A carbon-based perovskite solar cell and its fabrication method
By adding DPGME to the conductive carbon paste of carbon-based perovskite solar cells and performing hot-pressing densification, the problems of uneven carbon electrode thickness and high porosity were solved, achieving more efficient carbon electrode etching quality and improved cell performance.
Patent Information
- Application Number
- CN202611078720.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-20
- Publication Date
- 2026-11-17
AI Technical Summary
In the large-area module fabrication process of existing carbon-based perovskite solar cells, the uneven thickness of the carbon electrode and the high internal porosity lead to incomplete or excessive etching, affecting the quality and reliability of the cells. Existing laser process adjustments are insufficient to completely solve these problems.
Dipropylene glycol methyl ether (DPGME) is added to conductive carbon paste as a slow-volatile solvent, and combined with hot pressing densification treatment, the rheological properties and film uniformity of carbon paste are improved, the internal porosity is reduced, and the uniformity and density of carbon electrode are improved by hot pressing molding.
It significantly improves the thickness uniformity and structural density of carbon electrodes, reduces etching difficulty, obtains P3 isolation lines with smooth edges, improves component efficiency and fill factor, reduces short-circuit risk, and is easy to promote and apply.
Smart Images

Figure CN123124651A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of perovskite solar cell technology, and in particular to a carbon-based perovskite solar cell and its fabrication method. Background Technology
[0002] Perovskite solar cells have become a research hotspot in next-generation photovoltaic technology due to their high photoelectric conversion efficiency and low-cost solution processing characteristics. Among them, carbon-based perovskite solar cells use carbon materials, such as conductive carbon paste, graphene, and carbon nanotubes, to replace precious metals like gold and silver as the counter electrode. This significantly reduces material costs while effectively suppressing ion migration and electrode corrosion by utilizing the inherent chemical inertness and hydrophobicity of carbon materials, thereby greatly improving the long-term operational stability of the device in humid and hot environments. Therefore, carbon-based perovskite solar cells are considered an important candidate solution to resolve the "efficiency-lifetime-cost" triangle in photovoltaic technology.
[0003] In the fabrication of large-area carbon-based perovskite solar cell modules, achieving reliable monolithic interconnection between sub-cells is a core factor determining the overall performance of the module. Currently, the mainstream interconnection architecture employs a three-line scribing process: P1 scribing is used to divide the transparent conductive oxide layer of the bottom electrode, forming lateral isolation between sub-cells; P2 scribing aims to remove the perovskite layer and carrier transport layer covering the TCO, exposing the bottom electrode to achieve electrical conduction between sub-cells; and P3 scribing is used to isolate the back electrodes of adjacent sub-cells, i.e., carbon electrodes, to prevent short circuits. This process needs to be completed with micron-level precision, requiring extremely high scribing quality.
[0004] The fabrication method of the carbon electrode directly affects the P3 etching quality. Large-area carbon electrodes are mainly produced using screen printing, a mature and low-cost process, but it has the following inherent drawbacks:
[0005] Firstly, the thickness uniformity is poor. During screen printing, when the squeegee squeezes the carbon paste through the screen, factors such as screen tension, squeegee pressure, and the rheological properties of the carbon paste (shear thinning and thixotropic recovery) can easily cause local thickness fluctuations or surface undulations in the film layer. Especially when printing over large areas (300mm × 300mm or more), the thickness difference between the edge and the center can reach several micrometers. This non-uniformity leads to inconsistent absorption and heat conduction behavior of laser energy in different areas during subsequent P3 laser etching, resulting in the contradictory phenomenon of some areas being under-etched while others are over-etched. Under-etching easily creates carbon bridge residues, affecting the etching effect and cell quality; while over-etching easily damages the underlying perovskite or TCO layer, directly damaging the cell and affecting its quality. Therefore, under-etching and over-etching remain an irreconcilable contradiction in perovskite solar cells.
[0006] Secondly, it has high internal porosity. Traditional carbon pastes typically use low-boiling-point solvents such as ethanol and isopropanol as diluents. During the annealing and curing process, the solvents evaporate rapidly, leaving pores at the micron or even submicron scale. These pores not only increase the surface resistance of the carbon electrode and reduce the lateral carrier transport efficiency, but also become centers of heat accumulation and energy scattering during laser etching. They easily induce local melting and spatter, forming "crater"-like defects or carbon particle adhesion, severely compromising the smoothness and isolation reliability of the etched edges.
[0007] To address the aforementioned issues, existing technologies offer solutions to improve P3 etching quality by optimizing laser parameters such as wavelength, power, pulse width, and scanning speed, or by employing scanning strategies like overlapping lines and offset overlapping lines. However, these methods are all "post-hoc compensations," meaning they only attempt to compensate for etching unevenness by adjusting the laser process based on existing carbon electrode defects. They fail to fundamentally solve the problems of poor uniformity and numerous internal pores in the carbon electrode itself. When the carbon electrode thickness fluctuation exceeds the tolerance range of the laser process window, even the most refined laser parameter optimization struggles to achieve a consistently etched effect across the entire surface area.
[0008] Therefore, how to fundamentally improve the uniformity of carbon electrode thickness and the density of its structure has become a key technical challenge to overcome the yield bottleneck of carbon-based perovskite solar cell modules and promote their industrialization. Summary of the Invention
[0009] The purpose of this application is to provide an improved method for preparing carbon-based perovskite solar cells, and the carbon-based perovskite solar cells prepared therefrom.
[0010] To achieve the above objectives, this application adopts the following technical solution:
[0011] This application discloses a method for preparing a carbon-based perovskite solar cell, which includes adding dipropylene glycol methyl ether (DPGME) to a conductive carbon paste printed by screen printing, annealing and curing after screen printing, hot pressing densifying the carbon electrode layer after curing and cooling to room temperature, and then performing P3 scribing.
[0012] It should be noted that this application innovatively adds dipropylene glycol methyl ether (DPGME) as a slow-volatile solvent additive to the conductive carbon paste for screen printing before P3 scribing, thereby achieving the following three effects: (1) Regulating the rheological properties of the carbon paste. DPGME is a high-boiling-point (approximately 190 °C) and slow-volatile solvent, which also regulates the viscosity of the carbon paste and improves the uniformity of screen printing. (2) Improving the uniformity of film formation. The slow evaporation characteristics of DPGME provide sufficient "open time" for carbon particles to flow and rearrange, forming a smoother and more uniform carbon electrode surface, significantly reducing local thickness fluctuations. (3) Reducing internal porosity. The slow evaporation of DPGME avoids the formation of a large number of micropores inside the carbon film due to the rapid escape of solvent, reducing resistance and abnormal points in laser etching from the source.
[0013] The preparation method of this application, by adding DPGME to the conductive carbon paste, can regulate the paste properties and improve the problem of numerous micropores left by rapid solvent evaporation during annealing. Subsequent hot pressing treatment, through the synergistic effect of both, effectively improves the uniformity of the carbon electrode, reduces the etching difficulty of the carbon electrode in the P3 laser scribing process, and effectively improves the photoelectric conversion performance of the product. This fundamentally solves the industrialization problems and technical pain points commonly found in screen-printed carbon electrodes, such as uneven thickness and internal porosity; it lays the foundation for stably obtaining P3 isolation lines with smooth edges and no craters, thereby achieving controllable dead area and low short-circuit risk. In one implementation of this application, the carbon-based perovskite solar cell prepared using this method achieves a module efficiency of 16.18% and a fill factor of 61.3%, which are improvements of 14.67% and 13.52% respectively compared to the control example without DPGME and hot pressing treatment. Furthermore, the preparation method of this application, in the preparation of carbon electrode, further adds DPGME to conductive carbon slurry and performs a hot pressing process after carbon electrode curing, without changing the original main production process, and is easy to promote and apply.
[0014] In some implementations, the hot pressing densification process of this application takes 5 to 15 minutes.
[0015] It should be noted that short-time hot-pressing of the cured carbon electrode layer is an existing technology. Its purpose is to improve the contact between the carbon electrode and the perovskite layer. For example, hot-pressing for 1-60 seconds mainly affects the carbon electrode surface and does not solve the P3 etching quality problem caused by intrinsic defects in the carbon electrode. The hot-pressing densification process in this application, compared to existing hot-pressing processes, has a longer densification time. Combined with the effects of DPGME, it can effectively eliminate deep internal micropores, correct thickness inhomogeneities, fundamentally improve the thickness uniformity and structural density of the carbon electrode, reduce the etching difficulty of the carbon electrode in the P3 laser scribing process, and thus solve the technical problem of P3 etching quality caused by intrinsic defects in the carbon electrode.
[0016] In some implementations, the pressure for hot pressing densification is 15~60 kPa.
[0017] In some implementations, the temperature for hot pressing densification is 100~120 ℃.
[0018] In some implementations, DPGME is added during the preparation of the conductive carbon paste. For example, the amount of dipropylene glycol methyl ether is 100~500 µL of dipropylene glycol methyl ether per 100 g of conductive carbon paste, that is, 100~500 µL of dipropylene glycol methyl ether is contained in every 100 g of prepared conductive carbon paste.
[0019] In some implementations, the annealing and curing conditions are annealing at 100~130 ℃ for 10~30 min.
[0020] In some implementations, P3 scribing is performed using laser etching.
[0021] In some implementations, laser etching scribing involves using a flat-top picosecond laser to etch P3 lines using an offset overlay process.
[0022] In some implementations, the offset of the offset line is between 75 and 150 µm to obtain an effective isolation linewidth of 175 to 100 µm.
[0023] In some implementations, the preparation method of this application further includes selecting ITO conductive glass with pre-etched P1 lines, sequentially preparing a SnO2 electron transport layer, a perovskite light-absorbing layer, and a P3HT hole transport layer on the ITO surface, and performing P2 line etching to obtain a semi-finished substrate, and screen printing conductive carbon paste on the surface of the semi-finished substrate.
[0024] This application also discloses a carbon-based perovskite solar cell prepared using the preparation method described in this application.
[0025] It should be noted that the carbon-based perovskite solar cell of this application, due to the preparation method of this application, fundamentally improves the uniformity of carbon electrode thickness and the density of structure, has smooth edges and no crater-like P3 isolation lines, controllable dead area, low short-circuit risk, and higher yield of carbon-based perovskite solar cell modules, laying the foundation for promoting the industrialization of carbon-based perovskite solar cells.
[0026] Due to the adoption of the above technical solutions, the beneficial effects of this application are as follows:
[0027] The carbon-based perovskite solar cell fabrication method of this application effectively improves the rheological properties of the conductive carbon paste by adding dipropylene glycol methyl ether. After the carbon electrode is cured, hot pressing densification treatment improves the uniformity and density of the carbon electrode, reducing the etching difficulty of the carbon electrode in the P3 laser scribing process. It fundamentally solves the industrialization problems and technical pain points such as uneven thickness and internal porosity that are common in screen-printed carbon electrodes. It lays the foundation for stably obtaining P3 isolation lines with smooth edges and no crater, thereby achieving the effects of controllable dead area and low short-circuit risk. Moreover, the fabrication method of this application does not change the original front-end production process and is easy to promote and apply. Attached Figure Description
[0028] Figure 1 These are optical microscope images of the laser scribing morphology, scanning electron microscope images of the carbon electrode cross-section, and battery efficiency test results of Comparative Example 1 of this application;
[0029] Figure 2 These are optical microscope images of the laser scribing morphology, scanning electron microscope images of the carbon electrode cross-section, and battery efficiency test results of Comparative Example 2 of this application;
[0030] Figure 3 These are optical microscope images of the laser scribing morphology, scanning electron microscope images of the carbon electrode cross-section, and battery efficiency test results of Embodiment 1 of this application;
[0031] Figure 4 These are optical microscope images of the laser scribing morphology, scanning electron microscope images of the carbon electrode cross-section, and battery efficiency test results of Embodiment 2 of this application. Detailed Implementation
[0032] Intrinsic defects in the carbon electrode layer are the main cause of P3 etching quality problems. Current technology lacks research on pretreatment of the cured carbon electrode layer to improve its intrinsic defects. Therefore, this application creatively proposes adding DPGME to the conductive carbon paste to improve its rheological properties, followed by hot-pressing densification after carbon electrode curing. This hot-pressing plasticity of the carbon electrode layer improves its uniformity, increases its density, and reduces the etching difficulty of the carbon electrode in the P3 laser scribing process.
[0033] In some implementations of this application, the fabrication method of carbon-based perovskite solar cells includes the following steps:
[0034] S1: Fabrication of functional layer and etching of P1 and P2 lines
[0035] The P1 line was pre-etched (using a Gaussian spot picosecond laser for scribing, power 4.4W, frequency 50kHz, pulse width 20ns, wavelength 1064nm, scan speed 400mm / s). A 300mm×300mm ITO conductive glass (sheet resistance ~15 Ω / □) was used. SnO2 layer (tin oxide nanocolloidal particles, annealed at 160℃ for 30 min in a tunnel furnace), perovskite layer (vacuum-assisted crystallization, 1 Pa low-pressure holding for 10 s, annealed at 160℃ for 30 min), and P3HT layer (poly(3-hexylthiophene-2,5-dimethyl), annealed at 120℃ for 10 min) were sequentially prepared on the ITO surface using slit coating. P2 line etching was then performed (using a Gaussian spot picosecond laser for scribing, power 3.3 W, frequency 20 kHz, pulse width 20 ns, wavelength 1064 nm, scan speed 300mm / s). (mm / s, 10 lines stacked, linewidth approximately 130 µm) to obtain a semi-finished substrate.
[0036] S2: Prepare carbon paste and screen print carbon electrodes
[0037] Commercial conductive carbon paste (DD-10) and dipropylene glycol methyl ether (DPGME, D108833) were mixed and dispersed in a specific ratio to form a homogeneous carbon paste. The preferred volumetric amount of DPGME in the carbon paste was 100–500 µL / 100 g of conductive carbon paste. Seven layers of carbon paste were printed using screen printing and then cured in a tunnel oven at 120 °C for 30 min to form a carbon electrode layer.
[0038] S3: Hot-pressed carbon electrode
[0039] The annealed and cured carbon electrode is placed in a laminating equipment and subjected to hot pressing under set temperature, pressure and time conditions to reshape the carbon electrode layer, resulting in a denser and more uniform carbon electrode layer.
[0040] S4: Laser etching of P3 line
[0041] A flat-top picosecond laser (34 W power, 50 kHz frequency, 144 ns pulse width, 1064 nm wavelength, and 450 mm / s scanning speed) was used to etch the P3 line using an offset stacking process to achieve reliable isolation between sub-cells. The offset of the stacking line was set to 150 µm, and the two stacking lines could obtain an effective isolation linewidth of about 100 µm, which ensured the reliability of isolation while minimizing the dead area.
[0042] Mechanism of action and effects of dipropylene glycol methyl ether:
[0043] (1) Regulate the rheological properties of carbon paste. DPGME is a high-boiling-point (about 190 ℃) and slow-volatile solvent. It also regulates the viscosity of carbon paste, preventing the rapid evaporation of solvent during the printing process from causing carbon particles to block the mesh of the screen printing plate and improving the uniformity of screen printing.
[0044] (2) Improve film uniformity. The slow volatilization characteristics of DPGME provide sufficient "open time" for carbon particles to flow and rearrange, forming a smoother and more uniform carbon electrode surface, significantly reducing local thickness fluctuations.
[0045] (3) Reduce internal porosity. The slow evaporation of DPGME avoids the formation of a large number of micropores inside the carbon film due to the rapid escape of solvent, thereby reducing resistance and abnormal points of laser etching from the source.
[0046] In some implementations, the role of the long-duration hot pressing process is:
[0047] For example, the annealed substrate is hot-pressed at a temperature of 100~120℃, a pressure of 15~60 kPa, and a time of 5~15 min. The long-term hot pressing allows heat and pressure to fully penetrate into the carbon electrode, achieving overall densification and uniform thickness, thereby achieving the following effects:
[0048] (1) Improve the uniformity of carbon electrode thickness, make the surface morphology more uniform, and provide a uniform energy absorption interface for laser etching.
[0049] (2) Eliminate internal pores, reduce film surface resistance, and improve the transverse transport efficiency of charge carriers.
[0050] (3) Improve the P3 etching quality, with neat and smooth edges, no carbon particle adhesion and crater defects, and reduce the risk of short circuit.
[0051] (4) Ultimately improve the photoelectric conversion efficiency and fill factor of the component.
[0052] Therefore, compared with the prior art, the preparation method of this application has the following advantages:
[0053] (1) Solving technical pain points: In response to the common industrialization problems of uneven thickness and internal pores in screen-printed carbon electrodes, a simple and effective comprehensive solution is provided without changing the printing equipment or parameters.
[0054] (2) Controllable etching quality: Combined with offset laser process, P3 isolation lines with smooth edges and no crater are stably obtained, the dead area is controllable, and the risk of short circuit is small.
[0055] (3) Significant performance improvement: For example, the module efficiency of Example 2 (DPGME + 50 kPa hot pressing for 10 min) reached 16.18%, and the fill factor was 61.3%, which were 14.67% and 13.52% higher than the untreated control, respectively. To clarify the contribution of each process step, the inventors further conducted an effect breakdown analysis: the module efficiency of Comparative Example 2 (only 50 kPa hot pressing treatment, no DPGME addition) was 15.89%, which was 12.62% higher than the untreated control; while comparing Example 2 with Comparative Example 2, that is, on the basis of the same hot pressing process, only the additional addition of DPGME further increased the module efficiency from 15.89% to 16.18%, which was 1.83% higher than the untreated control. The above data fully demonstrate that the addition of DPGME and the hot pressing treatment produced a synergistic effect, and the two complemented each other. The mechanism lies in the following: DPGME regulates the rheological properties of the carbon paste at the source, improving the film uniformity of screen printing and providing a smoother initial carbon film with fewer structural defects for subsequent hot pressing. Hot pressing, on this basis, densifies the carbon electrode layer through the combined action of pressure and heat, further closing residual interconnected pores and smoothing surface undulations. It is this synergistic effect of "source modification" and "post-processing enhancement" that significantly improves module performance.
[0056] (4) Strong process compatibility: Adding DPGME to conductive carbon paste and adding a hot pressing process after carbon electrode curing does not change the original front-end production process and is easy to promote to other carbon-based perovskite battery systems.
[0057] The present application will be further described in detail below through specific embodiments. The following embodiments are only for further illustration of the present application and should not be construed as limiting the present application.
[0058] Unless otherwise specified, the techniques used in the embodiments are conventional methods well known to those skilled in the art. For example, where specific techniques or conditions are not specified in the embodiments, they are performed in accordance with the techniques or conditions described in the literature in this field or in accordance with the product instructions. Reagents or instruments whose manufacturers are not specified are all commercially available conventional products.
[0059] Example 1
[0060] In this example, dipropylene glycol methyl ether (DPGME) + 30 kPa hot pressing is used to pretreat the cured carbon electrode layer, as detailed below:
[0061] S1: Fabrication of functional layer and etching of P1 and P2 lines
[0062] The P1 line was pre-etched (using a Gaussian spot picosecond laser for scribing, power 4.4 W, frequency 50 kHz, pulse width 20 ns, wavelength 1064 nm, scan speed 400 mm / s). A 300 mm × 300 mm ITO conductive glass (sheet resistance ~15 Ω / □) was used. SnO2 layer (tin oxide nanocolloidal particles, annealed in a tunnel furnace at 160 ℃ for 30 min), perovskite layer (vacuum-assisted crystallization, 1 Pa low-pressure holding for 10 s, annealed at 160 ℃ for 30 min), and P3HT layer (poly(3-hexylthiophene-2,5-dimethyl), annealed at 120 ℃ for 10 min) were sequentially prepared on the ITO surface using slit coating. P2 line etching was then performed (using a Gaussian spot picosecond laser for scribing, power 3.3 W, frequency 20 kHz, pulse width 20 ns, wavelength 1064 nm, scan speed 300 mm / s). (mm / s, 10 lines stacked, linewidth approximately 130 µm) to obtain a semi-finished substrate.
[0063] S2: Prepare carbon paste and screen print carbon electrodes
[0064] Commercial conductive carbon paste (DD-10) was mixed and dispersed with dipropylene glycol methyl ether (DPGME, D108833-500 mL) in a specific ratio to form a homogeneous carbon paste. The preferred volumetric amount of DPGME in the carbon paste was 100-500 µL / 100 g; specifically, in this example, 300 µL of DPGME was present per 100 g of conductive carbon paste. Seven layers of carbon paste were printed using screen printing and cured by annealing in a tunnel oven at 120 °C for 30 min to form a carbon electrode layer.
[0065] S3: Hot-pressed carbon electrode
[0066] The annealed carbon electrode was placed in a laminating apparatus, preheated to 110 °C by the upper and lower heating plates, and subjected to a pressure of 30 kPa for 10 min of hot pressing. After hot pressing, the four-probe test showed a four-sided resistivity of 8.2 Ω / □. Scanning electron microscopy revealed a carbon electrode thickness of 21.88 µm and a smooth, dense surface.
[0067] S4: Etching P3 line
[0068] P3 scribe lines were performed using a flat-top picosecond laser (output power 200 W, pulse width 144 ns, wavelength 1064 nm). The settings were 34 W power, 50 kHz frequency, and 450 mm / s scanning speed. After the first scribe, a second scribe was performed, offset downwards by 150 µm. Microscopic observation showed an effective etched linewidth of approximately 100 µm, with smooth and even etched edges, free of crater-like inclusions and carbon particle adhesion.
[0069] Example 2
[0070] In this example, dipropylene glycol methyl ether (DPGME) + 50 kPa hot pressing was used to pretreat the cured carbon electrode layer, as detailed below:
[0071] Steps S1 and S2 are the same as in Example 1.
[0072] S3: Hot-pressed carbon electrode
[0073] The hot-pressing temperature was 110 ℃, the pressure was increased to 50 kPa, and the hot-pressing time was 10 min. After hot pressing, the surface resistivity of the film measured by four probes was 6.7 Ω / □. Scanning electron microscopy showed that the carbon electrode thickness was 17.42 µm, indicating a higher degree of densification.
[0074] S4: Etching P3 line
[0075] Using the same laser and offset overlay process as in Example 1, the effective etched line width was observed to be approximately 100µm under a microscope, with smooth and flat etched edges and no defects.
[0076] Comparative Example 1
[0077] This example does not involve any treatment of the carbon electrode layer, i.e., no DPGME or hot pressing, as detailed below:
[0078] Steps S1 and S2 are the same as in Example 1, and the prepared carbon film has a thickness of approximately 25 µm and a surface resistivity of 11.6 Ω / □. In particular, compared with Example 1, step S2 does not add DPGME, and the carbon electrode layer is prepared directly by screen printing using commercial conductive carbon paste (DD-10). The screen printing and annealing curing are the same as in Example 1.
[0079] S3: Direct P3 etching (without hot pressing process), laser parameters are the same as in Example 1. Microscopic observation shows that the etching linewidth is about 100µm, with residual carbon particles and slight cratering in some areas.
[0080] Comparative Example 2
[0081] This example only involves hot-pressing the carbon electrode layer, without adding DPGME; that is, no DPGME, only hot pressing. Details are as follows:
[0082] Steps S1 and S2 are the same as in Comparative Example 1.
[0083] S3: Hot pressing was performed under the conditions of 50 kPa, 110 ℃, and 10 min. After hot pressing, the film surface resistivity was 6.9 Ω / □, and the thickness was 17.98 µm.
[0084] S4: After hot pressing, P3 etching is performed with the same laser parameters as in Example 1. Microscopic observation shows that the etching linewidth is approximately 100 µm, the P3 etching edge is smooth and without residue, and the component efficiency is 15.89%, which is slightly lower than that in Example 2, indicating that the addition of DPGME provides additional gain.
[0085] Test Method Description
[0086] The testing methods for the relevant parameters in each embodiment and comparative example are as follows:
[0087] (1) Film surface resistance test: A four-probe resistivity tester was used. At least 5 different positions (four corners and center) were selected for each sample for measurement, and the arithmetic mean was taken.
[0088] (2) Photovoltaic conversion efficiency and fill factor test of the module: A steady-state solar cell module simulator, model GSIV-22A1210, was used. The AM1.5G spectrum was provided by LED lights, and the power of the light source was calibrated to 100 mW / cm² using a silicon standard cell. 2 The IV curve was scanned in reverse (from open-circuit voltage to short-circuit voltage) at a scan rate of 0.1 V / s, with a scan range of 75 V to -0.1 V. All tests were conducted under atmospheric conditions (25±5 ℃, 50±5%RH). Module efficiency (PCE) and fill factor (FF) were automatically calculated by the testing software.
[0089] (3) Characterization of P3 etching edge quality: The edge morphology of the etching line was observed under 50-100x magnification using a laser scribing device and an optical magnifying glass.
[0090] (4) Microscopic morphology characterization: Field emission scanning electron microscope was used to observe the cross-section of the sample, and the magnification was 1000-10000 times.
[0091] Performance Comparison
[0092] The photoelectric performance of the battery modules prepared in the above embodiments and comparative examples was tested, and the results are shown in Table 1.
[0093] Table 1. Comparison of carbon electrode performance and component efficiency between each embodiment and the comparative example.
[0094] sample film surface resistance P3 Etching Edge Quality PCE component FF Comparative Example 1 11.6 Ω / □ Localized residual carbon particles 14.11% 54.0% Comparative Example 2 6.9 Ω / □ Smooth and residue-free 15.89% 58.2% Example 1 8.2 Ω / □ Small amount of residual carbon particles 15.22% 58.2% Example 2 6.7 Ω / □ Smooth and residue-free 16.18% 61.3%
[0095] Figure 1This document presents optical microscope images of the laser scribing morphology, scanning electron microscope images of the carbon electrode cross-section, and cell efficiency test results for Comparative Example 1 (without DPGME and without hot pressing) of this application. Images a to c show laser scribing points spaced 6 cm apart from left to right, revealing residual carbon particles in some areas; image d is a magnified view of the laser scribing, showing significant residual carbon particles and a high risk of short circuits; image e is a cross-sectional view of the carbon electrode, with a thickness of 23.67 µm and a small number of internal pores; image f is the module efficiency curve, showing a photoelectric conversion efficiency of 14.11% for the untreated perovskite cell.
[0096] Figure 2 The images show optical microscope photographs of the laser scribing morphology, scanning electron microscope images of the carbon electrode cross-section, and cell efficiency test results for Comparative Example 2 (without DPGME + 50 kPa hot pressing) of this application. Figures a to c show randomly selected points at 6 cm intervals from left to right along the P3 laser scribing, with virtually no carbon electrode particle residue; Figure d is a magnified view of the laser scribing, showing no carbon particle residue; Figure e is a cross-sectional view of the carbon electrode, with a thickness of 17.98 µm; Figure f is the module efficiency curve, showing that the photoelectric conversion efficiency of the perovskite cell increased to 15.89% after hot pressing, an improvement of 12.62% compared to the untreated cell.
[0097] Figure 3 The images show optical microscope photographs of the laser scribing morphology, scanning electron microscope images of the carbon electrode cross-section, and cell efficiency test results for Example 1 of this application (DPGME treatment + 30 kPa hot pressing). Figures a to c show laser scribing points spaced 6 cm apart from left to right, with a small amount of carbon particles remaining at the edge of the P3 line; Figure d is a magnified view of the laser scribing, showing a small amount of carbon particles visible within the P3 line; Figure e is a cross-sectional view of the carbon electrode, with a thickness of 21.88 µm; Figure f is the module efficiency curve. After DPGME treatment and 30 kPa hot pressing, the photoelectric conversion efficiency of the perovskite cell increased to 15.22%, a 7.87% improvement compared to the untreated cell. Due to the relatively low hot pressing pressure (30 kPa / 110℃ / 10 min), the film surface resistance and carbon electrode interface thickness after hot pressing are slightly higher than those of Comparative Example 2, which explains its inferior performance.
[0098] Figure 4 This document presents optical microscope images of the laser scribing morphology, scanning electron microscope images of the carbon electrode cross-section, and cell efficiency test results for Example 2 (DPGME treatment + 50 kPa hot pressing) of this application. Images a to c show laser scribing points spaced 6 cm apart from left to right on P3, with no carbon particles remaining at the edge of the P3 line; image d is a magnified view of the laser scribing, showing no carbon particles within the P3 line; image e is a cross-sectional view of the carbon electrode, with a thickness of 17.42 µm; image f is the module efficiency curve, showing that the perovskite cell photoelectric conversion efficiency increased to 16.18% after DPGME treatment and 50 kPa hot pressing, representing a 14.67% improvement over the untreated cell, indicating optimal performance.
[0099] Example 3
[0100] To further verify the rationality and criticality of the hot pressing process parameters, a systematic parameter optimization experiment was conducted simultaneously in this example. Specifically, based on Example 1, the hot pressing pressure, hot pressing time, and DPGME dosage were optimized respectively.
[0101] (1) Hot pressing pressure optimization
[0102] Under the conditions of a fixed hot-pressing temperature of 110 ℃, a hot-pressing time of 10 min, and a DPGME addition amount of 300 µL / 100 g carbon paste, hot-pressing treatment was performed by applying pressures of 15 kPa, 30 kPa, 50 kPa, and 60 kPa, respectively. All other aspects were the same as in Example 1. Film surface resistance, module efficiency, fill factor, and P3 etching edge quality characterization were performed using the same methods as in Example 1. The results are shown in Table 2.
[0103] Table 2 Effect of different hot-pressing pressures on the performance of carbon electrodes
[0104] Hot pressing pressure film surface resistance PCE component FF P3 Etching Edge Quality 15 kPa 9.5Ω / □ 14.82% 55.1% Small amount of carbon particles remaining 30 kPa 8.2Ω / □ 15.22% 58.2% Small amount of carbon particles remaining 50 kPa 6.7Ω / □ 16.18% 61.3% Smooth and residue-free 60 kPa 6.7Ω / □ 15.87% 58.0% Slight cracks in carbon electrode
[0105] As shown in Table 2, as the hot-pressing pressure increases from 15 kPa to 50 kPa, the film surface resistance gradually decreases, and the module efficiency gradually increases. At a pressure of 50 kPa, the module efficiency reaches its optimal value of 16.18%, and the P3 etching edge is smooth and residue-free. When the pressure is further increased to 60 kPa, although the film surface resistance remains unchanged (6.7 Ω / □), the excessive pressure causes slight cracks in the carbon electrode. This indicates that there is an optimal range for the hot-pressing pressure; too low a pressure results in insufficient densification, while too high a pressure damages the carbon electrode structure. Therefore, the hot-pressing densification treatment pressure in this application is 15~60 kPa, preferably 30~50 kPa, and more preferably 50 kPa.
[0106] (2) Hot pressing time optimization
[0107] Under the conditions of a fixed hot-pressing temperature of 110 ℃, a hot-pressing pressure of 50 kPa, and a DPGME addition amount of 300 µL / 100g carbon paste, hot-pressing treatments were performed for 5 min, 10 min, 15 min, and 20 min, respectively, with all other parameters being the same as in Example 1. Film surface resistance, module efficiency, fill factor, and P3 etching edge quality characterization were performed using the same methods as in Example 1, and the results are shown in Table 3.
[0108] Table 3 Effect of different hot-pressing times on the performance of carbon electrodes
[0109] Hot pressing time film surface resistance PCE component FF P3 Etching Edge Quality 5 min 8.8Ω / □ 15.02% 54.8% Small amount of carbon particles remaining 10 min 6.7Ω / □ 16.18% 61.3% Smooth and residue-free 15 min 6.5Ω / □ 15.98% 58.3% Smooth and residue-free 20 min 6.8Ω / □ 15.31% 55.6% Slight cracks at the edges
[0110] As shown in Table 3, when the hot-pressing time was extended from 5 min to 10 min, the film surface resistivity decreased significantly from 8.8 Ω / □ to 6.7 Ω / □, and the module efficiency increased from 15.01% to 16.18%. Further extending the time to 15 min resulted in a slight decrease in module efficiency, indicating that 10 min was the optimal process point. However, when the hot-pressing time was extended to 20 min, the carbon electrode developed embrittlement cracks due to excessive hot pressing, and the module efficiency actually decreased. This indicates that there is also an optimal window for the hot-pressing time; if it is too short, heat and pressure cannot fully penetrate into the carbon electrode, while if it is too long, cracks will appear in the carbon film. Therefore, the hot-pressing densification treatment time in this application is 5–15 min, preferably 5–10 min, and more preferably 10 min.
[0111] (3) Optimization of DPGME addition amount
[0112] Under fixed hot-pressing conditions (50 kPa, 110 °C, 10 min), different volumes of DPGME were added to the conductive carbon paste, resulting in 0 µL, 100 µL, 300 µL, and 500 µL of DPGME per 100 g of conductive carbon paste, respectively. All other parameters were the same as in Example 1. The film surface resistance, module efficiency, fill factor, and P3 etching edge quality were characterized using the same methods as in Example 1. The results are shown in Table 4.
[0113] Table 4 Effect of DPGME addition amount on carbon electrode performance
[0114] DPGME addition amount film surface resistance PCE component FF P3 Etching Edge Quality 0 µL / 100g carbon paste 6.9 Ω / □ 15.89% 58.2% Smooth and residue-free 100 µL / 100g carbon paste 6.9 Ω / □ 15.93% 57.8% Smooth and residue-free 300 µL / 100g carbon paste 6.7 Ω / □ 16.18% 61.3% Smooth and residue-free 500 µL / 100g carbon paste 6.8 Ω / □ 15.65% 55.5% Slight burrs on the edges
[0115] As shown in Table 4, when the DPGME addition amount is in the range of 100-500 µL / 100g carbon paste, the module efficiency first increases and then decreases. The optimal effect is observed at 300 µL / 100g carbon paste. However, when the addition amount reaches 500 µL, the uniformity of the carbon film after screen printing decreases, and etching P3 causes burrs at the edges, reducing the module efficiency to 15.65%. Therefore, this application limits the DPGME addition amount to 100-500 µL per 100g conductive carbon paste, preferably 100-300 µL per 100g conductive carbon paste, and more preferably 300 µL per 100g conductive carbon paste.
[0116] Conclusion: This application improves the rheological properties and film uniformity of carbon paste by adding dipropylene glycol methyl ether (DPGME) during the carbon paste preparation process, utilizing its high boiling point and slow volatility to reduce porosity defects within the carbon electrode from the source. Furthermore, the cured carbon electrode layer undergoes long-term hot-pressing densification treatment to further close residual interconnected pores and smooth out surface thickness unevenness. The synergistic effect of DPGME addition and the hot-pressing process significantly improves the thickness uniformity and structural density of the screen-printed carbon electrode, reduces the etching difficulty of the carbon electrode in the P3 laser scribing process, and thus obtains smooth-edged, crater-free P3 isolation lines, effectively improving the fill factor and photoelectric conversion efficiency of the component, verifying the effectiveness and practicality of the technical solution presented in this application.
[0117] The above description, in conjunction with specific embodiments, provides a further detailed explanation of this application and should not be construed as limiting the specific implementation of this application to these descriptions. Those skilled in the art to which this application pertains can make several simple deductions or substitutions without departing from the concept of this application.
Claims
1. A method for preparing a carbon-based perovskite solar cell, characterized in that: This process involves adding dipropylene glycol methyl ether to the conductive carbon paste used for screen printing, annealing and curing after screen printing, hot pressing densifying the cured carbon electrode layer after it has cooled to room temperature, and then performing P3 scribing.
2. The preparation method according to claim 1, characterized in that: The hot pressing densification process takes 5 to 15 minutes.
3. The preparation method according to claim 1, characterized in that: The pressure for the hot-press densification process is 15~60 kPa.
4. The preparation method according to claim 1, characterized in that: The temperature for the hot pressing densification process is 100~120℃.
5. The preparation method according to claim 1, characterized in that: The amount of dipropylene glycol methyl ether used is 100~500 µL of dipropylene glycol methyl ether per 100 g of conductive carbon paste.
6. The preparation method according to claim 1, characterized in that: The annealing and curing conditions are annealing at 100~130 ℃ for 10~30 min.
7. The preparation method according to claim 1, characterized in that: The P3 scribing is performed using laser etching.
8. The preparation method according to claim 1, characterized in that: The laser etching process includes using a flat-top picosecond laser to etch the P3 line using an offset overlay process. Optionally, the offset of the offset line is between 75 and 150 µm to obtain an effective isolation linewidth of 175 to 100 µm.
9. The preparation method according to any one of claims 1-8, characterized in that: It also includes using ITO conductive glass with pre-etched P1 lines, sequentially preparing a SnO2 electron transport layer, a perovskite light-absorbing layer, and a P3HT hole transport layer on the ITO surface, and then etching the P2 lines to obtain a semi-finished substrate, and then screen printing conductive carbon paste on the surface of the semi-finished substrate.
10. A carbon-based perovskite solar cell prepared by the preparation method according to any one of claims 1-9.