A Low-Damage Micro / Nano Fabrication Method for YBCO High-Temperature Superconducting Thin Films

By depositing an Au protective layer on the surface of YBCO thin films and employing a low-temperature dry etching technique, the damage problem of YBCO thin films during micro-nano fabrication was solved, achieving efficient protection of the superconducting properties and morphological integrity of YBCO. This method is suitable for fabricating micro-nano devices such as Hall strips, microbridges, and superconducting detectors.

CN123124665APending Publication Date: 2026-11-17SHANGHAI TECH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611269500.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

YBCO high-temperature superconducting thin films are susceptible to chemical and physical damage during micro- and nano-fabrication, leading to a decline in superconducting performance. Existing etching methods are difficult to maintain the integrity of the film while ensuring patterning accuracy.

Method used

A dense Au protective layer is deposited on the surface of the YBCO thin film, and low-temperature dry etching technology is used to pattern the YBCO film through low-temperature IBE or low-temperature ICP etching processes. This avoids direct exposure of the YBCO film to air and the etching environment, thereby reducing thermal damage and chemical corrosion.

Benefits of technology

It effectively protects the superconducting properties of YBCO thin films, maintains the morphological integrity of micron-sized and small-sized patterns, reduces superconducting transition temperature degradation, and improves the ability of processed devices to retain superconducting characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124665A_ABST
    Figure CN123124665A_ABST
Patent Text Reader

Abstract

This invention relates to the field of single-photon detection technology, and in particular to a low-damage micro / nano fabrication method for YBCO high-temperature superconducting thin films. The fabrication method includes the following steps: (1) epitaxially growing a YBCO thin film on a substrate; (2) depositing a gold protective layer on the surface of the YBCO thin film using magnetron sputtering; (3) spin-coating photoresist on the surface of the gold protective layer and baking the photoresist, performing ultraviolet exposure and development to form a photoresist mask layer containing a preset pattern, and then performing low-temperature dry etching to remove the photoresist and complete the micro / nano fabrication; the low-temperature dry etching is selected from either low-temperature IBE etching or low-temperature ICP, and the low-temperature temperature is -20~10℃. This invention can significantly reduce water vapor erosion, oxygen desorption, thermally induced damage, and etching edge degradation of YBCO thin films during the fabrication process, and improve the Tc retention capability and process consistency of micron-scale and even submicron / micro / nano-scale YBCO devices after patterning.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of single-photon detection technology, and in particular to a low-damage micro / nano fabrication method for YBCO high-temperature superconducting thin films. Background Technology

[0002] YBCO, or yttrium barium copper oxide high-temperature superconducting material, typically has the chemical formula YBa₂Cu₃O. 7-δ YBCO is a type of high-temperature superconducting oxide material with broad application prospects. Compared with traditional low-temperature superconducting materials such as Nb and NbTi, YBCO's critical transition temperature (Tc) can reach approximately 92 K, which is higher than the boiling point of liquid nitrogen (77 K). Therefore, YBCO devices can operate in the liquid nitrogen temperature range without relying on expensive and complex liquid helium refrigeration systems, offering advantages such as low refrigeration costs, simple system structure, and great potential for engineering applications.

[0003] However, the micro / nano fabrication of YBCO thin films presents significant challenges. YBCO is a complex oxide high-temperature superconducting material, and its superconducting properties are highly dependent on oxygen content, lattice structure integrity, and surface / interface state. YBCO thin films are susceptible to surface degradation due to moisture in air; contact with water, acids, alkalis, or aqueous corrosive liquids containing ions can also lead to changes in oxygen content, surface chemical damage, and lattice structure disruption. Even slight oxygen loss or localized structural degradation can cause a significant decrease in Tc, and in severe cases, even the disappearance of the superconducting transition.

[0004] On the other hand, YBCO devices typically require processing steps such as thin film deposition, photolithography, patterning etching, resist stripping, and cleaning. Among these, patterning etching is a key challenge in fabricating micro / nano-scale YBCO devices. Existing YBCO patterning methods mainly include wet etching and dry etching.

[0005] While wet etching is a simple process, it typically exhibits isotropic corrosion characteristics, which can easily lead to lateral etching, pattern edge coarsening, and distortion of small-sized patterns. More importantly, YBCO comes into direct contact with water, acids, or corrosion reaction products during wet etching, which can easily cause chemical degradation of the film surface and a decrease in superconductivity. Therefore, the applicability of wet etching for micron-sized or smaller YBCO devices is limited.

[0006] Dry etching methods, such as ion beam etching (IBE) and inductively coupled plasma etching (ICP), can achieve good anisotropy and pattern transfer capabilities. However, dry etching processes are subject to problems such as ion bombardment, plasma irradiation, localized temperature rise, and surface oxygen desorption, which can still lead to damage to the YBCO thin film. In particular, oxygen atoms on the YBCO surface are more likely to desorb when etching at room temperature or higher temperatures, resulting in more significant lattice degradation and a decrease in crystal density (Tc).

[0007] Therefore, there is an urgent need to provide a micro / nano fabrication method for YBCO high-temperature superconducting thin films with low damage. Summary of the Invention

[0008] In view of the shortcomings of the prior art described above, the purpose of this invention is to provide a low-damage micro / nano fabrication method for YBCO high-temperature superconducting thin films, which solves the problem of damage that easily occurs when fabricating micro / nano-scale YBCO devices in the prior art.

[0009] To achieve the above and other related objectives, the present invention is obtained through the following technical solution.

[0010] The first aspect of this invention is to provide a low-damage micro / nano fabrication method for YBCO high-temperature superconducting thin films, the fabrication method comprising the following steps:

[0011] (1) Epitaxial growth of YBCO thin films on a substrate;

[0012] (2) A gold protective layer is deposited on the surface of the YBCO thin film by magnetron sputtering;

[0013] (3) Spin-coating photoresist onto the surface of the gold protective layer and baking the photoresist, then performing ultraviolet exposure and development to form a photoresist mask layer containing a preset pattern, followed by low-temperature dry etching to remove the photoresist and complete the micro-nano processing; the low-temperature dry etching is selected from either low-temperature IBE etching or low-temperature ICP, and the low temperature is -20~10℃.

[0014] A second aspect of the present invention is to provide a YBCO micro / nano device that can be used in a high-temperature superconducting infrared absorption detector, which is fabricated using the processing method described above.

[0015] As described above, the low-damage micro / nano fabrication method for YBCO high-temperature superconducting thin films of the present invention has the following beneficial effects:

[0016] (1) This invention provides a low-damage micro / nano fabrication method suitable for Au and YBCO composite thin films. This method forms a dense Au protective layer on the surface of YBCO and uses a low-temperature dry etching process adapted to the properties of Au and YBCO. This allows Au to continuously act as an in-situ protective barrier for YBCO throughout the patterning process while performing device functions. This enables patterning of the composite thin film, reduces chemical and thermal damage to YBCO during air exposure and processing, maintains the morphological integrity of micron-level and small-sized patterns, and minimizes the degradation of the superconducting transition temperature of the YBCO device after processing.

[0017] (2) This invention can be used to prepare Hall bars, microbridges, superconducting detectors, superconducting interconnects, superconducting filters, auxiliary structures for superconducting quantum devices and other micro- and nano-devices based on YBCO thin films. Attached Figure Description

[0018] Figure 1 This is a schematic diagram of the lateral damage caused by etching.

[0019] Figure 2 The graph shows a comparison of the test results of the superconducting stability of YBCO thin films after growing Au protective layers using different deposition methods. Sample 1 (Example 1c) is a newly grown YBCO thin film, which has been in the atmosphere for a short time and has not yet had an Au protective layer deposited, representing the initial state of the YBCO thin film; Sample 2 (Example 1a) is a YBCO thin film with 50 nm Au deposited by magnetron sputtering; and Sample 3 (Example 1b) is a YBCO thin film with 50 nm Au deposited by electron beam evaporation.

[0020] Figure 3 The diagram shown is a schematic diagram of the Hall bar / Hall target mirror and the four-end test structure in Embodiment 1 of the present invention.

[0021] Figure 4 The figure shows the Tc test results of devices with different linewidths after room temperature IBE etching of Au / YBCO in Embodiment 2 of the present invention.

[0022] Figure 5 The figure shown is a graph of Tc test results for devices with different linewidths after low-temperature IBE etching of Au / YBCO in Example 3 of the present invention.

[0023] Figure 6 The figure shown is a graph of Tc test results for devices with different linewidths after room temperature ICP etching of Au / YBCO in Example 4 of this invention.

[0024] Figure 7 The figure shown is a graph of Tc test results for devices with different linewidths after low-temperature ICP etching of Au / YBCO in Example 5 of this invention.

[0025] Figure 8 The figure shows the Tc test results of devices with different linewidths after wet etching Au / YBCO in Embodiment 6 of the present invention.

[0026] Figure 9 The graph shows the Tc test results of devices with different linewidths obtained by the dry-wet combined process of first ICP dry etching of Au and then wet etching of YBCO in Embodiment 7 of the present invention.

[0027] Figure 10 The graph shows the Tc test results of devices with different linewidths obtained by the wet-dry combined process of first wet etching Au and then ICP dry etching YBCO in Embodiment 8 of the present invention. Detailed Implementation

[0028] To make the inventive objectives, technical solutions, and beneficial effects of this invention clearer, the invention will be further described in detail below with reference to embodiments. Those skilled in the art can easily understand other advantages and effects of this invention from the content disclosed in this specification.

[0029] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the specification of this invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.

[0030] When using “including,” “having,” and “contains” as described herein, the intention is to cover non-exclusive inclusion, unless an explicit qualifying term such as “only,” “consisting of,” etc., is used, in which case another component may be added.

[0031] In this invention, the terms "preferredly," "more preferably," "better," and "even better" refer to embodiments of the invention that provide certain beneficial effects under certain circumstances. However, other embodiments may also be preferred under the same or other circumstances. Furthermore, the description of one or more preferred embodiments does not imply that other embodiments are unavailable, nor is it intended to exclude other embodiments from the scope of the invention. That is, in this invention, "preferredly," "more preferably," "better," and "even better" are merely descriptions of more effective implementations or examples, but do not constitute a limitation on the scope of protection of the invention.

[0032] In this invention, terms such as "further," "even more," and "particularly" are used for descriptive purposes and indicate differences in content, but should not be construed as limiting the scope of protection of this invention.

[0033] In this invention, "at least one" means one or more, such as one, two, or more. "Multiple" or "several" means at least two, such as two, three, etc., and "multi-layered" means at least two layers, such as two layers, three layers, etc., unless otherwise explicitly specified. In the description of this invention, "several" means at least one, such as one, two, etc., unless otherwise explicitly specified.

[0034] When a numerical range is disclosed herein, the range is considered continuous and includes the minimum and maximum values ​​of the range, as well as every value between the minimum and maximum values. Furthermore, when the range refers to integers, it includes every integer between the minimum and maximum values ​​of the range. Additionally, when multiple ranges are provided to describe a feature or characteristic, the ranges may be combined. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges to which they are incorporated.

[0035] Unless otherwise specified, all steps of this invention may be performed sequentially or randomly. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the method may also include step (c), indicating that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.

[0036] Unless otherwise stated, a singular term may include a plural term and should not be understood as having a quantity of one.

[0037] In this invention, "above" or "below" both include the number itself. For example, "below 1" includes 1.

[0038] In this invention, room temperature refers to 0~40°C, including but not limited to 10~40°C, or further to 20~30°C.

[0039] When the linewidth of YBCO devices shrinks to the submicron or even nanoscale, the superconducting properties of the material exhibit a significant size effect. Small-linewidth YBCO transport lines enable high-density integration and are therefore of great significance in the fabrication of micro and nano devices. In existing technologies, to prevent the rapid degradation of YBCO in air, amorphous YBCO or alumina is typically deposited on its thin film surface as a protective layer. In device fabrication, the superconducting performance at wide linewidths is contributed by the three-dimensional bulk state. As the linewidth decreases, the superconducting performance approaches the contribution of the two-dimensional bulk state. The shift from large-linewidth fabrication to small-linewidth fabrication represents a reduction in physical dimension. This amplifies the originally minor thermal damage during the process by tens of times, thus drastically reducing the "tolerance" of the superconducting performance.

[0040] In device fabrication, metal electrodes and inert oxide layers are typically deposited separately. Directly using Au as a protective layer presents challenges in patterning processes. Furthermore, during subsequent patterning, the protective layer often requires windowing or stripping, directly exposing the underlying YBCO to the etchant or plasma environment. This makes it difficult to simultaneously maintain patterning accuracy and superconducting performance, effectively weakening the protective layer's effectiveness in the processing stage. Therefore, the technical problem this invention aims to solve is the susceptibility of YBCO high-temperature superconducting thin films to performance degradation when exposed to moisture or aqueous etching solutions in air, and the significant decrease or even loss of superconducting transition temperature during room-temperature or high-temperature etching due to thermal effects, oxygen desorption, ion bombardment, and plasma irradiation.

[0041] To address the aforementioned issues, this invention proposes a technical concept for the functional integration of an Au layer with a YBCO thin film. This concept abandons the traditional design approach of separating the protective layer and the functional layer, instead depositing a dense Au layer directly on the surface of the grown YBCO thin film. This allows Au to simultaneously serve as a chemical barrier for YBCO in the air, an electrode or functional metal layer for subsequent devices, and an in-situ masking layer during the patterning process. Under this concept, the Au layer is no longer merely a passive protective coating, but is incorporated into the overall design of the patterning process; the processing itself constitutes a protective mechanism for the YBCO.

[0042] The core of the above-mentioned technical implementation lies in establishing a low-temperature dry etching process window adapted to the differences in the physical properties of Au and YBCO. This process, through the coordinated control of the types of active particles in the plasma, ion bombardment energy, and substrate temperature, enables the Au layer to undergo controllable anisotropic etching at a low temperature. Etching products and residual plasma are effectively blocked by the Au layer in the un-etched areas, preventing them from directly affecting the YBCO interface. Throughout the patterning process, YBCO remains completely physically shielded by the Au layer until pattern transfer is complete. Simultaneously, the low-temperature environment significantly inhibits oxygen desorption and thermal diffusion of YBCO under plasma irradiation, and low-energy ion bombardment limits the energy acting on the YBCO surface to below the lattice damage threshold. Therefore, while the Au layer is gradually patterned, the underlying YBCO remains under dual protection of shielding and low-temperature stabilization, fundamentally avoiding the chemical corrosion and plasma damage caused by direct exposure of YBCO to the etching environment in traditional processing.

[0043] Compared with the prior art, the present invention has at least the following beneficial effects:

[0044] First, this invention directly deposits an Au layer on the surface of a YBCO thin film, giving it the dual functions of an air protective film and a metal electrode, thus simplifying the process. YBCO has poor chemical stability and is easily degraded by contact with moisture and water in air. Existing technologies typically require the additional epitaxial growth of an amorphous YBCO or alumina layer as a protective film, making the process complex. This invention uses magnetron sputtering to deposit the Au layer. Compared to electron beam evaporation, magnetron sputtering offers better thickness uniformity and coverage integrity, forming a more continuous and stable protective film, thus providing more effective protection for YBCO. Experiments show that this Au protective layer can effectively inhibit the degradation of YBCO performance, reduce the drop in superconducting transition temperature, and make the transition curve steeper.

[0045] Secondly, regarding patterning, traditional methods often employ electron beam evaporation to deposit a metal layer followed by a liftoff process to fabricate electrodes. However, in this invention, the Au layer is directly deposited on the YBCO surface via magnetron sputtering, resulting in a strong bond with the substrate that is difficult to remove using a liftoff process. Therefore, etching is necessary for patterning. Conventional ion beam etching can easily damage the underlying YBCO layer when processing the Au layer, affecting its superconducting properties. To address this, this invention has developed an in-situ etching process by optimizing process parameters such as etching temperature, gas ratio, and operating pressure. This process allows for precise patterning of the Au layer without interrupting the vacuum environment, while effectively protecting the superconducting properties of the YBCO film. Compared to electron beam evaporation, magnetron sputtering deposition of the Au layer offers better thickness uniformity and coverage integrity, forming a more continuous and stable protective film, thus providing more effective protection for the YBCO.

[0046] Third, this invention preferably employs low-temperature dry etching technology, controlling the etching process temperature through low-temperature IBE or low-temperature ICP to significantly reduce thermally induced damage and oxygen desorption. The superconducting properties of YBCO are highly sensitive to oxygen content; localized temperature rises during room-temperature or high-temperature etching processes promote oxygen desorption and lattice degradation, leading to a significant decrease in the superconducting transition temperature. Low-temperature etching can effectively suppress the aforementioned thermal damage mechanisms, allowing the etched YBCO device to maintain better superconducting transition characteristics. Furthermore, this dry etching process avoids prolonged exposure of YBCO to water, acids, or wet etching products, preventing lateral corrosion, edge roughening, and chemical damage, making it particularly suitable for small-size pattern fabrication. During plasma etching, anisotropic etching cannot completely avoid lateral damage (such as...). Figure 1 As shown in the figure. Theoretically, the degree of lateral damage is similar for devices with different linewidths; however, experimental results show that as the device linewidth decreases, the impact of edge damage, lateral corrosion, and surface degradation on the effective superconducting channel significantly increases (e.g., ...). Figure 4As shown), this leads to a decrease in the superconducting transition temperature and a broadening of the transition curve in small-linewidth devices. This invention employs an Au protective layer combined with a low-temperature dry etching process, effectively suppressing the damage amplification effect caused by size reduction, and significantly improving the superconducting transition temperature retention capability and process consistency of micron-sized YBCO devices (e.g., ...). Figure 5 (As shown).

[0047] The first aspect of this invention is to provide a low-damage micro / nano fabrication method for YBCO high-temperature superconducting thin films, the fabrication method comprising the following steps:

[0048] (1) Epitaxial growth of YBCO thin films on a substrate;

[0049] (2) A gold protective layer is deposited on the surface of the YBCO thin film by magnetron sputtering;

[0050] (3) Spin-coating photoresist onto the surface of the gold protective layer and baking the photoresist, then performing ultraviolet exposure and development to form a photoresist mask layer containing a preset pattern, followed by low-temperature dry etching to remove the photoresist and complete the micro-nano processing; the low-temperature dry etching is selected from either low-temperature IBE etching or low-temperature ICP, and the low temperature is -20~10℃.

[0051] In some embodiments of the present invention, in step (1), the substrate is selected from any one of LaAlO3 single crystal substrate, SrTiO3 single crystal substrate or LSAT single crystal substrate; the LaAlO3 substrate has a small lattice mismatch with YBCO, a matching coefficient of thermal expansion, and a cubic perovskite structure, which is beneficial for the epitaxial growth of YBCO and obtaining a high critical current density.

[0052] In some embodiments of the present invention, in step (1), the thickness of the YBCO thin film is 10-13 nm; for example, 10-11 nm, 11-12 nm, or 12-13 nm.

[0053] In some embodiments of the present invention, in step (1), the growth method is pulsed laser deposition; the laser source for pulsed laser deposition is a 200-300 nm Nd:YAG solid-state laser, for example, 200-230 nm, 230-260 nm, or 260-300 nm; the oxygen partial pressure is 0.1-0.5 Torr, for example, 0.1-0.25 Torr or 0.25-0.5 Torr; the radiation heater temperature is 900-1100 ℃, for example, 900-970 ℃ or 970-1100 ℃; and the laser energy density is 2.3 J·cm⁻¹. -2 The laser repetition frequency is 1-4 Hz. For example, 1-2.5 Hz or 2.5-4 Hz.

[0054] In some embodiments of the present invention, in step (1), the thickness of the substrate is 0.5-1 mm. For example, 0.5-0.8 mm or 0.8-1 mm;

[0055] YBCO high-temperature superconducting thin films were prepared on LaAlO3(001) single-crystal substrates. Pulsed laser deposition (PLD) was used, employing a target material prepared from CuO, BaCO3, and Y2O3 powders through calcination and hot pressing at 50 MPa, to deposit YBCO thin films with a thickness of 10–13 nm. After deposition, in-situ cooling was performed to obtain the desired superconducting thin film.

[0056] In some embodiments of the present invention, in step (2), the thickness of the gold protective layer is 40-60 nm; for example, 40-47 nm, 47-53 nm, or 53-60 nm. The Au protective layer plays multiple key roles in the present invention. As a physical barrier, it effectively isolates moisture in the air from contacting the YBCO film, thereby significantly reducing the degradation of the YBCO surface caused by moisture absorption. In subsequent micro-nano processing, this protective layer can reduce the direct impact of photoresist coating, exposure and development, solvent cleaning, and plasma etching processes on the YBCO film, avoiding chemical erosion and physical damage. At the same time, the Au protective layer itself has excellent conductivity, which can provide a stable conductive cover layer for the device. In addition, in some device structures, the Au layer can also be directly used as an electrode, absorption layer, or other functional metal layer to achieve structural simplification and functional integration. The thickness of the Au protective layer is about 40-50 nm. This thickness can provide good moisture protection and process protection without excessively increasing the difficulty of subsequent Au patterning etching.

[0057] In some embodiments of the present invention, in step (2), the magnetron sputtering deposition is DC magnetron sputtering. Compared with electron beam evaporation, Au films formed by magnetron sputtering generally have better thickness uniformity, coverage integrity, and interface continuity, which is beneficial for more effectively isolating the influence of air, water vapor, and subsequent process media on YBCO.

[0058] In some embodiments of the present invention, the substrate temperature for DC magnetron sputtering is 20-25°C; for example, 20-23°C or 23-25°C; the sputtering power is 140-160W; for example, 140-150W or 150-160W; the working gas pressure is 2-4mT; for example, 2-3mT or 3-4mT; and the deposition time is 120-140s; for example, 120-130s or 130-140s.

[0059] After the YBCO thin film is prepared, its exposure to air should be minimized, especially prolonged exposure to high humidity environments should be avoided. Vacuum transfer, inert gas transfer, dry nitrogen protection, or transfer to a low-humidity clean environment can be used to transfer the YBCO thin film into the Au deposition equipment.

[0060] Low-temperature etching plays the following main roles in the entire patterning process: By reducing the local temperature rise during etching, it effectively suppresses the desorption of oxygen atoms in YBCO, reduces thermally induced lattice degradation, and mitigates damage propagation caused by plasma irradiation and ion bombardment, ultimately improving the ability to maintain the superconducting transition temperature after patterning of small-sized devices.

[0061] For the patterning requirements of the Au and YBCO composite thin films mentioned above, the following two preferred solutions can be adopted for low-temperature dry etching.

[0062] Option A: Low-temperature IBE etching of Au / YBCO

[0063] The Au protective layer and YBCO thin film were patterned using low-temperature ion beam etching (IBE).

[0064] IBE primarily relies on high-energy ion beams to bombard the material surface, removing the material through physical sputtering. Due to Au's strong chemical inertness, IBE is well-suited for patterning Au.

[0065] The advantage of low-temperature IBE lies in its strong etching ability for Au, a chemically inert metal, and the relatively direct etching mechanism, primarily manifested as a physical sputtering process. By lowering the sample temperature, oxygen desorption and thermal damage to YBCO can be significantly reduced, thus making it suitable for the integrated patterning transfer of Au and YBCO composite films.

[0066] Option B is low-temperature inductively coupled plasma etching (ICP), which consists of two steps. The first step involves etching an Au protective layer using a Cl2 / Ar mixed gas. Cl2 reacts with the Au surface, and argon ion bombardment aids in the desorption of reaction products and material removal via physical sputtering. Since Au chlorides have limited volatility at room temperature or low temperatures, the Au layer thickness should not be too large, preferably around 50 nanometers or thinner. The second step involves etching a YBCO thin film using a CHF3 / Ar mixed gas. CHF3 forms a fluorocarbon polymer passivation layer on the etching sidewalls, reducing lateral etching and improving pattern anisotropy and edge morphology. Argon ion bombardment provides auxiliary physical sputtering. The advantage of low-temperature ICP etching is that the plasma density and ion bombardment energy can be controlled by adjusting the inductive coupling power, bias power, gas pressure, and gas composition. Compared with room temperature processes, low temperature conditions can significantly reduce thermal damage. At about 5°C, it can effectively improve the superconducting performance retention of YBCO after patterning, and has a better anisotropic transfer capability for micron-sized patterns.

[0067] In some embodiments of the present invention, in step (3), when the low-temperature dry etching is low-temperature IBE etching, the etching conditions are: temperature -20~0℃, for example, -20~-15℃, -15~-10℃, -10~-5℃, -5~0℃; etching time is 800-1000s; for example, 800-867s, 867-933s, 933-1000s;

[0068] In some embodiments of the present invention, in step (3), when the low-temperature dry etching is low-temperature ICP etching, the etching operation is as follows: S1, etching the Au protective layer using Cl2 / Ar mixed gas; S2, etching the YBCO thin film using CHF3 / Ar mixed gas.

[0069] In some embodiments of the present invention, in step S1, the etching temperature is 3-7°C; for example, 3-5°C or 5-7°C; the etching time is 33-40s; for example, 33-36s or 36-40s; the etching power is 450-650W; for example, 450-516W, 517-582W, or 583-650W; the RF power is 140-160W; for example, 140-146W, 147-153W, or 154-160W; and the etching gas pressure is 4.5-5.5mTorr; for example, 4.5-4.8mTor, 4.9-5.1mTor, or 5.2-5.5mTor.

[0070] In some embodiments of the present invention, in step S1, the volume ratio of Cl2 to Ar in the mixed gas is 2-4:1; for example, 2-3:1 or 3-4:1.

[0071] In some embodiments of the present invention, in step S2, the etching temperature is 3-7°C; for example, 3-5°C, 5-6°C, or 6-7°C; the etching time is 80-120s; for example, 80-90s, 90-100s, 100-110s, or 110-120s; the etching power is 450-650W; for example, 450-516W, 517-582W, or 583-650W; the RF power is 140-160W; for example, 140-146W, 147-153W, or 154-160W; and the etching gas pressure is 4.5-5.5mTorr; for example, 4.5-4.8mTorr, 4.9-5.1mTorr, or 5.2-5.5mTorr.

[0072] In some embodiments of the present invention, in step S2, the volume ratio of CHF3 to Ar in the mixed gas is 1:1-2. For example, it is 1:1-1.3, 1:1.4-1.6, or 1:1.7-2.

[0073] In some embodiments of the present invention, in step (3), the preset pattern is selected from one or more of the following: Hall strip structure, four-terminal test structure, microbridge structure, narrow line structure, superconducting detector structure, and superconducting interconnect structure.

[0074] In some embodiments of the present invention, in step (3), the line width of the preset pattern is 1-100μm; for example, 1-1.5μm, 1.5-2μm, 2-2.5μm, 2.5-3μm, 3-3.5μm, 3.5-4μm, 4-5μm, 5-6μm, 6-7μm, 7-10μm, 10-20μm, 21-40μm, 41-60μm, 61-80μm, 81-100μm;

[0075] In some embodiments of the present invention, in step (3), the cryogenicity is achieved by one or more of the following methods: cooling platform, back helium cooling, circulating coolant, semiconductor refrigeration, or liquid nitrogen-assisted cooling.

[0076] In some embodiments of the present invention, during step (3), prolonged contact between the YBCO exposed area and water, acid, or alkali should be avoided as much as possible during the degumming and cleaning process. Methods such as degumming with organic solvents, low-moisture cleaning, nitrogen drying, low-temperature drying, or vacuum drying can be used to reduce further damage to the YBCO from moisture and residual ions.

[0077] A second aspect of the present invention is to provide a YBCO micro / nano device that can be used in a high-temperature superconducting infrared absorption detector, which is fabricated using the processing method described above.

[0078] In some embodiments of the present invention, the micro / nano devices are used in spectral analysis or plasma physics measurements.

[0079] The present invention will be further illustrated by the following examples, but these examples do not limit the scope of the invention.

[0080] When numerical ranges are given in the embodiments, it should be understood that, unless otherwise stated in the present invention, both endpoints of each numerical range and any value between the two endpoints may be selected. Unless otherwise defined, all technical and scientific terms used in this invention have the same meaning as commonly understood by one of ordinary skill in the art. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. All reagents or instruments whose manufacturers are not specified are conventional products that can be purchased commercially. In addition to the specific methods, equipment, and materials used in the embodiments, based on the knowledge of the prior art possessed by one of ordinary skill in the art and the description of this invention, any prior art methods, equipment, and materials similar to or equivalent to those described, used, and materials in the embodiments of this invention may be used to implement this invention.

[0081] Example

[0082] Example 1

[0083] Example 1a

[0084] This embodiment provides a method for fabricating YBCO high-temperature superconducting thin films using micro / nano techniques. The method includes the following steps:

[0085] (1) Epitaxial growth of YBCO thin films on a substrate by pulsed laser deposition; specifically as follows: A LaAlO3(001) single crystal substrate was selected as the growth substrate. The substrate was placed into the growth chamber of a 2-inch large-area pulsed laser deposition system, and then the nominal temperature of the radiation heater was raised to 995 °C. High-purity oxygen was introduced into the chamber, and the oxygen partial pressure was maintained at 0.3 Torr (approximately 40 Pa). A 266 nm Nd:YAG solid-state laser was used as the ablation source, and the laser energy density was set to 2.3 J / cm². 2 The pulse repetition frequency was 2 Hz, and the target material was a YBCO ceramic target prepared by solid-state reaction and hot pressing densification of CuO, BaCO3, and Y2O3 powders. Under the above conditions, pulsed laser deposition was performed to grow a YBCO thin film on the surface of a LaAlO3(001) substrate.

[0086] After deposition, the sample was cooled to 600 °C, and 500 Torr (approximately 6.67 × 10⁻⁶) was introduced into the chamber. 4The oxygen (Pa) was applied without setting a constant temperature annealing time, and then cooled by turning off the heater (furnace cooling) to obtain a 10nm YBCO thin film;

[0087] (2) A gold protective layer is deposited on the surface of the YBCO thin film by magnetron sputtering; specifically as follows: the substrate with the YBCO thin film is transferred to the magnetron sputtering equipment under vacuum to avoid exposing the YBCO thin film to the atmospheric environment. A DC magnetron sputtering process is used, with a 99% pure gold target as the sputtering target material, and the base vacuum of the sputtering chamber is evacuated to 2.4 × 10⁻⁶. -8 Below Torr. High-purity argon gas was introduced as the sputtering gas, the working pressure was controlled at 3 mTorr, the sputtering power was set to 150 W, and the substrate temperature was room temperature. Under the above process conditions, sputtering was performed for 120 s to deposit a 50 nm thick, complete and dense gold protective layer on the surface of the YBCO thin film.

[0088] (3) Photoresist is spin-coated onto the surface of the gold protective layer and baked, then exposed to ultraviolet light and developed to form a photoresist mask layer with a preset pattern. Low-temperature dry etching is then used to remove the photoresist, completing the micro / nano fabrication. Specifically: AZ5214 photoresist is spin-coated onto the surface of the gold protective layer to form a photoresist layer with a thickness of approximately 1.4 μm. The spin-coated sample is placed on a hot plate for pre-baking at 100°C for 180 s. After the sample cools to room temperature, contact exposure is performed using an ultraviolet lithography machine at an exposure dose of 140 mJ / cm² to transfer the preset micro / nano pattern to the photoresist layer. After exposure, development is performed using AZ300MIF for 90 s, followed by rinsing with deionized water and drying with high-purity nitrogen to obtain a photoresist mask layer with the preset pattern. The dried sample is placed on a hot plate for post-baking at 100°C for 90 s. Low-temperature dry etching was performed on the sample with the photoresist mask. This embodiment employs a low-temperature ion beam etching process. The sample was placed in the sample stage of the low-temperature ion beam etching equipment, and the stage temperature was controlled at -10°C using liquid nitrogen or a refrigerator. The ion beam acceleration voltage was set to 200 volts, and the ion beam current to 0.16 mA. Using the photoresist mask as protection, the exposed gold protective layer was etched for 900 s. During the etching process, endpoint detection technology was used to monitor the gold layer etching progress to synchronously transfer the pattern to the YBCO thin film.

[0089] (4) After etching, the sample is removed from the etching equipment and sonicated with acetone at 26°C (room temperature) for 10 minutes (power 0.48W), followed by sonication with isopropanol at 26°C (room temperature) for 3 minutes (power 0.48W). Nitrogen gas is then used to dry the sample to remove any residual photoresist mask layer. The sample surface is then rinsed sequentially with deionized water and anhydrous ethanol, and finally dried with high-purity nitrogen gas to obtain a patterned gold electrode and YBCO superconducting thin film composite structure, completing the low-damage micro / nano fabrication. Sample 2 is obtained. The linewidth of the preset pattern is 1.5 μm. The preset pattern is a Hall bar or a Hall target four-terminal test structure, such as... Figure 3 As shown, the structure includes a narrow line channel in the central region and four electrode pads extending from both sides of the channel. This four-terminal test structure reduces the influence of contact resistance and lead resistance on the test results, allowing for a more accurate characterization of the intrinsic electrical transport characteristics of the YBCO device.

[0090] Example 1b

[0091] This embodiment provides a micro / nano fabrication method for YBCO high-temperature superconducting thin films. The difference from Embodiment 1a is that in step (2), a gold protective layer is prepared on the surface of the YBCO thin film using electron beam evaporation; otherwise, it is the same as in Embodiment 1a. Specifically:

[0092] Step (1) is performed in the same manner as in Example 1a;

[0093] (2) A gold protective layer was deposited on the surface of the YBCO thin film using electron beam evaporation; the substrate with the deposited YBCO thin film was fixed on the sample stage of the electron beam evaporation equipment, and the vacuum chamber was evacuated to a background vacuum level of 2.5 × 10⁻⁶. - 8 Below Tor. Place a high-purity gold target with a purity of not less than 99% in an electron beam evaporation crucible. Adjust the electron beam current to 75mA and preheat the gold target, setting the electron beam power output to 12% of the equipment's maximum output power. Turn on the crystal oscillator film thickness monitor and set the evaporation rate to 0.5 nm per second. Begin evaporating the gold film, monitoring the film thickness in real time using the crystal oscillator film thickness monitor. Stop evaporation when the gold film thickness reaches 50 nm. Turn off the electron beam and allow the substrate to cool naturally to room temperature. Then, fill the vacuum chamber with dry nitrogen gas to atmospheric pressure and remove the sample, thus forming a gold protective layer on the YBCO thin film surface.

[0094] The operations of steps (3)-(4) are the same as in Example 1a.

[0095] Example 1c

[0096] This embodiment provides a method for micro / nano fabrication of YBCO high-temperature superconducting thin films. The difference between this embodiment and Embodiment 1a is that step (2) is omitted, while the rest is the same as in Embodiment 1a.

[0097] The superconducting stability test results of Examples 1a-1c are as follows: Figure 2 As shown in the figure. Experiments revealed that YBCO films without an Au protective layer are prone to performance degradation in air, manifested as a decrease in Tc or a broadening of the transition curve. After covering with an Au protective layer, the electrical properties of YBCO are significantly more stable.

[0098] Further comparison revealed that magnetron sputtered Au films exhibited better thickness uniformity and coverage integrity, providing superior protection for YBCO compared to electron beam evaporated Au films. Therefore, magnetron sputtering deposition of an Au protective layer (such as...) is the preferred method in subsequent processes. Figure 2 (As shown).

[0099] Example 2: Room temperature IBE etching of Au / YBCO

[0100] This embodiment provides a method for micro / nano fabrication of YBCO high-temperature superconducting thin films. The difference from Embodiment 1a is that step (3) uses room-temperature IBE etching, while the rest is the same as in Embodiment 1a. Specifically:

[0101] Steps (1)-(2) are performed in the same manner as in Example 1a;

[0102] (3) Photoresist is spin-coated onto the surface of the gold protective layer and baked, then exposed to ultraviolet light and developed to form a photoresist mask layer with a preset pattern. The photoresist is then removed by dry etching at room temperature to complete the micro / nano fabrication. Specifically: AZ5214 photoresist is spin-coated onto the surface of the gold protective layer to form a photoresist layer with a thickness of approximately 1.4 μm. The spin-coated sample is placed on a hot plate for pre-baking at 100°C for 180 s. After the sample cools to room temperature, contact exposure is performed using an ultraviolet lithography machine at an exposure dose of 140.5 mJ / cm² to transfer the preset micro / nano pattern to the photoresist layer. After exposure, development is performed using an AZ300MIF for 90 s, followed by rinsing with deionized water and drying with high-purity nitrogen to obtain a photoresist mask layer with the preset pattern. The dried sample is placed on a hot plate for post-baking at 100°C for 90 s. Samples with photoresist masks were subjected to room-temperature dry etching. This embodiment employs room-temperature ion beam etching (room-temperature IBE). The sample was placed in the sample stage of the room-temperature ion beam etching equipment, high-purity argon gas was introduced, and the gas flow rate was adjusted to 20 mBar. High-purity helium gas was introduced, and the gas flow rate was adjusted to 6 sccm. The ion beam acceleration voltage was set to 120 volts, the ion beam current to 8 mA, the ignition voltage to 260 volts, and the electron beam voltage to 200 volts. Using the photoresist mask as protection, the exposed gold protective layer was etched for 827 s. During the etching process, endpoint detection technology was used to monitor the gold layer etching progress, and etching was stopped promptly when the underlying LAO substrate was exposed.

[0103] Step (4) is performed in the same manner as in Example 1a. Subsequently, preset patterns with linewidths of 1.5 μm, 3 μm, 5 μm, 10 μm, and 50 μm were prepared using the same steps, and the Tc of each pattern was measured. The test results are shown in […]. Figure 4 The smaller the device linewidth, the more significant the impact of damage introduced by room-temperature ion beam etching (IBE) on the effective superconducting channel becomes, according to conventional fabrication methods. This is because ion bombardment forms a damage layer on the sidewalls with a thickness of several nanometers to tens of nanometers. When the linewidth is wide, the damage layer occupies only a small portion of the cross-section; however, when the linewidth shrinks, the damage layer occupies most of the cross-sectional area, severely compressing the effective superconducting channel. This leads to a sharp drop in the superconducting critical temperature (Tc), which can decrease by up to 40 K, while the superconducting transition width increases significantly. Transition edge widening means a slower device response speed, making it difficult to meet the fast response requirements of high-temperature superconducting detectors. In contrast, devices with larger linewidths are less affected by edge damage and thus maintain better superconducting transition characteristics. For example, when the linewidth is 50 μm, the device Tc can reach approximately 71 K. This result indicates that while room-temperature IBE can achieve Au / YBCO patterning, it causes significant damage to small-sized YBCO devices.

[0104] Example 3 Low-temperature IBE etching

[0105] This embodiment provides a method for micro / nano fabrication of YBCO high-temperature superconducting thin films. The difference between this method and Embodiment 1a is that the linewidth of the preset pattern is different from that in Embodiment 1a; otherwise, they are the same as in Embodiment 1a. Details are as follows:

[0106] Pre-defined patterns with linewidths of 1 μm, 1.5 μm, 3 μm, 5 μm, 10 μm, 50 μm, and 100 μm were prepared following the exact same steps as in Example 1a, and the Tc of each pattern was measured. The test results are shown in [Figure 1]. Figure 5 The overall etch resistance (Tc) of devices with different linewidths after low-temperature IBE is better than that after room-temperature IBE, and the Tc difference between small-linewidth and large-linewidth devices is reduced. This indicates that low-temperature IBE can effectively reduce the etching damage amplification effect caused by size reduction and improve the superconducting performance retention of small-sized YBCO devices after patterning. Therefore, low-temperature IBE is one of the preferred processes for low-damage patterning of Au / YBCO composite films, especially suitable for situations where the Au layer is chemically inert and requires physical sputtering removal.

[0107] Example 4: Room Temperature ICP Etching

[0108] This embodiment provides a method for micro / nano fabrication of YBCO high-temperature superconducting thin films. The difference from Embodiment 1a is that step (3) uses room-temperature ICP etching, while the rest is the same as in Embodiment 1a. Specifically:

[0109] Steps (1)-(2) are performed in the same manner as in Example 1a;

[0110] (3) Photoresist is spin-coated onto the surface of the gold protective layer and baked, then exposed to ultraviolet light and developed to form a photoresist mask layer with a preset pattern. The photoresist is then removed by dry etching at room temperature to complete the micro / nano fabrication. Specifically: AZ5214 photoresist is spin-coated onto the surface of the gold protective layer to form a photoresist layer with a thickness of approximately 1.4 μm. The spin-coated sample is placed on a hot plate for pre-baking at 100°C for 180 s. After the sample cools to room temperature, contact exposure is performed using an ultraviolet lithography machine at an exposure dose of 140.5 mJ / cm² to transfer the preset micro / nano pattern to the photoresist layer. After exposure, development is performed using an AZ300MIF for 90 s, followed by rinsing with deionized water and drying with high-purity nitrogen to obtain a photoresist mask layer with the preset pattern. The dried sample is placed on a hot plate for post-baking at 100°C for 90 s. The sample with the photoresist mask was subjected to room-temperature dry etching. This embodiment employs room-temperature inductively coupled plasma (ICP) etching. The sample with the photoresist mask was placed on the sample stage of the ICP etching equipment, and the stage temperature was controlled at 20°C. The etching process consisted of two steps. The first step was the etching of the gold protective layer. The etching gas was a mixture of chlorine and argon, with a chlorine flow rate of 15 sccm and an argon flow rate of 6 sccm. The chamber working pressure was 5 mTorr, the etching power was 500 W, the bias power was 150 W, and the etching time was 39 s, completing the patterning of the gold protective layer. The second step is the etching of the YBCO thin film. The etching gas is switched to a mixture of trifluoromethane and argon, with a trifluoromethane flow rate of 15 sccm and an argon flow rate of 15 sccm. The working pressure of the chamber is 5 mTorr, the etching power is 500 W, the bias power is 150 W, and the etching time is 120 s, thus completing the pattern transfer of the YBCO thin film.

[0111] Step (4) is performed in the same manner as in Example 1a. Subsequently, preset patterns with linewidths of 1 μm, 1.5 μm, 3 μm, 5 μm, 10 μm, 50 μm, and 100 μm were prepared according to the same steps, and the Tc of each pattern was measured. The test results are shown in […]. Figure 6Room-temperature ICP also leads to size-related damage. Room-temperature ICP etching causes more severe damage at small linewidths than at large linewidths. The heat generated by the chemical reactions during etching is difficult to dissipate at smaller linewidths, and the resulting polymer residues cause a sharp shrinkage of the effective superconducting channel, resulting in more significant performance degradation. When the original thin film is processed into nanowires, the impact of etching damage on the effective superconducting channel increases with decreasing linewidth, leading to a sharp drop in the superconducting critical temperature (Tc), which can decrease by up to 30 K. Simultaneously, the superconducting transition width increases significantly. Transition edge broadening means a slower device response speed, making it difficult to meet the fast response requirements of high-temperature superconducting detectors. For larger linewidth structures, such as 100 μm linewidth devices, Tc can reach approximately 78 K, indicating that room-temperature ICP has some applicability for large-size devices, but significant performance degradation still exists for small-size devices.

[0112] Example 5 Low-temperature ICP etching

[0113] This embodiment provides a method for micro / nano fabrication of YBCO high-temperature superconducting thin films. The difference from Embodiment 1a is that the etching in step (3) uses low-temperature ICP etching; otherwise, it is the same as Embodiment 1a. Specifically:

[0114] Steps (1)-(2) are performed in the same manner as in Example 1a;

[0115] (3) Photoresist is spin-coated onto the surface of the gold protective layer and baked, then exposed to ultraviolet light and developed to form a photoresist mask layer with a preset pattern. Low-temperature dry etching is then used to remove the photoresist, completing the micro / nano fabrication. Specifically: AZ5214 photoresist is spin-coated onto the surface of the gold protective layer to form a photoresist layer with a thickness of approximately 1.4 μm. The spin-coated sample is placed on a hot plate for pre-baking at 100°C for 180 s. After the sample cools to room temperature, contact exposure is performed using an ultraviolet lithography machine at an exposure dose of 140.5 mJ / cm², transferring the preset micro / nano pattern to the photoresist layer. After exposure, development is performed using AZ300MIF for 90 s, followed by rinsing with deionized water and drying with high-purity nitrogen to obtain a photoresist mask layer with the preset pattern. The dried sample is placed on a hot plate for post-baking at 100°C for 90 s. Dry etching is performed on the sample with the photoresist mask. In this embodiment, dry etching can also be performed using a low-temperature inductively coupled plasma etching process. The sample with the photoresist mask is placed on the sample stage of the low-temperature inductively coupled plasma etching equipment, and the stage temperature is controlled at 5°C. The etching process is performed in two steps. The first step is the etching of the gold protective layer. The etching gas is a mixture of chlorine and argon, with a chlorine flow rate of 15 sccm and an argon flow rate of 6 sccm. The chamber working pressure is 5 mTorr, the etching power is 500 W, the bias power is 150 W, and the etching time is 39 s, completing the patterning of the gold protective layer. The second step is the etching of the YBCO thin film. The etching gas is switched to a mixture of trifluoromethane and argon, with a trifluoromethane flow rate of 15 sccm and an argon flow rate of 15 sccm. The working pressure of the chamber is 5 mTorr, the etching power is 500 W, the bias power is 150 W, and the etching time is 120 s, thus completing the pattern transfer of the YBCO thin film.

[0116] Step (4) is performed in the same manner as in Example 1a. Subsequently, preset patterns with linewidths of 1 μm, 1.5 μm, 3 μm, 5 μm, 10 μm, 50 μm, and 100 μm were prepared according to the same steps, and the Tc of each pattern was measured. The test results are shown in […]. Figure 7 The superconducting properties of YBCO devices are significantly improved after low-temperature ICP. The Tc of larger linewidth devices is close to that of the original YBCO thin film; although small linewidth devices still have some etching damage, the difference in Tc between them and large linewidth devices is significantly smaller than that under room-temperature ICP conditions. This indicates that the heat generated by the chemical reaction during etching, which is difficult to eliminate in smaller linewidths, can be improved by reducing the etching temperature.

[0117] The results show that low-temperature ICP can effectively improve the Tc retention and process consistency of Au / YBCO thin films after patterning, and is another preferred process of the present invention.

[0118] Example 6 Wet Etching

[0119] This embodiment provides a micro / nano fabrication method for YBCO high-temperature superconducting thin films. The difference from Embodiment 1a is that wet etching is used in step (3), while the rest is the same as in Embodiment 1a. Specifically:

[0120] Steps (1)-(2) are performed in the same manner as in Example 1a;

[0121] (3) Spin-coat photoresist onto the surface of the gold protective layer and bake the photoresist, perform ultraviolet exposure and development to form a photoresist mask layer with a preset pattern, wet etch to remove the photoresist, and complete the micro-nano fabrication; specifically as follows: Spin-coat AZ5214 photoresist onto the surface of the gold protective layer to form a photoresist layer with a thickness of approximately 1.4 μm. Place the spin-coated sample on a hot plate for pre-baking at a temperature of 100°C for 180 s. After the sample cools to room temperature, perform contact exposure using an ultraviolet lithography machine at an exposure dose of 140.5 mJ / cm² to transfer the preset micro-nano pattern to the photoresist layer. After exposure, perform development using AZ300MIF for 90 s, then rinse with deionized water and dry with high-purity nitrogen to obtain a photoresist mask layer with a preset pattern. Place the dried sample on a hot plate for post-baking at a temperature of 100°C for 90 s. Wet etching was performed on the sample with the photoresist mask. This embodiment uses a wet etching process, which consists of two steps. The first step is gold protective layer etching, where the sample with the photoresist mask is placed in a KI / I2 dilution solution (GE-8110) for 13 seconds. The second step is YBCO etching, where the sample from the first step is immediately immersed in a 1% phosphoric acid solution for 6 seconds. It is then immediately rinsed with deionized water and dried with nitrogen gas to complete the pattern transfer of the YBCO thin film.

[0122] Step (4) is performed in the same manner as in Example 1a. Subsequently, preset patterns with linewidths of 3 μm, 5 μm, 10 μm, 50 μm, and 100 μm were prepared according to the same steps, and the Tc of each pattern was measured. The test results are shown in […]. Figure 8 Wet etching has poor ability to preserve small-sized patterns. When the linewidth is less than 3μm, the pattern is prone to disappearance, breakage, or severe deformation; even if some 3μm linewidth structures are preserved, they may not exhibit a significant superconducting transition.

[0123] This indicates that water, acid, ion residues, and isotropic lateral corrosion in wet etching can significantly damage small-sized superconducting channels in YBCO. Therefore, simple wet etching is not suitable as a preferred patterning method for small-sized Au / YBCO devices.

[0124] Example 7: Au first etched by ICP dry etching, then YBCO etched by wet etching

[0125] This embodiment provides a micro / nano fabrication method for YBCO high-temperature superconducting thin films. The difference from Embodiment 1a is that in step (3), the etching process involves first low-temperature ICP dry etching of Au followed by wet etching of YBCO; otherwise, it is the same as Embodiment 1a. Specifically:

[0126] Steps (1)-(2) are performed in the same manner as in Example 1a;

[0127] (3) Photoresist is spin-coated onto the surface of the gold protective layer and baked, then exposed to ultraviolet light and developed to form a photoresist mask layer with a preset pattern. Low-temperature dry etching is then used to remove the photoresist, completing the micro / nano fabrication. Specifically: AZ5214 photoresist is spin-coated onto the surface of the gold protective layer to form a photoresist layer with a thickness of approximately 1.4 μm. The spin-coated sample is placed on a hot plate for pre-baking at 100°C for 180 s. After the sample cools to room temperature, contact exposure is performed using an ultraviolet lithography machine at an exposure dose of 140.5 mJ / cm², transferring the preset micro / nano pattern to the photoresist layer. After exposure, development is performed using AZ300MIF for 90 s, followed by rinsing with deionized water and drying with high-purity nitrogen to obtain a photoresist mask layer with the preset pattern. The dried sample is placed on a hot plate for post-baking at 100°C for 90 s. The sample with the photoresist mask was etched. In this embodiment, the etching process involved first low-temperature ICP dry etching of Au, followed by wet etching of YBCO. Specifically, the sample with the photoresist mask was placed on the sample stage of a low-temperature inductively coupled plasma etching (ICP) apparatus, and the stage temperature was controlled at 5°C. The etching process consisted of two steps. The first step was dry etching of the gold protective layer, using a mixture of chlorine and argon gases. The chlorine flow rate was 15 sccm, the argon flow rate was 6 sccm, the chamber working pressure was 5 mTorr, the etching power was 500 W, the bias power was 150 W, and the etching time was 39 s, completing the patterning of the gold protective layer. The second step was wet etching of the YBCO thin film. The sample from the first step was immediately immersed in a 1% phosphoric acid solution for 6 s. It was then immediately rinsed with deionized water and dried with nitrogen, completing the pattern transfer of the YBCO thin film.

[0128] Step (4) is performed in the same manner as in Example 1a. Subsequently, preset patterns with linewidths of 1.5 μm, 3 μm, 5 μm, 50 μm, and 100 μm were prepared using the same steps, and the Tc of each pattern was measured. The test results are shown in […]. Figure 9 Because the Au layer is etched using a dry etching method, the pattern retention capability is improved compared to simple wet etching, and some small linewidth structures can be preserved in terms of morphology.

[0129] However, electrical test results show that ( Figure 9Structures with linewidths of 3 μm and below did not exhibit a significant superconducting transition, indicating that wet etching of YBCO still leads to severe edge degradation, lateral corrosion, or chemical damage, causing small-linewidth patterns to completely lose their superconducting properties. Only when the linewidth reaches 50 μm and above can the device achieve a relatively ideal Tc, with the highest Tc reaching approximately 79 K.

[0130] The results indicate that although the wet-dry process improves the patterning quality of Au, the superconducting performance of small-sized devices is still severely limited because YBCO is still subjected to aqueous acid corrosion.

[0131] Example 8: Wet etching of Au followed by ICP dry etching of YBCO

[0132] This embodiment provides a micro / nano fabrication method for YBCO high-temperature superconducting thin films. The difference from Embodiment 1a is that in step (3), the etching process involves wet etching of Au followed by ICP dry etching of YBCO; otherwise, it is the same as Embodiment 1a. Specifically:

[0133] Steps (1)-(2) are performed in the same manner as in Example 1a;

[0134] (3) Photoresist is spin-coated onto the surface of the gold protective layer and baked, then exposed to ultraviolet light and developed to form a photoresist mask layer containing a preset pattern. Low-temperature dry etching is used to remove the photoresist and complete the micro-nano fabrication. Specifically, the sample with the photoresist mask is placed in a KI / I2 dilution solution (GE-8110) for 13s, then immediately rinsed with deionized water for 30s, and dried with nitrogen to complete the patterning of the gold protective layer. The second step is the etching of the YBCO thin film. The sample after the first step of etching is placed on the sample stage of a low-temperature inductively coupled plasma etching device, and the temperature of the sample stage is controlled at 5 degrees Celsius. The etching gas is a mixture of trifluoromethane and argon, with a trifluoromethane flow rate of 15 sccm, an argon flow rate of 15 sccm, a chamber working pressure of 5 mTorr, an etching power of 500W, a bias power of 150W, and an etching time of 120s to complete the pattern transfer of the YBCO thin film. The KI / I2 dilution solution (GE-8110) was obtained by diluting the KI / I2 solution purchased from Transene (USA) by 2 times.

[0135] Step (4) is performed in the same manner as in Example 1a. Subsequently, preset patterns with linewidths of 1.5 μm, 3 μm, 5 μm, 10 μm, 50 μm, and 100 μm were prepared using the same steps, and the Tc of each pattern was measured. The test results are shown in […]. Figure 10 Because the YBCO layer is etched using a dry etching method, the YBCO layer avoids direct exposure to phosphoric acid wet etching. Therefore, this process provides better protection for the superconducting performance of small-sized devices compared to the "dry etching Au + wet etching YBCO" approach.

[0136] Experimental results show that ( Figure 10 The 1.5 μm linewidth structure can still be preserved in morphology and exhibit certain superconducting transition characteristics. This result indicates that when wet etching of Au is unavoidable, wet etching of YBCO should be avoided as much as possible, and dry etching methods such as ICP should be preferred to complete the YBCO pattern transfer.

[0137] However, compared with the full-process low-temperature dry etching, this process may still be affected by interface contamination, edge roughening or residual ions introduced by Au wet etching. Therefore, its overall performance is still not as good as the low-temperature IBE or low-temperature ICP full dry process.

[0138] The above embodiments are merely illustrative of the principles and effects of the present invention and are not intended to limit the invention. Any person skilled in the art can modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by those skilled in the art without departing from the spirit and technical concept disclosed in the present invention should still be covered by the claims of the present invention.

Claims

1. A low-damage micro-nano processing method for YBCO high-temperature superconducting thin films, characterized in that, The processing method includes the following steps: (1) Epitaxial growth of YBCO thin films on a substrate; (2) A gold protective layer is deposited on the surface of the YBCO thin film by magnetron sputtering; (3) Spin-coating photoresist onto the surface of the gold protective layer and baking the photoresist, then exposing and developing it under ultraviolet light to form a photoresist mask layer containing a preset pattern. Low-temperature dry etching is then used to remove the photoresist and complete the micro-nano processing. The low-temperature dry etching is selected from either low-temperature IBE etching or low-temperature ICP, and the low temperature is -20~10℃.

2. The method of claim 1, wherein: It also includes one or more of the following features: 11) In step (1), the substrate is selected from any one of LaAlO3 single crystal substrate, SrTiO3 single crystal substrate or LSAT single crystal substrate; 12) In step (1), the thickness of the YBCO thin film is 10-13 nm; 13) In step (1), the growth method is pulsed laser deposition; 14) In step (1), the thickness of the substrate is 0.5-1 mm.

3. The method of claim 2, wherein: In feature 13), the laser source of the pulsed laser deposition is a 200-300 nm Nd:YAG solid laser, the oxygen partial pressure is 0.1-0.5 Torr, the radiant heater temperature is 900-1100℃, the laser energy density is 2.3 J·cm -2 , and the laser repetition frequency is 1-4 Hz.

4. The method of claim 1 wherein: It also includes one or more of the following features: 21) In step (2), the thickness of the gold protective layer is 40-60 nm; 22) In step (2), the magnetron sputtering deposition is DC magnetron sputtering.

5. The method of claim 4, wherein: In feature 22), the substrate temperature of the DC magnetron sputtering is 20-25℃; the sputtering power is 140-160W; the working pressure is 2-4mT; and the deposition time is 120-140s.

6. The method of claim 1 wherein: It also includes any of the following features: 31) In step (3), when the low-temperature dry etching is low-temperature IBE etching, the etching conditions are: temperature -20~0℃, etching time 800-1000s; 32) In step (3), when the low-temperature dry etching is low-temperature ICP etching, the etching operation is as follows: S1, etching the Au protective layer with Cl2 / Ar mixed gas; S2, etching the YBCO thin film with CHF3 / Ar mixed gas.

7. The method of claim 6, wherein: It also includes one or more of the following features: 321) In feature 32), in step S1, the etching temperature is 3-7℃; the etching time is 33-40s; the etching power is 450-650W; the RF power is 140-160W; and the etching gas pressure is 4.5-5.5mTorr. 322) In feature 32), in step S1, the volume ratio of Cl2 to Ar in the mixed gas is 2-4:1; 323) In feature 32), in step S2, the etching temperature is 3-7℃; the etching time is 80-120s; the etching power is 450-650W; the RF power is 140-160W; and the etching gas pressure is 4.5-5.5mTorr. 324) In feature 32), in step S2, the volume ratio of CHF3 and Ar in the mixed gas is 1:1-2.

8. The method of claim 1 wherein: In step (3), the preset pattern is selected from one or more of the following: Hall strip structure, four-terminal test structure, microbridge structure, narrow line structure, superconducting detector structure, and superconducting interconnect structure.

9. The method of claim 1 wherein: In step (3), the line width of the preset pattern is 1-100 μm; and / or, the low temperature is achieved by one or more of the following methods: cooling stage, back helium cooling, circulating coolant, semiconductor refrigeration or liquid nitrogen-assisted cooling.

10. A YBCO micro- and nano-device useful for high temperature superconducting infrared absorption detectors, characterized by: It is processed using the processing method described in any one of claims 1-9.