Two-component acrylic structural adhesive compositions, and articles and components made therefrom.

By using a two-component acrylic structural adhesive composition containing a specific internal plasticizer, the problem of adhesive instability under high temperature and vibration conditions is solved, achieving rapid curing and crack resistance of magnets at high temperatures, making it suitable for applications such as loudspeakers.

CN123125296APending Publication Date: 2026-11-17HENKEL KGAA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202480090900.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-04-16
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing adhesives are difficult to maintain the bonding integrity of magnets under high temperature and vibration conditions, and have low productivity, failing to meet the requirements of heat resistance, vibration resistance and rapid curing for applications such as loudspeakers.

Method used

A two-component acrylic structural adhesive composition is used, comprising (meth)acrylate monomers, toughening agents, free radical initiators, catalysts, and internal plasticizers, wherein the internal plasticizer is a heterocyclic (meth)acrylate monomer with two or more oxygen atoms to balance heat resistance and crack resistance.

Benefits of technology

It maintains high bonding strength at high temperatures, has good vibration resistance, fast curing speed, good flexibility and moisture resistance, and is suitable for magnet bonding in high-temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention relates to a two-component acrylic structural adhesive composition comprising component A and component B. The two-component acrylic structural adhesive composition comprises at least one (meth)acrylate monomer, at least one toughening agent, a free radical initiator, a catalyst, and an internal plasticizer, wherein the internal plasticizer is a heterocyclic (meth)acrylate monomer having two or more oxygen atoms as cyclizing atoms. The two-component acrylic structural adhesive composition can be used as a structural adhesive, for example, as a structural adhesive in the bonding of speaker magnets, motor structures, and metal components, providing excellent crack resistance during thermal shock testing while also providing good thermal strength properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to two-component acrylic structural adhesive compositions suitable for structural adhesive applications, articles and components made therefrom, and particularly structural adhesive compositions exhibiting good crack resistance and good adhesive strength at high temperatures. The two-component acrylic structural adhesive compositions can be used, for example, in magnet bonding applications. Background Technology

[0002] Magnets are everywhere, and so is magnetic adhesive. It's an application used across a wide range of industries, including motors, power tools, the automotive industry, audio and video equipment, home appliances, and others. Innovative magnetic adhesives go beyond traditional methods, providing a reliable way to utilize magnetic force while ensuring a strong and durable bond. Whether in manufacturing electronics, automobiles, or even in creative projects, magnetic adhesives offer a unique way to create versatile connections that combine the strength of magnets with the versatility of adhesives.

[0003] To meet our customers' manufacturing and application needs, selecting the right adhesive is crucial. For example, the adhesive used to bond magnets in loudspeakers must be strong, durable, and heat-resistant because loudspeakers operate at high temperatures and experience significant internal stresses during use. Loudspeaker adhesives typically possess high-temperature resistance, meaning they can withstand elevated temperatures without losing their adhesive properties. Epoxy resins and cyanoacrylates are common choices because of their high modulus and resistance to temperature fluctuations; the high modulus provides high bond strength.

[0004] However, vibration resistance is also essential to ensure the speaker remains intact and maintains its sound quality over time. Speaker structural adhesives with good vibration resistance can maintain their bond even under the most demanding conditions. However, under external forces, high-modulus adhesives can generate internal stress, and excessive internal stress can cause the ferrite magnets bonded to the structural adhesive to break or crack.

[0005] Furthermore, advanced loudspeaker manufacturing processes require higher productivity, which necessitates adhesives with faster setting times and lower viscosity, requirements that epoxy resins struggle to meet.

[0006] Acrylic adhesives are known for their rapid setting and flexibility, making them ideal for applications where magnets must withstand stress and vibration. However, balancing the heat resistance and flexibility of these resins remains a significant challenge.

[0007] Therefore, there is a need to develop an acrylic structural adhesive composition with high temperature resistance, vibration resistance and low modulus to improve the crack resistance of bonded magnetic materials under fluctuating temperatures. Summary of the Invention

[0008] Therefore, the object of the present invention is to overcome the above-mentioned disadvantages by providing an acrylic structural adhesive composition that exhibits excellent heat resistance (high adhesive strength at high operating temperatures above 100°C, for example 150°C), good flexibility (it does not cause magnet cracking / shrinkage / displacement during thermal shock), short setting time (achieving 0.1 MPa shear strength within 1 minute), and low viscosity. Furthermore, the acrylic structural adhesive composition also exhibits good resistance to moisture and thermal aging.

[0009] Surprisingly, a two-component acrylic structural adhesive composition prepared from at least (meth)acrylate monomers, toughening agents, free radical initiators, catalysts, and internal plasticizers has been found to provide a very good balance between high-temperature resistance and crack resistance under fluctuating temperatures, wherein the internal plasticizer is a heterocyclic (meth)acrylate monomer having two or more oxygen atoms as cyclizing atoms.

[0010] According to one aspect, the present invention relates to a two-component acrylic structural adhesive composition comprising component A and component B. a) Free radical initiators in component A b) The catalyst in component B, The composition further comprises: c) At least one (meth)acrylate monomer in component A and component B, d) At least one toughening agent in component A and component B, and e) Internal plasticizers in component A and / or component B The internal plasticizer is a heterocyclic (meth)acrylate monomer having two or more oxygen atoms as cyclizing atoms.

[0011] According to one aspect, the present invention relates to structural adhesives comprising cured products of two-component acrylic structural adhesive compositions according to the present invention.

[0012] According to another aspect, the invention also relates to articles comprising a magnetic substrate and a structural adhesive bonded to the magnetic substrate, wherein the structural adhesive is a cured product of a two-component acrylic structural adhesive composition according to the invention.

[0013] According to another aspect, the invention also relates to loudspeakers, electric motors, or metal components that include the articles of the invention.

[0014] According to another aspect, the present invention also relates to a method for bonding two substrates, comprising: 1) Apply component A of the two-component acrylic structural adhesive composition according to the present invention to a first substrate to be bonded; 2) Apply component B of the two-component acrylic structural adhesive composition according to the present invention to the second substrate to be bonded; 3) Covering the first substrate onto the second substrate, or covering the second substrate onto the first substrate; and 4) The first substrate is bonded to the second substrate by mixing and curing the two-component acrylic structural adhesive composition, wherein components A and B are mixed and cured.

[0015] According to another aspect, the present invention also relates to another method of bonding two substrates, comprising: 1) Mix component A and component B of the two-component acrylic structural adhesive composition according to the present invention; 2) Apply the mixed two-component acrylic structural adhesive composition to the first substrate to be bonded; 3) Bring the second substrate into contact with the first substrate; and cure the composition.

[0016] According to another aspect, the present invention also relates to the use of the two-component acrylic structural adhesive composition according to the invention as a structural adhesive in the bonding of loudspeaker magnets, the bonding of electric motor structures, and the bonding of metal components. Detailed Implementation

[0017] The invention is described in more detail in the following paragraphs. Each aspect thus described may be combined with any one or more other aspects unless expressly indicated to the contrary.

[0018] In particular, any feature indicated as preferred or advantageous may be combined with any one or more other features indicated as preferred or advantageous.

[0019] In the context of this invention, the terminology used should be interpreted according to the following definitions, unless the context otherwise requires.

[0020] As used herein, the singular forms “a,” “an,” “the,” and “the” include both singular and plural references, unless the context clearly specifies otherwise. For example, references to “filler” cover embodiments having one, two, or more fillers. As used in this specification and the appended claims, the terms “or” and “or” are generally used to mean “and / or” and “as well as / or”, unless the context clearly specifies otherwise.

[0021] The terms “comprising” and “containing” as used herein are synonymous with “including” or “containing”, and are inclusive or open-ended and do not exclude additional, unlisted members, elements or method steps.

[0022] The term "ambient temperature" refers to the temperature in the range of 10 to 40°C, preferably 20 to 35°C (inclusive).

[0023] The term "high temperature" refers to a temperature in the range of 100°C or higher, preferably 100 to 150°C (inclusive).

[0024] The list of numerical endpoints includes all numbers and fractions that fall into the corresponding range, as well as the listed endpoints.

[0025] Unless otherwise defined, all terms (including technical and scientific terms) used in this disclosure have the meanings commonly understood by one of ordinary skill in the art to which this invention pertains. Further guidance, including terminology definitions, is provided to better understand the teachings of this invention.

[0026] In the context of this disclosure, several terms will be used.

[0027] The term "polymer" is used herein in accordance with its usual usage in chemistry. A polymer is composed of many repeating subunits. The term "polymer" is used to describe the material obtained by a polymerization reaction.

[0028] The term "acrylic acid" refers to either or both of the "acrylic acid" and "methacrylic acid" categories.

[0029] The term "acrylate" refers to either or both of "acrylate" and "methacrylate".

[0030] The term "curing" as used in this article refers to the process of material hardening. This term is intended to encompass the cross-linking of components within the material that have reactive groups.

[0031] As used herein, the term "one-component (1K) composition" refers to a composition in which all the components of the composition are mixed together during storage, but the properties of the composition (including viscosity) remain sufficiently consistent during the storage period to allow the composition to be successfully used later.

[0032] The term "two-component (2K) composition" is understood to be a composition in which the first component / part and the second component / part must be stored in separate containers due to their (high) reactivity. The two components / parts are mixed only shortly before application and then react, usually without further activation, with the formation of bonds and thus a polymer network.

[0033] The term "fixed time" refers to the amount of time it takes for an adhesive to not only bond but also reach handling strength, such as reaching a shear strength of 0.1 MPa within 1 minute.

[0034] For the purposes of this invention, the number-average molecular weight (Mn) was determined by gel permeation chromatography (GPC, also known as SEC) at 23°C using styrene standards according to DIN EN ISO 16014-5:2012-10.

[0035] The viscosity of the composition can be determined using a Brookfield viscometer of model RVT under standard conditions of 25°C and 50% relative humidity (RH). The viscometer is calibrated using silicone oil of known viscosity, varying between 5,000 cps and 300,000 cps. A set of RV rotors attached to the viscometer is used for calibration. Measurements of the damped composition are performed at 25°C using a No. 7 rotor at 20 revolutions per minute for 1 minute until the viscometer reaches equilibrium.

[0036] As used in this article, the glass transition temperature (T) g The measurements were determined according to DIN 53 765 using differential scanning calorimetry (DSC) with a ramp rate of 20 K / min and a midpoint measurement.

[0037] As previously discussed, embodiments of this disclosure relate to a two-component acrylic structural adhesive composition comprising component A (part A) and component B (part B). This two-component acrylic structural adhesive composition comprises at least one (meth)acrylate monomer, at least one toughening agent, a free radical initiator, a catalyst, and an internal plasticizer, wherein the internal plasticizer is a heterocyclic (meth)acrylate monomer having two or more oxygen atoms as cyclizing atoms.

[0038] The at least one (meth)acrylate monomer is present in component A and / or component B, and the at least one (meth)acrylate monomer present in component A may be the same as or different from the at least one (meth)acrylate monomer in component B. The same applies to the at least one toughening agent. The catalyst and optionally present reducing agent are present in a component different from the free radical initiator. The two-component acrylic structural adhesive composition further comprises an anti-shrinkage agent, and / or a urea acrylate monomer, and / or a reducing agent, and / or additives.

[0039] (Meth)acrylate monomers The compositions according to the invention comprise at least one (meth)acrylate monomer. The (meth)acrylate monomer is present in component A and / or component B of the composition, wherein the (meth)acrylate monomer in component A is the same as or different from the (meth)acrylate monomer in component B.

[0040] The (meth)acrylate monomers are preferably selected from 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isobutyl (meth)acrylate, cyclohexyl (meth)acrylate, 3,3,5-trimethylcyclohexyl (meth)acrylate, isobornyl (meth)acrylate, benzyl (meth)acrylate, 2-phenylethyl propionic acid, tetrahydrofurfuryl (meth)acrylate, bisphenol A ethoxylate dimethacrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, hexadecyl (meth)acrylate, octadecyl (meth)acrylate, docosyl (meth)acrylate, and mixtures thereof. 2-hydroxypropyl (meth)acrylate, isobornyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, benzyl (meth)acrylate, and 3,3,5-trimethylcyclohexyl (meth)acrylate are more preferred because they have relatively high Tg and / or good adhesion to magnetic materials.

[0041] Commercially available (meth)acrylate monomers suitable for use in this invention include, but are not limited to, SR 423 NS (isobornyl methacrylate) from Sartoma and HPMA (2-hydroxypropyl methacrylate) from Evonik.

[0042] The (meth)acrylate monomer may be present in component A in an amount of 30 to 80 parts by weight, or 40 to 70 parts by weight, or 42 to 65 parts by weight. And / or the (meth)acrylate monomer may be present in component B according to the invention in an amount of 20 to 70 parts by weight, or 25 to 55 parts by weight.

[0043] Based on the total weight of the composition, the (meth)acrylate monomer may be present in the composition in an amount of 20% to 80% by weight, or 30% to 70% by weight, or 30% to 60% by weight.

[0044] <Urea (meth)acrylate monomer> In some preferred embodiments of the invention, the (meth)acrylate monomer includes a urea (meth)acrylate monomer.

[0045] In some embodiments, the urea (meth)acrylate monomer comprises the product of the reaction of a -OH-terminated (meth)acrylate with a diisocyanate in a molar ratio of 2:1 to 2:3, and mixtures thereof. Here, the -OH-terminated (meth)acrylate is selected from 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and mixtures thereof. The diisocyanate is selected from 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, hexamethylene diisocyanate, and mixtures thereof.

[0046] In some embodiments, the urea (meth)acrylate monomer comprises one or more selected from the following: N-(2-(2-oxo-1-imidazolyl)ethyl)-(meth)acrylamide, (2,4,6-trioxo-1,3,5-triazinane-1,3,5-triyl)triethane-2,1-dimethyltriprop-2-olefin ester.

[0047] Examples of urea (meth)acrylate monomers include urea (meth)acrylate monomers with relatively low molecular weights, having a number average molecular weight (Mn) equal to or less than 1000, or between 100 and 700.

[0048] Commercially available urea (meth)acrylate monomers suitable for use in this invention include, but are not limited to, WAM from Solvay and SR 368 NS from Sartoma.

[0049] The urea (meth)acrylate monomer may be present in component A of the composition according to the invention in an amount of 0.5 to 8 parts by weight, or 0.5 to 5 parts by weight, or 0.8 to 4 parts by weight, or 1 to 3 parts by weight.

[0050] In some preferred embodiments, the urea (meth)acrylate monomer may be present in component A of the composition in an amount of less than 5 parts by weight, or less than 4.5 parts by weight, or less than 4.0 parts by weight, or less than 3.5 parts by weight. An excess of the urea (meth)acrylate monomer may result in a longer fixation time.

[0051] In some embodiments, the urea (meth)acrylate monomer may be present in amounts ranging from 0.25% to 4% by weight, or from 0.4% to 2% by weight, or from 0.5% to 1.5% by weight, based on the total weight of the composition.

[0052] toughening agent Rubber toughening agent The composition according to the invention comprises rubber. The rubber is present in part A of the composition and / or part B of the composition, wherein the rubber in part A may be the same as or different from the rubber in part B.

[0053] The rubber can be a liquid or solid natural or synthetic rubber elastomer polymer. Preferably, the rubber is selected from polybutadiene, functionalized polybutadiene, polyisobutylene, functionalized polyisobutylene, butadiene-acrylonitrile copolymer, functionalized butadiene-acrylonitrile copolymer, functionalized styrene-butadiene copolymer, styrene-butadiene copolymer, styrene-isoprene copolymer, functionalized styrene-isoprene copolymer, polyisoprene, methyl methacrylate-butadiene-styrene copolymer, and mixtures thereof, wherein the polybutadiene, polyisobutylene, butadiene-acrylonitrile copolymer, and styrene-butadiene copolymer are functionalized with functional groups selected from hydroxyl, carboxyl, carboxylic anhydride, epoxy, and mixtures thereof; more preferably, the rubber is selected from styrene-butadiene copolymer, butadiene-acrylonitrile copolymer, styrene-isoprene copolymer, methyl methacrylate-butadiene-styrene copolymer, and mixtures thereof.

[0054] The rubbers listed above are preferred because they offer good impact resistance, while the hydrophobic properties of the selected rubbers ensure that they do not affect their performance under high temperature and high humidity conditions.

[0055] Commercially available rubbers suitable for use in this invention include, but are not limited to, Kraton D1155ES from Kraton.

[0056] The rubber may be present in part A or part B of the composition according to the invention in an amount of 10 to 40 parts by weight, preferably 15 to 25 parts by weight, and more preferably 18 to 22 parts by weight.

[0057] In some embodiments, the rubber is present in an amount of 10% to 40% by weight, or 15% to 25% by weight, or 18% to 22% by weight, based on the total weight of the composition.

[0058] <Carbamate (meth)acrylate oligomer toughening agent> The compositions according to the invention comprise urethane (meth)acrylate oligomers as toughening agents. The urethane (meth)acrylate oligomers are present in component A and / or component B of the composition.

[0059] Suitable urethane (meth)acrylate oligomers for use in this invention can be aromatic urethane (meth)acrylate oligomers, aliphatic urethane (meth)acrylate oligomers, or cyclic aliphatic urethane (meth)acrylate oligomers. Preferably, the urethane (meth)acrylate oligomers are aromatic urethane (meth)acrylate oligomers or cyclic aliphatic urethane (meth)acrylate oligomers, and more preferably, the urethane (meth)acrylate oligomers are aromatic urethane (meth)acrylate oligomers. Suitable urethane (meth)acrylate oligomers for use in this invention can be formed in several ways.

[0060] Uraffinate (meth)acrylate oligomers can be formed by the reaction of diisocyanate and polyol, followed by a subsequent end-capping reaction with hydroxyl-functionalized (meth)acrylate.

[0061] The diisocyanate can be an aromatic diisocyanate, an aliphatic diisocyanate, or a cyclic aliphatic diisocyanate, wherein the aromatic diisocyanate can be selected from 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, 4,4-methylene di(phenylisocyanate), 2,4-methylene di(phenylisocyanate), 2,2-methylene di(phenylisocyanate), 1,5-naphthalene diisocyanate, and mixtures thereof; and wherein the aliphatic diisocyanate can be selected from tetramethylene diisocyanate, hexamethylene diisocyanate, pentamethylene diisocyanate, 1,4-diisocyanatobutane (1 The cyclic aliphatic diisocyanate may be selected from isophorone diisocyanate, 4,4-methylenebis(cyclohexyl isocyanate), 1,4-cyclohexane diisocyanate, and mixtures thereof; and the polyol may be selected from neopentyl glycol, trimethylolpropane, pentaerythritol, dipentaerythritol, polyethylene glycol, polytetramethylene ether glycol, and mixtures thereof; and the hydroxyfunctional (meth)acrylate may be selected from hydroxyethyl methacrylate, hydroxypropyl methacrylate, hydroxybutyl methacrylate, hydroxypentyl methacrylate, hydroxyheptyl methacrylate, hydroxynonyl methacrylate, hydroxydecyl methacrylate, and mixtures thereof.

[0062] Examples of polyols include relatively low molecular weight polyester polyols (with a number average molecular weight (Mn) of 50 to 500) and relatively high molecular weight polyols (with a number average molecular weight (Mn) of 500 to 30,000).

[0063] Alternatively, urethane (meth)acrylate oligomers can be formed by the reaction of diisocyanates with hydroxy-functional (meth)acrylates.

[0064] The diisocyanate can be an aromatic diisocyanate, an aliphatic diisocyanate, or a cyclic aliphatic diisocyanate, wherein the aromatic diisocyanate can be selected from 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, 4,4-methylene di(phenylisocyanate), 2,4-methylene di(phenylisocyanate), 2,2-methylene di(phenylisocyanate), 1,5-naphthalene diisocyanate, and mixtures thereof; and wherein the aliphatic diisocyanate can be selected from tetramethylene diisocyanate, hexamethylene diisocyanate, pentamethylene diisocyanate, 1 4-Diisocyanate butane and mixtures thereof; and wherein the cyclic aliphatic diisocyanate may be selected from isophorone diisocyanate, 4,4-methylenebis(cyclohexyl isocyanate), 1,4-cyclohexane diisocyanate and mixtures thereof; and wherein the hydroxyfunctional (meth)acrylate may be a hydroxy monofunctional (meth)acrylate, preferably selected from hydroxyethyl methacrylate, hydroxypropyl methacrylate, hydroxybutyl methacrylate, hydroxypentyl methacrylate, hydroxyheptyl methacrylate, hydroxynonyl methacrylate, hydroxydecyl methacrylate, and mixtures thereof.

[0065] T of urethane (meth)acrylate oligomers g Preferably -40 to 60°C, more preferably -20 to 20°C.

[0066] In some preferred embodiments, the urethane (meth)acrylate oligomers include (meth)acrylate oligomers based on polycarbonate urethane.

[0067] Commercially available urethane (meth)acrylate oligomers suitable for use in this invention include, but are not limited to, BR-7432GB and BRC-843S from Dymax.

[0068] The urethane (meth)acrylate oligomer may be present in component A and / or component B of the composition according to the invention in an amount of 20 to 60 parts by weight, preferably 30 to 55 parts by weight, and more preferably 35 to 50 parts by weight.

[0069] The urethane (meth)acrylate oligomer toughening agent may be present in part A or part B of the composition according to the invention in an amount of 20 to 60 parts by weight, preferably 30 to 55 parts by weight.

[0070] Based on the total weight of the composition, the urethane (meth)acrylate oligomer toughening agent may be present in the composition according to the invention in an amount of 20% to 60% by weight or 30% to 55% by weight.

[0071] The number-average molecular weight of the urethane (meth)acrylate oligomers is preferably 2,000 or greater. The number-average molecular weight of the urethane (meth)acrylate oligomers is preferably from 2,000 to 30,000.

[0072] If the amount of urethane (meth)acrylate oligomer in component A or component B is less than 20 parts by weight, it may result in excessively high composition rigidity, affecting thermal shock test failure. Conversely, an amount exceeding 60 parts by weight in component A or component B may result in high viscosity.

[0073] Free radical initiators The compositions according to the invention comprise a free radical initiator. Suitable free radical initiators for use in the invention are organic peroxides.

[0074] The free radical initiator is preferably selected from cyclic peroxides, diacyl peroxides, dialkyl peroxides, hydroperoxides, peroxycarbonates, peroxydicarbonates, peroxide esters, and peroxyketals; more preferably selected from cumene hydroperoxide (CHP), p-terpene hydroperoxide, tert-butyl hydroperoxide (TBH), tert-butyl peroxybenzoate, tert-butyl peroxypentanoate, di-tert-butyl peroxide, tert-butyl peracetate, tert-butyl peroxy-2-hexanoate, tert-pentyl hydroperoxide, and 1,2,3,4-tetramethylbutyl hydroperoxide. Benzoyl peroxide, dibenzoyl peroxide, 1,3-bis(tert-butylperoxyisopropyl)benzene, diacetyl peroxide, butyl 4,4-bis(tert-butylperoxy)valerate, p-chlorobenzoyl peroxide, tert-butylcumyl peroxide, di-tert-butyl peroxide, dicumyl peroxide, di(dodecanoyl) peroxide, 2,5-dimethyl-2,5-di-tert-butylperoxyhexane, 2,5-dimethyl-2,5-di-tert-butylperoxyhex-3-yne, 4-methyl-2,2-di-tert-butylperoxypentane, and mixtures thereof.

[0075] Commercially available free radical initiators suitable for use in this invention include, but are not limited to, Perbutyl Z from NOF Corp and Irgacure 184 from IGM Resins BV.

[0076] The free radical initiator may be present in component A of the composition according to the invention in an amount of 1 to 7 parts by weight, preferably 1.5 to 6 parts by weight, and more preferably 2 to 5 parts by weight.

[0077] If the amount of free radical initiator in component A is less than 1 part by weight, it may not have the desired curing speed; while an amount greater than 7 parts by weight may cause the adhesive to be unstable, and too high an amount may also cause the formation of low molecular weight polymers and brittle cured polymers.

[0078] In some embodiments, the free radical initiator is present in the composition in an amount of 0.5% to 3.5% by weight, or 0.7% to 3% by weight, or 1% to 3% by weight, or 1% to 2.5% by weight, based on the total weight of the composition.

[0079] catalyst The compositions according to the invention comprise a catalyst. Suitable catalysts for use in the invention are organometallic salts.

[0080] Preferably, the catalyst is selected from cobalt(II) naphthenate, copper carbonate, copper(II) acetylacetonate, copper naphthenate, silver nitrate, vanadium(III) acetylacetonate, iron(II) naphthenate, disodium copper ethylenediaminetetraacetic acid (EDTA.2Na.Cu(II)), copper naphthenate, vanadium acetylacetonate, vanadium acetylacetonate oxyacetate, iron(II) acetate, and mixtures thereof; preferably, the catalyst is selected from copper naphthenate, vanadium(III) acetylacetonate, and mixtures thereof.

[0081] Commercially available catalysts suitable for use in this invention include, but are not limited to, copper naphthenate 8 from OMG Americas Inc.

[0082] The catalyst may be present in component B of the composition according to the invention in an amount of 0.02 to 3 parts by weight, preferably 0.05 to 1 part by weight, and more preferably 0.08 to 0.5 parts by weight.

[0083] If the amount of catalyst is less than 0.02 parts by weight, it may not have the desired curing speed; while an amount greater than 3 parts by weight may cause the adhesive to be unstable.

[0084] Internal plasticizer The compositions according to the invention comprise an internal plasticizer. Suitable internal plasticizers for use in the invention are heterocyclic acrylate monomers having at least two oxygen atoms as cyclizing atoms. Surprisingly, it has been found that adding a heterocyclic ring having at least two oxygen atoms as cyclizing atoms can significantly reduce the modulus of the adhesive while maintaining similar heat resistance, thus giving the adhesive better thermal shock resistance (thermal shock resistance), particularly better crack and displacement resistance during thermal shock testing, which is considered more reliable.

[0085] In some embodiments, the internal plasticizer comprises an acrylate monomer having a heterocyclic ring having two or more oxygen atoms, such as dioxolane, dioxane, caprolactone, dioxane-heptane, trioxane-hexane, or crown ether ring. Among these heterocycles, heterocycles having two or more oxygen atoms as ring members are preferred, and / or heterocycles having at least five atoms as ring members are preferred. Furthermore, monocyclic heterocycles are preferred over fused heterocycles, and aliphatic heterocycles are preferred over aromatic heterocycles. More particularly, dioxolane and dioxane are especially preferred.

[0086] If the internal plasticizer contains only one oxygen atom as a cyclic atom, it cannot provide sufficient plasticizing properties. If the heterocyclic molecule has fewer than 5 cyclic atoms, the heterocycle is less stable for the purposes of this invention. When the heterocyclic molecule has more than 8 or more than 7 cyclic atoms, it may lead to a decrease in thermal strength or adhesion.

[0087] By including the internal plasticizer of the present invention in the adhesive composition, oxygen-containing heterocycles can be effectively plasticized and softened, which makes the adhesive have better thermal stability and thermal aging properties at similar moduli.

[0088] Specific examples of compound (A) include (meth)acrylate (2-methyl-2-ethyl-1,3-dioxolane-4-yl)methyl ester, (meth)acrylate (2,2-dimethyl-1,3-dioxolane-4-yl)methyl ester, (meth)acrylate (2-methyl-2-isobutyl-1,3-dioxolane-4-yl)methyl ester, acrylate (5-ethyl-2,2-dimethyl-1,3-dioxane-5-yl)methyl ester, and (meth)acrylate cyclohexanespiro-2-(1,3-dioxale-4-yl)methyl ester. (meth)acrylate), 5-ethyl-1,3-dioxane-5-yl acrylate, (2-oxo-1,3-dioxane-4-yl)methyl acrylate, 1,3-dioxane-2-one-5-yl acrylate, 3-[(2'R)-spiro[1,3-dioxane-2,4'-2,3-dihydro-1H-naphthalene]-2'-yl]prop-2-enoic acid ethyl ester, etc.; and (2-methyl-2-ethyl-1,3-dioxane-4-yl)methyl acrylate and (meth)acrylate 5-ethyl-1,3-dioxane-5-yl methyl acrylate are preferred because they are excellent over a wide temperature range from high to low temperatures.

[0089] In some preferred embodiments, the internal plasticizers include cyclotrimethylolpropane methyl acrylate (CTFA) and 2-methyl-2-ethyl-1,3-dioxolane-4-yl)methyl acrylate (Medol-10).

[0090] The internal plasticizer may be present in component B of the composition according to the invention in an amount greater than 3 to less than 30 parts by weight, or 4 to 28 parts by weight, or 5 to 25 parts by weight, or 6 to 20 parts by weight, or 5 to 20 parts by weight.

[0091] Based on the total weight of the composition, the internal plasticizer may be present in the composition according to the invention in an amount greater than 1.5% by weight and less than 15% by weight, or 2% by weight and 14% by weight, or 2.5% by weight and 12.5% ​​by weight, or 3% by weight and 10% by weight, or 2.5% by weight and 10% by weight.

[0092] The internal plasticizers mentioned above have been found to offer rapid curing speed, good resistance to high humidity and high temperature aging, good crack resistance during thermal shock, and high operating temperature.

[0093] additive The curable two-component adhesive composition according to the invention may further include optional additives in component A and / or component B of the composition.

[0094] Non-limiting examples of optional additives include: anti-shrinkage agents, reducing agents, stabilizers (e.g., metal chelating agents); free radical stabilizers, such as butylated hydroxytoluene, ethylenediaminetetraacetic acid (EDTA), p-benzoquinone; thickeners; fluorescent additives; dyes; and mixtures thereof.

[0095] Components A and B of the composition according to the invention may be mixed in a weight ratio of 0.5 to 2.0:1, or 0.8:1 to 1.2:1, or 0.9:1 to 1.1:1, preferably 1:1.

[0096] Preparation method of two-component acrylic structural adhesive composition Two-component acrylic structural adhesive compositions are formulated by simply mixing the various components of component A and component B separately. While there is no intention to restrict the mixing order of the components, it may be prudent to keep the initiator and catalyst / reducing agent in separate components.

[0097] The present invention also relates to the use of the two-component acrylic structural adhesive composition according to the invention as a structural adhesive in the bonding of loudspeaker magnets, the bonding of electric motor structures, and the bonding of metal components.

[0098] This invention relates to a method for bonding two substrates, comprising the following steps: 1) Apply component A of the two-component acrylic structural adhesive composition according to the present invention to a first substrate to be bonded; 2) Apply component B of the two-component acrylic structural adhesive composition according to the present invention to the second substrate to be bonded; 3) Covering the first substrate onto the second substrate, or covering the second substrate onto the first substrate; and 4) The first substrate is bonded to the second substrate by mixing and curing the two-component acrylic structural adhesive composition, wherein components A and B are mixed and cured.

[0099] The compositions according to the invention can be applied to a variety of magnetic substrates to achieve the desired benefits and advantages described herein. For example, suitable substrates may consist of AlNiCo magnets, ferrite magnets, sintered neodymium magnets, steel, zinc dichromate-coated steel, zinc chromate-coated steel, nickel, nickel-coated steel, galvanized steel, zinc phosphate-coated steel, zinc-flake coated steel, and mixtures thereof.

[0100] No pretreatment is required on the relevant surface before applying the composition. The composition is then applied to the preferably pretreated, optionally primed, surface of the substrate using conventional application methods, such as dispensing, printing, and spraying methods, including but not limited to air atomization spraying, air-assisted spraying, airless spraying, and high-volume low-pressure spraying.

[0101] The thickness of the adhesive applied in this invention can be adjusted to ensure that the final cured composition is effective in achieving the desired level of thermal shock resistance and bond strength. In many cases, the composition is applied to a wet film thickness of 0.05 to 0.5 mm. Applying thinner layers within this range is more economical and reduces the possibility of harmful thick cured areas. However, good control must be exercised during the application of thinner coatings or layers to avoid the formation of discontinuous cured films.

[0102] The curing of the compositions of the present invention typically occurs at temperatures ranging from 10°C to 40°C, 20°C to 30°C, and preferably 23°C to 27°C. A suitable temperature depends on the specific compound present and the desired curing rate, and can be determined by those skilled in the art in individual cases, using simple preliminary tests if necessary.

[0103] List of Implementation Plans 1. A two-component acrylic structural adhesive composition comprising component A and component B, a) Free radical initiators in component A b) The catalyst in component B, The composition further comprises: c) At least one (meth)acrylate monomer in component A and component B, d) At least one toughening agent in component A and component B, and e) Internal plasticizers in component A and / or component B The internal plasticizer is a heterocyclic (meth)acrylate monomer having two or more oxygen atoms as cyclizing atoms.

[0104] 2. The two-component acrylic structural adhesive composition according to embodiment 1, wherein the heterocycle of the internal plasticizer has at least five atoms as cyclizing atoms.

[0105] 3. The two-component acrylic structural adhesive composition according to any one of the foregoing embodiments, wherein the internal plasticizer comprises methyl cyclotrimethylolpropane acrylate or alkoxylated tetrahydrofuran acrylate.

[0106] 4. The two-component acrylic structural adhesive composition according to any one of the foregoing embodiments, wherein the internal plasticizer is present in an amount greater than 1.5% by weight to less than 15% by weight, or 2% by weight to 14% by weight, or 2.5% by weight to 12.5% ​​by weight, or 3% by weight to 10% by weight, or 2.5% by weight to 10% by weight, based on the total weight of the composition.

[0107] 5. The two-component acrylic structural adhesive composition according to any one of the foregoing embodiments, wherein the at least one (meth)acrylate monomer comprises a urea acrylate monomer with a number average molecular weight (Mn) equal to or less than 1000, preferably 100 to 700.

[0108] 6. The two-component acrylic structural adhesive composition according to any one of the foregoing embodiments, wherein the urea acrylate monomer is present in an amount of 0.25% to 4% by weight, or 0.4% to 2% by weight, or 0.5% to 1.5% by weight, based on the total weight of the composition.

[0109] 7. A two-component acrylic structural adhesive composition according to any one of the foregoing embodiments, wherein the toughening agent comprises a polyester polyurethane-based (meth)acrylate oligomer and a rubber.

[0110] 8. The two-component acrylic structural adhesive composition according to embodiment 7, wherein the polyester polyurethane-based (meth)acrylate oligomer may be present in an amount of 20% to 60% by weight or 30% to 55% by weight, based on the total weight of the composition.

[0111] 9. The two-component acrylic structural adhesive composition according to embodiment 7, wherein the rubber is present in an amount of 10% to 40% by weight or 15% to 25% by weight, based on the total weight of the composition.

[0112] 10. A two-component acrylic structural adhesive composition according to any one of the foregoing embodiments, wherein the free radical initiator comprises 1 to 7 parts by weight, or 1.5 to 6 parts by weight, or 2 to 5 parts by weight of a peroxide compound in component A.

[0113] 11. The two-component acrylic structural adhesive composition according to any one of the foregoing embodiments, wherein the catalyst is an organometallic salt.

[0114] 12. The two-component acrylic structural adhesive composition according to any one of the foregoing embodiments, wherein the two-component acrylic structural adhesive composition comprises: 20% to 80% by weight of (meth)acrylate monomers, 10% to 60% by weight toughening agent, 0.5% to 3.5% by weight of free radical initiator, and Effective amount of catalyst, 2% to 14% by weight of internal plasticizer, 0.25% to 4% by weight of urea (meth)acrylate.

[0115] 13. A structural adhesive comprising a cured product of a two-component acrylic structural adhesive composition according to any one of embodiments 1 to 12.

[0116] 14. The structural adhesive according to embodiment 13, wherein the structural adhesive retains 70% or more of its capacity after a thermal shock test (40 to 85°C, 30 minutes per cycle, 300 cycles) without magnet cracking or displacement.

[0117] 15. The structural adhesive according to embodiment 13, wherein the structural adhesive retains a retention rate of 70% or greater after high-temperature aging (150°C, 336 hours).

[0118] 16. An article comprising a magnet substrate and a structural adhesive bonded to the magnet substrate, wherein the structural adhesive is a cured product of a two-component acrylic structural adhesive composition according to any one of embodiments 1 to 12.

[0119] 17. A loudspeaker, an electric motor, or a metal component, including the article described in embodiment 16.

[0120] 18. A method for bonding two substrates, comprising: 1) Apply component A of the two-component acrylic structural adhesive composition according to any one of embodiments 1 to 12 to the first substrate to be bonded; 2) Apply component B of the two-component acrylic structural adhesive composition according to any one of embodiments 1 to 12 to the second substrate to be bonded; 3) Covering the first substrate onto the second substrate, or covering the second substrate onto the first substrate; and 4) The first substrate is bonded to the second substrate by mixing and curing the two-component acrylic structural adhesive composition, wherein components A and B are mixed and cured.

[0121] 19. A method for bonding two substrates, comprising: 1) Mix component A and component B of the two-component acrylic structural adhesive composition according to any one of embodiments 1 to 12; 2) Apply the mixed two-component acrylic structural adhesive composition to the first substrate to be bonded; 3) Bring the second substrate into contact with the first substrate; and cure the composition.

[0122] 20. Use of the two-component acrylic structural adhesive composition according to any one of embodiments 1 to 12 as a structural adhesive in the bonding of loudspeaker magnets, the bonding of motor structures, and the bonding of metal parts.

[0123] Example: The present invention will be further described and illustrated in detail below with reference to the embodiments. These embodiments are intended to help those skilled in the art better understand and practice the invention, but are not intended to limit the scope of the invention. All figures in the embodiments are based on weights unless otherwise stated.

[0124] raw materials

[0125] * All raw materials are used directly without any special treatment.

[0126] Example 1 <Preparation of Two-Component Acrylic Structural Adhesive Compositions> The composition of the present invention comprises raw materials at the levels shown below. The composition is obtained by: first, adding acrylate monomers to a container and mixing at 5°C to 25°C for 5 to 20 minutes. Then, adding toughening agents and anti-shrinkage agents and mixing at 20°C to 40°C until a smooth, homogeneous liquid is obtained. Then, adding plasticizers and adhesion promoters at 10°C to 40°C for 5 to 15 minutes. Then, adding catalysts and initiators at 5°C to 25°C for 5 to 10 minutes. Vacuum is preferred during mixing to reduce entrained air bubbles.

[0127] <Curing of Two-Component Acrylic Structural Adhesive Compositions> The composition is applied to the substrate by dispensing. The thickness is controlled from about 0.05 mm to about 0.5 mm. After application to the substrate, the composition is typically cured at ambient temperature for at least about 0.5 minutes, more typically about 0.75 to about 1.5 minutes.

[0128] Examples 2 to 11 and CE1 to CE8 The compositions of E2 to E11 and CE1 to CE8 were prepared according to Example 1. The compositions of E2 to E11 and CE1 to CE8 were cured according to Example 1. Further details are listed in the Results section below. For E2 to E11 and CE1 to CE8, the curing of the compositions was carried out at ambient temperature for 0.5 to 5 minutes.

[0129] Test methods <Heat Intensity Test> Thermal strength testing was performed using an Instron universal testing machine, and the test method was in accordance with ASTM D1002-2010. The substrate was galvanized steel with dimensions of 101.6 mm × 25.4 mm × 2.0 mm. An adhesive was used to bond the material to a diameter of 322.6 mm. 2 Two of the above-mentioned substrates were bonded together, and cured for at least 24 hours. Prior to testing, the sample and testing machine were heated to 130°C and held for 30 minutes. The thermal strength (shear strength) test was then performed at 130°C. The test results are shown in the table below.

[0130] Record the thermal intensity results and classify them as follows: - Fail: Shear strength less than 1.5 MPa at 130℃; - Pass: Shear strength equal to or greater than 1.5 MPa at a temperature of 130°C.

[0131] <Modulus and Elongation Test> Modulus and elongation tests were performed using an Instron universal testing machine, and the test methods were in accordance with ASTM D638-22. Specimen preparation methods included injection molding and die-cutting. In this case, the die-cutting mold was a Type III mold according to ASTM D638-22. Prior to testing, the width and thickness of each specimen were measured to an accuracy of 0.025 mm using the applicable method in ASTM D5947. Modulus and elongation tests were then performed at 50 mm / min, and the data were automatically calculated by the testing machine. The test results are shown in the table below.

[0132] Record the modulus results and classify them as follows: - Failed: Modulus greater than 400 MPa; - Pass: Modulus equal to or less than 400 MPa; - Good: Modulus equal to or less than 350 MPa.

[0133] Record the elongation results and classify them as follows: - Failed: Elongation less than 50%; - Passed if modulus equals or is greater than 50%; <Retention Rate Test> Retention rate tests were conducted to determine the reliability of the structural adhesive. The adhesive was used to bond zinc-coated steel to ferrite steel and cured for 24 hours. The zinc-coated steel had dimensions of Φ45mm × 5mm, and the ferrite steel had dimensions of Φ60mm × 15mm with a Φ15mm × 15mm hollow core. Thrust tests were performed to determine the force required to separate the zinc-coated steel from the ferrite steel using an Instron universal testing machine. Retention rate was calculated using the following equation under different aging conditions: Retention rate = (Thrust after aging / Initial thrust) × 100% - Initial thrust: The thrust prior to aging test.

[0134] - Thrust after aging: Thrust value after aging test.

[0135] The aging conditions are as follows: Thermal shock test Place the test specimen into the thermal shock environment test chamber. Set the temperature of the upper chamber to 85°C, and correspondingly set the temperature of the lower chamber to -40°C. Keep the test specimen in the upper chamber for 30 minutes, then keep it in the lower chamber for another 30 minutes. This is recorded as one cycle. The test specimen must be transferred from one chamber to the other within 15 seconds. After 300 cycles, the aging test is completed. For more stringent conditions, set the temperature of the upper chamber to 95°C, and extend the residence time in each chamber to 1 hour. After 200 cycles, the aging is completed.

[0136] Record the thermal shock test results and grade them as follows: - Fail: The sample dislocates or shifts, or breaks, or forms a crack extending deep to the substrate, or the retention rate is less than 70%; - Pass: No dislocation, no cracking, and the retention rate is equal to or greater than 70%; - Good: No dislocation, no cracking, and the retention rate is equal to or greater than 75%; - Excellent: No dislocation, no cracking, and the retention rate is equal to or greater than 90%.

[0137] <High Temperature Aging Test> Place the test specimen in an oven set at a temperature of 150°C. After 336 hours, the aging is completed.

[0138] Record the high temperature aging results and grade them as follows: - Fail: The retention rate is less than 70%; - Pass: No dislocation, no cracking, and the retention rate is equal to or greater than 70%; - Good: No dislocation, no cracking, and the retention rate is equal to or greater than 80%.

[0139] <HTHH (High Temperature High Humidity) Aging Test> Place the test specimen into an environment test chamber set at a temperature of 60°C and a humidity of 90%. After 168 hours, the aging is completed. In more stringent tests, the aging test lasts for 500 hours.

[0140] Record the high temperature high humidity aging results and grade them as follows: - Fail: The retention rate is less than 30%; - Pass: No dislocation, no cracking, no red rust, and the retention rate is equal to or greater than 30%; - Good: No dislocation, no cracking, no red rust, and the retention rate is equal to or greater than 50%.

[0141] <Fixed-Time Test> The fixed-time test determines the time required for the adhesive to bond and achieve operational strength. In this test, a sufficient amount of adhesive is applied to a prepared surface of an lap shear specimen, such that when the mating lap shear specimen is placed on the adhesive, the bond strength is 322.6 mm. 2 (0.5 in.) 2 The area is completely covered. The components are then clamped approximately 6.4 mm from each side of the adhesive area, and the adhesive is allowed to cure for a specific time. After this, a 3 kg object is suspended from the lap shear test specimen, and the specimen is lifted for 5 seconds. If the mating lap shear test specimen does not separate, the result is recorded as "pass". The shortest time to pass this type of test is recorded as the final "curing time" of the adhesive.

[0142] If the fixed time is equal to or less than 90 minutes, the result is marked as "Pass"; if the fixed time is equal to or less than 60 minutes, the result is marked as "Good"; if the fixed time is equal to or less than 50 minutes, the result is marked as "Excellent".

[0143] Table 1

[0144] Table 1 shows the structural adhesive compositions for E1 to E5 and E11.

[0145] Table 2.

[0146] Table 2 shows the test results for structural adhesive compositions E1 to E5 and E11.

[0147] Table 3.

[0148] Table 3 shows the structural adhesive compositions for E1, E6 to E10.

[0149] Table 4.

[0150] Table 4 shows the test results for structural adhesive compositions E1, E6 to E10.

[0151] In Examples 1 to 11, the structural adhesive compositions were prepared according to the formulations provided by the present invention. These formulations particularly comprise (meth)acrylate monomers, toughening agents, specific internal plasticizers, initiators, and catalysts. It can be seen that when the content of the components claimed by the present invention (especially the internal plasticizers) is within a certain range, the structural adhesive samples exhibit improved crack resistance, good thermal strength properties, and good anti-aging properties during thermal shock testing.

[0152] Sample E2 showed improved crack resistance in the thermal shock test, but failed in the more stringent thermal shock test. Samples E3 through E4 showed improved crack resistance in the more stringent thermal shock test with the addition of internal plasticizer. Sample E5 passed the thermal shock test, but failed in the more stringent thermal shock test due to the absence of an anti-shrinkage agent. Sample E11 showed that using rubber as a toughening agent can also enable the composition to pass the thermal shock test.

[0153] As can be seen from E6 to E8, structural adhesive compositions containing urea acrylate monomers passed more stringent high temperature and high humidity (HTHH) resistance tests. Urea (meth)acrylate monomers work in conjunction with specific internal plasticizers to further improve heat aging resistance and HTHH resistance. To ensure good HTHH resistance and short setting time, the structural adhesive composition contains urea acrylate monomers in component A in an amount of up to 5 parts by weight, or less than 2.5% by weight based on the total weight of the composition. Excessive urea acrylate monomers also negatively affect setting time.

[0154] Table 5.

[0155] Table 5 shows the structural adhesive compositions for CE1 to CE8.

[0156] Table 6.

[0157] Table 6 shows the test results for structural adhesive compositions CE1 to CE8.

[0158] In Comparative Example CE1, the amount of internal plasticizer was higher than required. Excessive internal plasticizer negatively impacted thermal strength, thermal shock resistance (displacement) in the thermal shock test, and resistance to high temperature and humidity. In the absence of internal plasticizer, the sample in CE2 exhibited an excessively high modulus and poor thermal shock resistance in the thermal shock test. In Comparative Example CE4, the amount of internal plasticizer was less than required, and the aqueous acoustic damping composition with insufficient internal plasticizer failed the thermal shock test and also failed the thermal aging test.

[0159] CE3 contains a polyether-based urethane (meth)acrylate oligomer as a toughening agent. The composition has a suitable modulus value and acceptable retention, but the sample shifts after a thermal shock test. Furthermore, CE3 failed both the more stringent thermal shock test and the thermal aging test. Regarding CE3, the instantaneous thermal strength (i.e., thermal strength) was improved by introducing a high-Tg acrylate monomer, but thermal aging performance remained difficult to improve. It is very difficult for CE3 to simultaneously achieve excellent performance in both thermal shock and thermal aging. If a high-Tg oligomer is used, whether it is a polyester or a polyether urethane (meth)acrylate oligomer, it is very difficult to pass thermal and thermal shock tests unless a large amount of internal plasticizer is added. However, such a large amount of internal plasticizer leads to poor thermal strength performance. In this case, it is preferable to use a polyester urethane (meth)acrylate oligomer because it has better thermal stability. The claimed internal plasticizer and urea-based monomer can compensate for the shortcomings of polyester in terms of thermal shock while maintaining thermal stability and improving hydrolysis resistance.

[0160] CE5 contains a heterocyclic plasticizer, wherein the heterocycle has only one oxygen atom as a cyclizing atom. CE6 contains a plasticizer with a polyether group. The thermal shock test results of CE5 and CE6 show that the lack of the claimed heterocyclic (meth)acrylate monomer (wherein the heterocycle has two or more oxygen atoms as cyclizing atoms) leads to failure in crack resistance. CE7 and CE8 use plasticizers with long carbon chains, which exhibit visible plasticizing properties. However, such plasticizers negatively impact thermal strength and impact resistance, making them unsuitable for such high-temperature operating and thermal shock environments. With increasing amounts of long-chain plasticizers in the composition, the settling time increases. Comparing the settling time values ​​of CE1 and CE8, conventional long-chain plasticizers can increase settling time and reduce production efficiency. Claims (as amended under Article 19 of the Treaty) 1. A two-component acrylic structural adhesive composition comprising component A and component B, a) Free radical initiators in component A b) The catalyst in component B, The composition further comprises: c) At least one (meth)acrylate monomer in component A and component B, d) At least one toughening agent in component A and component B, and e) Internal plasticizers in component A and / or component B The internal plasticizer is a heterocyclic (meth)acrylate monomer having two or more oxygen atoms as cyclizing atoms. 2. The two-component acrylic structural adhesive composition according to claim 1, wherein the heterocycle of the internal plasticizer has at least five atoms as cyclizing atoms. 3. The two-component acrylic structural adhesive composition according to claim 1, wherein the internal plasticizer comprises methyl cyclotrimethylolpropane acrylate. 4. The two-component acrylic structural adhesive composition of claim 1, wherein the internal plasticizer is present in an amount greater than 1.5% by weight to less than 15% by weight, or 2% by weight to 14% by weight, or 2.5% by weight to 12.5% ​​by weight, or 3% by weight to 10% by weight, or 2.5% by weight to 10% by weight, based on the total weight of the composition. 5. The two-component acrylic structural adhesive composition according to claim 1, wherein the at least one (meth)acrylate monomer comprises a urea acrylate monomer with a number average molecular weight (Mn) equal to or less than 1000, preferably 100 to 700. 6. The two-component acrylic structural adhesive composition according to claim 5, wherein the urea acrylate monomer is present in an amount of 0.25% to 4% by weight, or 0.4% to 2% by weight, or 0.5% to 1.5% by weight, based on the total weight of the composition. 7. The two-component acrylic structural adhesive composition of claim 1, wherein the toughening agent comprises a polyester polyurethane-based (meth)acrylate oligomer and a rubber. 8. The two-component acrylic structural adhesive composition according to claim 7, wherein the polyester polyurethane-based (meth)acrylate oligomer may be present in an amount of 20% to 60% by weight or 30% to 55% by weight, based on the total weight of the composition. 9. The two-component acrylic structural adhesive composition of claim 7, wherein the rubber is present in an amount of 10% to 40% by weight or 15% to 25% by weight, based on the total weight of the composition. 10. The two-component acrylic structural adhesive composition according to claim 1, wherein the free radical initiator comprises 1 to 7 parts by weight, or 1.5 to 6 parts by weight, or 2 to 5 parts by weight of a peroxide compound in component A. 11. The two-component acrylic structural adhesive composition according to claim 1, wherein the catalyst is an organometallic salt. 12. The two-component acrylic structural adhesive composition according to claim 1, wherein the two-component acrylic structural adhesive composition comprises: 20% to 80% by weight of (meth)acrylate monomers, 10% to 60% by weight toughening agent, 0.5% to 3.5% by weight of free radical initiator, and Effective amount of catalyst, 2% to 14% by weight of internal plasticizer, 0.25% to 4% by weight of urea (meth)acrylate. 13. A structural adhesive comprising a cured product of a two-component acrylic structural adhesive composition according to any one of claims 1 to 12. 14. The structural adhesive of claim 13, wherein the structural adhesive retains 70% or more of its original value after a thermal shock test (40 to 85°C, 30 minutes per cycle, 300 cycles) without any magnet cracking or displacement. 15. The structural adhesive according to claim 13, wherein the structural adhesive retains 70% or more after high-temperature aging (150°C, 336 hours). 16. An article comprising a magnet substrate and a structural adhesive bonded to the magnet substrate, wherein the structural adhesive is a cured product of a two-component acrylic structural adhesive composition according to any one of claims 1 to 12. 17. A loudspeaker, an electric motor, or a metal component, including the article according to claim 16. 18. A method for bonding two substrates, comprising: 1) Applying component A of the two-component acrylic structural adhesive composition according to any one of claims 1 to 12 to the first substrate to be bonded; 2) Apply component B of the two-component acrylic structural adhesive composition according to any one of claims 1 to 12 to the second substrate to be bonded; 3) Covering the first substrate onto the second substrate, or covering the second substrate onto the first substrate; and 4) The first substrate is bonded to the second substrate by mixing and curing the two-component acrylic structural adhesive composition, wherein components A and B are mixed and cured. 19. A method for bonding two substrates, comprising: 1) Mixing component A and component B of the two-component acrylic structural adhesive composition according to any one of claims 1 to 12; 2) Apply the mixed two-component acrylic structural adhesive composition to the first substrate to be bonded; 3) Bring the second substrate into contact with the first substrate; and cure the composition. 20. Use of the two-component acrylic structural adhesive composition according to any one of claims 1 to 12 as a structural adhesive in the bonding of loudspeaker magnets, the bonding of motor structures, and the bonding of metal parts.

Claims

1. A two-component acrylic structural adhesive composition comprising component A and component B, a) The free radical initiator in component A, b) The catalyst in component B, The composition further comprises: c) at least one (meth)acrylate monomer in component A and component B, d) At least one toughening agent in component A and component B, and e) Internal plasticizers in component A and / or component B The internal plasticizer is a heterocyclic (meth)acrylate monomer having two or more oxygen atoms as cyclizing atoms.

2. The two-component acrylic structural adhesive composition according to claim 1, wherein the heterocycle of the internal plasticizer has at least five atoms as cyclizing atoms.

3. The two-component acrylic structural adhesive composition according to claim 1, wherein the internal plasticizer comprises methyl cyclotrimethylolpropane acrylate and alkoxylated tetrahydrofuran acrylate.

4. The two-component acrylic structural adhesive composition of claim 1, wherein the internal plasticizer is present in an amount greater than 1.5% by weight to less than 15% by weight, or 2% by weight to 14% by weight, or 2.5% by weight to 12.5% ​​by weight, or 3% by weight to 10% by weight, or 2.5% by weight to 10% by weight, based on the total weight of the composition.

5. The two-component acrylic structural adhesive composition according to claim 1, wherein the at least one (meth)acrylate monomer comprises a urea acrylate monomer with a number average molecular weight (Mn) equal to or less than 1000, preferably 100 to 700.

6. The two-component acrylic structural adhesive composition according to claim 5, wherein the urea acrylate monomer is present in an amount of 0.25% to 4% by weight, or 0.4% to 2% by weight, or 0.5% to 1.5% by weight, based on the total weight of the composition.

7. The two-component acrylic structural adhesive composition of claim 1, wherein the toughening agent comprises a polyester polyurethane-based (meth)acrylate oligomer and a rubber.

8. The two-component acrylic structural adhesive composition according to claim 7, wherein the polyester polyurethane-based (meth)acrylate oligomer may be present in an amount of 20% to 60% by weight or 30% to 55% by weight, based on the total weight of the composition.

9. The two-component acrylic structural adhesive composition of claim 7, wherein the rubber is present in an amount of 10% to 40% by weight or 15% to 25% by weight, based on the total weight of the composition.

10. The two-component acrylic structural adhesive composition according to claim 1, wherein the free radical initiator comprises 1 to 7 parts by weight, or 1.5 to 6 parts by weight, or 2 to 5 parts by weight of a peroxide compound in component A.

11. The two-component acrylic structural adhesive composition according to claim 1, wherein the catalyst is an organometallic salt.

12. The two-part acrylic structural adhesive composition of claim 1, wherein, The two-component acrylic structural adhesive composition comprises: 20% to 80% by weight of (meth)acrylate monomers, 10% to 60% by weight toughening agent, 0.5% to 3.5% by weight of free radical initiator, and Effective amount of catalyst, 2% to 14% by weight of internal plasticizer, 0.25% to 4% by weight of urea (meth)acrylate.

13. A structural adhesive comprising a cured product of a two-component acrylic structural adhesive composition according to any one of claims 1 to 12.

14. The structural adhesive of claim 13, wherein, The structural adhesive retains 70% or more of its properties after a thermal shock test (40 to 85°C, 30 minutes per cycle, 300 cycles) without any magnet cracking or displacement.

15. The structural adhesive of claim 13, wherein, The structural adhesive retains 70% or more of its properties after high-temperature aging (150°C, 336 hours).

16. An article comprising a magnet substrate and a structural adhesive bonded to the magnet substrate, wherein the structural adhesive is a cured product of a two-component acrylic structural adhesive composition according to any one of claims 1 to 12.

17. A loudspeaker, an electric motor, or a metal component, including the article according to claim 16.

18. A method for bonding two substrates, comprising: 1) Applying component A of the two-component acrylic structural adhesive composition according to any one of claims 1 to 12 to the first substrate to be bonded; 2) Apply component B of the two-component acrylic structural adhesive composition according to any one of claims 1 to 12 to the second substrate to be bonded; 3) Cover the first substrate onto the second substrate, or cover the second substrate onto the first substrate; as well as 4) The first substrate is bonded to the second substrate by mixing and curing the two-component acrylic structural adhesive composition, wherein components A and B are mixed and cured.

19. A method for bonding two substrates, comprising: 1) Mixing component A and component B of the two-component acrylic structural adhesive composition according to any one of claims 1 to 12; 2) Apply the mixed two-component acrylic structural adhesive composition to the first substrate to be bonded; 3) Make the second substrate come into contact with the first substrate; The composition is then cured.

20. Use of the two-component acrylic structural adhesive composition according to any one of claims 1 to 12 as a structural adhesive in the bonding of loudspeaker magnets, the bonding of motor structures, and the bonding of metal parts.