A perovskite solar module with a dynamic interface functional layer and its fabrication method, and a tandem photovoltaic module.

By introducing a photo-induced heterogeneous self-assembled monolayer into perovskite solar cells and using ultraviolet light to modulate the molecular configuration, dynamic filtering of ultraviolet light and reversible control of the electrode work function were achieved, solving the problems of ultraviolet aging and interface energy level mismatch, and improving the stability and performance of the module.

CN123124564APending Publication Date: 2026-11-17CNNC OPTOELECTRONICS TECH (SHANGHAI) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611619047.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing perovskite solar cells face problems such as Pb-I bond breaking, iodine ion migration, interface defect accumulation, and the disconnect between ultraviolet protection and energy level regulation under ultraviolet light irradiation, lacking a dynamic regulation mechanism.

Method used

A photoinduced isomeric self-assembled monolayer is set between the transparent electrode and the charge transport layer. Diarylethylene, azobenzene, or spiropyran derivatives are used as organic molecules. Molecular configuration changes are achieved through ultraviolet light irradiation, which dynamically filters ultraviolet light and modulates the electrode work function.

Benefits of technology

Dynamic filtering of ultraviolet light and reversible control of electrode work function were achieved, solving the problems of ultraviolet aging and interface energy level mismatch in perovskite solar modules, and improving the stability and performance of the modules.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124564A_ABST
    Figure CN123124564A_ABST
Patent Text Reader

Abstract

This invention discloses a perovskite solar module with a dynamic interface functional layer and its preparation method, as well as a tandem photovoltaic module, comprising: a transparent electrode, a photo-induced heterogeneous self-assembled monolayer, a first charge transport layer, a perovskite light absorption layer, a second charge transport layer, and a back electrode, sequentially stacked along the incident light direction; the photo-induced heterogeneous self-assembled monolayer includes organic molecules; the organic molecules are one or more of diarylethylene derivatives, azobenzene derivatives, and spiropyran derivatives; the organic molecules contain one or more of phosphonic acid groups, carboxyl groups, and silane groups; the organic molecules undergo a reversible molecular configuration transformation under ultraviolet light irradiation, accompanied by reversible changes in ultraviolet absorption characteristics and molecular dipole moments, enabling the photo-induced heterogeneous self-assembled monolayer to simultaneously achieve dynamic filtering of incident ultraviolet light and reversible control of the work function of the transparent electrode, thereby simultaneously solving the problems of ultraviolet aging and interface energy level mismatch in perovskite solar modules.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of perovskite photovoltaic technology, and in particular to a perovskite solar module with a dynamic interface functional layer, its preparation method, and a tandem photovoltaic module. Background Technology

[0002] Perovskite solar cells (PSCs) have become a research hotspot in third-generation photovoltaic technology due to their excellent photoelectric performance and low-cost solution processing potential. Typical device structures include two types: the nip structure and the pin structure. Both consist of a transparent conductive oxide (TCO) substrate, an electron transport layer, a perovskite light-absorbing layer, a hole transport layer, and a back electrode, in sequence. Self-assembled monolayer (SAM) interface manipulation is an important technological advancement in recent years. It modulates the electrode work function and optimizes energy level matching by forming oriented molecular dipoles on the TCO surface. SAM hole transport materials such as 2PACz and Me-4PACz have been widely used in pin devices.

[0003] Photoisomers are a class of functional molecules that undergo reversible configurational changes under irradiation with light of specific wavelengths. Typical examples include spiropyran, diarylethenes, and azobenzenes, and their isomerization process is accompanied by a significant change in molecular dipole moment. Previous studies have shown that depositing diarylethene molecules as photoisomerized molecule-as-aluminum (SAM) molecules on the surface of indium oxycarbonate (ITO) allows for reversible modulation of the ITO work function to approximately 60 meV under alternating UV / Vis light irradiation, confirming the feasibility of photoinduced dynamic modulation of electrode electronic properties using photoisomerized SAM.

[0004] However, existing perovskite modules still face the following problems: First, ultraviolet light (300 nm~400 nm) induces Pb-I bond breaking and iodine ion migration, causing continuous material degradation; second, ultraviolet-induced interface defect accumulation causes the electrode / transport layer energy levels to gradually deviate from the optimal state, while the work function regulation of existing SAMs is static and one-time, unable to dynamically compensate; third, ultraviolet protection and energy level regulation are disconnected, lacking a synergistic mechanism. Although some schemes introduce photoresponsive molecules on the hole transport layer surface to regulate wettability, these do not contact the transparent electrode, and dipole changes cannot act on the work function, thus the photo- and electrical regulation functions remain disconnected.

[0005] In summary, current technologies lack a scheme for simultaneously achieving dynamic ultraviolet light filtering and reversible control of the electrode work function by placing photo-induced heterogeneous SAMs between transparent electrodes and charge transport layers and using ultraviolet light as the same trigger signal. Therefore, it is necessary to develop a novel perovskite solar module and its fabrication method. Summary of the Invention

[0006] In view of this, this application provides a perovskite solar module with a dynamic interface functional layer and its preparation method, as well as a tandem photovoltaic module. The perovskite solar module includes a photo-induced heterogeneous self-assembled monolayer. The photo-induced heterogeneous self-assembled monolayer can undergo a reversible molecular configuration transformation under ultraviolet light irradiation, accompanied by reversible changes in ultraviolet absorption characteristics and molecular dipole moments, thereby simultaneously solving the problems of ultraviolet aging and interface energy level mismatch in perovskite solar modules.

[0007] This application provides a perovskite solar module with a dynamic interface functional layer, comprising: a transparent electrode, a photo-induced heterogeneous self-assembled monolayer, a first charge transport layer, a perovskite light absorption layer, a second charge transport layer, and a back electrode, which are sequentially stacked along the incident light direction. The photoinduced isomeric self-assembled monolayer includes organic molecules; The organic molecule is one or more of diarylethylene derivatives, azobenzene derivatives, and spiropyran derivatives; the organic molecule contains one or more of phosphonic acid groups, carboxyl groups, and silane groups.

[0008] In some specific implementations, the first charge transport layer is an electron transport layer, and the component is a formal structure.

[0009] In some specific implementations, the first charge transport layer is a hole transport layer, and the component is an inverse structure.

[0010] In some specific implementations, the thickness of the photoinduced heterogeneous self-assembled monolayer is 1 nm to 10 nm; The photo-induced heterogeneous self-assembled monolayer has a transmittance of 90% to 100% in the visible light band.

[0011] In some specific implementations, the diarylethene derivative is diarylethene phosphonate; The azobenzene derivative is carbazole-azobenzene-phosphonic acid; The spiropyran derivative is 1',3',3'-trimethyl-spiro[2H-1-benzopyran-2,2'-indoline]-6-methylphosphonic acid.

[0012] Furthermore, this application also provides a tandem photovoltaic module, including the perovskite solar module described above.

[0013] In some specific implementations, the tandem photovoltaic module is one or more of the following: perovskite / silicon two-terminal tandem module, perovskite / silicon four-terminal tandem module, all-perovskite tandem module, perovskite / organic tandem module, and perovskite / CIGS tandem module.

[0014] Furthermore, this application also provides a method for preparing the above-mentioned perovskite solar module, comprising the following steps: 1) Provide transparent electrodes; 2) A photo-induced isomeric self-assembled monolayer is formed on the surface of the transparent electrode; 3) A first charge transport layer, a perovskite light absorption layer, a second charge transport layer, and a back electrode are sequentially prepared on the surface of the photo-induced heterogeneous self-assembled monolayer.

[0015] In some specific implementations, the method for forming the photo-induced heterogeneous self-assembled monolayer is one or more of spin coating, vapor deposition, and solution immersion.

[0016] In some specific implementations, the fabrication temperature of the first charge transport layer is 100℃~150℃.

[0017] This application provides a perovskite solar module with a dynamic interface functional layer, comprising: a transparent electrode, a photo-induced heterogeneous self-assembled monolayer, a first charge transport layer, a perovskite light-absorbing layer, a second charge transport layer, and a back electrode, sequentially stacked along the incident light direction; the photo-induced heterogeneous self-assembled monolayer includes organic molecules; the organic molecules are one or more of diarylethylene derivatives, azobenzene derivatives, and spiropyran derivatives; the organic molecules contain one or more of phosphonic acid groups, carboxyl groups, and silane groups; the organic molecules undergo a reversible molecular configuration transformation under ultraviolet light irradiation, accompanied by reversible changes in ultraviolet absorption characteristics and molecular dipole moments, enabling the photo-induced heterogeneous self-assembled monolayer to simultaneously achieve dynamic filtering of incident ultraviolet light and reversible control of the work function of the transparent electrode, thereby simultaneously solving the problems of ultraviolet aging and interface energy level mismatch in perovskite solar modules; the perovskite solar module provided in this application is suitable for single-junction modules and tandem photovoltaic modules. Attached Figure Description

[0018] Figure 1 This is a schematic diagram of the structure of the perovskite solar module of this application (a is a schematic diagram of the formal device structure, and b is a schematic diagram of the inverse device structure). Figure 2 This is a schematic diagram illustrating the working mechanism of the photoinduced isomeric self-assembly of monolayers in this application; Figure 3 This is a schematic diagram of the preparation process of the photo-induced heterogeneous self-assembled monolayer of this application. Detailed Implementation

[0019] It should be understood that the expression “one or more of…” individually includes each of the objects described after the expression, as well as various different combinations of two or more of the described objects, unless otherwise understood from the context and usage. The expression “and / or” combined with three or more described objects should be understood to have the same meaning, unless otherwise understood from the context.

[0020] The terms “including,” “having,” or “containing,” including the use of their grammatical synonyms, should generally be understood as open-ended and non-restrictive, for example, not excluding other unstated elements or steps, unless otherwise specifically stated or understood from the context.

[0021] It should be understood that the order of steps or the sequence of actions is not important as long as this application remains operational. Furthermore, two or more steps or actions can be performed simultaneously.

[0022] This application provides a perovskite solar module with a dynamic interface functional layer, comprising: a transparent electrode, a photo-induced heterogeneous self-assembled monolayer, a first charge transport layer, a perovskite light-absorbing layer, a second charge transport layer, and a back electrode, sequentially stacked along the light incident direction; the photo-induced heterogeneous self-assembled monolayer includes organic molecules; the organic molecules are one or more of diarylethylene derivatives, azobenzene derivatives, and spiropyran derivatives; the organic molecules contain one or more of phosphonic acid groups, carboxyl groups, and silane groups.

[0023] Figure 1 This is a schematic diagram of the perovskite solar module structure of this application; in some specific implementations, when the first charge transport layer is an electron transport layer, the module is a formal device (nip), and its structure is as follows. Figure 1 As shown in a, Figure 1 In the diagram, 'a' represents a schematic of the formal device structure. The component, along the light-incident direction, sequentially includes: a transparent electrode, a dynamic interface functional layer (photoinduced heterogeneous self-assembled monolayer), an electron transport layer, a perovskite light-absorbing layer, a hole transport layer, a back electrode, and an encapsulating film and a backplate glass. In some specific implementations, when the first charge transport layer is a hole transport layer, the component is an inverted device (pin), and its structure is as follows: Figure 1 As shown in b, Figure 1 b in the diagram is a schematic diagram of the inverted device structure. The components, along the light incident direction, include, in sequence: a glass substrate, a transparent electrode, a dynamic interface functional layer (photoinduced heterogeneous self-assembled monolayer), a hole transport layer, a perovskite light absorption layer, an electron transport layer, a back electrode, and an encapsulating film and a backplate glass.

[0024] The perovskite solar module provided in this application includes a transparent electrode. This transparent electrode serves as a substrate, acting as a window for incident light to enter the device, a collection and extraction end for photogenerated charges, and an anchoring substrate for photo-induced heterogeneous self-assembly of monolayers, as well as the object of its work function regulation. In some specific implementations, the transparent electrode is one or more of FTO and ITO conductive glasses. In some embodiments of this application, the transparent electrode is either FTO or ITO conductive glass. The change in the work function of the transparent electrode before and after ultraviolet irradiation, ΔΦ, is 0.05 eV to 0.5 eV, preferably 0.05 eV to 0.30 eV, and more preferably 0.10 eV to 0.25 eV. The FTO conductive glass described in this application refers to conductive glass made by depositing a fluorine-doped tin oxide transparent conductive film on the glass surface; the ITO conductive glass refers to conductive glass made by depositing a tin-doped indium oxide transparent conductive film on the glass surface.

[0025] The perovskite solar module provided in this application also includes a photo-induced heterogeneous self-assembled monolayer (i.e., a dynamic interface functional layer). This photo-induced heterogeneous self-assembled monolayer is disposed between the transparent electrode and the first charge transport layer. On one hand, it acts as a molecular film anchored to the surface of the transparent electrode, undergoing a reversible molecular configuration transformation upon ultraviolet light irradiation. On the other hand, the reversible change in its molecular dipole moment directly affects the surface energy level of the transparent electrode. The photo-induced heterogeneous self-assembled monolayer includes organic molecules. In some specific implementations, the organic molecules are one or more of diarylethylene derivatives, azobenzene derivatives, and spiropyran derivatives, preferably diarylethylene phosphonate, carbazole-azobenzene-phosphonic acid, or 1',3',3'-trimethyl-spiropyran[2H- 1-Benzopyran-2,2'-indoline]-6-methylphosphonic acid; the organic molecule contains one or more of phosphonic acid group, carboxyl group and silane group, preferably phosphonic acid group, carboxyl group or silane group. In some embodiments of this application, the organic molecule contains phosphonic acid group; the above-mentioned groups contained in the organic molecule provided in this application are anchoring groups, which can chemically bond with the transparent electrode surface, so that the organic molecule is firmly anchored to the transparent electrode surface, preventing the molecule from migrating and aggregating during subsequent processes and long-term service, and making the organic molecule oriented and densely arranged on the electrode surface, thereby forming a structurally stable photoinduced isomeric self-assembled monolayer, ensuring that the ultraviolet absorption characteristics and reversible changes of molecular dipole moment of the monolayer can be cyclically carried out over a long period of time. In some specific implementations, the thickness of the photo-induced heterogeneous self-assembled monolayer is 1 nm to 10 nm, preferably 2 nm to 3 nm; the transmittance of the photo-induced heterogeneous self-assembled monolayer in the visible light band is 90% to 100%, preferably 93% to 98%, more preferably 94% to 97%; in some specific implementations, the photo-induced heterogeneous self-assembled monolayer contains organic molecules that simultaneously possess hole transport capability and photo-induced heterogeneity.

[0026] Figure 2 This is a schematic diagram illustrating the working mechanism of the photoinduced isomeric self-assembly of a bifunctional monolayer in this application; as shown below. Figure 2 As shown, under dark or visible light irradiation, the organic molecules are in the first configuration (the diarylethylene derivative is a closed ring, and the azobenzene derivative is a trans structure). At this time, the monolayer absorbs ultraviolet light weakly, and the work function of the transparent electrode is in its initial state. When ultraviolet light irradiates from the incident light side, the organic molecules undergo a reversible configurational transition to the second configuration (the diarylethylene derivative is an open ring, and the azobenzene derivative is a cis structure). The second configuration has a larger ultraviolet light absorption coefficient than the first configuration, especially for incident ultraviolet light, particularly in the 300 nm to 400 nm range. Dynamic filtering in the nm band weakens the ultraviolet light flux reaching the perovskite light absorption layer. Simultaneously, the second configuration has a different molecular dipole moment compared to the first configuration. Since organic molecules are oriented and densely bonded to the transparent electrode surface through anchoring groups, the change in molecular dipole moment directly alters the interfacial dipole layer on the transparent electrode surface, causing a reversible shift in the vacuum energy level of the transparent electrode, thus achieving reversible control of the work function of the transparent electrode. After the ultraviolet light is removed, the organic molecules recover to the first configuration through thermal recovery, and the ultraviolet absorption characteristics and work function synchronously return to their initial state, thus repeating the cycle.

[0027] The perovskite solar module provided in this application further includes a first charge transport layer, which is disposed between the photo-induced heterogeneous self-assembled monolayer and the perovskite light-absorbing layer. This first charge transport layer selectively extracts and transports one type of charge carrier from the perovskite light-absorbing layer while blocking the passage of another type of charge carrier. In some specific implementations, the first charge transport layer is an electron transport layer or a hole transport layer, wherein the material of the electron transport layer is SnO2, TiO2, ZnO, or PC. 61 One or more of BM; the thickness of the electron transport layer is 10 nm to 50 nm. Wherein, when the electron transport layer is SnO2, the thickness is preferably 10 nm to 20 nm; when the electron transport layer is PC... 61 In BM, the thickness is preferably 20 nm to 40 nm; the material of the hole transport layer is NiO. x One or more of Spiro-OMeTAD and PTAA, preferably NiO x Spiro-OMeTAD or PTAA; the thickness of the hole transport layer is 7 nm to 200 nm; wherein, when the hole transport layer is NiO xWhen the hole transport layer is PTAA, the thickness is preferably 7 nm to 15 nm; when the hole transport layer is Spiro-OMeTAD, the thickness is preferably 50 nm to 150 nm.

[0028] The perovskite solar module provided in this application also includes a perovskite light-absorbing layer, which is the core functional layer of the module, used to absorb sunlight transmitted through the layers on the light-incident side and generate photogenerated carriers; in some specific implementations, the material of the perovskite light-absorbing layer is Cs. x FA 1-x PbI3, FA 1-x MA x PbI3, Cs x FA 1-x Pb(I 1-y Br y One or more of C3 and MAPbI3, preferably Cs 0.05 FA 0.95 PbI3, FA 0.85 MA 0.15 PbI3 or Cs 0.05 FA 0.85 MA 0.10 Pb(I 0.95 Br 0.05 3; The thickness of the perovskite light-absorbing layer is 300 nm to 600 nm, preferably 400 nm to 600 nm, and can be 400 nm, 450 nm, 500 nm, 550 nm or 600 nm. In some embodiments of this application, the thickness of the perovskite light-absorbing layer is 500 nm. When the perovskite solar module is a tandem module, the perovskite light-absorbing layer is a wide bandgap perovskite (bandgap 1.60 eV to 1.75 eV) with a thickness of 150 nm to 350 nm, preferably 200 nm to 300 nm.

[0029] The perovskite solar module provided in this application further includes a second charge transport layer, which is disposed between the perovskite light-absorbing layer and the back electrode. This second charge transport layer is used to extract and transport a different type of charge carrier opposite to that of the first charge transport layer, cooperating with the first charge transport layer to complete the separation and directional transport of photogenerated charge carriers. In some specific implementations, when the first charge transport layer is an electron transport layer, the second charge transport layer is a hole transport layer; when the first charge transport layer is a hole transport layer, the second charge transport layer is an electron transport layer. The electron transport layer is made of SnO2, TiO2, and C. 60One or more of the following, preferably SnO2, TiO2, or ZnO, are used. In some embodiments of this application, the electron transport layer is made of SnO2 and C. 60 The hole transport layer is made of NiO. x One or more of Spiro-OMeTAD and PTAA, preferably NiO x In some embodiments of this application, the hole transport layer is made of Spiro-OMeTAD or NiO. x .

[0030] The perovskite solar module provided in this application also includes a back electrode, which, together with a transparent electrode, constitutes two current leads of the module for collecting charge carriers transferred from the second charge transport layer and leading them to an external circuit. In some specific implementations, the back electrode is a metal electrode or a transparent conductive oxide. The material of the back electrode is one or more of gold, silver, copper, and ITO thin film, preferably silver, copper, or ITO thin film. A diffusion barrier layer is disposed between the back electrode and the second charge transport layer, and the diffusion barrier layer is made of MoO. x The electrode is made of BCP, chromium, titanium, or molybdenum, with a thickness of 3 nm to 10 nm. The thickness of the back electrode is 50 nm to 150 nm, preferably 60 nm to 100 nm, and can be 60 nm, 70 nm, 80 nm, 90 nm, or 100 nm. In some embodiments of this application, the thickness of the back electrode is 80 nm.

[0031] Furthermore, this application also provides a tandem photovoltaic module, including the aforementioned perovskite solar module; the perovskite solar module serves as the perovskite top cell of the tandem photovoltaic module, and the photo-induced heterogeneous self-assembled monolayer is located on the light-incident side of the perovskite top cell, so that the incident ultraviolet light is dynamically filtered before entering the perovskite light-absorbing layer of the top cell and the bottom cell, thereby simultaneously providing ultraviolet protection for both the top and bottom cells; and the photo-induced heterogeneous self-assembled monolayer is a single-layer thickness, does not introduce additional refractive index mismatch interfaces, and does not affect the optical design of the tandem photovoltaic module. In some specific implementations, the tandem photovoltaic module is one or more of the following: a perovskite / silicon two-terminal tandem module, a perovskite / silicon four-terminal tandem module, an all-perovskite tandem module, a perovskite / organic tandem module, and a perovskite / CIGS tandem module, preferably a perovskite / silicon two-terminal tandem module or a perovskite / silicon four-terminal tandem module, more preferably a perovskite / silicon two-terminal tandem module.

[0032] Furthermore, this application also provides a method for preparing the above-mentioned perovskite solar module, comprising the following steps: 1) Provide transparent electrodes; 2) A photo-induced isomeric self-assembled monolayer is formed on the surface of the transparent electrode; 3) A first charge transport layer, a perovskite light absorption layer, a second charge transport layer, and a back electrode are sequentially prepared on the surface of the photo-induced heterogeneous self-assembled monolayer.

[0033] This application first provides a transparent electrode, the material of which is as described above and will not be repeated here. In some specific implementations, the transparent electrode can be pre-treated before use, specifically including the following steps: A pretreated transparent electrode is obtained by washing, drying, and treating with ultraviolet-ozone. In some specific implementations, the washing includes washing sequentially in a detergent aqueous solution, deionized water, acetone, and isopropanol. The detergent is a neutral detergent or a special cleaning solution for conductive glass. The washing is ultrasonic cleaning. The washing time for the detergent aqueous solution, deionized water, acetone, and isopropanol is 10 min to 30 min, preferably 10 min to 20 min, but can be 10 min, 15 min, or 20 min. In some embodiments of this application, the washing time is 15 min. The drying is preferably done with nitrogen. The ultraviolet-ozone treatment time is 10 min to 30 min, preferably 10 min to 20 min, but can be 10 min, 15 min, or 20 min. In some embodiments of this application, the ultraviolet-ozone treatment time is 15 min.

[0034] After obtaining the pretreated transparent electrode, this application forms a photo-induced isomeric self-assembled monolayer on its surface; in some specific implementations, the formation method is one or more of spin coating, vapor deposition, and solution immersion, preferably solution immersion; specifically, it includes the following steps: The pretreated transparent electrode is immersed in an organic molecular solution, then rinsed with the solvent of the organic molecular solution and dried with nitrogen gas, thus forming a photoinduced isomeric self-assembled monolayer on the surface of the transparent electrode. The types of organic molecules are as described above and will not be repeated here. In some specific implementations, the concentration of the organic molecular solution is 0.5 mM to 1.5 mM, preferably 0.5 mM to 1.0 mM, and can be 0.5 mM, 0.6 mM, 0.7 mM, 0.8 mM, 0.9 mM, or 1.0 mM. In some embodiments of this application, the concentration of the organic molecular solution is 0.5 mM or 1.0 mM. The solvent of the organic molecular solution includes, but is not limited to, anhydrous THF solution and anhydrous ethanol, preferably anhydrous THF solution or anhydrous ethanol. The immersion conditions are room temperature and protection from light. The immersion time is 1 h to 48 h, preferably 1 h to 10 h, and can be 1 h, 2 h, 3 h, 4 h, 5 h, 6 h, 7 h, 8 h, 9 h, etc. The soaking time is 2 hours or 10 hours. In some embodiments of this application, the soaking time is 2 hours. The number of solvent rinses is 1 to 5 times, preferably 2 to 4 times, and can be 2, 3 or 4 times. In some embodiments of this application, the number of solvent rinses is 3 times.

[0035] Figure 3 This is a schematic diagram of a typical preparation process for the photo-induced isomeric self-assembled monolayer of this application; such as Figure 3 As shown, the preparation process of the photo-induced heterogeneous self-assembled monolayer is as follows: First, the transparent electrode is ultrasonically cleaned sequentially with detergent aqueous solution, deionized water, acetone, and isopropanol, dried with nitrogen, and then treated with ultraviolet-ozone to obtain a transparent electrode with a clean and hydroxylated surface; then, the photo-induced heterogeneous organic molecules are dissolved in the corresponding solvent to prepare an organic molecule solution; next, the pretreated transparent electrode is immersed in the organic molecule solution and soaked at room temperature in the dark. The organic molecules form chemical bonds with the hydroxyl groups on the electrode surface through a condensation reaction, and are oriented and densely arranged on the electrode surface to self-assemble into a monolayer; finally, the electrode is taken out of the solution, rinsed several times with the corresponding solvent to remove physically adsorbed molecules, and dried with nitrogen to obtain a transparent electrode with a photo-induced heterogeneous self-assembled monolayer formed on the surface.

[0036] After obtaining the transparent electrode with the photo-induced heterogeneous self-assembled monolayer, this application prepares a first charge transport layer on its surface; in some specific implementations, the preparation method is one or more of spin coating, blade coating, and spray coating, preferably spin coating; specifically, it includes the following steps: A precursor solution is spin-coated onto the surface of the photo-induced heterogeneous self-assembled monolayer, and then annealed to form a first charge transport layer. The type, material, and thickness of the first charge transport layer are as described above and will not be repeated here. In some specific implementations, when the component is a formal device, i.e., the first charge transport layer is an electron transport layer, the concentration of the precursor solution is 2 wt% to 3 wt%, preferably 2 wt% to 2.5 wt%, and can be 2 wt%, 2.2 wt%, 2.5 wt%, or 3 wt%. In some embodiments of this application, the concentration of the precursor solution is 2.5 wt%. When the component is a trans device, i.e., the first charge transport layer is a hole transport layer, the concentration of the precursor solution is 5 mg / mL to 15 mg / mL, preferably 8 mg / mL to 12 mg / mL. In some embodiments of this application, the concentration of the precursor solution is 10 mg / mL. The spin-coating speed is 1000 rpm to 5000 rpm, preferably 2000 rpm to 4000 rpm. The rotation speed (rpm) can be 2000 rpm, 2500 rpm, 3000 rpm, 3500 rpm, or 4000 rpm. In some embodiments of this application, the spin coating speed is 3000 rpm. The spin coating time is 20 s to 60 s, preferably 20 s to 40 s, and can be 20 s, 25 s, 30 s, 35 s, or 40 s. In some embodiments of this application, the spin coating time is 30 s. The annealing temperature is 100°C to 150°C, preferably 120°C to 150°C, and can be 100°C, 110°C, 120°C, 130°C, 140°C, or 150°C. In some embodiments of this application, the annealing temperature is 100°C or 120°C. The annealing time is 10 min to 60 min, preferably 20 min to 40 min, and can be 20 min, 25 min, 30 min, 40 min, 50 min, 60 min, 70 min, 80 min, 90 min, 1 ... In some embodiments of this application, the annealing time is 20 min or 30 min, or 35 min or 40 min. By controlling the annealing temperature, this application can prevent the organic molecules in the photo-induced isomerization self-assembled monolayer from undergoing thermal decomposition, desorption, or aggregation, thereby maintaining its reversible isomerization capability and ensuring that the dynamic ultraviolet filtering and reversible work function regulation functions of the dynamic interface functional layer are realized.

[0037] After obtaining the transparent electrode with the first charge transport layer, this application prepares a perovskite light absorption layer on its surface; in some specific implementations, the preparation method is an anti-solvent method or a spin-coating method, preferably an anti-solvent method; specifically, it includes the following steps: A perovskite precursor solution is spin-coated onto the surface of the first charge transport layer. An antisolvent is added dropwise during the spin-coating process, followed by annealing to form the perovskite light-absorbing layer. The material of the perovskite light-absorbing layer is as described above and will not be repeated here. In some specific implementations, the concentration of the perovskite precursor solution is 1.0 M to 1.6 M, preferably 1.2 M to 1.5 M, and can be 1.2 M, 1.3 M, 1.4 M, or 1.5 M. In some embodiments of this application, the concentration of the perovskite precursor solution is 1.4 M. This application does not specifically limit the type of solvent for the perovskite precursor solution, but a mixed solution of N,N-dimethylformamide (DMF) and dimethyl sulfoxide (DMSO) is preferred. The volume ratio of DMF to DMSO is 4:1. The antisolvent includes, but is not limited to, chlorobenzene. The amount of the antisolvent is 150 μL to 200 μL, preferably 150 μL. The amount of antisolvent used is 150 μL in some embodiments of this application, ranging from μL to 180 μL; the annealing temperature is 100°C to 150°C, preferably 120°C to 150°C, and can be 100°C, 110°C, 120°C, 130°C, 140°C, or 150°C. In some embodiments of this application, the annealing temperature is 100°C or 150°C; the annealing time is 5 min to 30 min, preferably 8 min to 15 min, and can be 8 min, 10 min, 12 min, or 15 min. In some embodiments of this application, the annealing time is 10 min.

[0038] After obtaining the substrate with the perovskite light-absorbing layer, this application prepares a second charge transport layer on its surface; in some specific implementations, when the component is a formal device, i.e., the second charge transport layer is a hole transport layer, the specific preparation steps are as follows: A second charge transport layer solution is spin-coated onto the surface of the perovskite light-absorbing layer to form the second charge transport layer. The type and material selection of the second charge transport layer are as described above and will not be repeated here. The concentration of the second charge transport layer solution is 50 mM to 100 mM, preferably 60 mM to 80 mM, and can be 60 mM, 65 mM, 72.3 mM, 75 mM or 80 mM. In some embodiments of this application, the concentration of the second charge transport layer solution is 72.3 mM. This application does not have specific limitations on the solvent of the second charge transport layer solution, but it is preferably a solution of acetonitrile solution of lithium bis(trifluoromethanesulfonyl)imide (Li-TFSI) and 4-tert-butylpyridine (tBP). The amount of acetonitrile is preferably 17.5 μL and the amount of tBP is preferably 28.8 μL.

[0039] In some specific implementations, when the component is an inverted device, i.e., the second charge transport layer is an electron transport layer, it is preferable to prepare the second charge transport layer by thermal evaporation. The specific preparation steps are as follows: The substrate with the prepared perovskite light-absorbing layer was transferred to a vacuum thermal evaporation system, and after evacuation, the C2000 was turned on. 60 Evaporation source C 60 Then switch the BCP evaporation source to deposit BCP, obtaining the second charge transport layer; in some specific implementations, the pressure after vacuuming is 1×10⁻⁶. -4 Pa ~ 9×10 -4 Pa, preferably 3×10 -4 Pa ~ 8×10 -4 In some embodiments of this application, the pressure after vacuuming is 5 × 10 Pa. -4 Pa; the C 60 The evaporation rate is 0.1 Å / s to 0.5 Å / s, preferably 0.1 Å / s to 0.3 Å / s. In some embodiments of this application, the C... 60 The evaporation rate is 0.2 Å / s; the C 60 The thickness of the BCP is preferably 25 nm; the evaporation rate of the BCP is 0.1 Å / s to 0.4 Å / s, preferably 0.1 Å / s to 0.2 Å / s, and in some embodiments of this application, the evaporation rate of the BCP is 0.15 Å / s; the thickness of the BCP is preferably 5 nm.

[0040] After obtaining the substrate with the second charge transport layer, this application fabricates a back electrode on its surface; in some specific implementations, the fabrication method is thermal evaporation or magnetron sputtering, preferably thermal evaporation. When the fabrication method is thermal evaporation, specifically, it includes the following steps: The substrate device with the back electrode is prepared in the same vacuum cavity as the second charge transport layer. The evaporation source baffle of the back electrode material is opened for evaporation deposition. After evaporation deposition, the baffle is closed, the substrate is cooled, and nitrogen gas is introduced to obtain the substrate device. In some specific implementations, the back electrode material can be one of silver, gold, copper, and aluminum, preferably copper or silver. When the back electrode material is copper, the evaporation rate is preferably 0.5 Å / s, and the evaporation thickness is preferably 80 nm. When the back electrode material is silver, the evaporation rate is preferably 0.1 Å / s, and the evaporation thickness is preferably 80 nm.

[0041] In some specific implementations, it should be noted that in the 2T stacked module structure, the tunneling composite layer is usually composed of an ITO thin film. This ITO thin film also serves as the transparent back electrode of the perovskite top cell and acts as an electrical series connection between the top and bottom cells. In this case, the preferred method for preparing the tunneling composite layer is magnetron sputtering, specifically including the following steps: A magnetron sputtering deposition is performed on the substrate surface where the second charge transport layer is formed under an inert atmosphere to obtain a stacked intermediate structure with an ITO thin film deposited on the surface. The ITO thin film serves simultaneously as the transparent back electrode of the perovskite top cell and the tunneling composite layer of the 2T stacked assembly. In some specific implementations, the back electrode is made of an ITO thin film; the thickness of the back electrode is 20 nm to 60 nm, preferably 20 nm to 40 nm, and in some embodiments of this application, the thickness of the back electrode is 30 nm; the inert atmosphere is an argon atmosphere with an operating pressure of 0.3 Pa; and the power density of the magnetron sputtering deposition is 1 W / cm³. 2 ~5 W / cm 2 Preferably 1 W / cm 2 ~3 W / cm 2 In some embodiments of this application, the power density of the magnetron sputtering deposition is 2 W / cm². 2 The deposition rate of the magnetron sputtering deposition is 0.1 Å / s to 0.8 Å / s, preferably 0.1 Å / s to 0.5 Å / s. In some embodiments of this application, the deposition rate of the magnetron sputtering deposition is 0.3 Å / s.

[0042] In some specific implementations, after obtaining the perovskite solar module, this application can further perform lamination and encapsulation processing; specifically, it includes the following steps: The perovskite solar module is laminated and encapsulated with an encapsulating film and a backsheet glass. In some specific implementations, the lamination and encapsulation are performed in a laminator. The lamination temperature is 140℃~160℃, preferably 150℃. The lamination time is 10 min~20 min, preferably 15 min.

[0043] This application provides a perovskite solar module with a dynamic interface functional layer, comprising: a transparent electrode, a photo-induced heterogeneous self-assembled monolayer, a first charge transport layer, a perovskite light-absorbing layer, a second charge transport layer, and a back electrode, sequentially stacked along the incident light direction; the photo-induced heterogeneous self-assembled monolayer includes organic molecules; the organic molecules are one or more of diarylethylene derivatives, azobenzene derivatives, and spiropyran derivatives; the organic molecules contain one or more of phosphonic acid groups, carboxyl groups, and silane groups; the organic molecules undergo a reversible molecular configuration transformation under ultraviolet light irradiation, accompanied by reversible changes in ultraviolet absorption characteristics and molecular dipole moments, enabling the photo-induced heterogeneous self-assembled monolayer to simultaneously achieve dynamic filtering of incident ultraviolet light and reversible control of the work function of the transparent electrode, thereby simultaneously solving the problems of ultraviolet aging and interface energy level mismatch in perovskite solar modules; the perovskite solar module provided in this application is suitable for single-junction modules and tandem photovoltaic modules.

[0044] The present application is further illustrated below with reference to embodiments. The scope of protection of the present application is not limited to the following embodiments.

[0045] Example 1

[0046] 1) The ITO conductive glass was ultrasonically cleaned in detergent aqueous solution, deionized water, acetone and isopropanol for 15 min each, dried with nitrogen, and then treated with ultraviolet-ozone for 15 min.

[0047] 2) Immerse the cleaned ITO glass in an anhydrous THF solution containing 1 mM diarylethene phosphonate (PA-DAE) for 2 hours at room temperature in the dark; after removal, rinse 3 times with anhydrous THF and dry with nitrogen to obtain an ITO substrate modified with PA-DAE SAM; the thickness of the SAM is about 2 nm to 3 nm.

[0048] 3) On the PA-DAE SAM surface, a SnO2 nanoparticle dispersion with a concentration of 2.5 wt% was deposited by spin coating at a speed of 3000 rpm for 30 s, followed by annealing at 120°C for 30 min to obtain a SnO2 electron transport layer; the thickness of the SnO2 electron transport layer was 30 nm.

[0049] 4) A perovskite precursor solution is deposited on the SnO2 surface using a one-step antisolvent method, wherein the solute in the perovskite precursor solution is FA. 0.85 MA 0.15PbI3 at a concentration of 1.4 M was used in a mixed solvent of DMF and DMSO (volume ratio 4:1). During spin coating, 150 μL of chlorobenzene was added dropwise as an antisolvent between 8 and 10 seconds after the start of spin coating (or 5 to 8 seconds before the end of spin coating), and the addition was completed within 1 to 2 seconds. The film was then annealed at 150°C for 10 minutes to obtain a perovskite film with a thickness of approximately 500 nm.

[0050] 5) Spin-coating a Spiro-OMeTAD solution onto the perovskite surface. The Spiro-OMeTAD solution was prepared by dissolving 72.3 mg Spiro-OMeTAD in 1 mL of chlorobenzene, adding 17.5 μL of acetonitrile solution of Li-TFSI (concentration 520 mg / mL) and 28.8 μL of tBP. The spin-coating speed was 4000 rpm and the spin-coating time was 30 s, thus forming a Spiro-OMeTAD hole transport layer.

[0051] 6) Transfer the prepared Spiro-OMeTAD hole transport layer substrate to a vacuum thermal evaporation coating system, using Ag wire with a purity ≥99.99% as the evaporation source, and load it into a molybdenum boat. After closing the cavity, evacuate to 5×10⁻⁶. -4 Pa. After the vacuum level stabilizes, the current in the evaporation boat is slowly increased to pre-melt Ag and wet the molybdenum boat. The baffle is closed during the pre-melting stage. After the baffle is opened, Ag is deposited at a rate of 0.1 Å / s, and the deposition rate is monitored in real time using a quartz crystal film thickness monitor. When the film thickness reaches 80 nm, the baffle is closed and heating is stopped. After the chamber cools naturally to room temperature, nitrogen is introduced to atmospheric pressure, and the device is removed.

[0052] 7) The above-mentioned device, EVA film, and backing glass are laminated and encapsulated in a laminator at a lamination temperature of 150°C for 15 minutes.

[0053] Example 2

[0054] 1) The FTO conductive glass was ultrasonically cleaned in detergent aqueous solution, deionized water, acetone and isopropanol for 15 min each, dried with nitrogen, and then treated with ultraviolet-ozone for 15 min.

[0055] 2) Immerse the cleaned FTO glass in an anhydrous THF solution containing 1 mM diarylethene phosphonate (PA-DAE) for 2 h at room temperature in the dark; after removal, rinse 3 times with anhydrous THF and dry with nitrogen to obtain a PA-DAE SAM-modified FTO substrate (SAM thickness approximately 2 nm to 3 nm).

[0056] 3) Spin-coating NiO onto the PA-DAE SAM surface xThe nanoparticle dispersion (10 mg / mL) was spin-coated at 3000 rpm for 30 s, followed by annealing at 100°C for 20 min to obtain NiO. x Hole transport layer, the NiO x The hole transport layer is 15 nm thick.

[0057] 4) A perovskite precursor solution with a concentration of 1.4 M was deposited on the surface of the nickel oxide layer using an antisolvent method. The solute in the perovskite precursor solution was FA. 0.85 MA 0.15 PbI3 at a concentration of 1.4 M was prepared in a mixed solvent of DMF and DMSO (volume ratio 4:1). During spin coating, 150 μL of chlorobenzene was added dropwise as an anti-solvent between 8 and 10 seconds after the start of spin coating (or 5 to 8 seconds before the end of spin coating), and the addition was completed within 1 to 2 seconds. Subsequently, the film was annealed at 150°C for 10 minutes to obtain a perovskite film with a thickness of approximately 500 nm.

[0058] 5) Transfer the prepared perovskite layer substrate to a vacuum thermal evaporation system and evacuate to a vacuum level of 5 × 10⁻⁶. -4 Pa. Open C 60 An evaporation source was used to deposit 25 nm of C at a rate of 0.2 Å / s. 60 Without breaking the vacuum, switch to the BCP evaporation source and deposit 5 nm of BCP at a rate of 0.15 Å / s.

[0059] 6) Continue to deposit 80 nm Cu as the back electrode in the vacuum chamber at a rate of 0.5 Å / s. After the deposition is complete, wait for the chamber to cool to room temperature, then fill it with nitrogen and remove the device.

[0060] 7) The above-mentioned device, EVA film, and backing glass are laminated and encapsulated in a laminator at a lamination temperature of 150°C for 15 minutes.

[0061] Example 3

[0062] 1) The FTO conductive glass was ultrasonically cleaned in detergent aqueous solution, deionized water, acetone and isopropanol for 15 min each, dried with nitrogen, and then treated with ultraviolet-ozone for 15 min.

[0063] 2) The cleaned FTO glass was immersed in an anhydrous ethanol solution containing 0.5 mM carbazole-azobenzene-phosphonic acid (Cz-Azo-PA) for 2 h at room temperature in the dark; after removal, it was rinsed 3 times with anhydrous ethanol and dried with nitrogen to obtain an FTO substrate modified with Cz-Azo-PA SAM (thickness of about 2 nm to 3 nm); the Cz-Azo-PA SAM serves as both a hole transport layer and a dynamic interface functional layer, without the need for additional hole transport layer deposition.

[0064] 3) A perovskite precursor solution was deposited on the Cz-Azo-PA SAM surface using an antisolvent method, wherein the solute in the perovskite precursor solution was FA. 0.85 MA 0.15 PbI3 at a concentration of 1.4 M was used in a mixed solvent of DMF and DMSO (volume ratio 4:1). During spin coating, 150 μL of chlorobenzene was added dropwise as an antisolvent, followed by annealing at 150°C for 10 min to obtain a perovskite film with a thickness of approximately 500 nm.

[0065] 4) Transfer the prepared perovskite layer substrate to a vacuum thermal evaporation system and evacuate to a vacuum level of 5 × 10⁻⁶. -4 Pa. Open C 60 An evaporation source baffle was used to deposit C at a rate of 0.2 Å / s. 60 When the film thickness reaches 25 nm, the baffle is turned off. Without disrupting the vacuum, the system is switched to the BCP evaporation source, and BCP is deposited at a rate of 0.15 Å / s. When the film thickness reaches 5 nm, the baffle is turned off.

[0066] 5) Continue in the same vacuum chamber (without breaking the vacuum), open the Cu evaporation source baffle, and evaporate Cu at a rate of 0.5 Å / s. When the film thickness reaches 80 nm, close the baffle. After the chamber cools to room temperature, fill it with nitrogen and remove the device.

[0067] 6) The above-mentioned device, EVA film, and backing glass are laminated and encapsulated in a laminator at a lamination temperature of 150°C for 15 minutes.

[0068] Example 4

[0069] 1) The ITO conductive glass was ultrasonically cleaned in detergent aqueous solution, deionized water, acetone and isopropanol for 15 min each, dried with nitrogen, and then treated with ultraviolet-ozone for 15 min.

[0070] 2) Immerse the cleaned ITO glass in an anhydrous THF solution containing 1 mM diarylethene phosphonate (PA-DAE) for 2 h at room temperature in the dark; after removal, rinse 3 times with anhydrous THF and dry with nitrogen to obtain PA-DAE SAM modified ITO substrate (SAM thickness about 2 nm~3 nm).

[0071] 3) On the PA-DAE SAM surface, a SnO2 nanoparticle dispersion with a concentration of 2.5 wt% was deposited by spin coating at a speed of 3000 rpm for 30 s, followed by annealing at 120°C for 30 min to obtain a SnO2 electron transport layer with a thickness of approximately 30 nm.

[0072] 4) A wide-bandgap perovskite precursor solution was deposited on the SnO2 surface using an antisolvent method. The precursor solute was CsO. 05 FA0. 85 MA0. 10 Pb(I0). 95 Br0. 05 The perovskite film (with a band gap of approximately 1.65 eV) was prepared at a concentration of 1.4 M using a mixed solvent of DMF and DMSO (volume ratio 4:1). The spin-coating procedure was as follows: spin-coating at 1000 rpm for 5 s, followed by spin-coating at 4000 rpm for 30 s. Twenty seconds after the start of the second spin-coating step, 150 μL of chlorobenzene was added dropwise as an anti-solvent. After spin-coating, the film was annealed at 100°C for 10 min to obtain a perovskite film (approximately 250 nm thick).

[0073] 5) A Spiro-OMeTAD solution was spin-coated onto the perovskite surface. The solution was prepared by dissolving 72.3 mg Spiro-OMeTAD in 1 mL of chlorobenzene, adding 17.5 μL of acetonitrile solution of Li-TFSI (concentration 520 mg / mL) and 28.8 μL of tBP. The spin-coating speed was 4000 rpm and the spin-coating time was 30 s to obtain a Spiro-OMeTAD hole transport layer with a thickness of 130 nm.

[0074] 6) A 30 nm ITO thin film was deposited on the Spiro-OMeTAD surface by magnetron sputtering. This ITO film serves as both the transparent back electrode and the tunneling composite layer for the perovskite top cell. The sputtering conditions were: argon atmosphere, operating pressure 0.3 Pa, power density 2 W / cm², and deposition rate 0.3 Å / s. The ITO layer of the perovskite top cell was then combined with the p-type back electrode of the crystalline silicon bottom cell. + -Si emitter surfaces are in direct contact, and the top and bottom cells are electrically connected in series through mechanical stacking to form a 2T tandem module. The crystalline silicon bottom cell adopts a bifacial TOPCon structure, and its p + -The Si emitter is located on the incident light side.

[0075] 7) 80 nm Ag was deposited on the back of the crystalline silicon bottom cell as the back electrode (molybdenum boat evaporation, vacuum degree 5×10⁻⁶). -4 Pa, rate 0.1 Å / s). The above-mentioned laminated assembly, EVA film, and backing glass were laminated and encapsulated in a laminator at a lamination temperature of 150°C for 15 min.

[0076] The above description is merely a preferred embodiment of this application, but the scope of protection of this application is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in this application, based on the technical solution and application concept of this application, should be included within the scope of protection of this application.

Claims

1. A perovskite solar module with a dynamic interface functional layer, characterized in that, include: A transparent electrode, a photo-induced isomeric self-assembled monolayer, a first charge transport layer, a perovskite light-absorbing layer, a second charge transport layer, and a back electrode are stacked sequentially along the incident light direction. The photoinduced isomeric self-assembled monolayer includes organic molecules; The organic molecule is one or more of diarylethylene derivatives, azobenzene derivatives, and spiropyran derivatives; the organic molecule contains one or more of phosphonic acid groups, carboxyl groups, and silane groups.

2. The perovskite solar module according to claim 1, characterized in that, The first charge transport layer is an electron transport layer, and the component is a formal structure.

3. The perovskite solar module according to claim 1, characterized in that, The first charge transport layer is a hole transport layer, and the component has an inverse structure.

4. The perovskite solar module according to claim 1, characterized in that, The thickness of the photoinduced heterogeneous self-assembled monolayer is 1 nm to 10 nm. The photo-induced heterogeneous self-assembled monolayer has a transmittance of 90% to 100% in the visible light band.

5. The perovskite solar module according to claim 1, characterized in that, The diarylethylene derivative is diarylethylene phosphonate; The azobenzene derivative is carbazole-azobenzene-phosphonic acid; The spiropyran derivative is 1',3',3'-trimethyl-spiro[2H-1-benzopyran-2,2'-indoline]-6-methylphosphonic acid.

6. A multilayer photovoltaic module, characterized in that, Includes the perovskite solar module as described in any one of claims 1 to 5.

7. The tandem photovoltaic module according to claim 6, characterized in that, The tandem photovoltaic module is one or more of the following: perovskite / silicon two-terminal tandem module, perovskite / silicon four-terminal tandem module, all-perovskite tandem module, perovskite / organic tandem module, and perovskite / CIGS tandem module.

8. A method for preparing a perovskite solar module as described in any one of claims 1 to 5, characterized in that, Includes the following steps: 1) Provide transparent electrodes; 2) A photo-induced isomeric self-assembled monolayer is formed on the surface of the transparent electrode; 3) A first charge transport layer, a perovskite light absorption layer, a second charge transport layer, and a back electrode are sequentially prepared on the surface of the photo-induced heterogeneous self-assembled monolayer.

9. The preparation method according to claim 8, characterized in that, The method for forming a photo-induced heterogeneous self-assembled monolayer is one or more of spin coating, vapor deposition, and solution immersion.

10. The preparation method according to claim 8, characterized in that, The first charge transport layer is prepared at a temperature of 100℃~150℃.