Hydraulic compositions and hardeners

By using fine and highly hydrophilic fibers to control the hydraulic composition and form a dense network, the problem of insufficient reaction caused by moisture evaporation in additive manufacturing is solved, thereby improving the strength and uniformity of the hardened material.

CN123125089APending Publication Date: 2026-11-17KURARAY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202580029180.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-04-22
Filing Date
2025-04-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing hydraulic compositions are prone to insufficient reaction due to moisture evaporation in additive manufacturing, especially near complex-shaped surfaces, resulting in insufficient strength or cracks in the hardened material, and the moisture content deviation is difficult to control.

Method used

A hydraulic composition using hydrophilic fibers with a single filament fineness of less than 50 dtex or a single filament fiber diameter of less than 70 μm and an equilibrium moisture regain of more than 1.5% is formed by controlling the aspect ratio, length and volume ratio of the fibers to form a dense network to retain moisture and react uniformly.

Benefits of technology

It effectively suppresses the water content deviation in the hydraulic composition, ensures that the hydraulic reaction at complex shaped surfaces is fully carried out, and improves the mechanical properties and strength of the hardened material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention relates to a hydraulic composition for additive manufacturing, comprising hydrophilic fibers having a monofilament fineness of 50 dtex or less or a monofilament diameter of 70 μm or less, and an equilibrium moisture regain of 1.5% or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a hydraulic composition for additive manufacturing and a cured form of the hydraulic composition. Background Technology

[0002] Additive manufacturing technology, also known as 3D printing, includes a known technique that involves extruding a fluid material from a nozzle and layering it. In additive manufacturing techniques using material extrusion, materials such as thermoplastic resins and hydraulic compositions like cement and mortar are used.

[0003] Additive manufacturing technology using hydraulic compositions as materials does not require the molds typically needed to shape and harden the hydraulic composition. Therefore, it offers advantages such as simplifying the manufacturing process of hardened hydraulic compositions and enabling free-form shaping without mold limitations, thus attracting considerable attention. For example, Patent Document 1 discloses a fiber-reinforced mortar for extrusion lamination using an additive manufacturing apparatus (Patent Document 1). Additionally, as a conventional hydraulic composition not used in additive manufacturing, a hydraulic composition with added fibers is disclosed (Patent Document 2).

[0004] Existing technical documents

[0005] Patent documents

[0006] Patent Document 1: Japanese Patent Application Publication No. 2022-124859

[0007] Patent Document 2: International Publication No. 2020 / 137466 Summary of the Invention

[0008] The problem that the invention aims to solve

[0009] While it is known that modified polyvinyl alcohol and other resin fibers can be added to conventional hydraulic compositions not used in additive manufacturing to improve the strength of the resulting cured material, conventional hydraulic compositions cannot be directly used in additive manufacturing. In particular, sometimes materials need to be extruded from nozzles, and the shape of the cured material is often complex and large, making it difficult to directly apply conventional hydraulic compositions to additive manufacturing technology.

[0010] While additive manufacturing technology offers advantages such as reduced manufacturing steps and the ability to create free-form shapes without mold constraints, the absence of a mold makes it prone to moisture evaporation from surfaces, especially near areas with low moisture content, sometimes resulting in incomplete hydraulic reactions. Furthermore, despite its ability to achieve complex shapes, the increased surface area exposed to air due to these complexities can lead to variations in moisture content within the molded body, causing deviations in the hydraulic reaction. This can result in insufficient strength in the hardened material or cracking due to strength variations.

[0011] Therefore, the objective of this invention is to provide a hydraulic composition that easily suppresses deviations in the amount of moisture in the hydraulic composition during curing after molding, and in particular, enables sufficient hydraulic reaction to occur at surfaces where moisture is easily insufficient.

[0012] Methods for solving problems

[0013] To solve the aforementioned problems, the inventors conducted repeated and careful research and completed the present invention. Specifically, the present invention includes the following preferred embodiments.

[0014] [1] A hydraulic composition, wherein the hydraulic composition is used in additive manufacturing,

[0015] The hydraulic composition comprises hydrophilic fibers, wherein the monofilament fineness of the hydrophilic fibers is less than 50 dtex or the monofilament fiber diameter is less than 70 μm, and the equilibrium moisture regain is greater than 1.5%.

[0016] [2] The hydraulic composition according to [1], wherein,

[0017] The single filament fineness of the above-mentioned hydrophilic fibers is less than 15 dtex.

[0018] [3] The hydraulic composition according to [1] or [2], wherein,

[0019] The water absorption rate of the above-mentioned hydrophilic fibers is above 6.0%.

[0020] [4] The hydraulic composition according to any one of [1] to [3], wherein,

[0021] The aspect ratio of the above-mentioned hydrophilic fibers is 50~400.

[0022] [5] The hydraulic composition according to any one of [1] to [4], wherein,

[0023] The fiber length of the aforementioned hydrophilic fibers is less than 10 mm.

[0024] [6] The hydraulic composition according to any one of [1] to [5], wherein,

[0025] When the volume of the matrix of the above-mentioned hydraulic composition is set to 100, the volume ratio of the above-mentioned hydrophilic fibers is 0.1 to 10%.

[0026] [7] The hydraulic composition according to any one of [1] to [6], wherein,

[0027] The single filament fineness of the above-mentioned hydrophilic fibers is above 0.1 dtex.

[0028] [8] The hydraulic composition according to any one of [1] to [7], wherein,

[0029] The fiber length of the above-mentioned hydrophilic fibers is 0.5 mm or more.

[0030] [9] The hydraulic composition according to any one of [1] to [8], wherein,

[0031] The dispersion of the hydrophilic fibers in the above-mentioned hydraulic composition is 60% or more.

[0032]

[10] The hydraulic composition according to any one of [1] to [9], wherein,

[0033] In the above-mentioned hydraulic composition, the ratio of the mass of water (W) to the total mass of cementitious material (B) (W / B) is 0.1 to 0.40.

[0034]

[11] A hardener, which is a hardener of any one of the hydraulic compositions described in [1] to

[10] .

[0035]

[12] A hydrophilic fiber used in the additive manufacturing of a hydraulic composition molded article, wherein the hydrophilic fiber has an equilibrium moisture regain of 1.5% or more and / or a water absorption of 6.0% or more, a monofilament fineness of 50 dtex or less and / or a monofilament fiber diameter of 70 μm or less.

[0036]

[13] A bundled filament, which is used in the additive manufacturing of a hydraulic composition molded body, wherein the bundled filament has an equilibrium moisture regain of 1.5% or more and / or a water absorption of 6.0% or more, a filament fineness of 50 dtex or less and / or a filament fiber diameter of 70 μm or less.

[0037]

[14] A hydraulic composition, wherein the hydraulic composition is used in additive manufacturing,

[0038] The above-mentioned hydraulic composition contains hydrophilic fibers, wherein the diameter of the monofilament of the hydrophilic fibers is less than 70 μm and the water absorption rate is more than 6.0%.

[0039]

[15] The hydraulic composition according to

[14] , wherein

[0040] The length of the hydrophilic fibers in the above-mentioned hydraulic composition is 16 mm or less.

[0041]

[16] The hydraulic composition according to

[14] or

[15] , wherein,

[0042] The aspect ratio of the above-mentioned hydrophilic fibers is 50~400.

[0043]

[17] The hydraulic composition according to any one of

[14] to

[16] , wherein,

[0044] The fiber length of the aforementioned hydrophilic fibers is less than 10 mm.

[0045]

[18] The hydraulic composition according to any one of

[14] to

[17] , wherein,

[0046] When the volume of the matrix of the above-mentioned hydraulic composition is set to 100, the volume ratio of the above-mentioned hydrophilic fibers is 0.1 to 10%.

[0047]

[19] The hydraulic composition according to any one of

[14] to

[18] , wherein,

[0048] The single filament fineness of the above-mentioned hydrophilic fibers is above 0.1 dtex.

[0049]

[20] The hydraulic composition according to any one of

[14] to

[19] , wherein,

[0050] The fiber length of the above-mentioned hydrophilic fibers is 0.5 mm or more.

[0051]

[21] The hydraulic composition according to any one of

[14] to

[20] , wherein,

[0052] The dispersion of the hydrophilic fibers in the above-mentioned hydraulic composition is 60% or more.

[0053]

[22] The hydraulic composition according to any one of

[14] to

[21] , wherein,

[0054] In the above-mentioned hydraulic composition, the ratio of the mass of water (W) to the total mass of cementitious material (B) (W / B) is 0.1 to 0.40.

[0055]

[23] A hardener, which is a hardener of any one of the hydraulic compositions described in

[14] to

[22] .

[0056] The effects of the invention

[0057] According to the present invention, a hydraulic composition can be provided that easily suppresses deviations in the amount of moisture in the hydraulic composition during hardening after molding, and in particular enables sufficient hydraulic reaction to occur at surfaces where moisture is easily insufficient. Detailed Implementation

[0058] The embodiments of the present invention will now be described in detail. It should be noted that the present invention is not intended to be limited to the following embodiments.

[0059] (fiber)

[0060] The hydraulic composition of the present invention is a hydraulic composition for additive manufacturing, comprising fibers having a monofilament fineness of 50 dtex or less or a monofilament fiber diameter of 70 μm or less, and an equilibrium moisture regain of 1.5% or more.

[0061] The hydraulic composition of the present invention contains fibers with a single filament fineness of 50 dtex or less, or a single filament fiber diameter of 70 μm or less. If neither of these conditions is met, i.e., the single filament fineness exceeds 50 dtex and the single filament fiber diameter exceeds 70 μm, deviations in the hydraulic reaction within the molded body of the hydraulic composition cannot be sufficiently suppressed. The reason for this is not yet clear, but it can be understood that by giving the fiber a certain degree of fineness, the total surface area of ​​the fibers capable of retaining moisture can be increased, and the fibers with surface moisture retention form a dense network in the hydraulic composition. Therefore, it can be considered that deviations in the amount of moisture in the hardening hydraulic composition can be suppressed after molding, deviations in the hydraulic reaction can be suppressed, and ultimately a hardened product with excellent mechanical properties can be manufactured. When the single filament fineness exceeds 50 dtex and the single filament fiber diameter exceeds 70 μm, the fibers are coarse and long, and therefore it is considered difficult to form a dense network of moisture-retaining fibers. Furthermore, it can be argued that, compared to the case of adding, for example, particulate hydrophilic substances, the addition of fibrous hydrophilic substances, based on the formed network, can more easily reduce the deviation of the hydraulic response.

[0062] From the viewpoint of suppressing deviations in the moisture content of the hydraulic composition during curing after molding, and from the viewpoint of fiber dispersibility, the fiber monofilament fineness is preferably 50 dtex or less, more preferably 20 dtex or less, further preferably 15 dtex or less, even more preferably 12 dtex or less, and may also be 9 dtex or less. Furthermore, from the viewpoint of suppressing deviations in the moisture content of the hydraulic composition during curing after molding, the fiber monofilament fineness is preferably 0.1 dtex or more, more preferably 0.3 dtex or more, and even more preferably 0.5 dtex or more.

[0063] It should be noted that the fineness of the fiber is expressed as the weight of 10,000m of fiber, and can be determined according to JIS L1015 "Test Method for Short Fibers of Chemical Fibers (8.5.1)".

[0064] From the viewpoint of moisture retention, the diameter of the single filament of the fiber is preferably 70 μm or less, more preferably 5 to 70 μm, even more preferably 5 to 39 μm, even more preferably 5 to 38.5 μm, particularly preferably 6 to 35 μm, even more preferably 6 to 30 μm, and especially preferably 7 to 27 μm. The diameter of the single filament of the hydrophilic fiber is the average fiber diameter, which can be determined by the method described in the above-mentioned aspect ratio calculation.

[0065] The cross-sectional shape of the fiber can be circular, elliptical, or irregular, and can be selected according to the purpose. From the viewpoint of increasing the surface area of ​​the fiber and improving the water retention effect brought by the fiber, an irregular cross-section is preferred; from the viewpoint of improving fluidity, circular or elliptical cross-sections are preferred. It should be noted that in the determination of the diameter of the monofilament fiber, the diameter is measured when the cross-sectional shape is circular, and the cross-sectional area is measured when the cross-sectional shape is irregular. The diameter of a circle with the same cross-sectional area as the obtained diameter is calculated and used as the conversion diameter.

[0066] The equilibrium moisture regain of the fiber is 1.5% or more. When the equilibrium moisture regain is less than 1.5%, moisture cannot be retained in the hydraulic composition during curing after molding, and deviations in moisture content cannot be adequately suppressed. As a result, the curing reaction is particularly insufficient near the surface, leading to deviations in the curing reaction. The reason for this is not yet clear, but it can be considered that when the equilibrium moisture regain of the fiber is less than 1.5%, the fiber cannot retain moisture, and therefore, even when the moisture content near the surface decreases due to drying, moisture cannot be distributed to the surface portion. From the viewpoint of moisture retention, the equilibrium moisture regain of the fiber is preferably 1.8% or more, more preferably 2.0% or more, and even more preferably 2.2% or more. Furthermore, from the viewpoint of poor curing at the fiber interface due to excessive water retention, the equilibrium moisture regain of the fiber is preferably 10.0% or less, more preferably 8.0% or less, and even more preferably 6.0% or less. The equilibrium moisture regain of a fiber refers to the moisture content after 72 hours of adjustment at 20°C and 65% RH following absolute drying, according to JIS L1015 "Test Methods for Chemical Short Fibers". It should be noted that an equilibrium moisture regain of 1.5% or higher indicates that the fiber is a hydrophilic fiber; in this specification, fibers with an equilibrium moisture regain of 1.5% or higher are also referred to as hydrophilic fibers. In one embodiment of the present invention, the equilibrium moisture regain of the fiber is preferably 1.5% to 10.0%, more preferably 1.8% to 8.0%, further preferably 2.0% to 6.0%, and even more preferably 2.2% to 6.0%.

[0067] The water absorption rate of the fiber is preferably 6.0% or higher. When the water absorption rate of the fiber is 6.0% or higher, the retention of moisture in the hydraulic composition during curing after molding can be improved, and deviations in the amount of moisture can be sufficiently suppressed. Therefore, it is particularly preferable from the viewpoint of improving the curing reaction near the surface and suppressing deviations in the curing reaction. The reason for this is not yet clear, but it can be considered that when the water absorption rate of the fiber is 6.0% or higher, the fiber has a high moisture retention capacity, so even if the moisture content near the surface decreases due to drying, moisture can still be distributed to the surface portion. From the viewpoint of moisture retention, the water absorption rate of the fiber is preferably 6.0% or higher, more preferably 7.0% or higher, further preferably 8.0% or higher, and even more preferably 9.0% or higher. Furthermore, from the viewpoint of poor curing at the fiber interface due to excessive water retention, the water absorption rate of the fiber is preferably 100.0% or lower, more preferably 50.0% or lower, further preferably 30.0% or lower, even more preferably 20.0% or lower, and can be 15.0% or lower, or 10.0% or lower. In one embodiment of the present invention, the water absorption rate of the fiber is preferably 6.0% to 100.0%, more preferably 7.0% to 50.0%, even more preferably 8.0% to 30.0%, even more preferably 9.0% to 20.0%, and particularly preferably 9.0% to 10.0%.

[0068] Water absorption rate refers to the value calculated by the following formula: after stirring the fiber in a 0.1 mol / L NaOH aqueous solution (pH 13) at 30°C for 4 minutes, dehydrating it three times by centrifugation at 3000 rpm for 5 minutes each time, let's call the fiber mass A. After centrifugation and dehydration, let's call the fiber mass B. Then, let's call the fiber mass B.

[0069] Formula: Water absorption rate = 100 × (AB) / B (%)

[0070] From the viewpoint of suppressing deviations in the hydraulic reaction, the aspect ratio of the hydrophilic fiber is preferably 50-400, more preferably 60-350, further preferably 10-300, even more preferably 70-300, even more preferably 100-300, particularly preferably 150-300, and may also be 200-250. Specifically, the aspect ratio can be 10, 20, 30, 40, 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 200, 210, 220, 230, 240, 250, 260, 270, 280, etc. It can be considered that when the hydrophilic fiber has an aspect ratio within the above range, it is easy to form a network for distributing moisture to the areas of insufficient moisture in the hydraulic composition.

[0071] The aspect ratio is the ratio of fiber length (L) to fiber diameter (D) (L / D). For the aspect ratio, the average fiber length is calculated according to JIS L1015 "Test Method for Short Fibers of Chemical Fibers (8.5.1)," and then the ratio is used to calculate the aspect ratio. It should be noted that the average fiber diameter can be obtained by randomly selecting 20 fibers and measuring the diameter of the central portion of each fiber along its length using an optical microscope.

[0072] From the viewpoint of suppressing deviations in the hydraulic reaction, the fiber length of the hydrophilic fiber is preferably 10 mm or less, more preferably less than 10 mm, even more preferably 0.5 mm or more and 10 mm or less, even more preferably 0.5 mm or more and less than 10 mm, and particularly preferably 0.5 mm to 9 mm or 0.5 mm to 8 mm. From the same viewpoint, the fiber length of the hydrophilic fiber is preferably 0.5 mm or more and less than 8 mm, but can also be 1.0 to 6.0 mm or 1.5 to 5.0 mm. When the fiber length is 10 mm or less, the network of moisture-retaining fibers becomes denser, making it easier to suppress deviations in the moisture content of the hydraulic composition. The fiber length of the hydrophilic fiber is the average fiber length, which can be determined by the method described in the above-described aspect ratio calculation.

[0073] There are no particular limitations on fibers as long as they meet the above requirements for monofilament fineness and equilibrium moisture regain. Examples include: polyvinyl alcohol (hereinafter sometimes referred to as PVA) fibers, polyamide fibers (including aramid fibers), acrylic fibers, and man-made fibers (polynosic fibers, solvent-spun cellulose fibers, etc.) and other synthetic polymer fibers.

[0074] Alternatively, fibers composed of hydrophobic resins can be used, which have been hydrophilicized through surface treatment or coating.

[0075] PVA-type fibers are fibers containing vinyl alcohol polymers. From the viewpoints of mechanical properties, adhesion to hydraulic materials, and alkali resistance, it is preferable that the fiber contains 30% by mass or more of this vinyl alcohol polymer, more preferably 60% by mass or more, and even more preferably 80% by mass or more. From the viewpoints of retaining moisture in the hydraulic composition during curing after molding, and ensuring a sufficient and uniform hydraulic reaction, thus easily improving the strength of the resulting molded article, PVA-type fibers are preferred. When the fiber is a PVA-type fiber, the density after curing is not compromised, and the strength of the molded article is less likely to decrease. Furthermore, when the fiber is a PVA-type fiber, due to its molecular structure, it has high hydrophilicity. Through the interaction between the hydroxyl groups of the fiber and the Ca of the cement, the affinity between the fiber and the cement can be improved, easily increasing chemical adhesion and readily suppressing cracking in the final cured product.

[0076] The vinyl alcohol polymer constituting PVA fibers can be a homopolymer of vinyl alcohol, or, without impairing the effects of the present invention, a copolymer of vinyl alcohol and other monomers, and can also be modified. From the viewpoint of easily improving the mechanical strength, alkali resistance, and hot water resistance of the fibers, when the total amount of all monomer units constituting the vinyl alcohol polymer is set to 100 mol%, the total amount of structural units derived from optionally contained modified polyvinyl alcohol monomers and the amount of optionally contained monomers other than vinyl alcohol is preferably 30 mol% or less, more preferably 10 mol% or less.

[0077] From the viewpoint of easily improving the mechanical strength, alkali resistance, and hot water resistance of the fibers, the viscosity-uniform polymerization degree of the vinyl alcohol polymer constituting the PVA fibers is preferably 1000 or more, more preferably 1500 or more. From the viewpoint of easily reducing the manufacturing cost of the vinyl alcohol polymer, this viscosity-uniform polymerization degree is preferably 10000 or less, more preferably 5000 or less, and even more preferably 3000 or less. For modified polyvinyl alcohol, the viscosity-uniform polymerization degree is as described below.

[0078] From the perspective of fiber heat resistance, durability, and dimensional stability, the degree of saponification of the vinyl alcohol polymer constituting PVA fibers is preferably 99 mol% or more, more preferably 99.5 mol% or more, and even more preferably 99.8 mol% or more. It should be noted that the upper limit of the degree of saponification is 100 mol% or less. For modified polyvinyl alcohol, the method for determining the degree of saponification is described below.

[0079] The fibers contained in the hydraulic composition of the present invention can be fibers composed of one polymer or composite fibers composed of two or more polymers. Examples of composite fiber shapes include island-type, core-sheath type, and side-by-side type.

[0080] The method for manufacturing the fibers contained in the hydraulic composition of the present invention is not particularly limited, and conventional melt spinning, solution spinning, dry spinning, etc., can be used. The fibers contained in the hydraulic composition of the present invention can be manufactured, for example, by the following method. For example, when the fiber is a PVA-type fiber, a vinyl alcohol polymer is prepared into aqueous flakes with a concentration of 40-60% by mass, and then dissolved and degassed using an extruder. Then, a crosslinking agent is added to the aqueous solution of the vinyl alcohol polymer. Examples of crosslinking agents include ammonium sulfate, sulfuric acid, ammonium phosphate, phosphoric acid, hydrochloric acid, nitric acid, acetic acid, and oxalic acid. From the viewpoint of not corroding pipes, not producing unpleasant odors, and not causing the fibers to foam, ammonium sulfate is preferred. The amount of crosslinking agent added is preferably 0.5-10% by mass relative to the vinyl alcohol polymer. The temperature of the spinning solution is preferably 90-140°C. The spinning solution with the added crosslinking agent is pressurized and sprayed into the air through a nozzle orifice for dry spinning. The nozzle orifice can be circular, or it can be any shape other than a circle, such as flat, cross-shaped, T-shaped, Y-shaped, L-shaped, triangular, quadrilateral, or star-shaped. It should be noted that the spinning method can be any of the following: wet, dry-wet, or dry.

[0081] Next, the fibers obtained from spinning are dried. The drying temperature is usually below 100°C, but it is preferable to dry them completely at a temperature above 100°C when the drying process has progressed to a certain point.

[0082] After drying, the fibers are stretched. Stretching is typically performed at 200–250°C, preferably at 220–240°C. The stretch ratio is typically 5 times or more, preferably 6 times or more. Stretching can be carried out in a hot air stretching oven for approximately 20 seconds to 3 minutes. The stretched fibers can then be heat-treated as needed to achieve a fixed length or shrinkage. The resulting fibers can be crimped or coated with an oil agent as required. In the case of polyvinyl alcohol (PVA) fibers, during stretching, the crosslinking agent added to the spinning solution reacts with the OH groups of the PVA to form crosslinking bonds.

[0083] (Hydraulic composition)

[0084] The hydraulic composition of the present invention is a hydraulic composition for additive manufacturing, comprising fibers having a monofilament fineness of 15 dtex or less and an equilibrium moisture regain of 1.5% or more. In addition to the aforementioned fibers, the hydraulic composition may also comprise cementitious materials, aggregates, other components, and water.

[0085] Cementitious materials are substances that undergo a hydration reaction in the presence of water to form solid hydrates or hydrated phases. Examples of cementitious materials include cement components. Cement components include, for example, ordinary Portland cement, early-strength Portland cement, ultra-early-strength Portland cement, and intermediate-heat Portland cement, as well as alumina cement, blast furnace cement, silica cement, and fly ash cement. Other cementitious materials besides cement include slag, fly ash, silica fume, volcanic ash, and hydraulic lime.

[0086] These cementing materials can be used alone or in combination of two or more.

[0087] As aggregates, various types of aggregates can be used as needed. Examples of such aggregates include fine aggregates, lightweight aggregates, and coarse aggregates. These aggregates can be used alone or in combination of two or more.

[0088] Fine aggregates can be those with a particle size of 5 mm or less. Examples include sand with a particle size of 5 mm or less; fine aggregates made by pulverizing or granulating inorganic materials such as silica, fly ash, blast furnace slag, volcanic ash-based white sand, various sludge, and rock minerals. These fine aggregates can be used alone or in combination of two or more. Examples of sand types include: river sand, mountain sand, sea sand, crushed sand, silica sand, slag, glass sand, iron sand, lime sand, calcium carbonate, and artificial sand. These fine aggregates can be used alone or in combination of two or more.

[0089] Examples of lightweight aggregates include natural lightweight aggregates such as volcanic sand and gravel, expanded slag, and coal ash, as well as artificial lightweight aggregates such as foamed perlite, foamed obsidian, MESALITE (Mitsui Expanded Shale Light-Weight Aggregate), vermiculite, Shirasu balloons, and fly ash microspheres. These lightweight aggregates can be used alone or in combination of two or more.

[0090] Coarse aggregate is aggregate containing at least 85% by mass of particles with a diameter of 5 mm or larger. Coarse aggregate can be formed from particles with a diameter greater than 5 mm. Examples of coarse aggregate include various sands and gravels, artificial aggregates (such as blast furnace slag), and recycled aggregates (such as recycled aggregates from construction waste). These coarse aggregates can be used alone or in combination of two or more.

[0091] In addition to the aggregates mentioned above, the hydraulic composition may also contain functional aggregates. Examples of functional aggregates include colored aggregates, hard aggregates, elastic aggregates, and aggregates with specific shapes, such as layered silicates (e.g., mica, talc, kaolin), alumina, and silica. The ratio of functional aggregates to aggregates can be appropriately set according to their respective types. For example, the mass ratio of aggregates to functional aggregates (aggregate / functional aggregate) can be 99 / 1 to 70 / 30, preferably 98 / 2 to 75 / 25, and more preferably 97 / 3 to 80 / 20. These functional aggregates can be used alone or in combination of two or more.

[0092] The mass ratio of the total amount of aggregate (S) to the total mass of cementitious material (B) (aggregate (S) / cementitious material (B)) is preferably 1 / 10 to 5 / 1, more preferably 1 / 8 to 4 / 1, and even more preferably 1 / 6 to 3 / 1.

[0093] Hydraulic compositions may contain various additives as needed. Examples of additives include: AE agents, flow agents, water-reducing agents, high-performance water-reducing agents, AE water-reducing agents, high-performance AE water-reducing agents, thickeners, water-retaining agents, water-repellent agents, swelling agents, curing accelerators, retarders, and polymer emulsions [acrylic emulsions, ethylene-vinyl acetate emulsions, and SBR (styrene-butadiene rubber) emulsions]. Additives may be included individually or in combination of two or more. It should be noted that polymer emulsions not only enhance the final molded article but also strengthen the adhesion between components within the molded article. Furthermore, by combining polymer emulsions, not only can the water-repellency of the molded article be improved, but excessive drying can also be inhibited.

[0094] In a preferred embodiment, the hydraulic composition preferably includes an admixture, more preferably an AE water-reducing agent. In this case, the mass ratio of the total mass (B) of the cementitious material contained in the hydraulic composition to the mass of the admixture (SP) (cementitious material (B) / admixture (SP)) is preferably 1 / 0.001 to 1 / 0.05, more preferably 1 / 0.002 to 1 / 0.03, and even more preferably 1 / 0.005 to 1 / 0.02.

[0095] The hydraulic composition may include water-soluble polymers as needed. It should be noted that the water-soluble polymers in this method exclude hydrophilic fibers with a monofilament fineness of less than 15 dtex and an equilibrium moisture regain of more than 1.5%. Examples of water-soluble polymers include: cellulose ethers such as methylcellulose, hydroxymethylcellulose, hydroxyethylcellulose, carboxymethylcellulose, and hydroxypropyl methylcellulose; polyvinyl alcohol; polyacrylic acid; and lignin sulfonates. These water-soluble polymers may be used alone or in combination of two or more.

[0096] The amount (by weight) of hydrophilic fibers contained in the hydraulic composition can be appropriately set according to the type, length, and aspect ratio of the hydrophilic fibers. For example, based on the volume of the final molded body (cured material), it can preferably reach 1~70 kg / m³. 3 More preferably, it can reach 2~40kg / m 3 Further optimization to achieve 2~30kg / m 3 The amount of hydrophilic fiber added is within the above range. When the amount of hydrophilic fiber added is within the above range, it is easy to improve the water retention and distribution effect brought about by the hydrophilic fiber, and it is easy to suppress the entanglement of fibers caused by excessive fiber content. From this point of view, it is easy to further improve the above-mentioned effects brought about by the hydrophilic fiber.

[0097] Furthermore, when the volume of the matrix of the hydraulic composition is set to 100, the volume ratio of hydrophilic fibers contained in the hydraulic composition is preferably 0.1 to 10%, more preferably 0.3 to 8%, even more preferably 0.5 to 6%, and particularly preferably 1.0 to 5%. Here, the volume of the matrix of the hydraulic composition refers to the sum of volumes calculated based on the weight and density of the materials constituting the hydraulic composition. When the volume ratio of hydrophilic fibers is within the above range, the water retention and distribution effect brought about by the hydrophilic fibers can be improved, and the above-mentioned effect can also be improved by suppressing the entanglement of fibers due to the excessive presence of fibers.

[0098] From the viewpoint of the water retention and distribution effect brought about by the hydrophilic fibers, the dispersion of the aforementioned hydrophilic fibers in the hydraulic composition is preferably 60% or more, more preferably 70% or more, even more preferably 80% or more, and even more preferably 90% or more. The dispersion can be measured by the method described in the examples, specifically by the method described in the examples.

[0099] The final molded body preferably contains 0 to 5 fiber spheres, more preferably 0 to 1. When the number of fiber spheres in the mortar concrete is within the above range, the water retention and distribution effect brought about by the hydrophilic fibers can be sufficiently improved, allowing the hydraulic reaction to proceed fully and improving the mechanical strength of the molded body. From this perspective, it is preferred. It should be noted that the fiber spheres are formed due to poor mixing of the fibers and cement components in the hydraulic composition, resulting in the fibers becoming entangled and forming a spherical shape. The number of fiber spheres can be determined by the method described in the examples.

[0100] The slump loss of the molded concrete is preferably less than 6 cm, more preferably less than 4 cm, and even more preferably less than 2 cm. When the slump loss is below the upper limit mentioned above, the mixability of the fiber and cement components is high, thus improving workability. The lower limit of the slump loss mentioned above is not particularly limited and is usually more than 1 cm. It should be noted that the slump loss can be determined by performing a slump test according to the slump test method for concrete based on JIS A1101:2020.

[0101] The hydraulic composition of the present invention can be manufactured by mixing the aforementioned hydrophilic fibers with a monofilament fineness of 50 dtex or less and an equilibrium moisture regain of 1.5% or more with water, cement components, aggregates, and other components such as various additives added as needed without impairing the effects of the present invention. Then, by hardening the hydraulic composition, molded articles (hardened products) such as mortar concrete can be manufactured.

[0102] The hydraulic composition can be mixed using a known or conventional mixing apparatus such as a mixer. Furthermore, the mixing order of the constituent materials is not particularly limited, but can be appropriately adjusted according to the composition of the hydraulic composition, the water / cementing material ratio (W / B), etc., in order to minimize physical impact on the fibers.

[0103] From the viewpoint of balancing fluidity and shape retention, in the above-mentioned hydraulic composition, the ratio of the mass of water (W) to the total mass of the cementitious material (B) (W / B) is preferably 0.1 to 0.40, more preferably 0.15 to 0.38, and even more preferably 0.20 to 0.36. Here, the total mass of the cementitious material refers to the total mass of the substances exhibiting hydraulic properties contained in the hydraulic composition.

[0104] There is no particular limitation on the method of supplying the hydrophilic fibers to the hydraulic composition. For example, various metering devices (such as vibrating feeders, screw feeders, or belt feeders) can be used as devices for supplying the fibers while controlling the amount and / or speed of fiber input.

[0105] There are no particular limitations on the state of the fibers when supplying them to the hydraulic composition; the fibers can be added directly or as bundled fibers. It should be noted that bundled fibers refer to the following: multiple fibers with a single filament fineness of less than 15 dtex and an equilibrium moisture regain of more than 1.5% are integrated by a bundling agent, and when added to the hydraulic composition, the bundling agent dissolves, and these multiple fibers separate and disperse.

[0106] The present invention also provides hydrophilic fibers and bundled yarns, wherein the hydrophilic fibers are hydrophilic fibers used in the additive manufacturing of hydraulic composition molded articles, having an equilibrium moisture regain of 1.5% or more and / or a water absorption rate of 6.0% or more, and a single filament fineness of 50 dtex or less; and the bundled yarns are bundled yarns used in the additive manufacturing of hydraulic composition molded articles, having an equilibrium moisture regain of 1.5% or more and / or a water absorption rate of 6.0% or more, and a single filament fineness of 50 dtex or less.

[0107] The bundled yarn of the present invention comprises multiple fibers and the aforementioned specific bundling agent, wherein the multiple fibers are integrated by the bundling agent. The integration of multiple fibers by the bundling agent refers to the state in which multiple fibers are bonded together by the bundling agent to form a bundle.

[0108] When adding fibers as bundled yarns, a water-soluble resin is preferably used as the bundling agent. In this specification, the water-soluble resin is preferably a resin having a solubility of 16 g / L or more at room temperature (20°C) relative to alkaline water at pH 12. From the viewpoint of easily improving the fiber opening property of the bundled yarns and easily improving the toughness of the molded body, the solubility of the water-soluble resin is preferably 18 g / L or more, more preferably 20 g / L or more. From the viewpoint of easily improving the fiber bundling property and easily preventing the formation of buckling portions, it is preferably 50 g / L or less, more preferably 45 g / L or less, and even more preferably 40 g / L or less. In addition, from the viewpoint of easily improving the fiber opening property of the bundled yarns and easily improving the toughness of the molded body, the water-soluble resin is preferably a resin having a solubility of 18 g / L or more, more preferably 20 g / L or more, and even more preferably 22 g / L or more at room temperature relative to water at pH 12. The solubility of alkaline water at room temperature (20°C) relative to pH 12 is, for example, the amount of water-soluble resin that dissolves when stirred at room temperature (20°C) without producing dissolved residue when a film-like water-soluble resin is added to alkaline water adjusted to pH 12 with sodium hydroxide.

[0109] As a water-soluble resin, any resin that dissolves upon addition to a hydraulic composition is acceptable, without particular limitation. Examples include: polyvinyl alcohol resins (resins containing structural units derived from vinyl alcohol), ethyleneimine resins (resins containing structural units derived from ethyleneimine), acrylic resins, urethane resins, epoxy resins, etc.

[0110] From the viewpoint of solubility in cement composite materials, the water-soluble resin is preferably selected from polyvinyl alcohol resins, ethylene imine resins, acrylic resins and epoxy resins, and more preferably from polyvinyl alcohol resins, ethylene imine resins and acrylic resins.

[0111] The water-soluble resin is preferably a vinyl alcohol resin containing structural units derived from vinyl alcohol, and more preferably a modified polyvinyl alcohol.

[0112] For example, the water-soluble resin can be modified polyvinyl alcohol. This modified polyvinyl alcohol preferably has at least a plurality of structural units derived from vinyl ester monomers and structural units (X) derived from unsaturated carboxylic acids or their derivatives. In this case, when the total amount of all monomer units of the modified polyvinyl alcohol is set to 100 mol%, the amount of structural unit (X) is preferably 0.1 to 10 mol%.

[0113] From the viewpoint of easily improving fiber opening rate, easily reducing fiber cohesion, and easily improving the effect of moisture retention and distribution brought by hydrophilic fibers, the amount of structural unit (X) is more preferably 0.5~10 mol%, more preferably 1~9.5 mol%, and even more preferably 2~9 mol%. It should be noted that the amount of structural unit (X) derived from unsaturated carboxylic acids or their derivatives in the modified polyvinyl alcohol can be adjusted according to the modified polyvinyl alcohol content. 1 The peaks can be determined by H-NMR, or by the monomer feed ratio during the production of modified polyvinyl alcohol.

[0114] From the viewpoint of easily and sufficiently improving the solubility of modified polyvinyl alcohol in water, the degree of saponification of the modified polyvinyl alcohol is preferably 85 mol% or more, more preferably 88 mol% or more, further preferably 90 mol% or more, even more preferably 95 mol% or more, and particularly preferably 98 mol% or more. The upper limit of the degree of saponification can be 100 mol% or less, and from the viewpoint of improving solubility in water due to the reduction in the crystallinity of the modified polyvinyl alcohol, it is preferably 99.9 mol% or less, more preferably 99.8 mol% or less. The degree of saponification can be determined by the method described in JIS K 6726 (1994).

[0115] The viscosity-uniform polymerization degree of the modified polyvinyl alcohol is preferably 100 to 5000, more preferably 100 to 4000, and even more preferably 300 to 3500. When the viscosity-uniform polymerization degree is above the lower limit mentioned above, it is easy to improve the fiber's bundle properties as a bundler. In addition, when the viscosity-uniform polymerization degree is below the upper limit mentioned above, the solubility of the modified polyvinyl alcohol in water can be improved, and it is easy to obtain rapid and sufficient fiber opening. The viscosity-uniform polymerization degree can be determined by the method described in JIS K 6726 (1994). Specifically, when the degree of saponification is less than 99.5 mol%, the viscosity-uniform polymerization degree (P) can be calculated by the following formula using the limiting viscosity [η] (L / g) of PVA saponified to a degree of saponification of 99.5 mol% or more in water at 30°C.

[0116] P=([η]×104 / 8.29) (1 / 0.62)

[0117] Examples of unsaturated carboxylic acids that impart structural unit (X) to modified polyvinyl alcohol include olefinic unsaturated carboxylic acids such as acrylic acid, methacrylic acid, phthalic acid, maleic acid, and itaconic acid. Examples of their derivatives include alkyl esters and metal salts of the aforementioned olefinic unsaturated carboxylic acids. In modified polyvinyl alcohol used as a bridging agent, the structural unit (X) derived from the unsaturated carboxylic acid or its derivative may have one structural unit, two or more structural units, or other structural units.

[0118] From the viewpoint of easily improving the fiber opening rate when using bundled yarns mixed with hydraulic materials and easily reducing the cohesion of the fibers after opening, unsaturated carboxylic acids or their derivatives are preferably selected from at least one of (meth)acrylic acid, alkyl (meth)acrylic acid esters, and metal salts of (meth)acrylic acid. It should be noted that the term "(meth)acrylic acid" as used in this specification refers to "acrylic acid and / or methacrylic acid".

[0119] Examples of alkyl methacrylates include esters formed from (meth)acrylic acid and straight-chain or branched alcohols having 1 to 5 carbon atoms, such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, and pentyl (meth)acrylate. Examples of alkali metal salts of (meth)acrylic acid include lithium, sodium, and potassium.

[0120] Here, considering that when the total amount of monomer units in the modified polyvinyl alcohol is set to 100 mol%, the structural units (X) derived from unsaturated carboxylic acids or their derivatives in the modified polyvinyl alcohol are preferably 0.1 to 10 mol%, and it can be assumed that most of them exist adjacent to the structural units derived from vinyl ester monomers. In this case, the structural units (X) and the structural units derived from vinyl ester monomers can exist as separate structural units (monomer units), but at least a portion of the plurality of structural units (X) can also be included as structural units that form closed rings with the hydroxyl groups contained in the structural units derived from vinyl ester monomers.

[0121] It should be noted that structural units (X) derived from unsaturated carboxylic acids or their derivatives, such as those containing carboxyl groups, which undergo cyclization with hydroxyl groups contained in structural units derived from vinyl alcohol, are also structural units containing structural unit (X), and are also structural units derived from unsaturated carboxylic acids or their derivatives. Here, in this specification, when calculating the total amount of monomer units in modified polyvinyl alcohol, the cyclized structural unit is not considered as a single structural unit; instead, the uncyclized structural unit (X) and the structural unit from vinyl alcohol, which are structural units corresponding to the monomers, are considered as separate monomer units.

[0122] When modified polyvinyl alcohol is used as a bridging agent, the modified polyvinyl alcohol has a structural unit (X) derived from an unsaturated carboxylic acid or its derivative, and / or a structural unit (X) obtained by cyclic closure with an adjacent structural unit derived from a vinyl ester monomer. When polyvinyl alcohol is modified by a structural unit (X) derived from an unsaturated carboxylic acid or its derivative, its performance as a bridging agent, particularly the bridging properties of the fibers, is excellent when the modified polyvinyl alcohol is not dissolved in water. Therefore, fiber damage is easily prevented when the bridging yarn is dry-mixed with hydraulic materials. Polyvinyl alcohol modified with structural unit (X) has high solubility relative to water due to carboxyl groups, etc. Therefore, bridging yarn containing such modified polyvinyl alcohol as a bridging agent has the characteristic of rapid dissolution of the bridging agent when mixed with water, enabling rapid and sufficient fiber opening. It should be noted that the required speed of fiber opening can vary depending on the amount of bundled yarn used, the application of the hydraulic material, etc. In the embodiments of this specification, for example, the fiber opening performance was evaluated when the mixing was carried out in a very short time of tens of seconds.

[0123] Especially when the modified polyvinyl alcohol has a structural unit (X) derived from an unsaturated carboxylic acid or its derivative, and / or a structural unit (X) obtained by ring-closing with an adjacent structural unit derived from an ethylene ester monomer, the modified polyvinyl alcohol exhibits very low solubility in water in the ring-closed state. Therefore, it performs excellently as a filament binder, easily suppressing fiber damage during dry mixing. This ring-closed structure exhibits particularly high ring-opening properties when dissolved in water under alkaline conditions, and the ring-opened modified polyvinyl alcohol with structural unit (X) has high solubility relative to water. Therefore, bundled yarns containing such modified polyvinyl alcohol as a filament binder have the following characteristics: the filament binder dissolves rapidly when mixed with water, facilitating rapid and thorough fiber opening.

[0124] From the perspective of easily improving the fiber opening rate of bundled yarns and easily suppressing fiber aggregation, modified polyvinyl alcohol preferably contains structural units (X) derived from unsaturated carboxylic acids or their derivatives, including structural units shown in formula (X1) and / or formula (X2).

[0125] [Chemical Formula 1]

[0126]

[0127] [In formula (X1), X is a hydrogen atom or a methyl group],

[0128] [Chemical Formula 2]

[0129]

[0130] [In formula (X2), X is a hydrogen atom or a methyl group, and Y is a hydrogen atom, an alkali metal atom, or an alkyl group with 1 to 5 carbon atoms].

[0131] The structural unit shown in formula (X2) is a structural unit selected from at least one of (meth)acrylic acid, alkyl (meth)acrylic acid, and metal salts of (meth)acrylic acid. When structural unit (X2) is ring-closed with an adjacent structural unit from a vinyl ester monomer, it becomes structural unit (X1). When modified polyvinyl alcohol includes structural units shown in formula (X1) and / or formula (X2) as structural units (X), rapid fiber opening is easily achieved when bundled fibers are mixed with hydraulic materials such as cement and water, the fiber opening rate is easily improved, and fiber aggregation after opening is easily prevented.

[0132] The modified polyvinyl alcohol may contain one structural unit as shown in formula (X1), or it may contain two structural units as shown in formula (X1). In addition, the modified polyvinyl alcohol may contain one structural unit as shown in formula (X2), or it may contain two or more structural units as shown in formula (X2).

[0133] When the modified polyvinyl alcohol contains the structural unit shown in formula (X1) and / or the structural unit shown in formula (X2), the ratio of the molar amount of the structural unit shown in formula (X1) to the total molar amount of the structural units shown in formula (X1) and (X2) (X1 / (X1+X2)) is preferably 0.65 or more and 1.0 or less, more preferably 0.70 or more and 0.99 or less, even more preferably 0.85 or more and 0.99 or less, and particularly preferably 0.90 or more and 0.99 or less. When the content ratio of the structural unit shown in formula (X1) is above the aforementioned lower limit, it is easy to improve the performance as a bundling agent, for example, it is easy to suppress fiber damage when the bundled yarn is dry-mixed with the hydraulic material. It should be noted that the content (molar amount) of the structural unit (X1) and structural unit (X2) contained in the modified polyvinyl alcohol can be adjusted according to the modified polyvinyl alcohol. 1 The peaks can be determined by H-NMR, or by the monomer feed ratio during the production of modified polyvinyl alcohol.

[0134] The modified polyvinyl alcohol preferably contains at least the structural unit shown in formula (X1). In this case, when the total amount of all monomer units of the modified polyvinyl alcohol is set to 100 mol%, the amount of the structural unit shown in formula (X1) is preferably 0.1 to 10 mol%, more preferably 0.5 to 10 mol%, even more preferably 1 to 9.5 mol%, and particularly preferably 2 to 9 mol%. When the amount of the structural unit shown in formula (X1) is within the above range, it is easy to improve the performance as a bundling agent (e.g., fiber adhesion), for example, it is easy to suppress fiber damage when dry mixing the bundled yarn and the hydraulic material. In addition, it is easy to achieve rapid and sufficient fiber opening when mixing the bundled yarn with water. As a result, it is easy to increase the fiber opening rate of the bundled yarn, easy to suppress fiber agglomeration, and easy to improve the mechanical strength of the molded article.

[0135] The method for dispersing the fibers after they are added is not particularly limited as long as it allows the fibers to be dispersed in a state where they do not exist in the form of fiber aggregates. For example, when using a mixer or kneader with high mixing performance, such a mixer or kneader can be a double-arm kneader, a pressure kneader, an Eirich mixer, a high-speed mixer, a planetary mixer, a Banbury mixer, a continuous mixer, or a continuous mixing mill. This allows the manufacture of hydraulic compositions containing specific hydrophilic fibers.

[0136] In another embodiment of the present invention, as a hydraulic composition that easily suppresses deviations in the moisture content of the hydraulic composition during curing after molding, and particularly enables sufficient hydraulic reaction at surfaces prone to moisture deficiency, the present invention also provides a hydraulic composition for additive manufacturing, which is a hydraulic composition comprising hydrophilic fibers with a monofilament diameter of 70 μm or less and a water absorption rate of 6.0% or more. Regarding this hydraulic composition of another embodiment, from the viewpoint that the water absorption rate of the contained hydrophilic fibers is 6.0% or more, it has the same high moisture retention capacity as the hydraulic composition described above that comprises hydrophilic fibers with an equilibrium moisture regain of 1.5% or more, easily suppressing deviations in the moisture content of the hydraulic composition during curing after molding, and particularly enabling sufficient hydraulic reaction at surfaces prone to moisture deficiency. Regarding this hydraulic composition of another embodiment, the description and preferred features of the hydraulic composition of the present invention described above also apply.

[0137] <Water Hardening Compositions and Hardeners for Additive Manufacturing>

[0138] The hydraulic composition of the present invention is a hydraulic composition for additive manufacturing. Additive manufacturing apparatus (3D printers) typically extrude photocurable resin and hydraulic compositions from nozzles, stacking the uncured compositions into a desired shape and allowing them to harden, ultimately forming a pre-designed three-dimensional shape. In additive manufacturing using hydraulic compositions, moisture easily evaporates from surfaces exposed to air because the molds typically used in hydraulic composition manufacturing are not employed. Furthermore, the resulting three-dimensional shapes are often complex or large, making curing methods, such as sheet covering, impractical. However, the hydraulic composition according to the present invention enables uniform distribution of moisture in the cured hydraulic composition, allowing for internal curing and ensuring a thorough and uniform hydraulic reaction.

[0139] A method for manufacturing a three-dimensional shape based on an additive manufacturing apparatus includes the following method: supplying the hydraulic composition of the present invention to an additive manufacturing apparatus, and extruding it from a nozzle of the additive manufacturing apparatus to form a three-dimensional shape. For example, in order to finally obtain a pre-designed three-dimensional shape read into a computer or the like for controlling the additive manufacturing apparatus, the hydraulic composition is first ejected or extruded from a nozzle to form a two-dimensional layer. Then, the hydraulic composition is ejected or extruded from a nozzle onto the layer to form a second layer. This operation is repeated to eventually form a cured product of the hydraulic composition having the designed three-dimensional shape. The present invention also provides a cured product of the hydraulic composition of the present invention.

[0140] In the formed three-dimensional shape, a hydraulic reaction occurs, resulting in a hardened hydraulic composition. Here, the hydraulic reaction is the reaction of cement or similar materials in the hydraulic composition with water, resulting in hydration and hardening. To ensure a uniform and sufficient hydraulic reaction, it is considered necessary to retain and distribute water within the formed, hardening three-dimensional shape. If the hydraulic reaction is insufficient, the strength of the final hardened product may be low. Furthermore, if the hydraulic reaction is not uniform, cracks or fissures may sometimes occur in the final hardened product. According to the hydraulic composition of the present invention, since the hydrophilic fibers retain moisture on their surface and form a dense network within the hydraulic composition, the distribution of moisture in the hardened, molded hydraulic composition can be made uniform. Even on surfaces of molded bodies where moisture is easily lost, the hydraulic reaction can proceed sufficiently and uniformly.

[0141] By using the hydraulic composition of the present invention, it is possible to manufacture various civil / construction structures, such as embedded mold frames for bridge piers and abutments, exterior walls of buildings, and precast concrete structures with complex shapes.

[0142] Example

[0143] The present invention will be described below through examples, but the present invention is not limited to these examples. It should be noted that, unless otherwise specified, the percentages in the examples are related to quality. First, the measurement method and evaluation method are shown below.

[0144] <Mortar Mixtures>

[0145] Referring to Marchment, T. et al.: Method of enhancing interlayer bond strength in construction scale 3D printing with mortar by effective bond area amplification, Materials and Design, Vol.169, pp.1-9, 2019, mortar mixtures with the following mixing ratios were prepared.

[0146] • Cementitious material: Ordinary Portland cement (AS3972-22)

[0147] • Aggregate: Fine aggregate (average particle size 500μm and 800μm)

[0148] Other: High-performance AE water-reducing agent (polycarboxylate compound)

[0149] • Water / cementing material ratio = 0.36 / 1 (W / B)

[0150] Aggregate / Cementitious Material = 1.5 / 1 (S / B)

[0151] Water-reducing agent / cementing material = 0.02 / 1

[0152] <fiber>

[0153] (Examples 1-2, 5, 7-8 and Comparative Example 2)

[0154] PVA fibers with the physical properties shown in Table 1 were used.

[0155] (Example 3)

[0156] Rayon fibers with the physical properties shown in Table 1 were used.

[0157] (Examples 4, 6, 9 and Comparative Example 1)

[0158] Clustering agent

[0159] Bundling agent 1: Modified polyvinyl alcohol with a viscosity-uniform polymerization degree of 1500, a saponification degree of 99.5 mol%, a content of 5 mol% of structural unit (X) derived from acrylic acid, a content of 4.8 mol% of structural unit (X1), a content of 0.2 mol% of structural unit (X2), and a ratio of (X1) to the total amount of structural units (X1) and (X2) of 0.96. The functional groups X and Y in structural units (X1) and (X2) are both hydrogen atoms.

[0160] · Bundled filament

[0161] Bundled yarn 1: For each fiber having the monofilament fineness, equilibrium moisture regain, and water absorption rate described in Examples 4, 6, 9 and Comparative Examples 1 and 5 of Table 1, an aqueous solution containing bundling agent 1 at an amount of 80 g / L was added by contact at an amount of 5.5% by weight relative to the fiber mass, followed by drying to allow the bundling agent 1 to adhere to the fiber. Then, the fibers were cut to an average fiber length of 6 mm in Example 4, 8 mm in Example 6, 16 mm in Example 9, 12 mm in Comparative Example 1, and 15 mm in Comparative Example 5, thus obtaining bundled yarn.

[0162] (Comparative Example 3)

[0163] PP fibers with the physical properties shown in Table 1 were used.

[0164] <Evaluation Methods>

[0165] The single filament fineness of the fiber was determined according to JIS L1015:2021 "Test method for short chemical fibers (8.5.1)".

[0166] [Fiber length, fiber diameter, aspect ratio]

[0167] The aspect ratio is the ratio of fiber length (L) to fiber diameter (D) (L / D). In this invention, the average fiber length is calculated according to JIS L1015:2021 "Test method for short chemical fibers (8.4.1)", and the aspect ratio of the fiber is calculated by the ratio of the average fiber diameter to the average fiber length.

[0168] For the average fiber diameter, 20 fibers were randomly selected, and the fiber diameter (monofilament diameter) at the center of the length direction of each fiber was measured using an optical microscope.

[0169] [Equilibrium moisture regain]

[0170] The above-mentioned fibers were used as test samples, and their equilibrium moisture regain was determined by the following method. Referring to the test method in JIS L1015:2021 "Test Method (8.3) for Short Chemical Fibers", the samples were absolutely dried in a dryer at 105°C, and then conditioned at 20°C and 65%RH for 72 hours. The moisture content in the sample relative to the mass of the absolutely dried sample was calculated and expressed as a percentage (%). In the above determination, fibers with an equilibrium moisture regain of 1.5% or higher were considered hydrophilic fibers.

[0171] Water absorption rate

[0172] The above-mentioned fibers were used as test samples, and the water absorption rate was determined by the following method. The water absorption rate refers to the value obtained by calculating the following formula: After stirring the fibers in a 0.1 mol / L NaOH aqueous solution (pH 13) at 30°C for 4 minutes, the fibers were dehydrated by centrifugation at 3000 rpm for 5 minutes for 3 times. The mass of the fibers after centrifugation and dehydration was then dried in a dryer at 100°C for 16 hours.

[0173] Formula: Water absorption rate = 100 × (AB) / B (%)

[0174] <Example 1>

[0175] The mortar compound prepared as described above was mixed with PVA fibers having the physical properties shown in Table 1, such that the volume ratio of hydrophilic fibers in the hydraulic composition reached 2%, thus producing a hydraulic composition. This hydraulic composition was then poured into a mold frame with internal dimensions of a cuboid (W240mm × D60mm × H10mm), and cured for 28 days at 20°C and 40% RH with the upper surface open, yielding a hardened product.

[0176] <Examples 2-9 and Comparative Examples 1-3 and Comparative Example 5>

[0177] By replacing the PVA fibers with fibers having the properties shown in Table 1, the hydraulic composition and the cured product were obtained in the same manner as in Example 1. It should be noted that in Examples 4, 6, 9 and Comparative Examples 1 and 5, the hydraulic composition was prepared by mixing the complex with bundled filaments of fibers having the properties shown in Table 1.

[0178] <Comparative Example 4>

[0179] PVA particles with the physical properties shown in Table 1 were used instead of PVA fibers. Otherwise, the hydraulic composition and the hardened product were obtained in the same manner as in Example 1.

[0180] <Comparative Example 6>

[0181] Without the addition of PVA fibers, the hydraulic composition and hardened material were obtained in the same manner as in Example 1.

[0182] <Evaluation Methods for Hydraulic Compositions and Hardened Products>

[0183] The fibers, hydraulic compositions of the examples and comparative examples, and hardened products obtained as described above were evaluated as follows. The results are shown in Table 1.

[0184] [Liquidity]

[0185] The flowability of the hydraulic compositions manufactured in the examples and comparative examples was evaluated using the flow test, section 12 of JIS R 5201:2015 "Physical Test Methods for Cement". The flow values ​​were evaluated according to the following evaluation criteria.

[0186] ○:120mm or more

[0187] △: 100mm or more and less than 120mm

[0188] ×: Less than 100mm

[0189] [Dispersion]

[0190] The dispersion of fibers in the hydraulic composition was determined by the following steps.

[0191] 20g of the hydraulic composition was collected and coated onto a 40-mesh metal mesh with uniform thickness. It was immediately washed with water to remove the cementitious material. Fibers were extracted from the residue on the metal mesh. For each fiber, dispersed fibers and undispersed fibers (fibers that were not opened or had aggregated) were collected separately using tweezers. After drying at 100°C for 24 hours, the mass (W) of the dispersed fibers was measured. f(Unit: g) and the mass of undispersed bundled fibers (W) g (Unit: g). The dispersion is calculated using the following formula.

[0192] Dispersion [%] = (W f / (W f +W g ))×100

[0193] The following evaluation criteria were used to assess the degree of dispersion.

[0194] ○:More than 80%

[0195] △: 60% or more but less than 80%

[0196] ×: Less than 60%

[0197] [Volume ratio of hydrophilic fibers]

[0198] For the volume ratio of the fibers when the volume of the hydraulic composition is set to 100, the total volume V of the hydraulic composition and the fiber volume V are calculated based on the specific gravity and weight of the materials constituting the hydraulic composition. f And use them to perform calculations using the following formula.

[0199] Fiber volume ratio = V f / V×100(%)

[0200] [W / B]

[0201] The ratio of W to B (W / B) is calculated based on the total mass (B) [g] of the cementitious material (cement) and the mass (W) [g] of the water in the hydraulic composition.

[0202] [Surface / Internal Reaction Rate Ratio (Cure Effectiveness)]

[0203] For the hardened products obtained in the examples and comparative examples, the reaction rate R of the cement on the upper surface corresponding to the surface was determined by small-angle scattering (SAXS). A And the reaction rate R of the cement on the inner bottom surface. B The reaction rate ratio (R) of the upper surface to the bottom surface was calculated. A / R B ×100)[%], the maintenance effect was evaluated using the following evaluation criteria.

[0204] ○:More than 80%

[0205] △: 70% or more but less than 80%

[0206] ×: Less than 70%

[0207]

[0208] It has been confirmed that the hydraulic composition of the present invention exhibits a high surface / internal reaction ratio even under dry curing conditions. The reason for this is not yet clear, but it can be considered that the fine fibers with low monofilament fineness or small monofilament diameter dispersed in the hydraulic composition sufficiently increase the fiber surface area and form a fiber network, resulting in excellent water retention and water diffusivity, thus exhibiting a high surface / internal reaction ratio even under dry curing conditions. Furthermore, the cured product manufactured in this way has high and consistent strength. In contrast, in the cases of hydraulic compositions containing fibers with high monofilament fineness in Comparative Examples 1, 2, and 5, the coarse fibers cannot sufficiently ensure the fiber surface area, failing to improve the curing effect brought by the fibers, resulting in a low surface reaction ratio. Additionally, in the case of the hydraulic composition in Comparative Example 3 containing fibers with low equilibrium moisture regain, the weak moisture retention also prevents the improvement of the curing effect brought by the fibers, resulting in a low surface reaction ratio. Furthermore, in the case of Comparative Example 4 using PVA particles, it can be considered that since they are not fibers, a network cannot be formed, and water diffusivity cannot be obtained, resulting in a low surface reaction ratio. In addition, in Comparative Example 6 where no hydrophilic fibers were added, insufficient moisture was present during curing, resulting in inadequate hardening reaction on the surface.

Claims

1. A hydraulic composition, which is used in additive manufacturing. The hydraulic composition comprises hydrophilic fibers, wherein the monofilament fineness of the hydrophilic fibers is less than 50 dtex or the monofilament fiber diameter is less than 70 μm, and the equilibrium moisture regain is greater than 1.5%.

2. The hydraulic composition according to claim 1, wherein, The hydrophilic fiber has a single filament fineness of less than 15 dtex.

3. The hydraulic composition according to claim 1 or 2, wherein, The hydrophilic fiber has a water absorption rate of 6.0% or higher.

4. The hydraulic composition according to claim 1 or 2, wherein, The aspect ratio of the hydrophilic fiber is 50 to 400.

5. The hydraulic composition according to claim 1 or 2, wherein, The hydrophilic fiber has a fiber length of less than 10 mm.

6. The hydraulic composition according to claim 1 or 2, wherein, When the volume of the matrix of the hydraulic composition is set to 100, the volume ratio of the hydrophilic fibers is 0.1~10%.

7. The hydraulic composition according to claim 1 or 2, wherein, The hydrophilic fiber has a single filament fineness of 0.1 dtex or higher.

8. The hydraulic composition according to claim 1 or 2, wherein, The hydrophilic fiber has a fiber length of 0.5 mm or more.

9. The hydraulic composition according to claim 1 or 2, wherein, The hydrophilic fibers in the hydraulic composition have a dispersion of 60% or more.

10. The hydraulic composition according to claim 1 or 2, wherein, In the hydraulic composition, the ratio of the mass of water (W) to the total mass of the cementitious material (B) (W / B) is 0.1 to 0.

40.

11. A hardened material, which is a hardened form of the hydraulic composition according to claim 1 or 2.

12. A hydrophilic fiber used in the additive manufacturing of a hydraulic composition molded article, wherein the hydrophilic fiber has an equilibrium moisture regain of 1.5% or more and / or a water absorption of 6.0% or more, a monofilament fineness of 50 dtex or less and / or a monofilament fiber diameter of 70 μm or less.

13. A bundled filament used in the additive manufacturing of a hydraulic composition molded article, said bundled filament having an equilibrium moisture regain of 1.5% or more and / or a water absorption of 6.0% or more, a filament fineness of 50 dtex or less and / or a filament fiber diameter of 70 μm or less.

14. A hydraulic composition for additive manufacturing, The hydraulic composition comprises hydrophilic fibers, wherein the monofilament diameter of the hydrophilic fibers is less than 70 μm and the water absorption rate is greater than 6.0%.

15. The hydraulic composition according to claim 14, wherein, The hydrophilic fibers in the hydraulic composition have a fiber length of 16 mm or less.

Citation Information

Patent Citations

  • Extrusion lamination method for fiber-reinforced mortar

    JP2022124859A

  • Bundled yarn, hydraulic composition and molded body

    WO2020137466A1