Metal compounds for ALD applications
By using scandium complexes with specific alkyl-substituted formamidinyl ligands as precursors, the problems of high melting point and low vapor pressure of existing scandium compounds in the ALD process were solved, and high-quality scandium-containing thin films were deposited efficiently.
Patent Information
- Application Number
- CN202580028500.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-04-19
- Filing Date
- 2025-04-16
- Publication Date
- 2026-11-17
AI Technical Summary
Existing scandium compounds used in ALD processes have high melting points, low vapor pressures, and insufficient thermal stability, making it difficult to form high-quality, uniform scandium-containing films.
Scandium complexes with specific alkyl-substituted formamidinyl ligands, such as tris(N,N'-diethyl-formamidinyl)scandium, are used as precursors for chemical vapor deposition and atomic layer deposition to lower the melting point and increase the vapor pressure, ensuring high thermal stability and volatility.
Scandium complexes with high vapor pressure and high thermal stability that are liquid at room temperature or slightly above room temperature have been developed, enabling the high-productivity formation of high-quality scandium-containing thin films suitable for CVD and ALD methods.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] The present invention relates to scandium complexes and, in particular, to a method for depositing scandium-containing films using these complexes as precursors by atomic layer deposition. Background Technology
[0002] Metal-containing films are used in semiconductor and electronic applications. Chemical vapor deposition (CVD) and atomic layer deposition (ALD) have been used as the main deposition techniques for producing thin films for semiconductor devices. These methods enable conformal films (metals, metal oxides, metal nitrides, metal silicides, etc.) to be formed via a chemical reaction of a metal-containing compound (precursor). This chemical reaction occurs on surfaces and other surfaces that may contain metals, metal oxides, metal nitrides, metal silicides, etc. In CVD and ALD, precursor molecules play a crucial role in achieving high-quality films with high conformability and low impurities. The precursor needs to have an appropriate vapor pressure and sufficient thermal stability. Additionally, it needs to be able to vaporize at a stable supply to form a thin film via CVD or ALD. The substrate temperature in CVD and ALD processes is an important consideration in selecting precursor molecules. Precursor molecules should preferably be stable at typical substrate temperatures (e.g., in the range of 150°C to 600°C). Furthermore, it is preferable that the precursor can be delivered to the reaction vessel in either the liquid or gas phase. Liquid-phase delivery of precursors at their evaporation temperatures generally delivers the precursor to the reaction vessel more uniformly than solid-phase precursors. While it is sufficient for the precursor to be liquid at the delivery temperature, it is preferable that the precursor is liquid at or near room temperature. This has the advantage that condensation is less likely to occur if any cold spots exist in the precursor delivery system. Additionally, handling compounds that are liquid at or slightly above room temperature is technically easier, for example, by filling the container to which the precursor is applied.
[0003] The ALD process uses two or more different vapor phase precursors to deposit thin layers of solid material. The substrate surface to be deposited is exposed to a specific dose of a first precursor vapor. Any excess unreacted vapor from that precursor is then removed, for example, by purging with an inert gas. Next, a second vapor dose of the precursor is brought to the surface and allowed to react. This cycle can be repeated to build thicker films. A particularly important aspect of this process is that the ALD reaction is self-limiting, meaning that only a certain maximum thickness can be formed in each cycle, and no further deposition occurs during that cycle, even if excess reactant is available. Due to this self-limiting characteristic, the ALD reaction produces coatings with highly uniform thickness not only on flat substrate surfaces but also in narrow holes and trenches, as well as other three-dimensional surfaces, making this technology indispensable to the semiconductor industry.
[0004] Scandium-containing thin films hold significant technological importance for the semiconductor industry. Such films can contain metallic scandium or scandium compounds, such as scandium(III) Sc₂O₃, scandium(III) Sc₂S₃ sulfide, scandium(III) ScN nitride, or mixed metal materials including scandium. Due to the increasing demand for highly conformal, polar thin films containing scandium in semiconductor manufacturing processes (especially dielectric film deposition), it is advantageous to use highly volatile compounds with low melting points and low and wide ALD windows as precursors for scandium-containing ALDs. Scandium-containing ALDs have been used to deposit electrically insulating materials with high dielectric constants (high-k dielectrics), serving as gate insulators in high-speed transistors and as ultrathin gate interlayers in the integration of new channel materials and high-performance capacitors.
[0005] Amidinate metal (AMD) complexes are commonly referred to as precursors for scandium-containing films deposited via ALD. For example, WO2004 / 046417 discloses the use of volatile amidinate metals in ALD applications and covers a variety of metals and different substituted amidinate ligands, wherein the amidinate ligands may be substituted, for example, with alkyl, aryl, or alkynyl groups. Examples disclose complexes having various transition metals and group metals, wherein the amidinate ligands are substituted with isopropyl, sec-butyl, and / or tert-butyl groups. Examples containing scandium are not disclosed. Furthermore, it is suggested to use longer alkyl chains and / or alkyl chains having more than one stereoisomer as substituents on the amidinate group to lower the melting point.
[0006] US2023 / 0058025A1 discloses amido-scandium complexes, particularly acetamipridonium complexes, wherein the substituents on each nitrogen atom of the ligand are distinct from one another. The compound disclosed in example Sc(Amd-Me,Et)3 (i.e., tris(N-methyl-N'-ethyl-acetamipridonium)scandium) has a melting point of 67°C, and the TGA... 50% The temperature at which 50% weight loss occurs is 215°C. Significant decomposition occurs during evaporation, as can be seen from the residue that cannot be evaporated. Complexes containing formamidinyl ligands are not disclosed in the examples.
[0007] KR10-2614467B1 discloses various amido-scandium complexes, some of which are liquids at room temperature. Examples of the complexes disclosed are Sc(Et2nPr-AMD)3 (i.e., tris(N,N'-diethyl-butylamidine)scandium) and Sc(Et2Et-AMD)3 (i.e., tris(N,N'-diethyl-propanedi)scandium).
[0008] Other amido-scandium complexes are known, such as tris(N,N'-diisopropyl-ethamidinyl)scandium from P. de Rouffignac et al., Electrochemical and Solid State Letters 2006, 9(6), F45-F48, or tris(N,N'-diethyl-ethamidinyl)scandium from H. Wang et al., Electrochemical and Solid State Letters 2009, 12(4), G13-G15, or KHKim et al., Applied Physics Letters 2006, 89, 133512. These materials exhibit high evaporation temperatures. Additionally, tris(N,N'-diisopropyl-methamidinyl)scandium is commercially available. This compound has a melting point of 269 °C.
[0009] In methods for forming thin films via compound vaporization (e.g., CVD or ALD methods), the compounds used as film formation precursors (reactants) need to possess the following important properties: high vapor pressure; low melting point, and preferably being liquid at or slightly above room temperature; high thermal stability; and the ability to produce high-quality films with high productivity, i.e., high reactivity to surfaces, co-reactants, and deposition materials, and a clean reaction, i.e., the reaction substantially does not produce any undesirable byproducts on the surface. As discussed above, there is still room for improvement regarding prior art scandium compounds. Therefore, the objective of this invention is to provide novel compounds that, compared to prior art scandium compounds, have high vapor pressure, low melting point, and can produce high-quality films with high productivity when used as film formation feedstocks.
[0010] Surprisingly, compared to scandium complexes known in the prior art, scandium complexes comprising specific alkyl-substituted formamidinyl ligands were found to significantly reduce the melting temperature and, in particular, the evaporation temperature of the scandium complexes. Furthermore, these compounds exhibit suitable thermal stability and volatility and can be used in CVD or ALD processes to form scandium-containing films. Thus, such compounds are the subject of this invention. Summary of the Invention
[0011] The disclosed and claimed subject matter relates to compounds of the following formula (1):
[0012]
[0013] Equation (1)
[0014] Where R N1 R N2 Each time it appears, it is either ethyl or n-propyl, and the compound may be partially or completely deuterated.
[0015] In compound (1), the group [R] N1 N-CH-NR N2 ] - Each of them is called a "ligand" or "formamidinyl ligand".
[0016] The disclosed and claimed subject matter further includes compositions and formulations containing compounds of formula (1), methods for depositing scandium-containing films using compounds of formula (1) as precursors, and scandium-containing films derived from compounds of formula (1). Detailed Implementation
[0017] All references cited in this article (including publications, patent applications and patents) are incorporated herein by reference to the extent that each reference is explicitly stated to be incorporated herein by reference and described in its entirety.
[0018] Unless otherwise specified herein or expressly contradictory, the use of the terms “a,” “an,” “the,” and similar indicators in the context of describing the disclosed and claimed subject matter (especially in the context of the following claims) shall be construed as covering both singular and plural. Unless otherwise stated, the terms “comprising,” “having,” “including,” and “containing” shall be construed as open-ended terms (i.e., meaning “including but not limited to”). Unless otherwise specified herein, the description of value ranges herein is merely intended as a shorthand for each individual value falling within that range, and each individual value is incorporated into this specification as if it were individually cited herein. Unless otherwise specified herein or expressly contradictory, all methods described herein may be performed in any suitable order. Unless otherwise claimed, the use of any and all instances or exemplary language (e.g., “such as”) provided herein is intended only to better set forth the disclosed and claimed subject matter and does not constitute a limitation on the scope of the disclosed and claimed subject matter. No language in this specification shall be construed as indicating any non-claimed element necessary to practice the disclosed and claimed subject matter. The use of the terms “comprising” or “including” in this specification and claims includes the narrower language of “consisting substantially of” and “comprises of”.
[0019] This document describes embodiments of the disclosed and claimed subject matter, including the best practices known to the inventors for carrying out the disclosed and claimed subject matter. Variations of these embodiments will become apparent to those skilled in the art upon reading the foregoing description. The inventors expect those skilled in the art to appropriately employ such variations, and the inventors expect to practice the disclosed and claimed subject matter in ways other than those specifically described herein. Therefore, the disclosed and claimed subject matter includes all modifications and equivalents of the subject matter listed in the appended claims permitted by applicable law. Furthermore, unless otherwise specified herein or otherwise clearly contradicted, the disclosed and claimed subject matter encompasses any combination of the foregoing elements in all possible variations.
[0020] When describing the use of the compounds in CVD or ALD deposition techniques, the compounds of the present invention are also referred to as “precursors” or “reactants”.
[0021] For ease of reference, "microelectronic device" or "semiconductor device" refers to semiconductor wafers on which integrated circuits, memory, and other electronic structures are fabricated, as well as flat panel displays, phase-change memory devices, solar panels, and other products manufactured for use in microelectronic, integrated circuit, or computer chip applications (including solar substrates, photovoltaic devices, and microelectromechanical systems (MEMS)). Solar substrates include, but are not limited to, silicon, amorphous silicon, polycrystalline silicon, monocrystalline silicon, CdTe, copper indium selenide, copper indium sulfide, and gallium arsenide. Solar substrates may be doped or undoped. It should be understood that the terms "microelectronic device" or "semiconductor device" are not intended to be limited in any way and include any substrate that will ultimately become a microelectronic device or microelectronic assembly.
[0022] As defined herein, the term "barrier material" refers to any material in the art used to seal metal wires (e.g., copper interconnects) to minimize the diffusion of that metal (e.g., copper) into dielectric materials. Preferred barrier layer materials include tantalum, titanium, ruthenium, hafnium, and other refractory metals and their nitrides and silicides.
[0023] "Substantially contains" is defined herein as less than 0.001 wt%. "Substantially contains" also includes 0.000 wt%. The term "containing" means 0.000 wt%. As used herein, "about" or "approximately" is intended to correspond to within ± 5% of the stated value.
[0024] In all such compositions, where the specific components of the composition are discussed with reference to a range including a lower limit of 0 for weight percentages (or “weight%” or “wt%”), it should be understood that such a component may or may not be present in the various specific embodiments of the composition, and where such a component is present, it may be present at a concentration as low as 0.001 wt% based on the total weight of the composition employing that component. All percentages of components are weight percentages and are based on the total weight of the composition, i.e., 100%.
[0025] Furthermore, when referring to the compositions described herein by weight % or wt%, it should be understood that the sum of the wt% of all components (including non-essential components, such as impurities) should not exceed 100 wt%. In compositions “consisting substantially of the listed components,” such components may total 100 wt% or may total less than 100 wt%. When the total components are less than 100 wt%, such compositions may contain small amounts of non-essential contaminants or impurities. For example, in one embodiment, the formulation may contain 2 wt% or less of impurities. In another embodiment, the formulation may contain 1 wt% or less of impurities. In yet another embodiment, the formulation may contain 0.05 wt% or less of impurities. In other such embodiments, the ingredients may form at least 90 wt%, more preferably at least 95 wt%, more preferably at least 99 wt%, more preferably at least 99.5 wt%, and most preferably at least 99.9 wt%, and may contain other components that do not affect or significantly affect the performance of the formulation. Otherwise, if there are no significant non-essential impurity components, it should be understood that all the basic components of the composition are substantially totaled 100 wt%.
[0026] Any reference to “one or more” or “at least one” includes “two or more” and “three or more”, etc.
[0027] The headings used in this article are not intended to be restrictive; rather, they are included for organizational purposes only.
[0028] In a preferred embodiment of the invention, the three formamidinyl ligands in the compound of formula (1) are identical. Thus, preferably, all groups R... N1 The same and all groups R N2 Same. R N1 and R N2 They may be the same or different, but R is preferred. N1 and R N2 Same. In another preferred embodiment, R N1 It is an ethyl group.
[0029] R N1 and R N2 The suitable combinations are the compounds listed in Table 1.
[0030] Table 1:
[0031]
[0032] Compound 1, i.e., R, is particularly preferred. N1 = R N2 =A compound of ethyl groups.
[0033] Preferably, the compound of formula (1) or the preferred embodiment is substantially free of impurities. In particular, this refers to metallic impurities, organic byproducts, and halogen impurities. The content of each impurity metal element is preferably 10 ppm or less, more preferably 1 ppm or less, and their total content is preferably 50 ppm or less, more preferably 10 ppm or less. The total content of impurity halogens is preferably 100 ppm or less, more preferably 10 ppm or less, and most preferably 1 ppm or less.
[0034] Compounds of formula (1) and preferred embodiments can be synthesized by reacting a suitable scandium precursor ScX3 (where X is a counterion, such as a halogen (F, Cl, Br, I, preferably Cl); trifluoromethanesulfonate or toluenesulfonate) with a desired formamidinium salt (e.g., LifAMD, NafAMD, or KfAMD, preferably LifAMD, where fAMD represents the correspondingly substituted formamidinium group). Formamidinium salts can be prepared in situ from the corresponding formamidinium by deprotonation in a solvent, preferably a polar or nonpolar aprotic solvent, such as THF, dioxane, diethyl ether, methyl-tert-butyl ether, dibutyl ether, hexane, pentane, or toluene or mixtures thereof.
[0035] Therefore, the present invention further relates to a method for manufacturing a compound of formula (1) or a preferred embodiment, wherein the compound ScX3 (where X is a counterion, preferably F, Cl, Br, I; trifluoromethanesulfonate or toluenesulfonate, and especially preferably Cl) is reacted with a formamidinium salt (preferably Li, Na or K salt, and especially preferably Li salt).
[0036] How to use
[0037] The disclosed compounds can be used as precursors (reactants) for depositing scandium-containing films using any chemical vapor deposition process known to those skilled in the art. Precursors for film formation (also referred to as "film formation precursors") include the compounds of this invention and optionally other compounds, depending on the manufacturing process to which the precursor is applied. For example, when producing a film containing only scandium as a metal, the film formation precursors of this invention do not contain any metal compounds other than those represented by general formula (1). Meanwhile, when producing a film containing two or more metals, the film formation precursors of this invention may contain compounds containing desired metals other than those represented by general formula (1). The film formation precursors of this invention may further contain organic solvents. As explained above, the physical properties of the compounds represented by general formula (1) are suitable for use as precursors in CVD processes, and thus the film formation precursors of this invention can be used as CVD precursors. In particular, the film formation precursors of this invention are especially suitable for ALD processes because the compounds represented by general formula (1) exhibit self-limiting reaction behavior on the surface, i.e., they do not react with the adsorbed surface precursor material.
[0038] As used herein, the term "chemical vapor deposition process" (CVD) refers to any process that exposes a substrate to a reaction and / or decomposition on the substrate surface to produce one or more volatile precursors to be deposited. As used herein, the term "atomic layer deposition process" (ALD) refers to a self-limiting (e.g., the amount of film material deposited in each reaction cycle is constant) sequential surface chemistry for depositing a film of material onto a substrate of different compositions. Although precursors, reagents, and co-reagents used herein may sometimes be described as "gaseous," it should be understood that precursors may be liquid or solid at room temperature and / or high temperatures, and may be transported to the reactor via direct vaporization, bubbling, or sublimation, with or without the use of inert gases. In some cases, vaporized precursors may be transported via a plasma generator. As used herein, the term "reactor" includes, but is not limited to, reaction chambers (reaction vessels, deposition chambers).
[0039] Chemical vapor deposition processes in which the disclosed and claimed compounds can be used as precursors include, but are not limited to, those used for manufacturing semiconductor-type microelectronic devices (e.g., ALD, CVD, pulsed CVD, plasma-enhanced ALD (PEALD), and / or plasma-enhanced CVD (PECVD)). Examples of suitable deposition processes for the methods disclosed herein include, but are not limited to, circulating CVD (CCVD), MOCVD (metal-organic CVD), thermochemical vapor deposition, plasma-enhanced chemical vapor deposition (“PECVD”), high-density PECVD, photon-assisted CVD, plasma-photon-assisted (“PPECVD”), low-temperature chemical vapor deposition, chemical-assisted vapor deposition, hot-filament chemical vapor deposition, CVD of liquid polymer precursors, deposition from supercritical fluids, low-energy CVD (LECVD), roll-to-roll ALD, space ALD, and atmospheric pressure ALD. In some embodiments, scandium-containing films are deposited via atomic layer deposition (ALD), plasma-enhanced ALD (PEALD), or plasma-enhanced circulating CVD (PECCVD) processes.
[0040] In one embodiment, a scandium-containing film is deposited using an ALD process. In another embodiment, a scandium-containing film is deposited using a CCVD process. In yet another embodiment, a thermal CVD process is used to deposit the scandium-containing film.
[0041] There are no particular limitations on suitable substrates for depositing the disclosed and claimed precursors, and the choice varies depending on the intended end use. For example, the substrate may be selected from oxides, such as HfO2-based materials, TiO2-based materials, ZrO2-based materials, rare earth oxide-based materials, ternary oxide-based materials, etc.; or nitride-based materials. Other substrates may include solid substrates, such as metal substrates (e.g., Au, Pd, Rh, Ru, W, Al, Ni, Ti, Co, Pt), substrates containing metal silicides (e.g., TiSi2, CoSi2, and NiSi2); substrates containing metal nitrides (e.g., TaN, TiN, WN, TaCN, TiCN, TaSiN, and TiSiN); semiconductor materials (e.g., Si, SiGe, GaAs, InP, diamond, GaN, and SiC); insulators (e.g., SiO2, Si3N4, SiON, HfO2, Ta2O5, ZrO2, TiO2, Al2O3, and barium strontium titanate) and combinations thereof. Preferred substrates include TiN, Ru, and Si type substrates.
[0042] In such deposition methods and processes, co-reactants (e.g., oxidants) are typically used. The term "oxidant" in this application should be understood to refer to a chemical compound that transfers oxygen to the scandium-containing film. Oxidants are typically introduced in gaseous form. Examples of suitable oxidants include, but are not limited to, oxygen, water vapor, ozone, oxygen plasma, or mixtures thereof.
[0043] Other possible co-reactants are reducing agents, such as H2, H2 plasma, hydrazine, or aminoborane; nitrogen-containing co-reactants, such as hydrazine, NH3, N2, or N2 plasma; sulfur-containing co-reactants, such as H2S or elemental sulfur; or peroxides, such as H2O2 or HOOtBu.
[0044] Deposition methods and processes may also involve a purging step typically performed using one or more purge gases. The purge gas used to remove unconsumed reactants and / or reaction byproducts is an inert gas that does not react with the precursors and the formed film. Exemplary purge gases include, but are not limited to, argon (Ar), nitrogen (N2), helium (He), neon (Ne), and mixtures thereof. For example, a purge gas (e.g., Ar) is supplied to the reactor at a flow rate between about 10 sccm and about 2000 sccm for about 0.1 to 10000 seconds, thereby purging unreacted material and any byproducts that may remain in the reactor.
[0045] The deposition methods and processes require the application of energy to at least one of the precursors, co-reactants, or combinations thereof to induce a reaction and form a scandium-containing film or coating on a substrate. Such energy can be provided by, but is not limited to, temperature (thermally induced), plasma, pulsed plasma, helical wave plasma, high-density plasma, inductively coupled plasma, X-rays, electron beams, photons, remote plasma methods, and combinations thereof. In some processes, a secondary RF frequency source can be used to alter the plasma characteristics of the substrate surface. When utilizing plasma, the plasma generation process can include a direct plasma generation process where plasma is generated directly in a reactor, or alternatively, a remote plasma generation process where plasma is generated outside the reactor and supplied to the reactor.
[0046] When used in such deposition methods and processes, suitable precursors (e.g., the compounds of the present invention) can be delivered to the reaction chamber (e.g., a CVD or ALD reactor) in various ways. A preferred method of delivering the precursor to the reaction chamber is by vaporization, such as by vacuum-driven thermal vaporization or active vaporization using a carrier gas. In other cases, liquid delivery systems or combined liquid delivery and rapid vaporization process units can be employed to enable the volumetric delivery of low-volatility materials, resulting in reproducible transport and deposition without precursor thermal decomposition. The precursor compositions described herein can be effectively used as reagents to provide the vapor of the metal precursor to an ALD or CVD reactor via direct liquid injection (DLI) or vacuum-driven vaporization. Vacuum-driven vaporization is a preferred method for delivering the precursors of the present invention.
[0047] When used in this deposition method and process, the disclosed and claimed compounds may contain hydrocarbon solvents, which are particularly desirable because they can be dried to sub-ppm water content. Exemplary hydrocarbon solvents that may be used in the precursors include, but are not limited to, toluene, mesitylene, cumene, p-isopropyltoluene, 1,3-diisopropylbenzene, octane, dodecane, 1,2,4-trimethylcyclohexane, n-butylcyclohexane, and decahydronaphthalene. The disclosed and claimed compounds may also be stored and used in stainless steel containers. In some embodiments, the hydrocarbon solvent is a high-boiling solvent or has a boiling point of 100°C or higher. The disclosed and claimed compounds may also be mixed with other suitable metal compounds (which may be used as precursors), and the mixture may be used to simultaneously deliver two metals to grow a binary metal film.
[0048] During precursor pulsation, an argon stream and / or other gas stream may be used as a carrier gas to aid in the delivery of vapor containing at least one of the disclosed and claimed precursors to the reaction chamber. During precursor delivery, the process pressure in the reaction chamber is between 1 Torr and 50 Torr, preferably between 5 Torr and 20 Torr.
[0049] Substrate temperature is a crucial process variable in the deposition of high-quality scandium-containing films. Typically, the substrate temperature ranges from approximately 100°C to approximately 550°C. Higher temperatures can promote higher film growth rates but may result in bulk CVD rather than ALD. Additionally, at higher substrate temperatures, precursors risk desorption from the substrate, leading to lower growth rates. Conversely, if the substrate temperature is not high enough, it may be too low to allow sufficient reaction between the precursor and the surface, also resulting in lower growth rates, and / or precursor condensation on the surface, which could increase the growth rate.
[0050] In view of the foregoing, those skilled in the art will recognize that the disclosed and claimed subject matter further includes the use of the disclosed and claimed compounds as precursors in chemical vapor deposition (CVD) processes.
[0051] In one embodiment, the disclosed and claimed subject matter includes a method for forming a scandium-containing film on at least one surface of a substrate, comprising the following steps:
[0052] (a) Providing at least one surface of the substrate in the reaction vessel; and
[0053] (b) A scandium-containing film is formed on at least one surface using a deposition process selected from chemical vapor deposition (CVD) and atomic layer deposition (ALD) processes, with at least one compound of formula (1) or a preferred embodiment as a scandium source compound precursor for the deposition process.
[0054] In another aspect of this embodiment, the method includes introducing at least one co-reactant into a reaction vessel. The co-reactant is a reactant other than those used in the in vitro deposition of scandium-containing films prior to this invention. In another aspect of this embodiment, the method includes introducing at least one co-reactant into a reaction vessel, wherein the at least one co-reactant is selected from the group consisting of water, oxygen (O2), oxygen plasma, ozone (O3), NO, N2O, NO2, CO, CO2, and combinations thereof. These co-reactants are typically used to form metal oxide thin films. In another aspect of this embodiment, the method includes introducing at least one co-reactant into a reaction vessel, wherein the at least one co-reactant is selected from the group consisting of ammonia, hydrazine, monoalkylhydrazine, dialkylhydrazine, nitrogen, nitrogen / hydrogen, ammonia plasma, nitrogen plasma, nitrogen / hydrogen plasma, and combinations thereof. These co-reactants are typically used to form metal nitride thin films, but ammonia, hydrazine, monoalkylhydrazine, dialkylhydrazine, ammonia plasma, and combinations thereof can also be used to form metal films. In another aspect of this embodiment, the method includes introducing at least one co-reactant into a reaction vessel, wherein the at least one co-reactant is selected from the group consisting of hydrogen, hydrogen plasma, mixtures of hydrogen and helium, mixtures of hydrogen and argon, hydrogen / helium plasma, hydrogen / argon plasma, boron-containing compounds, silicon-containing compounds, and combinations thereof. These co-reactants are typically used to form metal films, i.e., to form elemental metals.
[0055] In one embodiment, the disclosed and claimed subject matter includes a method for forming a scandium-containing film via an atomic layer deposition (ALD) process or an ALD-like process, comprising the following steps:
[0056] (a) Providing a substrate in the reaction vessel;
[0057] (b) Introduce one or more of the compounds of formula (1) or those in the preferred embodiments as precursors into the reaction vessel;
[0058] (c) Purging procedure, particularly purging the reaction vessel with a first purging gas;
[0059] (d) Introduce the co-reactants into the reaction vessel;
[0060] (e) Purging steps, particularly purging the reaction vessel with a second purging gas;
[0061] (f) Repeat steps (b) to (e) in sequence until a scandium-containing film of the desired thickness is obtained.
[0062] Depending on the desired composition of the resulting scandium-containing film, steps (b), (c), (d), and (e) may also be repeated using the second co-reactant from step (d) and optionally the third or other co-reactants, and the purging steps may be repeated using the third purge gas and optionally the fourth or other purge gas.
[0063] Additionally, in step (b), two or more precursors may be introduced, at least one of which is a compound of formula (1) or a preferred embodiment. These two or more precursors may be introduced as a mixture from the same container or from different containers.
[0064] Additionally, two or more co-reactants may be introduced in step (d). These two or more co-reactants may be introduced as a mixture from a container of the same source or from different containers.
[0065] In another aspect of this embodiment, the co-reactant is selected from one or more oxygen-containing co-reactants, including water, O2, oxygen plasma, O3, NO, N2O, NO2, CO, CO2, and combinations thereof. In another aspect of this embodiment, the co-reactant is selected from one or more nitrogen-containing co-reactants, including ammonia, hydrazine, monoalkylhydrazine, dialkylhydrazine, nitrogen, nitrogen / hydrogen, ammonia plasma, nitrogen plasma, nitrogen / hydrogen plasma, and mixtures thereof. In another aspect of this embodiment, the co-reactant is selected from hydrogen, hydrogen plasma, mixtures of hydrogen and helium, mixtures of hydrogen and argon, hydrogen / helium plasma, hydrogen / argon plasma, boron-containing compounds, silicon-containing compounds, and combinations thereof. In another aspect of this embodiment, the first purge gas and the second purge gas of this method are each independently selected from one or more of argon, nitrogen, helium, neon, and combinations thereof. Alternatively or additionally, a vacuum may be used for one or more purge steps. In another aspect of this embodiment, the method further includes applying energy to at least one of the precursor, co-reactant, substrate, and combinations thereof, wherein the energy is one or more of heat, plasma, pulsed plasma, helical wave plasma, high-density plasma, inductively coupled plasma, capacitively coupled plasma, X-ray, electron beam, photon, remote plasma method, and combinations thereof. In a preferred aspect of this embodiment, step (b) of the method includes introducing the precursor into the reaction vessel using thermal energy and vacuum. In another aspect of this embodiment, step (b) of the method further includes introducing the precursor into the reaction vessel using a carrier gas flow to deliver the vapor of the precursor into the reaction vessel. In another aspect of this embodiment, step (b) of the method further includes using a solvent medium including toluene, mesitylene, isopropylbenzene, 4-isopropyltoluene, 1,3-diisopropylbenzene, octane, dodecane, 1,2,4-trimethylcyclohexane, n-butylcyclohexane, and decahydronaphthalene, and combinations thereof.
[0066] The shape of the substrate is not particularly limited and can be, for example, plate-shaped, spherical, fibrous, or scaly. The surface of the substrate can be planar or can have a three-dimensional structure (e.g., trench structure).
[0067] Furthermore, examples of the production conditions mentioned above include reaction temperature (substrate temperature), reaction pressure, and deposition rate. The reaction temperature is preferably room temperature to 500°C, more preferably 100°C to 300°C. Additionally, the reaction pressure is preferably 10 Pa to atmospheric pressure in the case of thermal CVD or optical CVD, and preferably 10 Pa to 2,000 Pa in the case of using plasma. For ALD, when performing this step, the pressure in the system (in the film formation chamber) is preferably 1 Pa to 10,000 Pa, more preferably 10 Pa to 1,000 Pa.
[0068] Furthermore, the deposition rate can be controlled by the precursor supply conditions (vaporization temperature and vaporization pressure), reaction temperature, and reaction pressure. At high deposition rates, the properties of the desired film may degrade. At low deposition rates, productivity issues may occur. Therefore, for CVD processes, the deposition rate is preferably from 0.01 nm / min to 100 nm / min, more preferably from 1 nm / min to 50 nm / min. In the case of the ALD method, the deposition rate is controlled by the number of cycles to obtain the desired film thickness. In the ALD process, typical deposition rates are 0.01 nm / cycle to 0.2 nm / cycle, more typically 0.05 nm / cycle to 1.3 nm / cycle. Additionally, as mentioned above, a given temperature and pressure exist when vaporizing the film-forming precursor to obtain the precursor gas. The step of vaporizing the film-forming precursor to obtain the precursor gas can be carried out in a precursor container or vaporization chamber. In any case, preferably, the film-forming precursor of the present invention is evaporated at a temperature between 0°C and 150°C. In addition, when a precursor gas is obtained by vaporizing a thin film in a precursor container or vaporization chamber to form a precursor, the pressure in the precursor container and the pressure in the vaporization chamber are preferably from 1 Pa to 10,000 Pa.
[0069] Furthermore, in the method for producing the thin film of the present invention, after film deposition, annealing can be performed under an inert atmosphere, an oxidizing atmosphere, or a reducing atmosphere to obtain more satisfactory electrical properties. The annealing temperature is from 200°C to 1,000°C, preferably from 250°C to 500°C. Attached Figure Description
[0070] Figure 1 The TGA curves of various compounds of the present invention and comparative scandium compounds are shown.
[0071] Figure 2 The thermal stability of Sc(Et2-fAMD)3 on Si(100) with 10 nm scandium oxide is shown, as illustrated in ALD Example 1.
[0072] Figure 3Saturation studies of Sc(Et2-fAMD)3 on Si(100) with native oxides are shown at 200°C, 250°C and 300°C, as illustrated in ALD Example 2.
[0073] Figure 4 The temperature dependence of the Sc(Et2-fAMD)3 / O3 process on Si(100) with native oxide is demonstrated, as illustrated in ALD Example 3.
[0074] Example
[0075] Reference will now be made to more specific embodiments of the invention and experimental results supporting those embodiments. The embodiments given below are provided to more fully illustrate the disclosed subject matter and should not be construed as limiting the disclosed subject matter in any way.
[0076] Those skilled in the art will appreciate that various modifications and variations can be made to the disclosed subject matter and the specific embodiments provided herein without departing from the spirit or scope of the disclosed subject matter. Therefore, it is intended that the disclosed subject matter (including the description provided in the following examples) be covered by any modifications and variations of the disclosed subject matter within the scope of any claims and their equivalents.
[0077] Materials and methods:
[0078] Unless otherwise indicated, all solvents and starting materials were purchased from Sigma-Aldrich.
[0079] General synthesis procedure:
[0080] In a Schlenk flask, the corresponding amidine (AMDH) (3 equivalents) for preparing the complex described below was dissolved in THF and cooled to -78°C. 1.6 M n-butyllithium (nBuLi) (3 equivalents) in hexane was added dropwise to the solution. The mixture was heated to room temperature and stirred for 2 h. The mixture was cooled to 0°C and slowly transferred via a sleeve to a 0°C cold solution of scandium chloride (ScCl3) (1 equivalent) in THF. After the addition, the reaction mixture was stirred overnight at room temperature. The solvent was removed under reduced pressure, and the crude mixture was extracted in toluene. The suspension was filtered, and the solvent in the filtrate was removed under reduced pressure. The crude product was distilled or sublimated under the conditions given below to obtain the spectroscopically pure complex. In the following terms, fAMD represents formamidinyl, MeAMD represents ethamidinyl, EtAMD represents propamidinyl, and nPrAMD represents butylamidinyl. The amidines used are known in the literature.
[0081] Example 1: Sc(Et2-fAMD)3
[0082] Tris(N,N'-diethyl-methylamidine)scandium; R N1 = RN2 =Ethyl compounds of formula (1).
[0083] 1 H NMR (500 MHz, C6D6) δ 8.08 (s, 3H), 3.14 (q, J = 7.2 Hz, 12H), 1.18(t, J = 7.2 Hz, 18H).
[0084] TGA: T 1% = 98℃, T 50% = 196℃, m 剩余 < 1%
[0085] DSC: T 熔点 = 27℃, T 分解起始 = 350℃
[0086] Vapor pressure: Lg(p(Pa)) = -2988.7(1 / T(K)) + 10.219 → T1 托 = 96℃
[0087] Example 2: Sc(nPr2-fAMD)3
[0088] Tris(N,N'-di-n-propyl-methylammonyl)scandium; R N1 = R N2 = n-propyl compound of formula (1).
[0089] 1 H NMR (500 MHz, C6D6) δ 8.10 (s, 3H), 3.11 (t, J = 6.8 Hz, 12H), 1.58 (h, J = 7.2 Hz, 12H), 0.96 (t, J = 7.4 Hz, 18H).
[0090] TGA: T 1% = 128℃, T 50% = 231℃, m 剩余 < 1%
[0091] DSC: T 熔点 = -22℃, T 分解起始 = 287℃
[0092] Vapor pressure: Lg(p(Pa)) = -3457.2(1 / T(K)) + 10.534 → T1 托 = 138℃
[0093] Comparative Example 1: Sc(Et,Me-MeAMD)3
[0094] Tris(N-methyl-N'-ethyl-acetamidine)scandium; according to the compound in US 2023 / 0058025 A1, corresponding to R N1 =Methyl, R N2 =Ethyl, but with methyl substituents on the carbon atom of the compound of formula (1).
[0095] 1 H NMR (500 MHz, C6D6) δ 3.24 - 3.10 (m, 6H), 3.01 - 2.93 (m, 9H), 1.62 - 1.51 (m, 9H), 1.38 - 1.21 (m, 9H).
[0096] TGA: T 1% = 123℃, T 50% = 215℃, m 剩余 = 9.3%
[0097] DSC: T 熔点 = 76℃, T 分解起始 = 265℃ (no clear peak)
[0098] Vapor pressure: Lg(p(Pa)) = -3832.7(1 / T(K)) + 11.868 → T1 托 = 120℃
[0099] Comparative Example 2: Sc(Et2-EtAMD)3
[0100] Tris(N,N'-diethyl-propanediyl)scandium; according to the compound of KR 102614467 B1, corresponding to R N1 = R N2 =Ethyl, but with an ethyl substituent on a carbon atom, of formula (1).
[0101] 1 H NMR (500 MHz, C6D6) δ 3.24 (q, J = 7.2 Hz, 12H), 2.16 (q, J = 7.7Hz, 6H), 1.27 (t, J = 7.2 Hz, 18H), 1.00 (t, J = 7.7 Hz, 9H).
[0102] TGA: T 1%= 116℃, T 50% = 243℃ (measured under the same conditions as in Examples 1 and 2; 232℃, measured under conditions according to the prior art), m 剩余 < 1%
[0103] T 熔点 > Room temperature
[0104] Comparative Example 3: Sc(Et2-nPrAMD)3
[0105] Tris(N,N'-diethyl-butamidine)scandium; according to the compound of KR 102614467 B1, corresponding to R N1 = R N2 =Ethyl, but with n-propyl substituents on the carbon atom of the compound of formula (1).
[0106] TGA: T 50% = 246℃ (according to existing technology).
[0107] Comparative Example 4: Sc(iPr2-fAMD)3
[0108] Tris(N,N'-di-isopropyl-methylamidine)scandium; a commercial compound, corresponding to R N1 = R N2 =Isopropyl compounds of formula (1).
[0109] 1 H NMR (500 MHz, C6D6) δ 8.18 (s, 3H), 3.17 (hept, J = 6.4 Hz, 6H), 1.23 (d, J = 6.5 Hz, 36H).
[0110] TGA: T 1% = 151℃, T 50% = 236℃, m 剩余 < 1%
[0111] DSC: T 熔点 = 269℃, T 分解起始 = 390℃, another endothermic peak at 146℃.
[0112] Vapor pressure: Lg(p(Pa)) = -4283.7(1 / T(K)) + 12.176 → T1 托 = 153℃
[0113] Analysis through TGA
[0114] The TGA curves of the compounds from Examples 1 and 2, and Comparative Examples 1, 2, and 4 were determined. The TGA curves were measured in 20 ml / min. -1 Using 10 K min at Ar flow rate -1 The sample was heated using a heating ramp. The sample mass for each compound in the TGA experiment was 10 mg. The TGA curves are shown on... Figure 1 middle.
[0115] Results Discussion
[0116] Table 1 compares the compounds of the present invention and their evaporation temperatures (T). 50% (i.e., the temperature at which 50% mass loss occurs). As can be seen from Comparative Example 2, the values cited in the prior art differ from the measured values, but it is known that these values depend on the exact conditions used for the TGA analysis. Because the TGAs of Examples 1 and 2, as well as Comparative Examples 1, 2, and 4, were performed under the same conditions, the values obtained can be directly compared with each other.
[0117] The compound of the present invention has the advantage of being able to evaporate with virtually no decomposition compared to the compound of Comparative Example 1, as evidenced by a residual mass of less than 1%. In contrast, the compound of Comparative Example 1 exhibits considerable decomposition, as can be seen from a residual mass of more than 9% (see also...). Figure 1 ).
[0118] In addition, the compounds of the present invention have the advantage of lower evaporation temperature compared with the compounds of Comparative Examples 2, 3 and 4, which is particularly evident for the compound of Example 1.
[0119] Compound 2 of this invention is the only compound that is liquid at room temperature, while compound 1 has a melting point slightly above room temperature, and the compounds of Comparative Examples 1, 2, and 4 are solids at room temperature. The only other reported compound in KR 102614467 B1 that is liquid at room temperature is the compound in Comparative Example 3, but its volatility is lower than that of the compound in Comparative Example 2. Therefore, compound 2 of this invention is the most volatile Sc complex, and it is also liquid at room temperature.
[0120] Table 1. Formamidinyl compounds of Examples 1 and 2 compared with compounds of Comparative Examples 1 to 4 at 50% mass loss (T 50% A comparison in terms of ).
[0121]
[0122] According to the value of existing technology
[0123] Based on self-measured values under the same conditions as in Examples 1 and 2 and Comparative Examples 1 and 4
[0124] ALD experiment
[0125] experiment:
[0126] Deposition was performed on a 2'' Si(100) wafer with native oxide using a Picosun R-200 Advanced tool. The precursor Sc(Et2-fAMD)3 was used, with a delivery temperature set to 100°C and an argon carrier gas flow rate set to 10 sccm. Ozone (O3) generated by an Anseros COM-AD-04 ozone generator at 50% power and an O2 flow rate of 800 sccm was used as a co-reactant. The tool was equipped with a Film Sense FS-1 in-situ ellipsometer to monitor the process, and the film thickness was determined using a Cauchy model. The refractive index was determined from the ex-situ measurements and set to 1.94. The film thickness was further verified by ex-situ ellipsometric analysis using a JA Woollam M2000D ellipsometer. Measurements were taken at five points on the 2'' wafer at three different angles (65°, 70°, and 75°), and the thickness and refractive index were determined using an oscillator model. The median of the measurements was used to optimize the process.
[0127] ALD Example 1: Thermal Stability of Sc(Et2-fAMD)3
[0128] For this experiment, a Si(100) wafer with a native oxide was first coated with 10 nm scandium oxide, as described in Example 3. These scandium oxide-coated wafers were used as substrates for thermal stability studies. In this experiment, Sc(Et2-fAMD)3 precursor vapor was delivered to the deposition chamber in a pulsed pattern separated by argon purging. For thermal stability studies, without the use of co-reactants, Sc(Et2-fAMD)3 was pulsed for 1 s, followed by Ar purging for 70 s. This pulse sequence was repeated 50 times. The observed growth points indicated thermal decomposition on the surface (CVD-like growth). Growth was monitored using an in-situ ellipsometry, and the thickness was determined by subtracting the initial precursor absorption from the final thickness. Although no growth was observed at 250 °C and 300 °C, a slight increase was noted in 50 cycles at 350 °C. This trend was further confirmed by the clear decomposition of the precursor at a process temperature of 400 °C, which led to measurable film growth. Therefore, the precursor Sc(Et2-fAMD)3 is stable at a maximum temperature of 300°C in the ALD process. Figure 2 The results of the thermal stability study are presented.
[0129] ALD Example 2: Saturation Study of Sc(Et2-fAMD)3
[0130] In this experiment, a scandium oxide film was deposited using atomic layer deposition (ALD), which includes the following steps:
[0131] a. Provide a Si substrate in the reaction vessel;
[0132] b. Introduce the Sc(Et2-fAMD)3 precursor into the reaction vessel;
[0133] c. Use argon to purge the reaction vessel;
[0134] d. Introduce ozone into the reaction vessel;
[0135] e. Use argon purging for reaction vessels; and
[0136] f. Repeat steps b to e in sequence until a scandium-containing film of the desired thickness is obtained.
[0137] Saturation studies of Sc(Et2-fAMD)3 were conducted at 200°C, 250°C, and 300°C. In this study, the precursor pulse time varied between 0.5 s and 7 s, while the remainder of the ALD cycle time remained constant to produce the following pulse / purge sequence: xs (precursor pulse) / 70 s (precursor purge) / 3 s (ozone pulse) / 30 s (ozone purge). At all three investigational temperatures, the precursor saturated at a 1 s pulse time, resulting in minimal variation in the in-situ and out-of-situ thicknesses measured at different pulse times. Precursor saturation occurred at a GPC of 0.43 Å at a deposition temperature of 200°C; at 250°C, at 0.64 Å; and at 300°C, at 0.92 Å, demonstrating ALD-like self-limiting behavior of Sc(Et2-fAMD)3. Figure 3 Presenting the results of saturation research.
[0138] ALD Example 3: Temperature Dependence of Sc(Et2-fAMD)3 / Ozone Process
[0139] In this experiment, a scandium oxide film was deposited using atomic layer deposition (ALD), which includes the following steps:
[0140] a. Provide a Si substrate in the reaction vessel;
[0141] b. Introduce the Sc(Et2-fAMD)3 precursor into the reaction vessel;
[0142] c. Use argon purging for reaction vessels;
[0143] d. Introduce ozone into the reaction vessel;
[0144] e. Use argon purging for reaction vessels; and
[0145] f. Repeat steps b to e in sequence until a scandium-containing film of the desired thickness is obtained.
[0146] To confirm the temperature dependence of the Sc(Et2-fAMD)3 / O3 process, deposition temperatures were varied between 150 °C and 400 °C using a 1 s precursor pulse followed by a 70 s purging, simultaneously with a 3 s pulsed ozone followed by a 30 s purging. A strong temperature dependence was observed, as GPC continuously increased with increasing deposition temperature. The following growth rate was found: 0.27 Å cycling at 150 °C. -1 Cycling at 0.43 Å at 200℃ -1 Cycling at 0.64 Å at 250°C -1 Cycling at 300°C for 0.92 Å -1 1.10 Å cycling at 350℃ -1 and 1.26 Å cycling at 400℃ -1 When Sc(Et2-fAMD)3 begins to decompose, growth rates above 1 Å / cycle are observed only above 350 °C, which generally leads to an increase in the growth rate. Figure 4 The results of the temperature dependence study are presented.
Claims
1. A compound of formula (1), Equation (1) The symbols used are as follows: R N1 R N2 Each time it appears, it is either the same or different ethyl or n-propyl, which may also be partially or completely deuterated.
2. The compound according to claim 1, characterized in that... All three formamidinyl ligands are identical.
3. The compound according to claim 1 or 2, wherein the compound is selected from compounds having the following... (a)R N1 =R N2 =Ethyl; (b)R N1 =Ethyl and R N2 =n-propyl; and (c)R N1 =R N2 =n-propyl.
4. A method for manufacturing a compound according to one or more of claims 1 to 3, characterized in that... The compound ScX3, in which X = F, Cl, Br, I, trifluoromethanesulfonate, or toluenesulfonate, reacts with formamidinium salts.
5. Use of a compound according to one or more of claims 1 to 3 for depositing a scandium-containing film.
6. A method for forming a scandium-containing film on at least one surface of a substrate, comprising the steps of: (a) Providing at least one surface of the substrate in a reaction vessel; and (b) A scandium-containing film is formed on at least one surface using a deposition process selected from chemical vapor deposition (CVD) and atomic layer deposition (ALD) using at least one of the compounds according to one or more of claims 1 to 3 as a scandium source compound precursor for the deposition process.
7. The method of claim 6, further comprising introducing at least one co-reactant into the reaction vessel.
8. The method according to claim 7, characterized in that... The co-reactants are selected from the group consisting of: water, oxygen, oxygen plasma, ozone, NO, N2O, NO2, CO, CO2, ammonia, hydrazine, monoalkylhydrazine, dialkylhydrazine, nitrogen, nitrogen / hydrogen, ammonia plasma, nitrogen plasma, nitrogen / hydrogen plasma, hydrogen, hydrogen plasma, mixtures of hydrogen and helium, mixtures of hydrogen and argon, hydrogen / helium plasma, hydrogen / argon plasma, boron-containing compounds, silicon-containing compounds, and combinations thereof.
9. A method for forming a scandium-containing film via atomic layer deposition (ALD) or an ALD-like process, the method comprising the following steps: (a) Providing a substrate in the reaction vessel; (b) Introducing one or more compounds according to one or more of claims 1 to 3 as precursors into the reaction vessel; (c) Purging procedure, in particular purging the reaction vessel with a first purging gas; (d) Introduce the co-reactants into the reaction vessel; (e) Purging steps, particularly purging the reaction vessel with a second purging gas; (f) Repeat steps (b) to (e) in sequence until the scandium-containing film of the desired thickness is obtained.
10. The method according to claim 9, characterized in that... In step (d), at least one co-reactant is selected from water, O2, O3, NO, N2O, NO2, CO, CO2, ammonia, hydrazine, monoalkylhydrazine, dialkylhydrazine, nitrogen, nitrogen / hydrogen, hydrogen, a mixture of hydrogen and helium, a mixture of hydrogen and argon, hydrogen / helium plasma, boron-containing compounds, silicon-containing compounds and combinations thereof, or plasmas of these co-reactants.
11. The method according to one or more of claims 6 to 10, characterized in that... The compound according to one or more of claims 1 to 3 is introduced into the reaction vessel by vaporization using thermal energy and vacuum.
Citation Information
Patent Citations
Precursor comprising for scandium or yttrium containg thin film, deposition method of film and semiconductor device of the same
KR102614467B1
Scandium precursor for sc2o3 or sc2s3 atomic layer deposition
US20230058025A1
Atomic layer deposition using metal amidinates
WO2004046417A2