steps (a), (c), and (b), steps (c), (a), and (b), etc.

[0035] Existing technology involves printing a specific pattern of photoresist onto the surface of a silicon wafer using a screen printing stencil. The photoresist's acid resistance helps to shield the etching solution, enabling localized etching of the glass layer. While this process boasts high production capacity, it relies heavily on high-precision screen printing stencils, resulting in high procurement and maintenance costs. Furthermore, the high viscosity of the photoresist makes it prone to adhering to the stencil mesh during printing, causing clogging. The stencil is also susceptible to irreversible deformation under prolonged tensile stress, directly leading to pattern misalignment and poor line quality. Additionally, uneven tension distribution on the screen results in significant differences in the amount of photoresist applied between the center and periphery of the silicon wafer. Areas with insufficient film thickness are easily penetrated during subsequent acid etching, failing to protect the BSG / PSG layer; areas with excessive film thickness are prone to incomplete curing and residual photoresist. Moreover, since screen printing is a contact-extrusion method, the photoresist is compressed and spreads outwards, often causing the patterned design to widen. This cumulative deviation directly impacts the alignment accuracy of subsequent electrodes, hindering improvements in battery conversion efficiency.

[0036] Therefore, in one or more embodiments of this application, a method for patterning a battery surface is provided, comprising the following steps: A silicon wafer that has undergone boron diffusion or phosphorus diffusion treatment is provided, and the surface of the silicon wafer is covered with a corresponding BSG layer or PSG layer; A metal mask is covered on the BSG layer or PSG layer, the metal mask including a patterned masking area and a cutout area; Ultraviolet photoresist is ultrasonically atomized and sprayed onto the side of the metal mask away from the silicon wafer to form a photoresist layer; The photoresist layer is cured with ultraviolet light, the metal mask is removed, a protective film layer is formed at the position corresponding to the hollow area, and the BSG layer or PSG layer is exposed at the position corresponding to the shielded area. The exposed BSG or PSG layer is removed by etching, and then the protective film layer is removed to obtain a patterned silicon wafer.

[0037] In this application, the BSG layer and PSG layer refer to the borosilicate glass layer (i.e., the BSG layer) and the phosphorus silicate glass layer (PSG layer) formed on the surface of the silicon wafer after boron diffusion treatment or phosphorus diffusion treatment. Unless otherwise specified, the surface of the silicon wafer targeted by each step in the method provided in this application refers to the surface with the BSG layer and PSG layer. For example, for a back contact cell (BC), boron diffusion and phosphorus diffusion are usually performed on the back side (i.e., the backlight side) of the silicon wafer, then the surface of the silicon wafer refers to the surface on the back side of the silicon wafer.

[0038] This application abandons the contact screen printing method and adopts an integrated solution of precise metal mask positioning, ultra-fine ultrasonic atomization spraying and instant UV curing. The microdroplets formed by ultrasonic atomization spray pass through the hollow area of ​​the metal mask and are directionally deposited on the silicon wafer surface, which suppresses the irregular spread of photoresist and produces only controllable leveling. Then, the density of the photoresist layer can be improved by high intensity short-time UV curing, thereby preparing an acid-resistant and alkali-soluble photoresist protective film layer. Thus, the acid resistance of the photoresist isolates the BSG / PSG layer from acid, and the photoresist can be quickly removed by alkaline solution after acid etching, which can completely replace the traditional screen printing process. Because the method of this application relies on the characteristics of metal mask limiting and non-contact spraying, it can effectively control the widening of the photoresist pattern, thereby improving accuracy. The pattern consistency is high, and there is no extrusion deformation problem. Moreover, the thickness of the photoresist layer and the protective film it forms is constant, effectively reducing film thickness deviation and avoiding problems such as acid penetration due to insufficient film thickness and residual defects due to excessive film thickness, achieving stable protection of the BSG or PSG layer. The method provided by this application has strong process adaptability. The ultraviolet photoresist has dual characteristics of acid resistance and easy alkali solubility, resulting in a protective film layer with few defects and high density, perfectly matching the complete wet acid etching and alkaline resist removal process. The method provided by this application can completely eliminate the consumables of screen printing stencils and the associated cleaning, replacement, and maintenance processes. A single GW of production capacity can save 1.6 million to 2.6 million yuan in stencil costs annually, reducing downtime for board replacement, increasing production line uptime, and achieving a production capacity of 3000 to 3200 pieces / hour, at the same level as screen printing, and is fully compatible with existing mass production lines.

[0039] In some embodiments, the silicon wafer may be N-type or P-type, and may be a monocrystalline silicon wafer.

[0040] In some embodiments, the method further includes cleaning and preheating the silicon wafer before covering it with the metal mask. The cleaning process removes surface dust and organic residues, and the preheating process eliminates surface temperature differences and improves photoresist adhesion.

[0041] In some embodiments, the cleaning process includes using oxygen plasma on the surface of the silicon wafer. In some embodiments, the cleaning time can be 30s to 90s, for example, 30s, 40s, 50s, 60s, 70s, 80s, or 90s.

[0042] In some embodiments, the temperature of the preheating treatment is 45°C to 55°C, for example, it can be 45°C, 48°C, 50°C, 52°C or 55°C.

[0043] In some embodiments, the preheating process is performed by fixing the silicon wafer onto a vacuum adsorption stage.

[0044] In some embodiments, the ultraviolet photoresist is a negative photoresist. The ultraviolet photoresist described in this application is a type of photoresist that can be cured by ultraviolet light irradiation. Negative ultraviolet photoresist is chemically resistant to acid corrosion but completely soluble in alkaline solutions. Therefore, after curing to form a protective film, it can isolate the underlying BSG or PSG layer from acidic etching solutions and can be quickly and completely removed subsequently by an alkaline solution.

[0045] In some embodiments, the viscosity of the ultraviolet photoresist is 50,000 mPa·s to 200,000 mPa·s, for example, it can be 50,000 mPa·s, 80,000 mPa·s, 100,000 mPa·s, 130,000 mPa·s, 150,000 mPa·s, 180,000 mPa·s, or 200,000 mPa·s, etc.

[0046] In some embodiments, the solid content of the ultraviolet photoresist is 30% to 50%, for example, it can be 30%, 33%, 35%, 38%, 40%, 43%, 45%, 48% or 50%, etc.

[0047] In this application, the viscosity of the photoresist affects the spreading ability of droplets after impacting the silicon wafer, while the solid content affects the thickness of the solid film after drying / curing. Too low a viscosity leads to easy lateral spreading of droplets on the silicon surface, resulting in excessive line widening and poor film thickness uniformity. Too high a viscosity makes the droplets difficult to flow, easily causing particles and pinholes, and increasing film thickness fluctuations. Higher solid content results in a thicker film after curing for the same amount of droplets. Fluctuations in solid content can lead to batch-to-batch differences in film thickness. Therefore, maintaining suitable viscosity and solid content in the UV photoresist of this application is beneficial for both ultrasonic atomization to generate microdroplets and for achieving controllable leveling after spraying with the aid of a metal mask.

[0048] In some embodiments, the metal photomask is made of stainless steel. The metal photomask described in this application, covering one side of the silicon wafer, means it can be in contact with the silicon wafer surface or positioned above it. This allows the atomized photoresist to be uniformly deposited as droplets through the cutout area onto the silicon wafer surface. The distance between the photomask and the silicon wafer surface should be appropriate to control the precision and uniformity of the film thickness during ultrasonic atomization spraying within the cutout area.

[0049] In some embodiments, the thickness of the metal mask is 0.1mm to 0.2mm, for example, it can be 0.1mm, 0.12mm, 0.14mm, 0.16mm, 0.18mm or 0.2mm, etc.

[0050] In some embodiments, the hollowed-out area includes straight through slots with a line width of 200μm to 400μm, such as 200μm, 230μm, 250μm, 280μm, 300μm, 330μm, 350μm, 380μm, or 400μm; and a straightness error of <1μm, such as 0.9μm, 0.8μm, 0.7μm, 0.6μm, 0.5μm, 0.2μm, or 0.1μm; and the straight through slots are arranged in parallel at equal intervals along the line width direction to form a pattern. In one embodiment, the number of straight through slots is 100 to 300, such as 100, 130, 150, 166, 180, 200, 230, 250, 280, or 300. For example, 166 straight through slots can be arranged in parallel at equal intervals to adapt to the cross-finger electrode structure on the back of the back contact battery.

[0051] In some embodiments, the ultrasonic atomization spraying and the ultraviolet curing are performed under inert gas protection. In one embodiment, the ultrasonic atomization spraying and ultraviolet curing can be completed in a sealed nitrogen chamber, with the oxygen content of the chamber controlled to ≤500ppm, to prevent pinhole defects caused by oxidation during the photoresist spraying and curing process, improve density, and ensure acid resistance.

[0052] In some embodiments, the ultrasonic frequency of the ultrasonic atomization spraying is 50kHz to 100kHz, for example, it can be 50kHz, 60kHz, 70kHz, 80kHz, 90kHz or 100kHz.

[0053] In some embodiments, the size of the microdroplets generated by ultrasonic atomization spraying is 3μm to 10μm, for example, 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, or 10μm. It should be noted that the 3μm to 10μm range mentioned in this application refers to the particle size range of a single atomized microdroplet and is only used to characterize the fineness of atomization, not the final formed linewidth.

[0054] In some embodiments, the ultrasonic atomization spraying speed is 90 mm / s to 300 mm / s, for example, 90 mm / s, 100 mm / s, 110 mm / s, 120 mm / s, 130 mm / s, 140 mm / s, 150 mm / s, 160 mm / s, 180 mm / s, 200 mm / s, 230 mm / s, 250 mm / s, 280 mm / s, or 300 mm / s. In some embodiments, when spraying to the edge area of ​​the silicon wafer, the spraying speed can be appropriately reduced, for example, to 60 mm / s to 80 mm / s, for example, 60 mm / s, 65 mm / s, 70 mm / s, 75 mm / s, or 80 mm / s. Therefore, zoned variable speed spraying is beneficial for controlling and improving the uniformity of film thickness on each surface area of ​​the silicon wafer.

[0055] In some embodiments, the vertical distance between the ultrasonic atomizing nozzle and the surface of the silicon wafer is 15mm to 25mm, for example, 15mm, 16mm, 17mm, 18mm, 19mm, 20mm, 21mm, 22mm, 23mm, 24mm, or 25mm, and the atomization column divergence angle is 8° to 15°, for example, 8°, 9°, 10°, 11°, 12°, 13°, 14°, or 15°. This facilitates the use of a metal mask to jointly limit droplet dispersion, achieve controllable leveling, and improve accuracy and film thickness uniformity.

[0056] In some embodiments, the method further includes using a visual closed-loop correction system to control the offset of the ultrasonic atomization spraying to be ≤20μm. For example, the offset can be controlled to be 20μm, 18μm, 15μm, 12μm, 10μm, 8μm, 6μm, 4μm, 2μm or 1μm, etc.

[0057] In this application, the offset of ultrasonic atomization spraying refers to the lateral position deviation (i.e., geometric deviation of the planar position) of the actual spraying trajectory of the nozzle relative to the theoretical center of the hollow area (such as a slot) of the metal mask. Typically, the hollow slot of the mask has a designed theoretical center line. Therefore, under ideal conditions, the center of the atomized spray column should move along the center line of the hollow slot. At this time, the distance (in the X / Y direction of the plane) of the center of the spray column relative to the theoretical center line of the hollow slot is the offset.

[0058] The offset can be identified by a visual closed-loop correction system. This system may include an image acquisition unit, which may include an industrial vision camera (including a lens and light source), or further include a two-dimensional translational motion platform servo driver, acting as an actuator to control the industrial vision camera. It may also include an image processing unit (vision controller), configured to be electrically connected to the image acquisition unit and used for image recognition, coordinate calculation, and offset calculation. A main system controller may also be included, electrically connected to the image acquisition unit and the image processing unit, configured to coordinate the spray nozzle, vision system, and servo based on the offset. Furthermore, to achieve alignment when the visual closed-loop correction system acquires images, in some embodiments, alignment reference marks (such as cross / dot marks) can be used on the metal mask.

[0059] The process of identifying and calculating the offset using a visual closed-loop correction system can include: selecting multiple photoresist lines on a silicon wafer and acquiring images using an industrial vision camera; identifying two reference points using software: the theoretical center line of the cutout groove on the metal mask (CAD design reference or alignment mark reconstruction reference on the mask), and the actual center of the photoresist lines after curing; then measuring the distance between the two points in the X and Y directions on a plane, which is the single-point offset; furthermore, measurements can be taken at multiple sampling locations such as the center and four corners of the silicon wafer, and the maximum absolute value is taken as the true value of the offset for this process for output, which is then fed back to the servo driver of the two-dimensional translational motion platform and the overall system controller for adjustment and correction for the next spraying time.

[0060] In some embodiments, the thickness of the photoresist layer can be 2μm to 6μm, for example, 2μm, 3μm, 4μm, 5μm or 6μm.

[0061] In some embodiments, the line width of the photoresist layer formed by ultrasonic atomization spraying in the hollowed-out area is ≤10μm, for example, it can be 10μm, 8μm, 6μm, 5μm, 4μm, 2μm or 1μm, etc.; the thickness uniformity difference is ≤15%, for example, it can be 15%, 13.5%, 12.5%, 11%, 10%, 8%, 6%, 4%, 2% or 1%, etc.; in some embodiments, the thickness uniformity difference is ≤0.5μm, for example, it can be 0.5μm, 0.4μm, 0.3μm, 0.2μm or 0.1μm, etc. After ultrasonic atomization spraying, the sprayed photoresist layer (i.e., wet film layer) can achieve the requirements of accuracy and thickness uniformity under the limitation of the metal mask and the natural leveling effect of the adhesive layer.

[0062] In some embodiments, the method further includes pre-baking the photoresist layer before UV curing to remove organic solvents from the photoresist layer and improve the density and acid resistance of the photoresist layer after forming the protective film. In some embodiments, the temperature of the pre-baking treatment is 75℃~90℃, for example, 75℃, 80℃, 85℃, 88℃ or 90℃; the time is 5s~120s, for example, 5s, 6s, 7s, 8s, 9s, 10s, 13s, 15s, 20s, 50s, 80s, 100s, 110s or 120s.

[0063] In some embodiments, the ultraviolet curing uses a single-wavelength ultraviolet light source with a wavelength selected from 355nm to 395nm, such as 355nm, 358nm, 360nm, 362nm, 365nm, 368nm, 370nm, 372nm, 380nm, 385nm, 390nm, or 395nm.

[0064] In some embodiments, the UV curing energy is 8000 mJ / cm². 2 ~12000mJ / cm 2 For example, it could be 8000mJ / cm 2 9000mJ / cm 2 10000mJ / cm 2 11000mJ / cm 2 Or 12000mJ / cm 2 The curing time is 1s to 5s, for example, 1s, 2s, 3s, 4s, or 5s. This application uses ultraviolet irradiation with appropriate curing energy, which can complete curing in a very short time, thus improving production efficiency.

[0065] In some embodiments, the etching process includes immersion in an acidic etching solution; the acidic etching solution includes a hydrofluoric acid solution with a concentration of 10% to 15%, for example, it can be 10%, 11%, 12%, 13%, 14%, or 15%. In some embodiments, the etching time is 15s to 60s, for example, it can be 15s, 20s, 30s, 40s, 45s, 50s, 55s, or 60s.

[0066] In some embodiments, the method for removing the protective film includes soaking in a mixed solution of a 1%–2.5% alkaline solution and a 3%–5% hydrogen peroxide solution, both concentrations being mass percentages. The concentration of the alkaline solution can be 1%, 1.3%, 1.5%, 1.8%, 2%, or 2.5%, etc.; the concentration of the hydrogen peroxide can be 3%, 3.5%, 4%, 4.5%, or 5%, etc. The alkaline solution includes sodium hydroxide solution. Therefore, by soaking in a mixed solution of suitable concentration at room temperature for a short time of 20s–60s, such as 20s, 25s, 30s, 35s, 40s, 45s, 50s, 55s, or 60s, the protective film can be completely peeled off.

[0067] As a further example, this application provides a system apparatus capable of implementing the aforementioned method. This system apparatus optionally includes a silicon wafer loading module, a constant temperature preheating module, a metal mask (including its clamping module), an array-type ultrasonic atomization spraying module, and a visual correction system. Further, at least one of a hot air pre-baking module, a UV curing module, an acid-base etching module, and a unloading module can be added for subsequent processes. Specifically, after the silicon wafer is coated with the corresponding pattern, it can pass through a UV curing oven, which includes hot air heating and UV lamps of a specific wavelength for curing. After curing, the silicon wafer undergoes acid-base cleaning for resist removal and pattern etching before being unloaded. Specifically, as shown... Figure 1 As shown, the loading module may include a silicon wafer support platform 1, a conveyor belt 3 on the silicon wafer support platform 1, and a silicon wafer preheating platform 2 on the conveyor belt 3. The silicon wafer preheating platform 2 is used to support silicon wafers 4. A metal mask 5 is placed above the silicon wafer 4 through a clamping module. Then, an ultrasonic atomizing spraying module controls ultrasonic atomizing nozzles 6 to perform ultrasonic atomizing spraying on the surface of the silicon wafer 4 through the metal mask 5. At this time, the visual correction system 7 is electrically connected to the ultrasonic atomizing spraying module to compensate for trajectory deviations caused by equipment vibration in real time. After ultrasonic atomizing spraying is completed, the silicon wafer 4 is transported to a UV lamp plate 8 with UV lamp beads 9 through the conveyor belt 3 for ultraviolet curing. The above module and the system device composed of it can be set in a nitrogen-sealed cavity and can be optionally adapted to silicon wafers of 166mm, 182mm, 210mm, etc.

[0068] One or more embodiments of this application provide a patterned silicon wafer, which is prepared according to the method described in the foregoing embodiments.

[0069] One or more embodiments of this application provide a back contact battery containing the patterned silicon wafer described in the foregoing embodiments.

[0070] Example 1 This embodiment provides a method for patterning the surface of a battery, including the following steps: S1. Substrate preparation: Select an N-type monocrystalline silicon wafer with a size of 182mm, which has a front and a back side. The back side is the backlight side. Perform boron diffusion and phosphorus diffusion processes on the back side to form corresponding BSG and PSG layers on the silicon wafer surface. S2. Pretreatment: The back of the silicon wafer is cleaned with O2 plasma for 60 seconds to remove surface impurities. Then, the silicon wafer is fixed by vacuum adsorption and preheated at 50°C. S3. Photoresist selection: Select negative ultraviolet photoresist with a viscosity of 120,000 mPa·s and a solid content of 45%. Its chemical properties include resistance to hydrofluoric acid corrosion and solubility in KOH alkaline solution with a concentration of more than 1%. S4. Mask-assisted spraying: A stainless steel metal mask is provided, with 166 sets of equally spaced parallel straight through slots (i.e., hollow areas) on the mask, and the line width of a single slot is designed to be 300μm; the metal mask is covered on the back of the silicon wafer. In a sealed cavity protected by nitrogen and with an oxygen content of 400 ppm, an ultrasonic atomization frequency of 80 kHz is set to ultrasonically atomize the photoresist and spray it through a nozzle as microdroplets with a particle size of 5 μm to 8 μm. The nozzle is 20 mm away from the silicon wafer, and the atomization column divergence angle is controlled at 10°. Spraying is performed on the side of the metal mask away from the silicon substrate, allowing the microdroplets to pass through the hollow area and be directionally deposited onto the surface of the silicon wafer. The spraying speed is controlled at 100 mm / s in the central area of ​​the silicon wafer and at 70 mm / s in the edge area of ​​the silicon wafer. At the same time, during the spraying process, the spraying position is adjusted by a visual closed-loop correction system to correct the deviation, so that the deviation is <20 μm, thus forming a photoresist layer. S5. Pre-baking treatment: Bake at 85℃ for 80 seconds to remove the solvent inside the photoresist layer; S6. UV Curing: Using a single UV light source with a wavelength of 365nm, the curing energy is 10000mJ / cm². 2 The photoresist layer is further cured under ultraviolet light for 3 seconds. After removing the metal mask, a protective film is formed on the photoresist layer at the corresponding position of the cutout area. The size and shape of the protective film correspond to the straight through groove. That is, the film is composed of several parallel lines arranged at equal intervals. The line width is 300μm, the spread is ≤10μm, and the film thickness is 4.0μm±0.5μm, that is, the thickness uniformity is ≤12.5%. S7. Selective etching: Use 12% hydrofluoric acid solution to etch at room temperature for 45 seconds to remove the BSG and PSG layers on the areas not covered by the protective film, so as to achieve complete etching of the exposed doped glass layer, while the BSG and PSG layers on the corresponding areas covered by the protective film are completely preserved. S8. Alkaline Resin Removal: Use a mixed solution of 1.5% NaOH and 3% hydrogen peroxide, immerse at room temperature for 40 seconds to completely dissolve and peel off the protective film formed by the photoresist, leaving no residual photoresist, thus completing the patterning process and obtaining a patterned silicon wafer.

[0071] Example 2 This embodiment provides a method for patterning the surface of a battery, including the following steps: S1. Substrate preparation: Select a 166mm N-type monocrystalline silicon wafer with a front and a back side. The back side is the backlight side. Perform boron diffusion and phosphorus diffusion processes on the back side to form corresponding BSG and PSG layers on the silicon wafer surface. S2. Pretreatment: The back of the silicon wafer is cleaned with O2 plasma for 30 seconds to remove surface impurities. Then, the silicon wafer is fixed by vacuum adsorption and preheated at 45°C. S3. Photoresist selection: Select negative ultraviolet photoresist with a viscosity of 50,000 mPa·s and a solid content of 30%. Its chemical properties include resistance to hydrofluoric acid corrosion and solubility in KOH alkaline solution with a concentration of more than 1%. S4. Mask-assisted spraying: A stainless steel metal mask is provided, with 248 sets of equally spaced parallel straight through slots (i.e., hollow areas) on the mask, with a single slot design line width of 200μm; the metal mask is covered on the back of the silicon wafer. In a sealed cavity protected by nitrogen and with an oxygen content of 200 ppm, photoresist is ultrasonically atomized at a frequency of 100 kHz and sprayed through a nozzle as microdroplets with a particle size of 3 μm to 6 μm. The nozzle is 15 mm away from the silicon wafer, and the atomization angle is controlled at 8°. Spraying is performed on the side of the metal mask away from the silicon substrate, allowing the microdroplets to pass through the hollowed-out area and be directionally deposited onto the surface of the silicon wafer. The spraying speed is controlled at 90 mm / s in the central area of ​​the silicon wafer and at 60 mm / s in the edge area. Simultaneously, during the spraying process, the spraying position is adjusted by a visual closed-loop correction system to correct the offset, ensuring that the offset is <10 μm, thus forming a photoresist layer. S5. Pre-baking treatment: Bake at 75℃ for 120 seconds to remove the solvent inside the photoresist layer; S6. UV Curing: Using a single UV light source with a wavelength of 375nm, the curing energy is 8000mJ / cm². 2 The photoresist layer is further cured under ultraviolet light for 5 seconds. After removing the metal mask, a protective film is formed on the photoresist layer at the corresponding position of the cutout area. The size and shape of the protective film correspond to the straight through groove. That is, the film is composed of several parallel lines arranged at equal intervals. The line width is 200μm, the spread is ≤8μm, and the film thickness is 3.0μm±0.35μm, that is, the thickness uniformity is ≤11.7%. S7. Selective etching: Use 10% hydrofluoric acid solution to etch at room temperature for 55 seconds to remove the BSG and PSG layers on the areas not covered by the protective film, achieving complete etching of the exposed doped glass layer, while the BSG and PSG layers on the corresponding areas covered by the protective film are completely preserved. S8. Alkaline Resin Removal: Use a mixed solution of 1% NaOH and 4% hydrogen peroxide, immerse at room temperature for 60 seconds to completely dissolve and peel off the protective film formed by the photoresist, leaving no residual photoresist, thus completing the patterning process and obtaining a patterned silicon wafer.

[0072] Example 3 This embodiment provides a method for patterning the surface of a battery, including the following steps: S1. Substrate preparation: Select an N-type monocrystalline silicon wafer with a size of 210mm, which has a front side and a back side. The back side is the backlight side. Perform boron diffusion and phosphorus diffusion processes on the back side to form corresponding BSG and PSG layers on the silicon wafer surface. S2. Pretreatment: The back of the silicon wafer is cleaned with O2 plasma for 90 seconds to remove surface impurities. Then, the silicon wafer is fixed by vacuum adsorption and preheated at 55°C. S3. Photoresist selection: Select negative ultraviolet photoresist with a viscosity of 200,000 mPa·s and a solid content of 50%. Its chemical properties include resistance to hydrofluoric acid corrosion and solubility in KOH alkaline solution with a concentration of more than 1%. S4. Mask-assisted spraying: A stainless steel metal mask is provided, with 124 sets of equally spaced parallel straight through slots (i.e., hollow areas) on the mask, and the line width of a single slot is designed to be 400μm; the metal mask is covered on the back of the silicon wafer. In a sealed cavity protected by nitrogen and with an oxygen content of 300 ppm, an ultrasonic atomization frequency of 50 kHz is set to ultrasonically atomize the photoresist and spray it through a nozzle as microdroplets with a particle size of 6 μm to 10 μm. The nozzle is 25 mm away from the silicon wafer, and the atomization column divergence angle is controlled at 15°. Spraying is performed on the side of the metal mask away from the silicon substrate, allowing the microdroplets to pass through the hollowed-out area and be directionally deposited onto the surface of the silicon wafer. The spraying speed is controlled at 200 mm / s in the central area of ​​the silicon wafer and at 80 mm / s in the edge area. Simultaneously, during the spraying process, the spraying position is adjusted by a visual closed-loop correction system to correct the offset, ensuring that the offset is less than 15 μm, thus forming a photoresist layer. S5. Pre-baking treatment: Bake at 90℃ for 45 seconds to remove the solvent inside the photoresist layer; S6. UV Curing: Using a single UV light source with a wavelength of 385nm, the curing energy is 12000mJ / cm². 2The photoresist layer is further cured under ultraviolet light for 2 seconds. After removing the metal mask, a protective film is formed on the photoresist layer at the corresponding position of the cutout area. The size and shape of the protective film correspond to the straight through groove. That is, the film is composed of several parallel lines arranged at equal intervals. The line width is 400μm, the width is ≤10μm, and the film thickness is 5.0μm±0.61μm, that is, the thickness uniformity is ≤12.2%. S7. Selective etching: Use 15% hydrofluoric acid solution to etch at room temperature for 20 seconds to remove the BSG and PSG layers on the areas not covered by the protective film, achieving complete etching of the exposed doped glass layer, while the BSG and PSG layers on the corresponding areas covered by the protective film are completely preserved. S8. Alkaline Resin Removal: Use a mixed solution of 2.5% NaOH and 5% hydrogen peroxide at room temperature for 20 seconds to completely dissolve and peel off the protective film formed by the photoresist, leaving no residual photoresist, thus completing the patterning process and obtaining a patterned silicon wafer.

[0073] Example 4 The difference from Example 1 is that the viscosity of the negative ultraviolet photoresist was adjusted from 120,000 mPa·s to 35,000 mPa·s. Apart from the above, the other conditions are exactly the same as those in Example 1.

[0074] Example 5 The difference from Example 1 is that the viscosity of the negative ultraviolet photoresist was adjusted from 120,000 mPa·s to 50,000 mPa·s. Apart from the above, the other conditions are exactly the same as those in Example 1.

[0075] Example 6 The difference from Example 1 is that the viscosity of the negative ultraviolet photoresist was adjusted from 120,000 mPa·s to 200,000 mPa·s. Apart from the above, the other conditions are exactly the same as those in Example 1.

[0076] Example 7 The difference from Example 1 is that the viscosity of the negative ultraviolet photoresist was adjusted from 120,000 mPa·s to 220,000 mPa·s. Apart from the above, the other conditions are exactly the same as those in Example 1.

[0077] Comparative Example 1 This comparative example uses screen printing technology to perform photoresist screen printing on a 182mm silicon wafer with the same specifications as in Example 1, and further processes the outer protective film layer. The screen film thickness is 20μm, the designed line width is 300μm, and the designed protective film layer after printing has a designed film thickness of 4μm and a designed line width of 300μm.

[0078] Comparative Example 2 This comparative example uses a conventional air pressure spraying process without using a photomask. A silicon wafer with the same 182mm specification as in Example 1 is coated with photoresist and further processed with an outer protective film layer. The protective film layer is designed to have a thickness of 4μm and a linewidth of 300μm.

[0079] Characterization and Testing 1) The thickness (actual average thickness) and thickness uniformity (percentage deviation from actual average thickness) of the protective film layers formed in the examples and comparative examples were measured and calculated.

[0080] 2) The linewidth (actual average linewidth) and linewidth widening (the amount exceeding the actual average linewidth) of the protective film layers formed in the embodiments and comparative examples are measured and calculated.

[0081] 3) Statistical analysis and calculation of the production capacity and overall yield of the examples and comparative examples.

[0082] The results are recorded in Table 1.

[0083] Table 1 As can be seen from Table 1: The protective film formed by the methods in Examples 1, 2, and 3 exhibits good uniformity in thickness and high dimensional accuracy. Furthermore, the acid etching process eliminates the problem of protective film penetration, and the alkaline removal leaves no residue, resulting in high-precision etched patterns. The methods provided in these examples do not require stencil consumables, achieving production capacity comparable to screen printing. Comparative Example 1 relies on a screen stencil, whose lifespan only supports a production volume of 50,000 pieces. The actual thickness of the protective film fluctuates between 3μm and 6μm, with a designed linewidth expansion of 30μm. This leads to issues such as stencil sticking, stencil deformation, and pattern misalignment, resulting in an overall yield of only 97.1%. Comparative Example 2 eliminates the metal mask and employs a conventional pneumatic spraying process. However, droplet dispersion is uncontrollable, resulting in a designed linewidth expansion >22μm, film thickness deviation >18%, and a susceptibility to pinhole defects. Protective film penetration occurs during the acid etching stage, failing to meet mass production requirements.

[0084] In summary, this application addresses the pain points of existing wet patterning processes for BC batteries after boron / phosphorus diffusion, which use screen printing photoresist to protect the BSG / PSG glass layer. These pain points include high material costs, easy deformation and adhesion of the screen, large film thickness fluctuations, large pattern linewidth expansion, and inability to monitor offset in real time. Furthermore, considering the specific process requirements for acid etching protection of the BSG / PSG layer, this application provides a non-contact ultrasonic atomization spraying method for preparing a protective film layer. This method uses a precision metal mask and an ultra-fine ultrasonic atomization spraying technique to prepare a protective film layer on the back side of a silicon wafer that has undergone boron and phosphorus diffusion and has a BSG / PSG doped glass layer attached to its surface. The protective photoresist pattern utilizes a negative ultraviolet photoresist that is acid-resistant and readily soluble in alkaline solutions. This allows for complete protection of the designated BSG / PSG layer during acid etching, and subsequent rapid stripping via alkaline solutions. The process method described in this application can precisely control the thickness uniformity deviation of the protective film formed by the photoresist to ≤12.5%, with a spread of ≤10μm. This improves pattern accuracy by 60%, and the overall production capacity can reach over 3000 wafers / hour, comparable to traditional screen printing. This method is suitable for mass production scenarios involving selective etching of the doped glass layer in BC batteries, which helps reduce production costs and improve battery yield and conversion efficiency.

[0085] The preferred embodiments of this application have been described in detail above. However, this application is not limited to the specific details of the above embodiments. Within the scope of the technical concept of this application, various simple modifications can be made to the technical solution of this application, and these simple modifications all fall within the protection scope of this application.

[0086] It should also be noted that the various specific technical features described in the above embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, this application will not describe the various possible combinations separately.

[0087] Furthermore, various different implementations of this application can be combined in any way, as long as they do not violate the spirit of this application, they should also be regarded as the content disclosed in this application.

Claims

1. A method for patterning a battery surface, characterized in that, Includes the following steps: A silicon wafer that has undergone boron diffusion or phosphorus diffusion treatment is provided, and the surface of the silicon wafer is covered with a corresponding BSG layer or PSG layer; A metal mask is covered on the BSG layer or PSG layer, the metal mask including a patterned masking area and a cutout area; Ultraviolet photoresist is ultrasonically atomized and sprayed onto the side of the metal mask away from the silicon wafer to form a photoresist layer; The photoresist layer is cured with ultraviolet light, the metal mask is removed, a protective film layer is formed at the position corresponding to the hollow area, and the BSG layer or PSG layer is exposed at the position corresponding to the shielded area. The exposed BSG or PSG layer is removed by etching, and then the protective film layer is removed to obtain a patterned silicon wafer.

2. The method for patterning the battery surface according to claim 1, characterized in that, The method further includes cleaning and preheating the silicon wafer before covering it with the metal mask. The preheating temperature is 45℃~55℃.

3. The method for patterning the battery surface according to claim 1, characterized in that, The ultraviolet photoresist is a negative photoresist; And / or, the viscosity of the ultraviolet photoresist is 50,000 mPa·s to 200,000 mPa·s; And / or, the solid content of the ultraviolet photoresist is 30%~50%.

4. The method for patterning the battery surface according to claim 1, characterized in that, The material of the metal mask includes stainless steel; And / or, the thickness of the metal mask is 0.1mm~0.2mm; And / or, the hollowed-out area includes straight through grooves, the line width of the straight through grooves is 200μm~400μm, the straightness error is <1μm, and the straight through grooves are arranged in parallel at equal intervals along the line width direction to form a pattern.

5. The method for patterning the battery surface according to claim 1, characterized in that, The ultrasonic atomization spraying and the ultraviolet curing are carried out under inert gas protection; And / or, the ultrasonic frequency of the ultrasonic atomization spraying is 50kHz~100kHz; And / or, the size of the microdroplets generated by the ultrasonic atomization spraying is 3μm~10μm; And / or, the spraying speed of the ultrasonic atomization spraying is 90mm / s to 300mm / s; And / or, the vertical distance between the ultrasonic atomizing spray nozzle and the surface of the silicon wafer is 15mm~25mm, and the atomization column divergence angle is 8°~15°.

6. The method for patterning the battery surface according to claim 1, characterized in that, The method also includes using a visual closed-loop correction system to control the offset of the ultrasonic atomization spraying to be ≤20μm; And / or, the line width of the photoresist layer formed by ultrasonic atomization spraying in the hollow area is ≤10μm, and the thickness uniformity difference is ≤15%.

7. The method for patterning the battery surface according to claim 1, characterized in that, The method further includes pre-baking the photoresist layer before UV curing, wherein the pre-baking temperature is 75℃~90℃ and the time is 5s~120s; And / or, the UV curing uses a single-wavelength UV light source, with the wavelength selected from 355nm to 395nm; And / or, the UV curing energy is 8000 mJ / cm². 2 ~12000mJ / cm 2 The curing time is 1s to 5s.

8. The method for patterning the surface of a battery according to claim 1, characterized in that, The etching process includes immersion in an acidic etching solution; the acidic etching solution includes a hydrofluoric acid solution with a concentration of 10% to 15%. And / or, the method for removing the protective film layer includes soaking in a mixed solution of a 1% to 2.5% alkaline solution and a 3% to 5% hydrogen peroxide solution; the alkaline solution includes a sodium hydroxide solution.

9. A patterned silicon wafer, characterized in that, Prepared by the method according to any one of claims 1-8.

10. A back-contact battery, characterized in that, A silicon wafer containing the patterned design as described in claim 9.