Semiconductor devices and their fabrication methods
By setting an etching selectivity with a gradient of nitrogen content in the mask layer and employing a single etching technique, the high cost and complexity of self-aligned dual patterning technology are solved, achieving higher density semiconductor device patterning structures and higher quality reliability.
Patent Information
- Application Number
- CN202611328999.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-28
- Publication Date
- 2026-11-17
AI Technical Summary
Existing self-aligned dual patterning technology suffers from high cost, long cycle time and complex process in the fabrication of semiconductor devices, making it difficult to achieve higher density patterned structures, and it has poor adaptability to non-uniform spacing and complex two-dimensional pattern designs.
By setting a nitrogen content gradient in the mask layer and adjusting the etching selectivity, smaller openings can be formed in a single etching process, simplifying the process flow and reducing costs.
It achieves higher density patterned structures, reduces fabrication costs and process complexity, improves defects in the mask pattern transfer process, and enhances device quality and structural reliability.
Smart Images

Figure CN123124766A_ABST
Abstract
Description
Technical Field
[0001] This disclosure relates to the field of semiconductor technology, and in particular to a semiconductor device and a method for fabricating the same. Background Technology
[0002] With the continuous iteration of semiconductor manufacturing processes and the continuous improvement of chip device density, self-aligned dual patterning technology has become the mainstream solution, especially in the Fin Field-Effect Transistor (FinFET) process, where it is widely used to prepare the core Fin structure.
[0003] However, self-aligned dual patterning technology has significant limitations. It involves multiple complex processes such as photolithography, multiple deposition and etching, which not only increases manufacturing costs and lengthens the production cycle, but also easily leads to problems such as increased pattern edge roughness and polymer residue, directly affecting transistor performance. Furthermore, self-aligned dual patterning technology is only suitable for unidirectional, equally spaced line arrays. It is difficult to implement independently when dealing with non-uniform spacing, bidirectional, or complex two-dimensional patterns, and often requires the combination with other photolithography technologies, further increasing process complexity and implementation costs.
[0004] Therefore, how to achieve higher density patterned structures without affecting the controllability of key dimensions, improve defects in the mask layer pattern transfer process, and reduce fabrication costs has become a problem to be solved in this field. Summary of the Invention
[0005] The purpose of this disclosure is to provide a semiconductor device and a method for fabricating the same, which enables higher density patterned structures without affecting the controllability of critical dimensions, improves defects in the mask pattern transfer process, and reduces fabrication costs.
[0006] To achieve the above objectives, the embodiments of this disclosure provide the following technical solutions: On one hand, a method for fabricating a semiconductor device is provided, the method comprising: forming a mask layer on a substrate. Along a first direction perpendicular to the substrate, the mask layer includes a first portion near the substrate and a second portion away from the substrate, wherein the nitrogen content in the first portion is greater than the nitrogen content in the second portion. The mask layer is etched to form a first opening penetrating the mask layer, the first opening exposing the substrate. The substrate is etched through the first opening to form an opening within the substrate.
[0007] The method for fabricating the aforementioned semiconductor device includes forming a mask layer on a substrate. Along a first direction perpendicular to the substrate, the nitrogen content in a first portion of the mask layer closer to the substrate is greater than the nitrogen content in a second portion of the mask layer farther from the substrate. Since a higher nitrogen content results in a higher etching selectivity, the etching selectivity of the first portion is greater than that of the second portion. By setting the nitrogen content in the first portion to be greater than that in the second portion, the etching selectivity of the mask layer is increased the closer it is to the substrate.
[0008] Furthermore, the mask layer is etched to form a first opening penetrating the mask layer, exposing the substrate. The substrate is etched through the first opening to form an aperture within the substrate, thereby achieving mask pattern transfer. Since the etching selectivity of the first part is greater than that of the second part, during the etching of the mask layer, the size of the portion of the first opening located in the first part is smaller than the size of the portion of the first opening located in the second part, thereby enabling the formation of a smaller aperture within the substrate.
[0009] It is understood that in the above-described fabrication method, by adjusting the nitrogen content in different locations of the mask layer, the etching selectivity of the mask layer at different locations is adjusted, thereby achieving a gradient change in the etching selectivity of the mask layer. This forms a first opening with a gradually decreasing size in the mask layer, resulting in a smaller aperture in the substrate. Without affecting the controllability of the critical aperture size, a patterned structure of a smaller, higher-density semiconductor device can be achieved through a single etching of a mask layer, reducing fabrication costs and process complexity. Furthermore, compared to defects such as poor aperture morphology and polymer residue caused by multiple etching processes, the fabrication method disclosed herein also improves upon these defects during the mask layer pattern transfer process, enhancing the quality and structural reliability of the subsequently formed semiconductor device.
[0010] In some embodiments, the difference between the nitrogen content in the first part and the nitrogen content in the second part is less than or equal to 25%.
[0011] In some embodiments, along the first direction, the thickness of the first part is greater than or equal to the thickness of the second part.
[0012] In some embodiments, the mask layer further includes a third portion disposed between the first and second portions along the first direction. The nitrogen content in the third portion is greater than the nitrogen content in the second portion and less than the nitrogen content in the first portion.
[0013] In some embodiments, the difference between the nitrogen content in the third part and the nitrogen content in the second part is less than or equal to 15%. The difference between the nitrogen content in the first part and the nitrogen content in the third part is less than or equal to 20%.
[0014] In some embodiments, along the first direction, the thickness of the third part is greater than or equal to the thickness of the second part, and less than or equal to the thickness of the first part.
[0015] In some embodiments, the material of the mask layer includes at least one of silicon nitride and silicon oxynitride.
[0016] In some embodiments, forming a mask layer on a substrate includes: employing a deposition process and adjusting the process parameters of the deposition process to form the mask layer. The nitrogen content in the mask layer gradually increases along a direction perpendicular to the substrate and pointing from the mask layer to the substrate.
[0017] In some embodiments, the width of the first opening gradually decreases along a direction perpendicular to the substrate and pointing from the mask layer to the substrate.
[0018] In some embodiments, before forming a mask layer on the substrate, the above preparation method further includes experimentally adjusting the nitrogen content in the first and second parts according to the size of the target aperture.
[0019] On the other hand, a semiconductor device is provided, which is prepared by the semiconductor device preparation method of any of the above embodiments.
[0020] The semiconductor devices described above have the same beneficial technical effects as the semiconductor devices provided in some of the above embodiments, and will not be repeated here. Attached Figure Description
[0021] To more clearly illustrate the technical solutions in this disclosure, the accompanying drawings used in some embodiments of this disclosure will be briefly described below. Obviously, the drawings described below are only drawings of some embodiments of this disclosure, and those skilled in the art can obtain other drawings based on these drawings. In addition, the drawings described below can be regarded as schematic diagrams and are not intended to limit the actual size of the product, the actual process of the method, etc. involved in the embodiments of this disclosure.
[0022] Figure 1 This is a flowchart of a method for fabricating a semiconductor device according to some embodiments; Figures 2-9 The diagram shows the steps of a method for fabricating a semiconductor device according to some embodiments. Detailed Implementation
[0023] The technical solutions in some embodiments of this disclosure will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this disclosure, and not all embodiments. All other embodiments obtained by those skilled in the art based on the embodiments provided in this disclosure are within the scope of protection of this disclosure.
[0024] Unless the context otherwise requires, throughout the specification and claims, the term "comprising" is interpreted as open-ended and encompassing, meaning "including, but not limited to." In the description of the specification, terms such as "one embodiment," "some embodiments," "exemplary embodiments," or "example" are intended to indicate that a particular feature, structure, material, or characteristic associated with that embodiment or example is included in at least one embodiment or example of this disclosure. The illustrative representations of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics mentioned may be included in any suitable manner in any one or more embodiments or examples.
[0025] Hereinafter, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of that feature. In the description of embodiments of this disclosure, unless otherwise stated, "a plurality of" means two or more.
[0026] "At least one of A, B and C" has the same meaning as "at least one of A, B or C", both including the following combinations of A, B and C: only A, only B, only C, combinations of A and B, combinations of A and C, combinations of B and C, and combinations of A, B and C.
[0027] "A and / or B" includes the following three combinations: A only, B only, and a combination of A and B.
[0028] The use of “applies to” or “configured to” in this article implies an open and inclusive language that does not preclude applicability to or configuration to devices that perform additional tasks or steps.
[0029] As used herein, “about,” “approximately,” or “approximately” includes the stated value and the average value within an acceptable range of deviation from the given value, wherein the acceptable range of deviation is determined by a person skilled in the art taking into account the measurement under discussion and the error associated with the measurement of the given quantity (i.e., the limitations of the measurement system).
[0030] As used herein, “parallel,” “perpendicular,” and “equal” include the described situation and situations that are similar to the described situation, within an acceptable deviation range, which is determined by those skilled in the art taking into account the measurement under discussion and the errors associated with the measurement of a particular quantity (i.e., the limitations of the measurement system). For example, “parallel” includes absolute parallelism and approximate parallelism, where an acceptable deviation range for approximate parallelism may be, for example, within 5°; “perpendicular” includes absolute perpendicularity and approximate perpendicularity, where an acceptable deviation range for approximate perpendicularity may also be, for example, within 5°; “equal” includes absolute equality and approximate equality, where an acceptable deviation range for approximate equality may be, for example, a difference between the two equals being less than or equal to 5% of either one.
[0031] It should be understood that when a layer or element is referred to as being on another layer or substrate, it can mean that the layer or element is directly on the other layer or substrate, or that there is an intermediate layer between the layer or element and the other layer or substrate.
[0032] This document describes exemplary embodiments with reference to cross-sectional views and / or plan views, which are idealized exemplary drawings. In the drawings, the thickness of layers and the area of regions are enlarged for clarity. Therefore, variations in shape relative to the drawings are contemplated due to, for example, manufacturing techniques and / or tolerances. Thus, exemplary embodiments should not be construed as being limited to the shapes of the regions shown herein, but rather include shape deviations due to, for example, manufacturing processes. For example, etched areas shown as rectangular would typically have curved features. Therefore, the regions shown in the drawings are schematic in nature, and their shapes are not intended to show the actual shapes of the areas of the device, nor are they intended to limit the scope of the exemplary embodiments.
[0033] In related technologies, with the continuous development of semiconductor manufacturing technology, integrated circuits are becoming smaller and denser. In order to improve the device density on the chip, self-aligned double patterning (SADP) technology has been widely used.
[0034] For example, in the FinFET (Fin Field-Effect Transistor) process platform, the formation of the fin is typically accomplished using SADP (Sacrificial Image Processing) technology. The complexity and controllability challenges of SADP are its most critical limitations, resulting in numerous process steps, high manufacturing costs, and long production cycles. SADP requires multiple masks, sacrificial layers, and spacer deposition layers, along with multiple etching operations. These repeated depositions and etchings lead to complex sidewall morphologies in the final pattern, potentially exacerbating edge roughness and impacting transistor performance. Furthermore, the risk of polymer residue from multiple etching processes also poses a challenge. Complex mask layer deposition and high-precision spacer control are both challenging, and fluctuations in each process step can narrow the etching process window.
[0035] Furthermore, SADP's process flow is more complex than single-pass lithography, typically involving multiple steps such as photolithography, core layer etching, spacer layer deposition, anisotropic etching, and core layer removal. More steps mean longer production cycles, higher costs, and more potential points of failure. Additionally, SADP is suitable for fabricating unidirectional (usually one-way) line arrays with uniform spacing. For designs requiring varying spacing, bidirectional structures, or complex two-dimensional patterns (such as chip interconnect layers), SADP implementation becomes extremely complex, or even impossible. It often needs to be combined with other technologies such as LELE (photolithography-etching-photolithography-etching), further increasing complexity and cost.
[0036] Therefore, how to achieve higher density patterned structures without affecting the controllability of the critical dimension (CD), while improving defects in the mask pattern transfer process, has become a pressing technical problem in the current semiconductor manufacturing field.
[0037] To address the aforementioned problems, in one aspect, embodiments of this disclosure provide a method for fabricating a semiconductor device. Figure 1 This is a flowchart of a method for fabricating a semiconductor device according to some embodiments; Figures 2-9 The diagram shows the steps of a method for fabricating a semiconductor device according to some embodiments.
[0038] The preparation method includes the following steps S1 to S3: Step S1: See Figure 2 A mask layer 2 is formed on substrate 1. See [link / reference] Figure 2 and Figure 3 Along a first direction Z perpendicular to the substrate 1, the mask layer 2 includes a first part 21 near the substrate 1 and a second part 22 away from the substrate 1. The nitrogen content in the first part 21 is greater than the nitrogen content in the second part 22. Figure 3for Figure 2 A magnified view of a portion of the mask layer.
[0039] For example, substrate 1 can be a wafer, and the material of substrate 1 can be silicon. Substrate 1 is not limited to a complete circular silicon wafer; discrete dies that have been thinned and diced also fall within the scope of this solution.
[0040] For example, see [link to example]. Figure 2 Before forming the mask layer 2 on the substrate 1, the above preparation method further includes forming a sacrificial layer 3 on the substrate 1. The sacrificial layer 3 can be used to protect the parts of the substrate 1 that do not need to be etched from damage during the etching process. In addition, the sacrificial layer 3 can provide a high etching selectivity ratio to prevent over-etching through the substrate 1.
[0041] For example, the material of the sacrificial layer 3 can be at least one of a-Si (amorphous silicon), C (carbon), and SiO2 (silicon oxide).
[0042] For example, in the nitrogen-containing mask layer 2, the relationship between the etching selectivity and the nitrogen content can be expressed as:
[0043] Where S is the etching selectivity, S0 is the basic selectivity, k is a coefficient, and [N%] is the percentage content of nitrogen.
[0044] For example, S0 can be the selection ratio of the mask material formed in the initial stage of the process, and the k value is obtained from multiple experimental experiences, with the k value ranging from approximately 0.15 to 0.25.
[0045] As can be seen from the above formula, the etching selectivity of the mask material gradually increases with the increase of nitrogen content.
[0046] Understandably, see Figure 3 Along the first direction Z, the nitrogen content in the first part 21 of the mask layer 2 is greater than the nitrogen content in the second part 22, meaning the etching selectivity of the first part 21 is greater than that of the second part 22. The first part 21 is the portion of the mask layer 2 closest to the substrate 1; that is, the closer to the substrate 1, the greater the etching selectivity of the mask layer 2. The first part 21 exhibits higher etching resistance, while the second part 22 is more easily etched.
[0047] For example, see [link to example]. Figure 2 A photoresist layer 4 is also formed on the side of the mask layer 2 away from the substrate 1. The photoresist layer 4 can be patterned by processes such as exposure and development. The patterned photoresist layer 4 can be used as a mask for etching the mask layer 2.
[0048] Step S2: See Figures 4-6The mask layer 2 is etched to form a first opening 20 penetrating the mask layer 2, exposing the substrate 1. Figure 6 for Figure 5 A magnified view of the mask layer 2 at point N.
[0049] For example, see Figure 4 The photoresist layer 4 can be patterned using processes such as exposure and development to form a through second opening 41 in the photoresist layer 4, which exposes the portion of the mask layer 2 that needs to be etched away.
[0050] Understandably, the first opening 20 of the required size can be formed on the mask layer 2 using only a single exposure process.
[0051] Next, see Figure 5 The mask layer 2 is etched through the second opening 41 to form a through first opening 20 in the mask layer 2. See also Figure 6 Since the first part 21 exhibits higher etching resistance, the second part 22 is more easily etched. Along the X direction, the width of the through first sub-opening 210 formed in the first part 2 is smaller than the width of the through second sub-opening 220 formed in the second part 22.
[0052] For example, see Figure 7 After etching the mask layer 2, the sacrificial layer 3 can be etched through the first opening 20 to form a through third opening 30 within the sacrificial layer 3. For example, along the plane XY, the size of the third opening 30 is the same as the size of the first sub-opening 210.
[0053] Step S3: See Figure 8 The substrate 1 is etched through the first opening 20 to form an opening 11 within the substrate 1, thereby forming a mask pattern transfer. The width H2 of the opening 11 along the X direction is the critical dimension (CD).
[0054] For example, see Figure 8 Along direction X, the width H1 of the second opening 41 can be 50nm, and the width H2 of the final formed opening 11 is approximately 37nm.
[0055] For example, see Figure 9 After forming the opening 11 in step S3 above, the photoresist layer 4, mask layer 2 and sacrificial layer 3 can be removed to form a substrate 1 with the opening 11.
[0056] For example, such as Figure 9 The semiconductor device 100 shown can be formed into a FinFET through subsequent processes. Alternatively, the embodiments of this disclosure are not limited to the type of semiconductor device 100, and any semiconductor device 100 with any structure is included within the scope of this disclosure.
[0057] For example, in subsequent processes, the opening 11 may be filled with semiconductor material, or it may be filled with electrode material, or it may not be filled with other materials. The embodiments of this disclosure do not limit the function of the opening 11.
[0058] The method for fabricating the semiconductor device 100 includes forming a mask layer 2 on a substrate 1. Along a first direction Z perpendicular to the substrate 1, the nitrogen content in the first portion 21 of the mask layer 2 closer to the substrate 1 is greater than the nitrogen content in the second portion 22 of the mask layer 2 farther from the substrate 1. Since a higher nitrogen content results in a higher etching selectivity, the etching selectivity of the first portion 21 is greater than that of the second portion 22. By setting the nitrogen content in the first portion 21 to be greater than that in the second portion 22, the etching selectivity of the mask layer 2 is greater the closer it is to the substrate 1.
[0059] Furthermore, the mask layer 2 is etched to form a first opening 20 penetrating the mask layer 2, exposing the substrate 1. The substrate 1 is etched through the first opening 20 to form an aperture 11 within the substrate 1, thereby achieving mask pattern transfer. Since the etching selectivity of the first portion 21 is greater than that of the second portion 22, during the etching of the mask layer 2, the size of the portion of the first opening 20 located in the first portion 21 is smaller than the size of the portion of the first opening 20 located in the second portion 22, thereby allowing a smaller aperture 11 to be formed within the substrate 1.
[0060] It is understood that in the above-described fabrication method, by adjusting the nitrogen content in different locations of the mask layer 2, the etching selectivity of the mask layer 2 at different locations is adjusted, thereby achieving a gradient change in the etching selectivity of the mask layer 2. This forms a first opening 20 with a gradually decreasing size in the mask layer 2, thereby forming a smaller aperture 11 in the substrate 1. Without affecting the controllability of the critical dimensions of the aperture 11, a smaller and higher-density semiconductor device 100 pattern structure can be achieved through only one etching of the mask layer 2, reducing fabrication costs and process complexity. Furthermore, compared to defects such as poor aperture morphology and polymer residue caused by multiple etching processes, the fabrication method disclosed herein also improves the aforementioned defects in the mask layer 2 pattern transfer process, improving the quality and structural reliability of the subsequently formed semiconductor device 100.
[0061] In some embodiments, see Figure 3 The difference between the nitrogen content in Part 1, 21 and the nitrogen content in Part 2, 22 is less than or equal to 25%.
[0062] For example, the difference between the nitrogen content in the first part 21 and the nitrogen content in the second part 22 can be 5%, 10%, 15%, 20%, or 25%.
[0063] For example, the nitrogen content in Part 1 21 can range from 20% to 30%, the nitrogen content in Part 2 22 can range from 5% to 10%, and the difference between the nitrogen content in Part 1 21 and Part 22 can range from 10% to 25%.
[0064] It is understandable that if the difference in nitrogen content between the first part 21 and the second part 22 is zero, the first part 21 with a relatively large etching selectivity cannot be formed, thus making it impossible to achieve the small size and high density of the opening 11. If the difference in nitrogen content between the first part 21 and the second part 22 is greater than 25%, it may lead to an excessively large etching selectivity of the first part 21, increasing the etching time for forming the first opening 20, and making it difficult to control the size of the first opening 20.
[0065] Therefore, by setting the difference in nitrogen content between the first part 21 and the second part 22 to be less than or equal to 25%, it is beneficial to shorten the fabrication cycle of the semiconductor device 100 and improve the controllability of the key dimensions of the opening 11 while achieving a smaller and denser patterned structure.
[0066] In some embodiments, see Figure 6 Along the first direction Z, the thickness d1 of the first part 21 is greater than or equal to the thickness d2 of the second part 22.
[0067] For example, along the first direction Z, the thickness d1 of the first part 21 can be 5nm, and the thickness d2 of the second part 22 can be 2nm.
[0068] It is understandable that by setting d1≥d2, and combining the etching selectivity of the first part 21 with that of the second part 22, the etching impedance of the first part 21 can be further improved, which is conducive to forming a first sub-aperture 210 with a smaller planar size. Thus, while ensuring the controllability of key dimensions, the planar size of the aperture 11 can be further reduced, which is conducive to further increasing the density of the pattern structure of the semiconductor device 100.
[0069] In some embodiments, see Figure 3 The mask layer 2 also includes a third part 23, which is disposed between the first part 21 and the second part 22 along the first direction Z. The nitrogen content in the third part 23 is greater than that in the second part 22 and less than that in the first part 21.
[0070] Understandably, along the direction -Z, perpendicular to substrate 1 and pointing from mask layer 2 to substrate 1, the nitrogen content in the second part 22, the third part 23, and the first part 21 gradually increases, and the etching selectivity of the second part 22, the third part 23, and the first part 21 gradually increases, further realizing a gradient change in the etching selectivity of mask layer 2. During the etching of mask layer 2 to form the first opening 20, the planar dimensions of the first opening 20 are gradually reduced, thereby increasing the smoothness of the sidewalls of the first opening 20, further improving the controllability of critical dimensions, and also contributing to increasing the structural reliability of the opening 11 formed after the pattern transfer process of mask layer 2, thereby further improving the quality and structural reliability of the subsequently formed semiconductor device 100.
[0071] In some embodiments, see Figure 3 The difference between the nitrogen content in Part 3, 23 and the nitrogen content in Part 2, 22 is less than or equal to 15%.
[0072] For example, the difference between the nitrogen content in the third part 23 and the nitrogen content in the second part 22 can be 1%, 5%, 7.5%, 12% or 15%.
[0073] For example, the nitrogen content in Part 3, Section 23 can range from 10% to 20%.
[0074] The difference between the nitrogen content in Part 1, 21 and the nitrogen content in Part 3, 23 is less than or equal to 20%.
[0075] For example, the difference between the nitrogen content in the first part 21 and the nitrogen content in the third part 23 can be 1%, 5%, 10%, 15% or 20%.
[0076] It is understandable that by setting the difference in nitrogen content between the third part 23 and the second part 22 to be less than or equal to 15%, and the difference in nitrogen content between the first part 21 and the third part 23 to be less than or equal to 20%, it is beneficial to further realize the gradient change of the etching selectivity of the mask layer 2. That is, the closer to the substrate 1, the greater the etching selectivity of the mask layer 2, thereby further improving the controllability of the critical dimensions.
[0077] In some embodiments, along the first direction Z, the thickness d3 of the third part 23 is greater than or equal to the thickness d2 of the second part 22, and less than or equal to the thickness d1 of the first part 21.
[0078] For example, along the first direction Z, the thickness d3 of the third part 23 can be 3nm.
[0079] It is understandable that by setting d1≥d3≥d2, and by gradually increasing the etching selectivity of the first part 21, the third part 23, and the second part 22, the etching resistance of the first part 21, the third part 23, and the second part 22 can be gradually increased, which is beneficial to forming a first sub-opening 210 with a smaller planar size and improving the controllability of critical dimensions.
[0080] In some embodiments, see Figures 2-7 The material of the mask layer 2 includes at least one of silicon nitride (Si3N4) and silicon oxynitride (SiCN).
[0081] For example, the material of mask layer 2 may also include any mask material containing nitrogen, and the material of mask layer 2 in this disclosure is not limited to silicon nitride and silicon oxynitride. For example, in the embodiments of this disclosure, silicon oxynitride is used as the material of mask layer 2 for illustrative purposes.
[0082] It is understandable that by setting the material of the mask layer 2 to at least one of silicon nitride and silicon oxynitride, the gradient distribution of nitrogen content in the mask layer 2 and its material composition can be adjusted to meet the structural requirements of different semiconductor devices 100, exhibiting good scalability. Furthermore, the creation of the opening 11 solely through the design of the mask layer 2 with a gradient change in etching selectivity and a single-exposure photoresist layer 4 process simplifies the fabrication process of the semiconductor device 100, improving production efficiency and equipment utilization while reducing fabrication costs.
[0083] In some embodiments, see Figure 2 and Figure 3 The step S1 above, forming a mask layer 2 on the substrate 1, includes: employing a deposition process and adjusting the process parameters of the deposition process to form the mask layer 2. Specifically, along the direction -Z, perpendicular to the substrate 1 and pointing from the mask layer 2 to the substrate 1, the nitrogen content in the mask layer 2 gradually increases.
[0084] For example, the mask layer 2 can be formed on the substrate 1 using atomic layer deposition (ALD) or chemical vapor deposition (CVD) processes.
[0085] For example, the process parameters of the above deposition process may include gas flow rate. The gas flow rate and / or gas ratio can be controlled by using a showerhead to optimize the composition distribution and density uniformity of the hard mask layer 2, thereby depositing a mask layer 2 with a reduced nitrogen content gradient on the substrate 1.
[0086] For example, the gas can be at least one of precursor gases such as SiH4, C2H2, and N2. By adjusting the flow rate and / or ratio of precursor gases such as SiH4, C2H2, and N2, a mask layer 2 with a gradually varying nitrogen content is formed.
[0087] For example, see Figure 3 The embodiments of this disclosure can adopt a sandwich structure of the first part 21, the third part 23 and the second part 22, or can adopt a superimposed design with more nitrogen element content gradient changes. Both can solve the problem that the traditional self-aligned dual patterning method is difficult to balance smaller spacing and design freedom in the same area of the substrate 1, and improve the density of semiconductor device 100.
[0088] For example, this disclosure, through the design of a mask layer 2 with a gradient etching selectivity ratio and a single-exposure photoresist layer 4 process, significantly reduces manufacturing costs and process complexity while ensuring high-quality fabrication of semiconductor devices, demonstrating promising industrialization prospects. Furthermore, the single-exposure photoresist layer 4 process and the mask layer 2 scheme with a gradient etching selectivity ratio offer significant cost advantages. Compared to related technologies that use SADP processes to form small-size, high-density openings within the substrate, the technical solution of this disclosure can reduce manufacturing costs by approximately 35% to 40%.
[0089] In some embodiments, see Figure 5 Along the direction -Z, which is perpendicular to the substrate 1 and points from the mask layer 2 to the substrate 1, the width of the first opening 20 gradually decreases.
[0090] For example, the width of the first opening 20 can be the size of the first opening 20 in the direction X.
[0091] For example, the cross-sectional shape of the first opening 20 can be an inverted trapezoid.
[0092] It is understandable that by adjusting the nitrogen content in different parts of the mask layer 2, the etching selectivity of the mask layer 2 at different locations is adjusted, thereby achieving a gradient change in the etching selectivity of the mask layer 2, so as to form a first opening 20 with a gradually decreasing width in the mask layer 2, that is, a first opening 20 with an inverted trapezoidal cross-sectional shape.
[0093] In some embodiments, before forming the mask layer 2 on the substrate 1 in step S1, the above preparation method further includes: experimentally adjusting the nitrogen content in the first part 21 and the second part 22 according to the size of the target opening 11.
[0094] Understandably, before forming the mask layer 2, the nitrogen content in the first part 21 and the second part 22 can be adjusted in advance according to the size of the target opening 11, so as to adjust the width of the first opening 20 and obtain the required nitrogen content in the first part 21 and the second part 22. Then, the mask layer 2 is formed according to the experimental data (i.e., the required nitrogen content in the first part 21 and the second part 22 obtained above), thereby achieving precise control over the size of the first opening 20.
[0095] On the other hand, see Figure 9 The present disclosure also provides a semiconductor device 100, which is prepared by the preparation method of the semiconductor device 100 in any of the above embodiments.
[0096] For example, the semiconductor device 100 may be a FinFET. Alternatively, the embodiments of this disclosure are not limited to the type of semiconductor device 100, and any semiconductor device 100 of any structure is included within the scope of this disclosure.
[0097] For example, the opening 11 can be a contact hole of the semiconductor device 100, or it can be a via with any function. The embodiments of this disclosure do not limit the function of the opening 11.
[0098] The above description is merely a specific embodiment of this disclosure, but the scope of protection of this disclosure is not limited thereto. Any variations or substitutions conceived by those skilled in the art within the scope of the technology disclosed in this disclosure should be included within the scope of protection of this disclosure. Therefore, the scope of protection of this disclosure should be determined by the scope of the claims.
Claims
1. A method for fabricating a semiconductor device, characterized in that, include: A mask layer is formed on the substrate; Along a first direction perpendicular to the substrate, the mask layer includes a first portion close to the substrate and a second portion away from the substrate, wherein the nitrogen content in the first portion is greater than the nitrogen content in the second portion; The mask layer is etched to form a first opening through the mask layer, the first opening exposing the substrate; The substrate is etched through the first opening to form an opening within the substrate.
2. The preparation method according to claim 1, characterized in that, The difference between the nitrogen content in the first part and the nitrogen content in the second part is less than or equal to 25%.
3. The preparation method according to claim 1, characterized in that, Along the first direction, the thickness of the first part is greater than or equal to the thickness of the second part.
4. The preparation method according to claim 1, characterized in that, The mask layer further includes a third part, which is disposed between the first part and the second part along the first direction; The nitrogen content in the third part is greater than the nitrogen content in the second part, but less than the nitrogen content in the first part.
5. The preparation method according to claim 4, characterized in that, The difference between the nitrogen content in the third part and the nitrogen content in the second part is less than or equal to 15%. The difference between the nitrogen content in the first part and the nitrogen content in the third part is less than or equal to 20%.
6. The preparation method according to claim 4, characterized in that, Along the first direction, the thickness of the third part is greater than or equal to the thickness of the second part, and less than or equal to the thickness of the first part.
7. The preparation method according to claim 1, characterized in that, The material of the mask layer includes at least one of silicon nitride and silicon oxynitride.
8. The preparation method according to any one of claims 1 to 7, characterized in that, The process of forming a mask layer on the substrate includes: A deposition process is employed, and the process parameters of the deposition process are adjusted to form the mask layer; The nitrogen content in the mask layer gradually increases along a direction perpendicular to the substrate and pointing from the mask layer to the substrate.
9. The preparation method according to claim 8, characterized in that, Along a direction perpendicular to the substrate and pointing from the mask layer to the substrate, the width of the first opening gradually decreases.
10. The preparation method according to claim 1, characterized in that, Before forming the mask layer on the substrate, the preparation method further includes: The nitrogen content in the first and second parts was experimentally adjusted according to the size of the opening described in the target.
11. A semiconductor device, characterized in that, It is prepared by the preparation method according to any one of claims 1 to 10.