Cyclic organosiloxanes containing free radical polymerizable groups, their manufacturing methods, and curable compositions containing them.
By introducing free radical polymerizable functional groups into the cyclic siloxane structure, low-viscosity cyclic organosiloxane compounds are prepared, solving the problems of operability and environmental burden in the prior art. This results in cured products with excellent hardness, impact resistance and adhesion, and low curing shrinkage.
Patent Information
- Application Number
- CN202580027832.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-04-24
- Filing Date
- 2025-03-17
- Publication Date
- 2026-11-17
AI Technical Summary
Existing cyclic siloxane compounds have problems with operability and environmental impact, making it difficult to form cured products with excellent hardness, impact resistance and adhesion to substrates, and they also have large curing shrinkage.
By introducing free radical polymerizable functional groups through Si-OC bonds in the cyclic siloxane structure and carrying out a dehydrogenation reaction using an amine catalyst, low-viscosity cyclic organosiloxanes containing free radical polymerizable groups are prepared and then combined with polymerization initiators and other compounds to form a curable composition.
It achieves the formation of low-viscosity cyclic siloxane compounds, resulting in cured products with excellent hardness, impact resistance, and adhesion to substrates, and with minimal curing shrinkage.
Smart Images

Figure CN123125243A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to cyclic organosiloxanes containing free radical polymerizable groups, methods for their manufacture, and curable compositions containing them. Background Technology
[0002] Compounds with cyclic siloxanes as the main skeleton and polymerizable organic functional groups are used as adhesives for electronic materials, lens molding materials, hard coatings and other coatings due to the excellent heat resistance, weather resistance and low curing shrinkage of their siloxane skeleton.
[0003] For example, in Patent Document 1, a technique was proposed to improve the hardness, impact-resistant softness, and weather resistance required for hard coatings, as well as their resistance to long-term outdoor exposure. The technique involves reacting a cyclic siloxane derivative having hydroxyl (-OH) groups with a compound having isocyanate groups (-N=C=O) and (meth)acryloyl groups to obtain a compound in which (meth)acryloyl groups, which are polymerizable functional groups, are introduced into the cyclic siloxane skeleton via urethane bonds [-O-(C=O)-NH-]. This compound is then applied to an adhesive in a photocurable coating composition using a multifunctional (meth)acrylate.
[0004] However, polyfunctional (meth)acrylate compounds containing urethane bonds are prone to aggregation and high viscosity due to intermolecular interactions at the urethane bond sites, requiring dilution with organic solvents, which poses problems in terms of operability and environmental impact.
[0005] In addition, in patent documents 2-4, organosilicon oligomers with polymerizable functional groups introduced by Si-OC bonds were proposed. However, these siloxane skeletons are all composed of condensates of tetrafunctional siloxane units such as tetrachlorosilane or silicates (esters), and therefore have random structures, making it difficult to control the main chain structure.
[0006] Existing technical documents
[0007] Patent documents
[0008] Patent Document 1: Japanese Patent Application Publication No. 2020-66577
[0009] Patent Document 2: Japanese Patent Application Publication No. 10-245247
[0010] Patent Document 3: Japanese Patent Application Publication No. 2005-258119
[0011] Patent Document 4: Japanese Patent Application Publication No. 2016-209874 Summary of the Invention
[0012] The problem that the invention aims to solve
[0013] The present invention was made in view of the above circumstances, and its object is to provide a cyclic siloxane containing free radical polymerizable groups that has low viscosity, excellent hardness, impact resistance and adhesion to substrates, and low curing shrinkage, a method for manufacturing the same, and a curable composition containing the same.
[0014] Methods for solving problems
[0015] In order to achieve the above objectives, the inventors conducted in-depth research and found that cyclic organosiloxanes obtained by introducing free radical polymerizable functional groups into the cyclic siloxane structure through Si-OC bonds have low viscosity despite having a small functional group equivalent. At the same time, they can form cured products with excellent hardness, impact resistance, and adhesion to the substrate, as well as low curing shrinkage, thus completing the present invention.
[0016] That is, the present invention provides:
[0017] 1. A cyclic organosiloxane containing a free radical polymerizable group, represented by the following formula (1),
[0018] [Chemistry 1]
[0019]
[0020] (where R) 1 Each independently represents a monovalent hydrocarbon group, R 2 Each independently represents a monovalent hydrocarbon group or a hydrogen atom, R 3 This represents a hydrogen atom or a methyl group, A represents a divalent hydrocarbon group with 1 to 10 carbon atoms, n is an integer from 2 to 6, m is an integer from 0 to 4, and the sum of n and m is 4 to 6. The arrangement of the siloxane units within the parentheses is arbitrary.
[0021] 2. The cyclic organosiloxane containing a free radical polymerizable group as described in 1 above, wherein A is a divalent saturated hydrocarbon group with 2 to 4 carbon atoms.
[0022] 3. The method for manufacturing the cyclic organosiloxane containing a free radical polymerizable group as described in 1 above, wherein the cyclic hydrosiloxane represented by formula (2) below and the compound represented by formula (3) below undergo a dehydrogenation reaction in the presence of an amine catalyst.
[0023] [Chemistry 2]
[0024]
[0025] (where R) 1 Each siloxane unit independently represents a monovalent hydrocarbon group, where p is an integer from 2 to 6, q is an integer from 0 to 4, and the sum of p and q is 4 to 6. The arrangement of the siloxane units within the parentheses is arbitrary.
[0026] [Chemistry 3]
[0027]
[0028] (where R) 3 (This indicates a hydrogen atom or a methyl group; A represents a divalent hydrocarbon group with 1 to 10 carbon atoms.)
[0029] 4. The method for manufacturing the cyclic organosiloxane containing free radical polymerizable groups described in 3 above, wherein the amine catalyst is diethylhydroxylamine.
[0030] 5. A curable composition comprising:
[0031] (A) The cyclic organosiloxane containing free radical polymerizable groups described in 1 above, and
[0032] (B) Polymerization initiator.
[0033] 6. The curable composition described in 5 above further contains a compound containing polymerizable unsaturated groups other than component (A) as component (C).
[0034] 7. The cured product of the curable composition described in 5 or 6 above,
[0035] 8. An article having a cured product of the curable composition described in 5 or 6 above.
[0036] Invention Effects
[0037] The cyclic organosiloxane containing free radical polymerizable groups of the present invention has a structure in which polymerizable unsaturated groups, represented by acryloyl and methacryloyl groups, are connected to the main skeleton of the cyclic siloxane via Si-OC bonds. Therefore, even if the equivalent of free radical polymerizable groups is small (high functional group density), it has low viscosity. The cured product obtained from the polymerizable composition containing the cyclic organosiloxane containing free radical polymerizable groups of the present invention has excellent hardness, impact resistance and adhesion to the substrate, and low curing shrinkage. Detailed Implementation
[0038] The present invention will now be described in detail.
[0039] The cyclic organosiloxane containing free radical polymerizable groups of the present invention is represented by formula (1). It should be noted that the arrangement of the siloxane units within parentheses is arbitrary.
[0040] [Chemistry 4]
[0041]
[0042] In equation (1), R 1 Each independently represents a monovalent hydrocarbon group, R2 Each independently represents a monovalent hydrocarbon group or a hydrogen atom, R 3 It can be a hydrogen atom or a methyl group.
[0043] As R 1 and R 2 Specific examples of the monovalent hydrocarbon group can be any of straight-chain, branched, or cyclic, and are preferably groups having 1 to 20 carbon atoms. Specific examples include: alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-hexyl, cyclohexyl, n-octyl, 2-ethylhexyl, and n-decyl; alkenyl groups such as vinyl, allyl (2-propenyl), 1-propenyl, isopropenyl, and butenyl; aryl groups such as phenyl, tolyl, xylyl, and naphthyl; and aralkyl groups such as benzyl, phenethyl, and phenylpropyl.
[0044] Among them, alkyl groups with 1 to 20 carbon atoms and aryl groups with 6 to 12 carbon atoms are preferred, alkyl groups with 1 to 10 carbon atoms are more preferred, alkyl groups with 1 to 5 carbon atoms are even more preferred, and from the viewpoint of the market availability of the raw materials used, methyl, ethyl and n-propyl are most preferred.
[0045] In formula (1), A is a divalent hydrocarbon group with 1 to 10 carbon atoms. As a divalent hydrocarbon group, it can be any of the following: straight-chain, branched, or cyclic. Specific examples include: methylene, ethylene, trimethylene, propylene, tetramethylene, isobutylene, dimethyl ethylene, pentamethylene, 2,2-dimethyltrimethylene, hexamethylene, heptamethylene, octamethylene, nonamethylene, decamethylene (decamethylene), etc., which are straight-chain or branched alkylene groups; 1,2-phenylene, 1,3-phenylene, 1,4-phenylene, toluenediyl, xylenediyl, naphthyl, etc., which are aryl groups.
[0046] Preferably, the divalent saturated hydrocarbon group with 2 to 4 carbon atoms is preferred, and more preferably, ethylene, trimethylene, propylene, or tetramethylene is preferred.
[0047] In equation (1), n is an integer from 2 to 6, m is an integer from 0 to 4, and the sum of n+m is 4 to 6. Preferably, n is an integer from 2 to 4, m is an integer from 0 to 2, and the sum of n+m is 4.
[0048] When n is less than 2, the hardness of the cured material is insufficient. When n exceeds 6, it becomes a structure with too many polymeric functional groups, which sometimes results in excessive crosslinking density and reduced impact resistance of the cured material.
[0049] From an operational point of view, the kinematic viscosity of the cyclic organosiloxane containing free radical polymerizable groups of the present invention is preferably 1 to 1,000 mm. 2 / s, more preferably 10~100mm 2 / s. It should be noted that kinematic viscosity is a value measured at 25°C, for example using an Ubbelohde viscometer or a Cannon-Fenske viscometer.
[0050] From the viewpoint of imparting sufficient hardness and impact resistance to the resulting cured product, the weight-average molecular weight of the cyclic organosiloxane containing free radical polymerizable groups of the present invention is preferably 400 to 4,000. It should be noted that the weight-average molecular weight in the present invention is a standard polystyrene conversion value determined by gel permeation chromatography (GPC).
[0051] From the viewpoint of imparting sufficient hardness and impact resistance to the obtained cured product, the functional group equivalent of the free radical polymerizable groups of the cyclic organosiloxane containing free radical polymerizable groups of the present invention is preferably 200 to 500 g / mol. If it is 200 g / mol or more, a cured product with excellent hardness can be obtained, and if it is 500 g / mol or less, a cured product with excellent flexibility and impact resistance can be obtained.
[0052] The cyclic organosiloxane containing free radical polymerizable groups of the present invention can be obtained, for example, by dehydrogenation reaction of a cyclic hydrosiloxane represented by the following formula (2) with a compound represented by the following formula (3) in the presence of an amine catalyst.
[0053] [Chemistry 5]
[0054]
[0055] [Chemistry 6]
[0056]
[0057] In the above formulas, R 1 R 3 A represents the same meaning as above, p is an integer from 2 to 6, preferably an integer from 2 to 4, q is an integer from 0 to 4, preferably an integer from 2 to 4, and the sum of p and q is 4 to 6, preferably 4. It should be noted that in the above formula (2), the arrangement of the siloxane units in parentheses is arbitrary.
[0058] Specific examples of cyclic hydrosiloxanes represented by the above formula (2) include: 1,3,5,7-tetramethylcyclotetrasiloxane, 1,3,5,7-tetramethyl-1,3-dipropylcyclotetrasiloxane, 1,3,5,7-tetramethyl-1,5-dipropylcyclotetrasiloxane, etc.
[0059] Specific examples of compounds represented by the above formula (3) include: 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, 2-hydroxypropyl methacrylate, 4-hydroxybutyl acrylate, 4-hydroxybutyl methacrylate, etc.
[0060] There are no particular limitations on the amine catalyst; commercially available products can be used. However, amine compounds without NH groups are preferred, with diethylhydroxylamine being more preferred from the viewpoint of basicity and availability.
[0061] It should be noted that although metal complexes, such as platinum and palladium complexes, can also act as catalysts for this reaction, they can also cause hydrosilylation reactions between the hydrosilyl group and the olefin site of the polymerizable group, and therefore are not preferred.
[0062] From the viewpoint of reaction efficiency, the amount of amine catalyst used is preferably 0.001 to 0.1 moles relative to 1 mole of Si-H group in cyclic hydrosiloxane, more preferably 0.005 to 0.05 moles.
[0063] Organic solvents can be used as needed in the dehydrogenation reaction.
[0064] There are no particular limitations on the type of organic solvent used; any organic solvent that does not react with the raw materials and can fully dissolve them is acceptable. Examples include: nonpolar hydrocarbon solvents such as hexane, heptane, and cyclohexane; ether solvents such as tetrahydrofuran, 4-methyltetrahydropyran, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, propylene glycol monomethyl ether monoacetate, and cyclopentyl methyl ether; ketone solvents such as methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, and cyclohexanone; and aromatic solvents such as toluene and xylene. From the perspective of reactivity and solubility, ether solvents and aromatic solvents are preferred. Organic solvents can be used alone or in appropriate mixtures.
[0065] The reaction time for the dehydrogenation reaction can be set appropriately according to the progress of the reaction, but it is preferred to be 1 to 10 hours, and more preferably 2 to 7 hours.
[0066] The reaction temperature can be adjusted according to the boiling points of the raw materials and the solvent used, but a range of 40~100℃ is preferred.
[0067] The curable composition of the present invention comprises (A) the cyclic organosiloxane containing free radical polymerizable groups of the present invention described above and (B) a polymerization initiator.
[0068] From the perspective of compatibility and curability of the curable composition, the polymerization initiator of component (B) can be appropriately selected. Specific examples include: benzoin, benzoin monomethyl ether, benzoin isopropyl ether, acetoin, benzoyl, benzophenone, p-methoxybenzophenone, diethoxyacetophenone, benzoyl dimethyl ketal, 2,2-diethoxyacetophenone, 1-hydroxycyclohexylphenyl ketone, methyl phenylglyoxylate, 2-hydroxy-2-methyl-1-phenylpropane-1-one, etc. (carbonylated). Sulfur compounds such as tetramethylthiuram monosulfide and tetramethylthiuram disulfide; phosphoric acid compounds such as 2,4,6-trimethylbenzoyl diphenylphosphine oxide, 2,4,6-trimethylbenzoylphenyl ethoxyphosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, and bis(2,6-dimethoxybenzoyl)-2,4,4-trimethyl-pentylphosphine oxide; and 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butane-1-one and camphorquinone, etc. These compounds can be used individually or in combination of two or more, and can be arbitrarily combined according to the required coating properties.
[0069] From the viewpoint of achieving a moderate curing speed for the resulting coating, improving the scratch resistance and adhesion to the substrate of the cured coating, and preventing coloring and weather resistance degradation, the content of the polymerization initiator in the composition is preferably 0.1 to 10 parts by mass relative to 100 parts by mass of the (meth)acrylate compound and the adhesive precursor, more preferably 1 to 8 parts by mass.
[0070] The curable composition of the present invention may contain, as needed, a compound containing polymerizable unsaturated groups other than component (A) as component (C).
[0071] As component (C), examples include monofunctional (meth)acrylates and polyfunctional (meth)acrylates with polymerizable unsaturated bonds, such as urethane (meth)acrylates, epoxy (meth)acrylates, polyester (meth)acrylates, etc., which can be appropriately selected according to the required performance of the coating film.
[0072] Specific examples of monofunctional (meth)acrylates include: methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, morpholine (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and glycidyl (meth)acrylate. Dimethylaminoethyl methacrylate, diethylaminoethyl methacrylate, tricyclodecane methacrylate, polyethylene glycol mono(meth)acrylate, cyclohexyl methacrylate, tetrahydrofurfuryl methacrylate, dicyclopentyl methacrylate, dicyclopentenyl methacrylate, isobornyl methacrylate, allyl methacrylate, 2-ethoxyethyl methacrylate, benzyl methacrylate, phenoxyethyl methacrylate, phenyl methacrylate, adducts of phthalic anhydride and 2-hydroxyethyl methacrylate, etc.
[0073] Specific examples of polyfunctional (meth)acrylates include: neopentyl glycol di(meth)acrylate, ethylene glycol di(meth)acrylate, polyethylene glycol (repeating unit number (hereinafter referred to as "k") = 2~15) di(meth)acrylate, polypropylene glycol (k=2~15) di(meth)acrylate, polybutane glycol (k=2~15) di(meth)acrylate, 2,2-bis(4-(meth)acryloyloxyethoxyphenyl)propane, and 2,2-bis(4-(meth)acryloyloxydiethoxyphenyl)propane. Trimethylolpropane diacrylate, bis(2-(meth)acryloyloxyethyl)-hydroxyethyl isocyanurate, trimethylolpropane tri(meth)acrylate, tri(2-(meth)acryloyloxyethyl) isocyanurate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and epoxy di(meth)acrylate formed by the reaction of bisphenol A type diepoxide with (meth)acrylic acid. The following are examples of carbamates reacting with 2-hydroxyethyl methacrylate to form trimethacrylates: isophorone diisocyanate reacting with 2-hydroxypropyl methacrylate to form dimethacrylates; isophorone diisocyanate reacting with pentaerythritol trimethacrylate to form hexamethacrylates; and dicyclohexyl diisocyanate reacting with 2-hydroxyethyl methacrylate to form carbamates. The carbamate reaction products of di(meth)acrylate, dicyclohexyl diisocyanate and poly(k=6~15)tetramethylene glycol, and then reacted with 2-hydroxyethyl (meth)acrylate to form carbamate di(meth)acrylate and other carbamate poly(meth)acrylates, polyester (meth)acrylates formed by reacting trimethylolethane with succinic acid and (meth)acrylate, polyester (meth)acrylates formed by reacting trimethylolpropane with succinic acid, ethylene glycol and (meth)acrylate, and other polyester poly(meth)acrylates, etc.
[0074] From the viewpoint of improving the scratch resistance and adhesion to the substrate of the cured product obtained from the composition, the content of component (C) is preferably 1 to 100 parts by mass relative to the total of 100 parts by mass of components (A) and (C), and more preferably 5 to 90 parts by mass.
[0075] It should be noted that component (C) can be used alone or in combination.
[0076] The curable composition of the present invention may contain inorganic fillers as needed.
[0077] Examples of inorganic fillers include oxide particles of Si, Ti, Al, Zn, Zr, In, Sn, Sb, and their composite oxide particles. Additionally, particles whose surfaces are coated with silica, alumina, or similar materials can also be used.
[0078] Specific examples of metal oxide particles include silica, alumina, zirconium oxide, and titanium oxide particles, with silica particles being preferred. Adding such metal oxide particles can further improve the wear resistance and other properties of the cured product.
[0079] Furthermore, other additives may be added to the curable composition of the present invention without impairing the effects of the present invention. Examples of such additives include: ultraviolet absorbers, antifouling agents, water repellents, leveling agents, colorants, pigments, antioxidants, antiyellowing agents, bluing agents, defoamers, thickeners, antisettling agents, antistatic agents, surfactants, adhesion promoters, infrared absorbers, light stabilizers, and curing catalysts other than the aforementioned photo- and thermal polymerization initiators.
[0080] Furthermore, the compositions of the present invention are preferably solvent-free forms that are substantially free of organic solvents (which are often harmful to humans and flammable), but solvents may be added for use and workability.
[0081] Here, "substantially" means that the solvent contained in the composition is less than 1% by mass, especially less than 0.1% by mass.
[0082] As a specific example of a solvent that can be used, the same solvent as the organic solvent used in manufacturing the cyclic organosiloxane containing free radical polymerizable groups of the present invention described above (A) can be cited.
[0083] It should be noted that solvents also include components that are not intentionally added to the curable composition, such as reaction solvents that could not be completely removed by vacuum distillation.
[0084] By heating and / or irradiating the curable composition of the present invention to cure it, a corresponding cured product can be obtained. Its form is not particularly limited; it can be a coating film applied to various substrates and cured, or a self-supporting molded product or sealant.
[0085] From a production standpoint, photocuring is preferred as the curing method. As the light source for photocuring, high-pressure mercury lamps, metal halide lamps, LED lamps, etc., are used to irradiate with ultraviolet light or an electron beam of a wavelength corresponding to the polymerization initiator. The irradiation atmosphere can be air or an inert gas such as nitrogen or argon. When irradiating with ultraviolet light, a concentration of 1~1000 mJ / cm² is preferred. 2 about.
[0086] Examples of suitable base materials include: organic resins such as plastic molded parts, wood-based products, fibers, ceramics, glass, metals, calcium phosphate (represented by hydroxyapatite) or their complexes, etc., without particular limitation, but suitable for various plastic materials and calcium phosphate. In particular, suitable for polycarbonate resins, polystyrene resins, acrylic resins, modified acrylic resins, urethane resins, thiourethane resins, condensates of halogenated bisphenol A and ethylene glycol, acrylic urethane resins, halogenated aryl acrylic resins, sulfur-containing resins, polyalkylene terephthalate resins, polyimide resins, polyamide resins, polycyclic olefin resins, polyphenylene sulfide resins, polyphenylene ether resins, cellulose resins, amorphous polyolefin resins, and their composite resins, etc.
[0087] Furthermore, substrates obtained by surface treatment of these substrates can also be used. Specifically, substrates treated by chemical conversion, corona discharge, flame treatment, plasma treatment, acid or alkali treatment can be used. In addition, laminates whose surface is coated with a different type of resin than the substrate body can also be used.
[0088] Specific examples of laminates include: laminates in which an acrylic resin layer or a urethane resin layer exists on the surface of a polycarbonate resin substrate manufactured by co-extrusion or lamination, and laminates in which an acrylic resin layer exists on the surface of a polyester resin substrate.
[0089] It should be noted that the curable composition can be applied directly to the substrate surface, or it can be applied as needed through a primer layer, ultraviolet absorption layer, printing layer, recording layer, heat radiation shielding layer, pressure-sensitive adhesive layer, inorganic vapor deposition film layer, etc.
[0090] Coating methods can be appropriately selected from known coating methods such as spin coaters, corner roller coaters, lip coaters, roller coaters, die coaters, doctor blade coaters, scraper coaters, bar coaters, kiss coaters, gravure coaters, screen coating, dip coating, and cast coating.
[0091] Furthermore, other coating layers such as adhesive layers, ultraviolet absorption layers, printing layers, recording layers, heat radiation shielding layers, pressure-sensitive adhesive layers, inorganic vapor deposition film layers, water-repellent and oil-repellent layers, and hydrophilic antifouling layers can be formed on the surface of the cured coating film of the curable composition of the present invention as needed.
[0092] As a method for producing a self-supporting cured molded article using the curable composition of the present invention, in addition to the method of using a mold, examples include casting film formation method, which is obtained by coating and curing a film having a release layer in advance, but is not limited to these.
[0093] The material of the molding mold is not particularly limited as long as it ensures the demolding property of the cured product. For example, it can be any of the following: metal, glass, plastic, silicone, or Teflon (registered trademark) molds. However, from the viewpoint of having excellent demolding property and being able to suppress breakage when removing the cured product, Teflon (registered trademark) molds are preferred.
[0094] The cured products obtained from the curable composition of the present invention can be applied to scratch-resistant hard coatings for plastic substrates, optical lens moldings, flexible display materials for electronic materials, optical sealing materials for LED devices, and dental and medical prosthesis molding materials, dental fillings, etc.
[0095] Example
[0096] The present invention will be described in more detail below with examples and comparative examples, but the present invention is not limited to these examples.
[0097] It should be noted that in the following examples, unless otherwise specified, "parts" and "%" represent "parts by mass" and "% by mass," respectively. Additionally, the kinematic viscosity is a value measured at 25°C using a Canon-Fensk viscometer, and the apparatus used in the examples is described below.
[0098] (1) GPC determination conditions
[0099] Device: HLC-8320GPC manufactured by Tosoh Corporation
[0100] Elution solvent: Tetrahydrofuran (THF)
[0101] Flow rate: 0.6 mL / min
[0102] Detector: Differential refractive index detector (RI)
[0103] Column: TSK Guardcolumn SuperH-H
[0104] TSKgel SuperHM-N (6.0mmI.D.×15cm×1)
[0105] TSKgel SuperH2500 (6.0mmI.D.×15cm×1)
[0106] (All are manufactured by Tosoh Corporation)
[0107] Column temperature: 40℃
[0108] Sample injection volume: 50 μL (2.0% by mass THF solution)
[0109] Standard: Monodisperse polystyrene
[0110] (2) Proton nuclear magnetic resonance (NMR) 1 H-NMR spectroscopy measurement conditions
[0111] Device: Burker Avance III 400
[0112] Solvent: CDCl3
[0113] Internal standard: Tetramethylsilane (TMS)
[0114] [1] Synthesis of cyclic organosiloxanes containing free radical polymerizable groups
[0115] [Example 1]
[0116] In a 1L three-necked flask equipped with a stirrer, condenser, dropping funnel, and thermometer, 476g (4.1 mol) of 2-hydroxyethyl acrylate and 400g of toluene were added, and the mixture was heated to 80°C in an oil bath. Then, 1.07g (0.012 mol) of diethylhydroxylamine was added, and while stirring, 240g (1 mol) of 1,3,5,7-tetramethylcyclotetrasiloxane was added dropwise within an internal temperature range of 80–90°C. After the addition was complete, the mixture was stirred at 80°C for 4 hours to confirm the desired effect. 1 The H-NMR spectrum showed a decrease in peaks originating from the reactants and a formation of peaks originating from the target compound. The mixture was then cooled to 25°C, and unreacted 2-hydroxyethyl acrylate and amine catalyst were removed by washing with water. The solvent toluene was removed by vacuum distillation, yielding a pale yellow, transparent liquid (A-1). The kinematic viscosity of this substance at 25°C was 39 mm⁻¹. 2 / s, acryloyl equivalent is 174g / mol, and weight average molecular weight is 855.
[0117] The above (A-1) 1 Analysis by H-NMR, GPC and other methods confirmed that it was a compound represented by the following formula (4).
[0118] [Chemistry 7]
[0119]
[0120] [Example 2]
[0121] In Example 1, 1,3,5,7-tetramethylcyclotetrasiloxane was replaced with an equimolar mixture of 1,3,5,7-tetramethyl-1,3-dipropylcyclotetrasiloxane and 1,3,5,7-tetramethyl-1,5-dipropylcyclotetrasiloxane in a 1:1 molar ratio. Otherwise, the same procedures as in Example 1 were performed to obtain a pale yellow transparent liquid (A-2). This substance has a kinematic viscosity of 13 mm at 25°C. 2 / s, acryloyl equivalent is 276g / mol, and weight average molecular weight is 731.
[0122] The above (A-2) 1 Analysis by H-NMR, GPC and other methods confirmed that it was a mixture of compounds represented by the following formulas (5) and (6).
[0123] [Chemistry 8]
[0124]
[0125] [Example 3]
[0126] In Example 1, 2-hydroxyethyl acrylate was replaced with an equimolar amount of 4-hydroxybutyl acrylate. Otherwise, the same steps as in Example 1 were performed to obtain a pale yellow, transparent liquid (A-3). This substance had a kinematic viscosity of 42 mmHg at 25°C. 2 / s, acryloyl equivalent is 202g / mol, and weight average molecular weight is 1010.
[0127] The above (A-3) 1 Analysis by H-NMR, GPC and other methods confirmed that it was a compound represented by the following formula (7).
[0128] [Chemistry 9]
[0129]
[0130] [Example 4]
[0131] In Example 2, 2-hydroxyethyl acrylate was replaced with an equimolar amount of 4-hydroxybutyl acrylate. Otherwise, the same steps as in Example 2 were performed to obtain a pale yellow, transparent liquid (A-4). This substance had a kinematic viscosity of 16 mmHg at 25°C. 2 / s, acryloyl equivalent is 306 g / mol, and weight average molecular weight is 755.
[0132] The above (A-4) 1 Analysis by H-NMR, GPC and other methods confirmed that it was a mixture of compounds represented by the following formulas (8) and (9).
[0133] [Chemistry 10]
[0134]
[0135] [Example 5]
[0136] In Example 1, 2-hydroxyethyl acrylate was replaced with an equimolar amount of 2-hydroxypropyl methacrylate. Otherwise, the same steps as in Example 1 were performed to obtain a pale yellow, transparent liquid (A-5). This substance has a kinematic viscosity of 65 mmHg at 25°C. 2 / s, the methacryloyl equivalent is 205 g / mol, and the weight-average molecular weight is 986.
[0137] The above (A-5) 1 Analysis by H-NMR, GPC and other methods confirmed that the compound was represented by the following formula (10).
[0138] [Chemistry 11]
[0139]
[0140] [Example 6]
[0141] In Example 2, 2-hydroxyethyl acrylate was replaced with an equimolar amount of 2-hydroxypropyl methacrylate; otherwise, the same steps as in Example 2 were performed to obtain a pale yellow transparent liquid (A-6). This substance has a kinematic viscosity of 16 mmHg at 25°C. 2 / s, the methacryloyl equivalent is 300g / mol, and the weight-average molecular weight is 731.
[0142] The above (A-6) 1 Analysis by H-NMR, GPC and other methods confirmed that it was a mixture of compounds represented by the following formulas (11) and (12).
[0143] [Chemistry 12]
[0144]
[0145] [2] Preparation of curable compositions
[0146] [Examples 7-13, Comparative Examples 1-3]
[0147] Mix the components according to the proportions (parts by mass) shown in Table 1 to prepare a curable composition.
[0148] [Table 1]
[0149]
[0150] The abbreviations in Table 1 are as follows.
[0151] PETA: Pentaerythritol Tetraacrylate
[0152] DPHA: Dipentaerythritol hexaacrylate
[0153] HDDA: Hexanediol diacrylate
[0154] Photopolymerization initiator: α-hydroxyacetophenone (manufactured by IGB Resin BV, Omnirad 1173)
[0155] The curable compositions in Table 1 were applied using a rod coater No. 14 to various substrates, including Mitsubishi Engineering Plastics Co., Ltd. polycarbonate (PC) NF-2000 sheets (4mm thick × 15cm long × 10cm wide), Toyobo Co., Ltd. polyethylene terephthalate (PET) film COSMOSHINE A4160 (50 microns thick), and polished steel plates. After air drying for 15 minutes, the mixture was further heated at 80°C for 1 minute, and then subjected to a high-pressure mercury lamp at 600mJ / cm². 2 The coating is irradiated with light to cure it, and a test piece is obtained.
[0156] The coatings obtained in the above embodiments and comparative examples were evaluated as follows. The results are shown in Table 2.
[0157] (1) Coating appearance (PC, polished steel plate, PET)
[0158] Visually inspect the coating to determine if there are any abnormalities.
[0159] ○: No abnormalities
[0160] ×: Abnormalities such as impurities, unevenness, or whitening are present.
[0161] (2) Initial fog (PC)
[0162] The haze value of the coated sheet was measured using a haze meter NDH5000SP manufactured by Nippon Denshoku Kogyo Co., Ltd., as the initial haze value.
[0163] (3) Scratch resistance (PC)
[0164] According to ASTM 1044, the wear wheel CS-10F was installed on the Tabor abrasion tester, and the haze value was measured after 100 rotations under a load of 500g. The difference in haze between the test and the test was taken as the abrasion resistance.
[0165] (4) Initial sealing performance (PC, polished steel plate)
[0166] According to JIS K5600-5-6:1999, use a razor blade to make 6 vertical and 6 horizontal cuts at 2mm intervals on the coating to create 25 checkerboard squares. After tightly attaching Cellotape (registered trademark, manufactured by Nichiban Co., Ltd.), peel it off sharply in a 90° forward direction. The number of squares (X) remaining after the coating is not peeled off is represented as X / 25.
[0167] (5) Boiling and sealing properties (PC, polished steel sheet)
[0168] The airtightness of the samples after immersion in boiling water for 2 hours was evaluated in the same way as the initial airtightness.
[0169] (6) Pencil hardness (PC)
[0170] The pencil scratch test method described in JIS K5600-5-4:1999 was performed by applying a load of 750g, and the results are shown.
[0171] (7) Impact resistance (polished steel plate)
[0172] The test was performed using a DuPont impact testing machine according to the drop hammer impact test method described in JIS K5600-5-3:1999, and the results are shown.
[0173] (8) Curing shrinkage (PET)
[0174] The test piece was cut into 10cm×10cm pieces. When the center point of the membrane was fixed on the horizontal plane, the distances from the four corners of the membrane that curled up due to shrinkage to the horizontal plane were measured, and the average value was taken and the results were shown.
[0175] [Table 2]
[0176]
[0177] As shown in Table 2, the coatings obtained by curing the curable compositions of Examples 7-13 containing the cyclic organosiloxanes with free radical polymerizable groups of the present invention have transparency, adhesion, hardness and impact resistance, and low curing shrinkage.
[0178] On the other hand, it can be seen that Comparative Example 1 using PETA and Comparative Example 2 using DPHA have poor abrasion resistance, low impact resistance, and very large curing shrinkage due to insufficient adhesion.
[0179] It can be seen that although Comparative Example 3 using HDDA has good adhesion and curing shrinkage, it has low hardness. In addition, the polycarbonate substrate is eroded, resulting in poor transparency.
Claims
1. A cyclic organosiloxane containing a free radical polymerizable group, represented by the following formula (1), [Chemistry 1] In the formula, R 1 Each independently represents a monovalent hydrocarbon group, R 2 Each independently represents a monovalent hydrocarbon group or a hydrogen atom, R 3 The symbol represents a hydrogen atom or a methyl group, A represents a divalent hydrocarbon group with 1 to 10 carbon atoms, n is an integer from 2 to 6, m is an integer from 0 to 4, and the sum of n and m is 4 to 6. The arrangement of the siloxane units in parentheses is arbitrary.
2. The cyclic organosiloxane containing free radical polymerizable groups according to claim 1, wherein, The A is a divalent saturated hydrocarbon group with 2 to 4 carbon atoms.
3. The method for manufacturing cyclic organosiloxanes containing free radical polymerizable groups according to claim 1, wherein, A cyclic hydrosiloxane represented by formula (2) is subjected to a dehydrogenation reaction with a compound represented by formula (3) in the presence of an amine catalyst. [Chemistry 2] In the formula, R 1 Each siloxane unit independently represents a monovalent hydrocarbon group, where p is an integer from 2 to 6, q is an integer from 0 to 4, and the sum of p and q is 4 to 6. The arrangement of the siloxane units within the parentheses is arbitrary. [Chemistry 3] In the formula, R 3 It represents a hydrogen atom or a methyl group, and A represents a divalent hydrocarbon group with 1 to 10 carbon atoms.
4. The method for manufacturing cyclic organosiloxanes containing free radical polymerizable groups according to claim 3, wherein, The amine catalyst is diethylhydroxylamine.
5. A curable composition comprising: (A) The cyclic organosiloxane containing a free radical polymerizable group according to claim 1, and (B) Polymerization initiator.
6. The curable composition according to claim 5, further comprising a compound containing polymerizable unsaturated groups other than component (A) as component (C).
7. The cured product of the curable composition according to claim 5 or 6.
8. An article having a cured product of the curable composition according to claim 5 or 6.
Citation Information
Patent Citations
Laminated glass
JP1998245247A
Curable resin composition for optical component, optical component and image display apparatus
JP2005258119A
Manufacturing method of coated article, coating and laminate
JP2016209874A
(METH)acrylate compound, and coating composition and coated article containing the same