Semiconductor wafers and their fabrication methods

By inserting a nitrogen-containing dielectric layer between polysilicon layers, the problem of polysilicon grain coarsening at high temperatures is solved by utilizing the diffusion of nitrogen and its interaction with the polysilicon layers, thus achieving high impedance characteristics and performance maintenance of RF devices.

CN123124777APending Publication Date: 2026-11-17XIAN ESWIN MATERIAL TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611235677.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-14
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the manufacturing of radio frequency devices, the grains of the polycrystalline silicon charge cutoff layer coarsen during high-temperature growth and thermal processes, resulting in a reduction in the number of effective capture grain boundaries, which affects the high-resistivity characteristics and performance of radio frequency devices.

Method used

By inserting a nitrogen-containing dielectric layer between polycrystalline silicon layers and utilizing the interaction between nitrogen diffusion and the polycrystalline silicon layers, the grain size of polycrystalline silicon can be controlled within the range of 50nm to 100nm through the synergistic effect of layered growth and nitrogen diffusion, thus suppressing grain coarsening.

Benefits of technology

It effectively improves the carrier trapping capability of the charge cutoff layer, slows down the decrease in the effective resistivity of the semiconductor wafer, and maintains the high-resistivity characteristics of the RF device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124777A_ABST
    Figure CN123124777A_ABST
Patent Text Reader

Abstract

This application provides a semiconductor wafer and a method for fabricating the same. The semiconductor wafer includes: a monocrystalline silicon substrate; a first polycrystalline silicon layer disposed on one side of the monocrystalline silicon substrate; a dielectric layer disposed on the side of the first polycrystalline silicon layer away from the monocrystalline silicon substrate and containing silicon, oxygen, and nitrogen; and a second polycrystalline silicon layer disposed on the side of the dielectric layer away from the first polycrystalline silicon layer. Both the first and second polycrystalline silicon layers contain nitrogen. The nitrogen concentration in the dielectric layer is higher than that in both the first and second polycrystalline silicon layers. The nitrogen concentration in the first polycrystalline silicon layer decreases from the interface between the first polycrystalline silicon layer and the dielectric layer in a direction away from the dielectric layer. The nitrogen concentration in the second polycrystalline silicon layer also decreases from the interface between the second polycrystalline silicon layer and the dielectric layer in a direction away from the dielectric layer. The grain size of the polycrystalline silicon grains in both the first and second polycrystalline silicon layers is in the range of 50 nm to 100 nm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of semiconductor manufacturing technology, and in particular to semiconductor wafers and methods for their fabrication. Background Technology

[0002] In the manufacturing of radio frequency devices, a polycrystalline silicon charge cutoff layer needs to be deposited on the surface of a high-resistivity single-crystal silicon substrate to reduce the accumulation of free carriers in the substrate, thereby maintaining the high-resistivity characteristics of the substrate and reducing the loss of radio frequency signals.

[0003] In related technologies, polycrystalline silicon charge cutoff layers are typically grown to the target thickness in a single process using chemical vapor deposition. Due to the high growth temperature and long growth time of polycrystalline silicon, grain coarsening occurs during the growth process and subsequent thermal processing. This leads to a reduction in the number of effectively trapped grain boundaries in the charge cutoff layer, resulting in a decrease in the high-resistivity characteristics of the substrate and consequently affecting the performance of RF devices. Summary of the Invention

[0004] This application provides a semiconductor wafer and a method for fabricating the same; by inserting a nitrogen-containing dielectric layer between two polysilicon layers, nitrogen diffuses from the dielectric layer to the polysilicon layers on both sides and interacts with vacancies, defects or grain boundaries in the polysilicon, thereby suppressing the coarsening of polysilicon grains and controlling the grain size of the polysilicon charge cutoff layer within the range of 50 nm to 100 nm.

[0005] This application provides a semiconductor wafer in one aspect. The semiconductor wafer includes: a monocrystalline silicon substrate, a first polycrystalline silicon layer, a dielectric layer, and a second polycrystalline silicon layer. The first polycrystalline silicon layer is disposed on one side of the monocrystalline silicon substrate. The dielectric layer is disposed on the side of the first polycrystalline silicon layer away from the monocrystalline silicon substrate and contains silicon, oxygen, and nitrogen. The second polycrystalline silicon layer is disposed on the side of the dielectric layer away from the first polycrystalline silicon layer. Both the first and second polycrystalline silicon layers contain nitrogen, with the nitrogen concentration in the dielectric layer being higher than and higher than the nitrogen concentration in the first and second polycrystalline silicon layers, respectively. The nitrogen concentration in the first polycrystalline silicon layer decreases from the interface between the first polycrystalline silicon layer and the dielectric layer in a direction away from the dielectric layer. The nitrogen concentration in the second polycrystalline silicon layer decreases from the interface between the second polycrystalline silicon layer and the dielectric layer in a direction away from the dielectric layer. The grain size of the polycrystalline silicon grains in the first and second polycrystalline silicon layers is in the range of 50 nm to 100 nm.

[0006] This application provides, in another aspect, a method for fabricating a semiconductor wafer. The method includes: depositing a first polycrystalline silicon layer on a single-crystal silicon substrate; depositing a dielectric layer on the first polycrystalline silicon layer, the dielectric layer comprising silicon, oxygen, and nitrogen elements, wherein the nitrogen concentration in the dielectric layer is higher than the nitrogen concentration in the first polycrystalline silicon layer; and depositing a second polycrystalline silicon layer on the dielectric layer at a temperature of 600°C to 1100°C, thereby allowing nitrogen elements in the dielectric layer to diffuse into both the first and second polycrystalline silicon layers. The nitrogen concentration in the first polycrystalline silicon layer decreases from the interface between the first polycrystalline silicon layer and the dielectric layer in a direction away from the dielectric layer. The nitrogen concentration in the second polycrystalline silicon layer decreases from the interface between the second polycrystalline silicon layer and the dielectric layer in a direction away from the dielectric layer. The grain size of the polycrystalline silicon grains in the first and second polycrystalline silicon layers is in the range of 50 nm to 100 nm.

[0007] This application provides a semiconductor wafer and a method for fabricating the same. According to embodiments of this application, by introducing a nitrogen-containing dielectric layer between a first polysilicon layer and a second polysilicon layer, on the one hand, the physical barrier effect of the dielectric layer allows the second polysilicon layer to re-nucleate on the surface of the dielectric layer, preventing grain growth along existing nuclei in the first polysilicon layer; on the other hand, nitrogen in the dielectric layer diffuses into both the first and second polysilicon layers under the drive of a concentration gradient. The nitrogen interacts with vacancies, defects, or grain boundaries in the polysilicon lattice, reducing the degree of vacancy and grain boundary migration. Based on these two aspects, the coarsening of polysilicon grains can be effectively suppressed through the synergistic effect of physical barrier and nitrogen diffusion, controlling the grain size within the range of 50nm to 100nm, increasing the density of effectively captured grain boundaries in the charge cutoff layer, helping to mitigate the decrease in the effective resistivity of the semiconductor wafer after thermal processing, and maintaining the high resistivity characteristics of the semiconductor wafer in radio frequency device applications. Attached Figure Description

[0008] Figure 1 This is a schematic diagram illustrating the coarsening process of polycrystalline silicon grains during thermal processing in related technologies.

[0009] Figure 2 This is a schematic diagram of a semiconductor wafer cross-section provided in an embodiment of this application.

[0010] Figure 3 This is a schematic diagram showing the distribution of nitrogen concentration with depth, provided in an embodiment of this application.

[0011] Figure 4 This is a schematic diagram illustrating the microscopic mechanism by which nitrogen element inhibits the coarsening of polycrystalline silicon grains in the embodiments of this application.

[0012] Figure 5 This is a flowchart of a semiconductor wafer fabrication method provided in an embodiment of this application.

[0013] Figure 6This is a SEM image of the cross-section of polycrystalline silicon grains after heat treatment in Example 1.

[0014] Figure 7 This is a SEM image of the cross-section of polycrystalline silicon grains after heat treatment in Example 2.

[0015] Figure 8 This is a SEM image of the cross-section of polycrystalline silicon grains after heat treatment in Example 3.

[0016] Figure 9 This is a SEM image of the cross-section of polycrystalline silicon grains after heat treatment in Example 4.

[0017] Figure 10 The image shows a cross-sectional SEM image of the polycrystalline silicon grains after heat treatment in Comparative Example 1.

[0018] Figure 11 This is a SEM image of the cross-section of polycrystalline silicon grains after heat treatment, as shown in Comparative Example 2.

[0019] Figure 12 The image shows a cross-sectional SEM image of the polycrystalline silicon grains after heat treatment in Comparative Example 3.

[0020] Figure 13 A graph showing the variation of polysilicon layer thickness with the measurement position along the wafer diameter direction for a polysilicon structure without a nitrogen-containing dielectric layer.

[0021] Figure 14 A graph showing the variation of the polysilicon layer thickness with the measurement position along the wafer diameter direction in the first polysilicon layer / nitrogen-containing dielectric layer / second polysilicon layer structure provided in the embodiments of this application. Detailed Implementation

[0022] The technical solutions in this application will now be clearly and completely described with reference to the accompanying drawings.

[0023] In the fabrication of radio frequency (RF) devices, the devices are typically fabricated on silicon-on-insulator (SOI) structures or high-resistivity single-crystal silicon substrates. To enable the substrate to effectively cut off charges, reduce parasitic capacitance, and lower the nonlinear distortion of RF signals, a polycrystalline silicon charge cutoff layer with grain boundary defects needs to be deposited on the surface of the single-crystal silicon substrate.

[0024] Polycrystalline silicon is composed of many fine grains. The grain boundary regions between the grains contain many dangling bonds and other lattice defects. These defects can capture and fix the free carriers generated or injected in the monocrystalline silicon substrate when the semiconductor device is working, thereby preventing the free carriers from accumulating in the monocrystalline silicon substrate and forming conductive channels, thus maintaining the high resistance characteristics of the substrate.

[0025] In fact, the number of effectively captured grain boundaries is related to the grain size. In polycrystalline silicon thin films of the same volume, the smaller the grain size, the larger the total grain boundary area, the more sites that can capture charge carriers, and the better the charge cutoff effect. Conversely, the larger the grains, the sparser the grain boundaries, and the worse the cutoff effect. Therefore, controlling the grain size in the polycrystalline silicon charge cutoff layer to a small range is a key technical goal for improving the high resistivity performance of the substrate.

[0026] See Figure 1 , Figure 1 The diagram illustrates the grain coarsening process of polycrystalline silicon grains before, during, and after the thermal processing in related technologies. Before the thermal processing, the grains in the polycrystalline silicon charge-stop layer are relatively small and densely distributed, with numerous grain boundaries forming between adjacent grains. During the thermal processing, under high temperatures, some small grains gradually disappear, adjacent grains merge or grow, and the number of grain boundaries begins to decrease. After the thermal processing, the polycrystalline silicon grains further coarsen, the grain size increases, and the number of grain boundaries per unit area decreases significantly.

[0027] In related technologies, polycrystalline silicon charge-stop layers are typically deposited in a single step to a target thickness, such as approximately 2.5 μm, using atmospheric pressure chemical vapor deposition (APCVD) or low pressure chemical vapor deposition (LPCVD) processes. Because a large thickness needs to be grown in one step, the wafer is exposed to high-temperature environments for extended periods during the growth process, such as temperatures between 600°C and 1100°C. These high temperatures promote the coarsening of the polycrystalline silicon grains.

[0028] The coarsening of polycrystalline silicon grains is due to the tendency of polycrystalline silicon thin films to reduce the total energy of the system. When the grain size is small, the total grain boundary area per unit volume is large, and the grain boundary energy in the system is high. Under the aforementioned high-temperature conditions, some small grains are in a relatively unstable state and tend to gradually disappear; adjacent grains will merge or grow to reduce the total grain boundary area and lower the total energy of the system. As this process continues, the grain size in the polycrystalline silicon charge-stop layer continuously increases. For example, in related technologies, the grain size of polycrystalline silicon charge-stop layers directly grown may reach 250 nm to 500 nm after thermal processing.

[0029] Grain coarsening reduces the number of effectively trapped grain boundaries per unit area. This decreases the charge cutoff layer's ability to block charge carriers, shrinking the effective high-resistivity range of the single-crystal silicon substrate. Ultimately, this leads to performance degradation in RF devices fabricated on this substrate, such as increased harmonic distortion and insertion loss.

[0030] See Figure 2 This application provides a semiconductor wafer 10. Along... Figure 2The semiconductor wafer, shown in the top-down direction, comprises, in sequence: a single-crystal silicon substrate 100, a first polycrystalline silicon layer 110, a dielectric layer 120, and a second polycrystalline silicon layer 130.

[0031] In this embodiment, a dielectric layer 120 containing silicon, oxygen, and nitrogen is disposed between the first polysilicon layer 110 and the second polysilicon layer 130. Through the synergistic effect of the layered growth forced independent nucleation mechanism and the nitrogen diffusion inhibition grain coarsening mechanism, the polysilicon grain size in the first polysilicon layer 110 and the second polysilicon layer 130 can be controlled within the range of 50 nm to 100 nm.

[0032] The single-crystal silicon substrate 100 can be a high-resistivity single-crystal silicon substrate for radio frequency devices. For example, the bulk resistivity of the single-crystal silicon substrate 100 is not less than 1000 Ω·cm to ensure that the radio frequency devices manufactured subsequently have sufficiently low substrate losses. The crystal orientation of the single-crystal silicon substrate 100 can be (100), (110), or (111), and the specific crystal orientation can be selected according to the device process requirements. This application embodiment does not limit this.

[0033] See Figure 2 A first polysilicon layer 110 is disposed on one side of the monocrystalline silicon substrate 100 as a first charge cutoff layer. For example, the thickness of the first polysilicon layer 110 is in the range of 0.5 μm to 1.5 μm.

[0034] By controlling the thickness of the first polysilicon layer 110 to within 1.5 μm, it is beneficial to keep the monolayer growth time within a reasonable range and reduce the risk of excessive grain growth during deposition. The lower limit of the thickness of the first polysilicon layer 110 is 0.5 μm, so that it has a certain grain boundary capture density and can function as a first charge cutoff layer.

[0035] The first polysilicon layer 110 contains nitrogen, which diffuses from the dielectric layer 120. The nitrogen concentration in the first polysilicon layer 110 decreases from the interface between the first polysilicon layer 110 and the dielectric layer 120 away from the dielectric layer 120; that is, the nitrogen concentration is higher on the side closer to the dielectric layer 120 and lower on the side farther away from the dielectric layer 120. This nitrogen concentration gradient distribution can be characterized, for example, by a secondary ion mass spectrometry (SIMS) depth profiling method.

[0036] See Figure 2 and Figure 3 The dielectric layer 120 is disposed on the side of the first polysilicon layer 110 away from the monocrystalline silicon substrate 100. The dielectric layer 120 contains silicon, oxygen, and nitrogen. The concentration of nitrogen in the dielectric layer 120 is higher than the concentration of nitrogen in the first polysilicon layer 110.

[0037] The dielectric layer 120 can serve as a physical barrier layer. The material structure of the dielectric layer 120 differs from that of polysilicon, causing the growth of the second polysilicon layer 130 on the surface of the dielectric layer 120 to no longer extend continuously along the existing grains in the first polysilicon layer 110, but to re-nucleate on the surface of the dielectric layer 120, thereby helping to reduce the degree of continuous grain growth.

[0038] Additionally, the dielectric layer 120 can also be used to provide nitrogen. The nitrogen concentration in the dielectric layer 120 is higher than that in the first polysilicon layer 110 and higher than that in the second polysilicon layer 130. Under the deposition temperature of the second polysilicon layer 130, nitrogen diffuses into both the first polysilicon layer 110 and the second polysilicon layer 130 driven by the concentration gradient, so that both polysilicon layers contain nitrogen.

[0039] It should be noted that the introduction of dielectric layer 120 causes a discontinuity between the first polysilicon layer 110 and the second polysilicon layer 130 in the stacking direction. In charge-stopping layer applications, this discontinuity does not weaken the charge-stopping function. This is because dielectric layer 120 itself is an insulating material. The presence of dielectric layer 120 increases the longitudinal resistivity of the stacked structure, helping to maintain the high-resistivity characteristics of the semiconductor wafer. Furthermore, interface defects exist at the heterogeneous interfaces formed between the first polysilicon layer 110 and dielectric layer 120, and between dielectric layer 120 and second polysilicon layer 130. These interface defects can also trap free carriers, similar to the effect of grain boundary defects.

[0040] In addition, by controlling the thickness of the dielectric layer 120 within the range of 0.5nm to 20nm, the interfacial stress caused by the difference in thermal expansion coefficients between the dielectric layer 120 and the polysilicon layer can be controlled within the allowable range of the process, thus avoiding wafer warping.

[0041] In this embodiment, the dielectric layer 120 can be made of silicon oxynitride. The silicon oxynitride film contains both silicon-oxygen bonds (Si-O) and silicon-nitrogen bonds (Si-N). The introduction of nitrogen gives the film a higher nitrogen content than pure silicon dioxide films, thereby providing sufficient nitrogen source driving force for subsequent nitrogen diffusion.

[0042] The thickness of the dielectric layer 120 is, for example, in the range of 0.5 nm to 20 nm. Setting the lower limit of the dielectric layer 120 thickness to 0.5 nm is beneficial for the dielectric layer 120 to form a continuous cover on the surface of the first polysilicon layer 110 and to play a physical isolation role. Setting the upper limit of the dielectric layer 120 thickness to 20 nm is beneficial to reduce the risk of the dielectric layer 120 introducing excessive thin film stress in the overall stack-up structure, and to avoid reliability problems such as wafer warpage or interlayer cracking caused by stress concentration.

[0043] In some embodiments, the thickness of the dielectric layer 120 is set to 1 nm to 10 nm. Atomic force microscopy (AFM) measurements show that the surface elevation difference of the first polysilicon layer 110 after deposition is within the range of 1 nm to 10 nm. Setting the thickness of the dielectric layer 120 to 1 nm to 10 nm facilitates the covering of the surface undulations of the first polysilicon layer 110 by the dielectric layer 120, thereby improving the continuity of the dielectric layer 120's coverage on the surface of the first polysilicon layer 110. Thus, the dielectric layer 120 can effectively function as a separator between the first polysilicon layer 110 and the second polysilicon layer 130, and as a source of nitrogen for both polysilicon layers.

[0044] See Figure 3 , Figure 3 The diagram schematically illustrates the distribution of nitrogen concentration with depth. In a direction perpendicular to the surface of the monocrystalline silicon substrate 100, the nitrogen concentration in the dielectric layer 120 is higher than that in the first polycrystalline silicon layer 110, and also higher than that in the second polycrystalline silicon layer 130. Nitrogen diffuses from the dielectric layer 120 into both the first and second polycrystalline silicon layers 110 and 130, resulting in nitrogen content in both layers. The nitrogen concentration in the first polycrystalline silicon layer 110 decreases from the interface between the first polycrystalline silicon layer 110 and the dielectric layer 120 in a direction away from the dielectric layer 120. The nitrogen concentration in the second polycrystalline silicon layer 130 also decreases from the interface between the second polycrystalline silicon layer 130 and the dielectric layer 120 in a direction away from the dielectric layer 120. This nitrogen concentration distribution can be characterized, for example, by secondary ion mass spectrometry depth profiling.

[0045] See Figure 2 The second polysilicon layer 130 is disposed on the side of the dielectric layer 120 away from the first polysilicon layer 110, serving as a second charge-blocking layer. The thickness of the second polysilicon layer 130 is, for example, in the range of 0.5 μm to 1.5 μm. The considerations for setting this thickness range are the same as those for the first polysilicon layer 110.

[0046] The second polysilicon layer 130 contains nitrogen, which also originates from nitrogen diffusion in the dielectric layer 120. The nitrogen concentration in the second polysilicon layer 130 decreases from the interface between the second polysilicon layer 130 and the dielectric layer 120 in a direction away from the dielectric layer 120.

[0047] The grain size of the polysilicon grains in the first polysilicon layer 110 and the second polysilicon layer 130 is in the range of 50 nm to 100 nm. This grain size can be observed and measured using a scanning electron microscope (SEM). The grain size range described in this application refers to the distribution range of grain sizes obtained by observing and measuring the grains in the polysilicon layer using a scanning electron microscope. For example, a grain size range of 50 nm to 100 nm means that the size distribution of the polysilicon grains obtained through the above observation and measurement is within the range of 50 nm to 100 nm.

[0048] Compared to polysilicon charge-stop layers grown directly in related technologies, the embodiments of this application can control the polysilicon grain size in the first polysilicon layer 110 and the second polysilicon layer 130 within the range of 50nm to 100nm. Due to the reduced grain size, the number of grain boundaries per unit area increases, and the polysilicon charge-stop layer can provide more grain boundary defect sites for capturing charge carriers. This improves the charge-stop layer's ability to capture charge carriers, slows down the decrease in the effective resistivity of the semiconductor wafer after thermal processing, and maintains its high-resistivity characteristics in radio frequency device applications. See also Figure 4 In this embodiment of the application, nitrogen element in dielectric layer 120 diffuses into first polysilicon layer 110 and second polysilicon layer 130, and the interaction between nitrogen element and vacancies, defects or grain boundaries is utilized to suppress the continuous coarsening of polysilicon grains at high temperature.

[0049] Specifically, vacancy migration is one of the key factors promoting grain coarsening in polycrystalline silicon. In the absence of nitrogen, vacancies in the polycrystalline silicon lattice at high temperatures have high migration capacity, easily accumulating near grain boundaries and forming migration paths. Based on thermodynamic principles, smaller grains, due to their larger specific surface area, are in a higher energy state and tend to gradually dissolve. The released silicon atoms migrate to neighboring larger grains and deposit on their surfaces, leading to the continuous growth of larger grains and the gradual disappearance of smaller grains.

[0050] In the presence of nitrogen, nitrogen atoms from the dielectric layer 120 diffuse into the polycrystalline silicon lattice and can occupy positions within the lattice or interact with vacancies and defects. Consequently, nitrogen atoms reduce the continuity of vacancy migration and hinder grain boundary migration, thus reducing the dissolution rate of small grains. With vacancy and grain boundary migration suppressed, the migration flux of silicon atoms available for the continued growth of large grains decreases, the coarsening rate of polycrystalline silicon grains decreases, and the grain size is maintained during the thermal process. This helps to maintain the grain size of polycrystalline silicon grains in the first polycrystalline silicon layer 110 and the second polycrystalline silicon layer 130 within the range of 50 nm to 100 nm after heat treatment.

[0051] See Figure 5 This application also provides a method for preparing a semiconductor wafer, which includes steps S100 to S160. The following will describe the structural features and preparation method in an integrated manner.

[0052] In step S100, a single-crystal silicon substrate 100 is prepared. The single-crystal silicon substrate 100 can be a high-resistivity single-crystal silicon substrate for radio frequency devices. For example, the bulk resistivity of the single-crystal silicon substrate 100 is not less than 1000 Ω·cm. The crystal orientation of the single-crystal silicon substrate 100 can be (100), (110) or (111), which is not limited in this embodiment.

[0053] Before depositing the polycrystalline silicon charge cutoff layer, the monocrystalline silicon substrate 100 needs to be cleaned to remove organic contaminants, metal ions, and the native oxide layer from its surface, ensuring that the subsequently deposited first polycrystalline silicon layer 110 can nucleate and grow on a clean silicon surface. The cleaning process can employ a standard RCA cleaning procedure, including SC-1 and SC-2 cleaning steps. After cleaning, the substrate is rinsed with deionized water and dried with nitrogen. The specific cleaning process can be adjusted according to actual process requirements; this application does not limit the specific method of the cleaning process.

[0054] In step S120, after cleaning and preparing the monocrystalline silicon substrate 100, a first polycrystalline silicon layer 110 is deposited on the monocrystalline silicon substrate 100. The first polycrystalline silicon layer 110 serves as a first charge cutoff layer.

[0055] The first polycrystalline silicon layer 110 is deposited using a chemical vapor deposition process, specifically APCVD or LPCVD. During the deposition of the first polycrystalline silicon layer 110, the silicon source gas used includes trichlorosilane (TCS, chemical formula SiHCl3), and the carrier gas includes hydrogen (H2). Trichlorosilane undergoes a thermal decomposition reaction at high temperature, depositing silicon atoms onto the surface of the monocrystalline silicon substrate 100, thereby forming a polycrystalline silicon thin film. Hydrogen, as the carrier gas, not only dilutes the silicon source gas and regulates the deposition rate, but also plays a role in reducing and cleaning the surface of the monocrystalline silicon substrate 100 during the deposition process, which is beneficial for obtaining a pure polycrystalline silicon thin film.

[0056] The process parameters for depositing the first polysilicon layer 110 can be set, for example, as follows: deposition temperature of 600°C to 1100°C, pressure of 10 Pa to 100 Pa, and growth time of 10 seconds to 240 seconds. Under these process parameters, the thickness of the first polysilicon layer 110 is deposited to be 0.5 μm to 1.5 μm. When the deposition temperature is higher than 1100°C, the deposition rate of polysilicon increases, and the nucleation and growth rate of grains accelerates significantly, which is not conducive to controlling the grain size in the first polysilicon layer 110 within the target range. Therefore, 1100°C is determined as the upper limit of the temperature for depositing the first polysilicon layer 110.

[0057] After the first polysilicon layer 110 is deposited, fine grains formed inside the first polysilicon layer 110 by multiple nucleation processes are formed. The grain size is kept within a small range due to the constraint of the single-layer growth time. The formation of the first polysilicon layer 110 provides a relatively flat and clean growth surface for the subsequent deposition of the dielectric layer 120.

[0058] It is understood that, in addition to trichlorosilane, silicon source gases can also include silane (SiH4), dichlorosilane (DCS, chemical formula SiH2Cl2), or silicon tetrachloride (SiCl4). Different silicon source gases have different thermal decomposition temperatures and deposition rates, and can be selected according to specific process equipment and process requirements. The specific composition of the gas system used in this application embodiment is not limited.

[0059] In step S140, after the first polysilicon layer 110 is deposited, a dielectric layer 120 is deposited on the first polysilicon layer 110. The dielectric layer 120 contains silicon, oxygen and nitrogen elements, and the concentration of nitrogen element in the dielectric layer 120 is higher than the concentration of nitrogen element in the first polysilicon layer 110.

[0060] Since no nitrogen source is introduced during the deposition of the first polysilicon layer 110, the initial nitrogen concentration of the first polysilicon layer 110 is essentially zero. By adjusting the atmospheric composition during the deposition of the dielectric layer 120, such as adjusting the ratio of N2O to ammonia, the nitrogen content in the dielectric layer 120 can be directly controlled, making the nitrogen concentration in the dielectric layer 120 higher than that in the first polysilicon layer 110, thereby establishing a concentration gradient that drives the diffusion of nitrogen from the dielectric layer 120 to the first polysilicon layer 110.

[0061] In this embodiment, the dielectric layer 120 is made of silicon oxynitride. The deposition process for the dielectric layer 120 can employ LPCVD, with the deposition temperature set to 800°C to 1000°C. It is understood that the deposition process can also employ plasma-enhanced chemical vapor deposition (PECVD), in which case the deposition temperature can be reduced to 300°C to 400°C. Low-temperature PECVD helps reduce thermal disturbance to the grain structure of the deposited first polycrystalline silicon layer 110 and is suitable for processes with strict thermal budget requirements. This embodiment does not limit the specific type of deposition process.

[0062] When depositing the dielectric layer 120, a mixed atmosphere containing nitrous oxide (N2O) and ammonia (NH3) can be used. N2O, as the main reactant gas, provides both oxygen and nitrogen atoms during decomposition, participating in the formation of the silicon oxynitride film. Introducing a small amount of ammonia into the N2O layer provides a nitrogen source during decomposition, working synergistically with N2O to further increase the nitrogen content in the silicon oxynitride film. This establishes a larger nitrogen concentration gradient between the dielectric layer 120 and the two adjacent polycrystalline silicon layers, enhancing the diffusion driving force of nitrogen to the polycrystalline silicon layers. The specific composition of the atmosphere used for depositing the dielectric layer 120 is not limited in this embodiment.

[0063] The thickness of the dielectric layer 120 is controlled, for example, in the range of 0.5 nm to 20 nm.

[0064] During the deposition of dielectric layer 120, the deposition temperature is between 300℃ and 1000℃. As dielectric layer 120 is formed, nitrogen begins to diffuse into the already deposited first polycrystalline silicon layer 110. Due to the short deposition time of dielectric layer 120, the amount of nitrogen diffused into the first polycrystalline silicon layer 110 during this stage is relatively limited, mainly serving to initially establish a concentration gradient.

[0065] In step S160, after the dielectric layer 120 is deposited, a second polysilicon layer 130 is deposited on the dielectric layer 120 at a temperature of 600°C to 1100°C. The second polysilicon layer 130 serves as a second charge cutoff layer.

[0066] Because the material structure of the dielectric layer 120 differs from that of polysilicon, the growth of the second polysilicon layer 130 on the surface of the dielectric layer 120 no longer extends continuously along the existing grains in the first polysilicon layer 110, but can re-nucleate on the surface of the dielectric layer 120, which helps to reduce the degree of continuous grain growth.

[0067] The deposition of the second polysilicon layer 130 is the main stage of nitrogen diffusion from the dielectric layer 120 to the polysilicon layers on both sides. At deposition temperatures between 600°C and 1100°C, the dielectric layer 120 is fully formed, the total nitrogen source is sufficient, and the high-temperature environment provides thermal activation energy for nitrogen atoms. Driven by the concentration gradient, nitrogen atoms diffuse simultaneously in two directions. Specifically, they enter the first polysilicon layer 110, replenishing the diffusion amount in step S140 and further deepening the nitrogen concentration gradient in the first polysilicon layer 110; they enter the growing second polysilicon layer 130, continuously diffusing into the newly deposited polysilicon as the thickness of the second polysilicon layer 130 increases, establishing a nitrogen concentration gradient decreasing from the interface outwards in the second polysilicon layer 130.

[0068] Since the nitrogen concentration of the second polysilicon layer 130 is zero at the initial deposition time, and the nitrogen concentration in the dielectric layer 120 is higher than that in the second polysilicon layer 130, the diffusion of nitrogen from the dielectric layer 120 to the second polysilicon layer 130 during the deposition of the second polysilicon layer 130 is determined by the process timing and does not require additional settings.

[0069] Below 600℃, during the deposition of the second polysilicon layer, the diffusion of nitrogen from the dielectric layer to both the first and second polysilicon layers is minimal, which is detrimental to forming the required nitrogen concentration gradient between the two polysilicon layers and thus hinders the suppression of polysilicon grain coarsening. Therefore, 600℃ was determined as the lower limit of the deposition temperature for the second polysilicon layer. The experimental results of Comparative Example 3 below further illustrate this point.

[0070] The upper temperature limit for depositing the second polysilicon layer 130 is primarily based on considerations of film quality. Above 1100℃, the deposition rate of polysilicon increases, the nucleation and growth processes become too rapid, the growth of the second polysilicon layer 130 on the surface of the dielectric layer 120 tends to be uneven, the film density decreases, making it difficult to form a uniform coverage of the dielectric layer 120, and there is a risk of voids forming between the dielectric layer 120 and the second polysilicon layer 130. Furthermore, there is a difference in the coefficient of thermal expansion between the dielectric layer 120 and the polysilicon layer. When the deposition temperature is too high, the thermal stress accumulated during the growth of the second polysilicon layer 130 increases, posing a risk of interlayer delamination between the second polysilicon layer 130 and the dielectric layer 120. These voids and interlayer delamination will disrupt the continuous interface between the dielectric layer 120 and the second polysilicon layer 130, hindering the uniform diffusion of nitrogen from the dielectric layer 120 to the second polysilicon layer 130. For these reasons, 1100℃ is determined as the upper temperature limit for depositing the second polysilicon layer 130.

[0071] The deposition pressure of the second polysilicon layer 130 is 10 Pa to 100 Pa, the growth time is 10 seconds to 240 seconds, the silicon source gas includes trichlorosilane, the carrier gas includes hydrogen, and the deposition method can be APCVD or LPCVD. Under the above process parameters, the thickness of the second polysilicon layer 130 is deposited to 0.5 μm to 1.5 μm.

[0072] Nitrogen diffusion can be roughly divided into three stages. Specifically, during the deposition of the dielectric layer 120, nitrogen begins to diffuse unidirectionally towards the first polysilicon layer 110, but to a limited extent. During the deposition of the second polysilicon layer 130, nitrogen diffuses bidirectionally towards both the first and second polysilicon layers 110 and 130 simultaneously under a temperature range of 600°C to 1100°C; this is the main stage of nitrogen diffusion. In subsequent thermal processes, nitrogen continues to diffuse towards both polysilicon layers, further consolidating the nitrogen concentration gradient and continuing to suppress grain coarsening.

[0073] In the above process, after nitrogen diffuses into the polycrystalline silicon layer, it can occupy a position in the polycrystalline silicon lattice or interact with vacancies and defects, thereby reducing the degree of vacancy migration and grain boundary migration, suppressing the continuous coarsening of polycrystalline silicon grains in the thermal process, and helping to maintain the grain size of polycrystalline silicon grains in the first polycrystalline silicon layer 110 and the second polycrystalline silicon layer 130 in the range of 50nm to 100nm.

[0074] After completing step S160, the first polysilicon layer 110, the dielectric layer 120, and the second polysilicon layer 130 can be heat-treated at a temperature of 750°C to 1100°C. This heat treatment step can be an independently set annealing step or an inherent thermal process step in subsequent process flows. It can be understood that step S180 is an optional step. Without setting an independent heat treatment step, various thermal processes in subsequent processes can also drive nitrogen to diffuse from the dielectric layer 120 to the polysilicon layers on both sides, achieving the technical effects of the embodiments of this application.

[0075] Examples and Comparative Examples To verify the technical effectiveness of the semiconductor wafer fabrication method provided in this application, the following examples and comparative experiments were designed. All samples used a single-crystal silicon substrate with a resistivity of 1000 Ω·cm and a crystal orientation of (100). After deposition, the substrate was heat-treated at 1100°C for 11 hours to simulate the thermal process environment that may be experienced in subsequent processes. After heat treatment, the grain size of the polycrystalline silicon was observed and measured by cross-sectional SEM. The grain size ranges described in each example and comparative example are the grain size distribution ranges of the corresponding samples obtained by the above measurements. The effective resistivity of the semiconductor wafer was also tested.

[0076] Example 1 Example 1 uses the preparation method provided in the embodiments of this application to sequentially deposit a first polycrystalline silicon layer, a dielectric layer and a second polycrystalline silicon layer on a single-crystal silicon substrate to form a stacked structure of first polycrystalline silicon layer / silicon oxynitride / second polycrystalline silicon layer.

[0077] For the first polycrystalline silicon layer, LPCVD was used with trichlorosilane as the silicon source gas and hydrogen as the carrier gas. The deposition temperature was 900℃, the pressure was 50Pa, the growth time was 120 seconds, and the thickness was 1.0μm. The initial nitrogen concentration of the first polycrystalline silicon layer was zero.

[0078] For the dielectric layer, an LPCVD process was used, with a reaction gas mixture of N₂O and ammonia, a deposition temperature of 900℃, and a thickness of 5 nm. The nitrogen concentration in the dielectric layer was higher than that in the first polycrystalline silicon layer.

[0079] For the second polycrystalline silicon layer, the LPCVD process was used, with trichlorosilane as the silicon source gas, hydrogen as the carrier gas, a deposition temperature of 900℃, a pressure of 50Pa, a growth time of 120 seconds, and a thickness of 1.0μm.

[0080] After heat treatment, based on the nitrogen concentration difference between the dielectric layer and the two polysilicon layers and the diffusion pattern during the thermal process, nitrogen can diffuse from the dielectric layer to the first and second polysilicon layers, resulting in a nitrogen concentration distribution in the first and second polysilicon layers that decreases from the interface with the dielectric layer in the direction away from the dielectric layer. See also... Figure 6 Cross-sectional SEM measurements showed that the grain size of the polysilicon in the first and second polysilicon layers ranged from 50 nm to 100 nm. Further testing of the effective resistivity revealed that the effective resistivity of the semiconductor wafer obtained in Example 1 was 830 Ω·cm.

[0081] Example 2 The difference between Example 2 and Example 1 is that the thickness of the dielectric layer is adjusted to 2nm, while the other process parameters are the same as in Example 1.

[0082] After heat treatment, based on the nitrogen concentration difference between the dielectric layer and the two polysilicon layers, and the diffusion pattern during the thermal process, nitrogen can diffuse from the dielectric layer to the first and second polysilicon layers. Because the dielectric layer is relatively thin, the total amount of nitrogen available for diffusion within it is relatively reduced. See also... Figure 7 Cross-sectional SEM measurements showed that the grain size ranged from 55 nm to 100 nm. Further testing of the effective resistivity revealed that the semiconductor wafer obtained in Example 2 had an effective resistivity of 800 Ω·cm.

[0083] Example 3 The difference between Example 3 and Example 1 is that the thickness of the dielectric layer is adjusted to 15nm, while the other process parameters are the same as those in Example 1.

[0084] After heat treatment, based on the nitrogen concentration difference between the dielectric layer and the two polysilicon layers, and the diffusion pattern during the thermal process, nitrogen can diffuse from the dielectric layer to the first and second polysilicon layers. (See also...) Figure 8 Cross-sectional SEM measurements showed that the grain size ranged from 50 nm to 90 nm. Further testing of the effective resistivity revealed that the semiconductor wafer obtained in Example 3 had an effective resistivity of 850 Ω·cm.

[0085] Example 4 The difference between Example 4 and Example 1 is that the deposition temperature of the second polysilicon layer is adjusted to 700°C, while the other process parameters are the same as in Example 1.

[0086] After heat treatment, based on the nitrogen concentration difference between the dielectric layer and the two polysilicon layers on either side, and the diffusion pattern during the thermal process, nitrogen can diffuse from the dielectric layer to the first and second polysilicon layers. In Example 4, the deposition temperature of the second polysilicon layer is lower than that in Example 1, resulting in a relatively lower degree of thermal activation for nitrogen diffusion. See also... Figure 9 Cross-sectional SEM measurements showed that the grain size ranged from 60 nm to 100 nm. Further testing of the effective resistivity revealed that the semiconductor wafer obtained in Example 4 had an effective resistivity of 850 Ω·cm.

[0087] Comparative Example 1 Comparative Example 1 uses the same layered structure as Example 1, but replaces the dielectric layer with a pure silicon dioxide thin film with a dielectric layer thickness of 5 nm. The remaining process parameters are the same as those in Example 1.

[0088] Pure silica films do not contain nitrogen, therefore they cannot supply nitrogen to the polycrystalline silicon layers on either side, serving only as a physical barrier. Since the dielectric layer in Comparative Example 1 does not provide a nitrogen source, it is difficult to form a nitrogen concentration gradient provided by the dielectric layer in the polycrystalline silicon layers on either side. See also Figure 10 The cross-sectional SEM measurements showed that the grain size was in the range of 150 nm to 250 nm, which was significantly larger than that in Examples 1 to 4.

[0089] The results of Comparative Example 1 show that, relying solely on physical isolation to reform the second polysilicon layer, under heat treatment conditions of 1100℃ and 11 hours, significant grain coarsening still occurred because the vacancy migration channels were not suppressed due to the absence of nitrogen in the polysilicon layers on both sides. This result indicates that the introduction of nitrogen into the dielectric layer is a key factor in achieving grain stability after thermal processing; a simple layered structure is insufficient to maintain the grain size within the 50nm to 100nm range during high-temperature thermal processing. Further testing of the effective resistivity revealed that the semiconductor wafer obtained in Comparative Example 1 had an effective resistivity of 420 Ω·cm.

[0090] Comparative Example 2 Comparative Example 2 uses the direct growth method in related technologies to deposit a polycrystalline silicon charge cutoff layer of about 2.5 μm thickness on a single-crystal silicon substrate in one step, without containing a dielectric layer. The deposition temperature is 900℃, the pressure is 50 Pa, the silicon source gas is trichlorosilane, and the carrier gas is hydrogen.

[0091] See Figure 11 After heat treatment, cross-sectional SEM measurements showed grain sizes ranging from 250 nm to 500 nm, with sparse grain boundaries and the lowest effective grain boundary density. Comparative Example 2 demonstrates the grain coarsening problem that occurs in the direct growth method under prolonged high-temperature heat treatment. Further testing of the effective resistivity revealed that the semiconductor wafer obtained in Comparative Example 2 had an effective resistivity of 400 Ω·cm.

[0092] Comparative Example 3 The difference between Comparative Example 3 and Example 1 is that the deposition temperature of the second polysilicon layer is adjusted to 500°C, which is lower than 600°C, while the other process parameters are the same as those in Example 1.

[0093] During the deposition of the second polysilicon layer, due to the lower deposition temperature, the diffusion of nitrogen from the dielectric layer into the first and second polysilicon layers was minimal. After deposition, Comparative Example 3 underwent heat treatment under the same conditions as Example 1. Experimental results showed that, under the above conditions, the coarsening degree of the polysilicon grains in Comparative Example 3 was still greater than that in Examples 1 to 4. See also Figure 12 Cross-sectional SEM measurements showed that the grain size ranged from 200 nm to 400 nm. Further testing of the effective resistivity revealed that the effective resistivity of the semiconductor wafer obtained in Comparative Example 3 was 380 Ω·cm.

[0094] The results of Comparative Example 3 show that controlling the deposition temperature of the second polysilicon layer within the range of 600℃ to 1100℃ is beneficial to promoting the diffusion of nitrogen elements in the dielectric layer to both sides of the polysilicon layer during the deposition of the second polysilicon layer, and is also beneficial to suppressing the coarsening of polysilicon grains during subsequent heat treatment.

[0095] Summary of Examples and Comparative Cases

[0096] The summary table above reveals the following patterns.

[0097] The comparison between Examples 1 to 4 and Comparative Examples 1 and 2 shows that by using a nitrogen-containing dielectric layer and depositing a second polycrystalline silicon layer at a temperature of 600°C to 1100°C, the grain size of the polycrystalline silicon after heat treatment can be controlled within the range of 50nm to 100nm; when only a nitrogen-free silicon dioxide dielectric layer is used or no dielectric layer is used, the grain size after heat treatment exceeds the above range.

[0098] A comparison between Example 1 and Comparative Example 3 shows that, under the same process conditions, the deposition temperature of the second polysilicon layer affects the polysilicon grain size after the final heat treatment. In Comparative Example 3, the deposition temperature of the second polysilicon layer was 500°C, and after subsequent heat treatment under the same conditions as in Example 1, the polysilicon grain size still reached 200 nm to 400 nm. In Example 1, the deposition temperature of the second polysilicon layer was 900°C, and after subsequent heat treatment under the same conditions, the polysilicon grain size was 50 nm to 100 nm. These results indicate that controlling the deposition temperature of the second polysilicon layer within the range of 600°C to 1100°C is beneficial for suppressing the coarsening of polysilicon grains during heat treatment.

[0099] The comparison of Examples 1 to 3 shows that, with dielectric layer thicknesses of 2 nm, 5 nm, and 15 nm, the grain size of polycrystalline silicon can be controlled within the range of 50 nm to 100 nm. These results indicate that, under the tested dielectric layer thickness conditions, the variation in dielectric layer thickness has a relatively limited impact on the grain size.

[0100] Furthermore, to verify the influence of the semiconductor wafer provided in the embodiments of this application on the thickness uniformity of the polysilicon layer, thickness uniformity tests were performed on the polysilicon structure without a nitrogen-containing dielectric layer and the semiconductor wafer provided in the embodiments of this application, respectively. The testing methods for the two structures are the same. Thickness uniformity can be used to characterize the degree of fluctuation in the thickness of the polysilicon layer along the wafer diameter direction. The smaller the thickness uniformity value, the smaller the fluctuation in the thickness of the polysilicon layer along the wafer diameter direction.

[0101] See Figure 13 , Figure 13 The curves showing the variation of polysilicon layer thickness along the wafer diameter at measurement locations in a polysilicon structure without a nitrogen-containing dielectric layer are presented. In the polysilicon structure without a nitrogen-containing dielectric layer, the polysilicon layer thickness exhibits significant fluctuations along the wafer diameter. Based on the polysilicon layer thickness test results at various measurement locations along the wafer diameter, the thickness uniformity of this polysilicon structure is found to be 3.36%.

[0102] See Figure 14 , Figure 14 The diagram illustrates the variation of polysilicon layer thickness with measurement positions along the wafer diameter in a semiconductor wafer provided in this embodiment. In the semiconductor wafer provided in this embodiment, the variability of polysilicon layer thickness along the wafer diameter direction decreases. Based on the polysilicon layer thickness test results at each measurement position along the wafer diameter direction, the thickness uniformity of the semiconductor wafer is determined to be 1.89%.

[0103] Therefore, compared to a polysilicon structure without a nitrogen-containing dielectric layer, this embodiment of the application, by providing a dielectric layer 120 between the first polysilicon layer 110 and the second polysilicon layer 130, can suppress polysilicon grain coarsening while reducing the variation in polysilicon layer thickness along the wafer diameter direction, thereby improving the thickness uniformity of the polysilicon layer. This improvement in thickness uniformity is beneficial for enhancing the consistency of charge cutoff layer performance within the semiconductor wafer surface and for reducing RF performance differences at different locations within the wafer surface.

[0104] It should be noted that the technical solutions described in this application can be combined arbitrarily without conflict.

[0105] The above description is merely a specific embodiment of this application, but the scope of protection of this application is not limited thereto. Any variations or substitutions that can be conceived by those skilled in the art within the scope of the technology disclosed in this application should be included within the scope of protection of this application. Therefore, the scope of protection of this application should be determined by the scope of the claims.

Claims

1. A semiconductor wafer, characterized in that, include: Single-crystal silicon substrate; A first polycrystalline silicon layer is disposed on one side of the monocrystalline silicon substrate; A dielectric layer is disposed on the side of the first polycrystalline silicon layer away from the monocrystalline silicon substrate, and contains silicon, oxygen, and nitrogen elements; and The second polysilicon layer is disposed on the side of the dielectric layer away from the first polysilicon layer; The first and second polysilicon layers contain nitrogen, and the nitrogen concentration in the dielectric layer is higher than that in the first polysilicon layer and also higher than that in the second polysilicon layer. The nitrogen concentration in the first polysilicon layer decreases from the interface between the first polysilicon layer and the dielectric layer in a direction away from the dielectric layer. The nitrogen concentration in the second polysilicon layer decreases from the interface between the second polysilicon layer and the dielectric layer in a direction away from the dielectric layer, and The grain size of the polysilicon grains in the first polysilicon layer and the second polysilicon layer is in the range of 50nm to 100nm.

2. The semiconductor wafer according to claim 1, characterized in that, The dielectric layer is made of silicon oxynitride.

3. The semiconductor wafer according to claim 1, characterized in that, The thickness of the dielectric layer is in the range of 0.5 nm to 20 nm; The thickness of the first polycrystalline silicon layer is in the range of 0.5 μm to 1.5 μm; The thickness of the second polycrystalline silicon layer is in the range of 0.5 μm to 1.5 μm.

4. The semiconductor wafer according to any one of claims 1 to 3, characterized in that, The bulk resistivity of the single-crystal silicon substrate is not less than 1000 Ω·cm.

5. A method for fabricating a semiconductor wafer, characterized in that, The preparation method includes: A first polycrystalline silicon layer is deposited on a monocrystalline silicon substrate; A dielectric layer is deposited on the first polysilicon layer, the dielectric layer comprising silicon, oxygen, and nitrogen elements, wherein the concentration of nitrogen element in the dielectric layer is higher than the concentration of nitrogen element in the first polysilicon layer; and At a temperature of 600°C to 1100°C, a second polysilicon layer is deposited on the dielectric layer, and nitrogen in the dielectric layer diffuses into the first polysilicon layer and the second polysilicon layer. The nitrogen concentration in the first polysilicon layer decreases from the interface between the first polysilicon layer and the dielectric layer in a direction away from the dielectric layer. The nitrogen concentration in the second polysilicon layer decreases from the interface between the second polysilicon layer and the dielectric layer in a direction away from the dielectric layer, and The grain size of the polysilicon grains in the first polysilicon layer and the second polysilicon layer is in the range of 50nm to 100nm.

6. The method for fabricating a semiconductor wafer according to claim 5, characterized in that, The dielectric layer is made of silicon oxynitride. The thickness of the dielectric layer is in the range of 0.5 nm to 20 nm.

7. The method for preparing a semiconductor wafer according to claim 6, characterized in that, When depositing the medium layer, an atmosphere containing nitrogen source gas and oxygen source gas is used for deposition.

8. The method for preparing a semiconductor wafer according to claim 7, characterized in that, The nitrogen source gas includes ammonia, and the oxygen source gas includes nitrous oxide.

9. The method for preparing a semiconductor wafer according to claim 5, characterized in that, When depositing the first polycrystalline silicon layer, the deposition temperature is 600°C to 1100°C, the pressure is 10Pa to 100Pa, and the growth time is 10 seconds to 240 seconds. When depositing the second polycrystalline silicon layer, the deposition temperature is 600°C to 1100°C, the pressure is 10Pa to 100Pa, and the growth time is 10 seconds to 240 seconds.

10. The method for preparing a semiconductor wafer according to claim 5, characterized in that, The thickness of the first polycrystalline silicon layer is in the range of 0.5 μm to 1.5 μm; The thickness of the second polycrystalline silicon layer is in the range of 0.5 μm to 1.5 μm.