Cobalt-titanium alloy sputtering target assembly and its manufacturing method

By employing a two-step diffusion bonding process, the thermal stress problem at the bonding interface caused by the difference in thermal expansion coefficients between the cobalt-titanium alloy sputtering target and the copper alloy backing plate is solved, thereby enhancing the bonding strength. This process is suitable for sputtering target components in high-power semiconductor manufacturing.

CN123125366APending Publication Date: 2026-11-17SOZOTEX PERFORMANCE MATERIALS AMERICA INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202580028827.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2025-04-09
Filing Date
2025-04-17
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The difference in thermal expansion coefficients between the cobalt-titanium alloy sputtering target and the copper alloy backing plate leads to thermal stress at the interface, which may cause the sputtering target to peel off or crack, affecting the stability and service life of the sputtering target.

Method used

A two-step diffusion bonding process is adopted. First, at a high bonding temperature, a high-purity cobalt-titanium alloy sputtering target is diffused and bonded to a copper layer to form an intermediate coated sputtering target. Then, at a low bonding temperature, it is further diffused and bonded to a copper alloy backing plate. The difference in thermal expansion coefficient is reduced by the copper layer in the intermediate layer, thereby enhancing the bonding strength.

Benefits of technology

It improves the bonding strength between the sputtering target and the backplate, enabling it to remain stable under high-power sputtering conditions and preventing target warping or cracking. It is suitable for high-power PVD chambers in semiconductor manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123125366A_ABST
    Figure CN123125366A_ABST
Patent Text Reader

Abstract

A method for manufacturing a cobalt-titanium sputtering target is provided, wherein the sputtering target comprises 0.5 atomic percent to 24.9 atomic percent titanium. A sputtering target assembly and a method for manufacturing the sputtering target assembly are also provided.
Need to check novelty before this filing date? Find Prior Art

Description

Cross-referencing of related patent applications

[0001] This application claims priority to U.S. Patent Application No. 19 / 174,301, filed April 9, 2025, and U.S. Provisional Patent Application No. 63 / 636,698, filed April 19, 2024, the entire contents of which are incorporated herein by reference. Technical Field

[0002] This disclosure relates to cobalt-titanium alloy sputtering target assemblies and methods for manufacturing such sputtering target assemblies. The cobalt-titanium alloy sputtering target assemblies discussed herein can be used in semiconductor manufacturing. Background Technology

[0003] Physical vapor deposition (PVD) is widely used to form thin films of materials on a variety of substrates. One important application of this deposition technology is semiconductor manufacturing. Figure 1 The diagram illustrates a portion of an exemplary physical vapor deposition (“PVD”) apparatus 8. In one configuration, the sputtering target assembly 10 includes a backplate 12 to which a target 14 is coupled. A substrate 18 (such as a semiconductive material wafer) is located within the PVD apparatus 8 and is positioned spaced apart from the target 14. The surface 16 of the target 14 is the sputtering surface. As shown, the target 14 is disposed above the substrate 18 and positioned such that the sputtering surface 16 faces the substrate 18. In operation, sputtering material 22 is displaced from the sputtering surface 16 of the target 14 and used to form a coating (or thin film) 20 on the substrate 18.

[0004] Cobalt-titanium alloys are next-generation candidates for barrier layers in interconnects. Power densities in sputtering target chambers will likely be high. Therefore, diffusion-bonded targets may be necessary. Copper alloys are the most commonly used backing material. However, cobalt-titanium alloys and copper alloys have different coefficients of thermal expansion (CTE), which can induce thermal stress at the interface between the cobalt-titanium sputtering target and the copper alloy backing, potentially leading to target delamination or cracking.

[0005] An improved sputtering target assembly is needed. Summary of the Invention

[0006] In embodiment 1, a method for manufacturing a cobalt-titanium sputtering target includes: combining cobalt metal powder and titanium metal powder to form a powder mixture containing 0.5 atomic percent (atomic %) titanium to 24.9 atomic % titanium and residual cobalt and impurities; and vacuum hot-pressing the powder mixture at about 800°C to about 1150°C under hydraulic pressure of about 2 ksi (13.8 MPa) to about 5 ksi (34.5 MPa) for a holding time of about 2 hours to about 5 hours to form a cobalt-titanium sputtering target having a density of at least 95%.

[0007] In embodiment 2, the method according to embodiment 1 is used, wherein the titanium powder has a purity of about 3N5 to about 5N.

[0008] In embodiment 3, according to the method of embodiment 1, the cobalt powder has a purity of about 3N5 to about 5N.

[0009] In embodiment 4, the method described in embodiment 1 is used, wherein the vacuum hot pressing is performed at approximately 1000°C to approximately 1150°C.

[0010] In embodiment 5, the method described in embodiment 4 is used, wherein the vacuum hot pressing is performed under hydraulic pressure of about 2.5 ksi (17.2 MPa) to about 4 ksi (27.6 MPa).

[0011] In implementation scheme 6, the method described in implementation scheme 5 is used, wherein the holding time is from about 2 hours to about 4 hours.

[0012] In implementation scheme 7, the method according to implementation scheme 1 is wherein the density is at least 99%.

[0013] In embodiment 8, the method according to embodiment 1 is wherein the powder mixture comprises 10 atomic percent (atomic %) titanium to 20 atomic percent titanium, and the remainder cobalt and impurities.

[0014] In embodiment 9, the sputtering target assembly includes a powder metallurgy high-purity cobalt-titanium alloy sputtering target having a density of at least 95%, a copper alloy backplate diffusely bonded to the sputtering target, and an intermediate layer positioned between the sputtering target and the backplate. The intermediate layer includes: an optional first layer directly adjacent to the sputtering target and composed of copper; a second layer, if the first layer is present, directly adjacent to the first layer, or if the first layer is absent, directly adjacent to the sputtering target, wherein the second layer is composed of copper; and a third layer, directly adjacent to the second layer on a first side and directly adjacent to the backplate on an opposite side, wherein the third layer is composed of copper.

[0015] In embodiment 10, the sputtering target assembly according to embodiment 9 is wherein the powder metallurgy high-purity cobalt-titanium alloy sputtering target is composed of 0.5 atomic percent (atomic %) titanium to 24.9 atomic percent titanium, as well as the remaining cobalt and impurities.

[0016] In Implementation Scheme 11, the sputtering target assembly according to Implementation Scheme 9 is wherein the powder metallurgy high-purity cobalt-titanium alloy sputtering target is composed of 10 atomic percent (atomic %) titanium to 20 atomic percent titanium.

[0017] In embodiment 12, the sputtering target assembly according to embodiment 9 is provided, wherein the sputtering target has a density of at least 99%.

[0018] In embodiment 13, the method of forming a sputtering target assembly includes diffusion bonding of a sputtering target to a second copper layer at a high bonding temperature to form an intermediate-plated sputtering target, the sputtering target consisting of 0.5 atomic percent (atomic %) titanium to 24.9 atomic percent titanium and the remainder cobalt and impurities; positioning a first side of a third copper layer adjacent to a backplate and positioning a side opposite to the first side of the third copper layer adjacent to a second layer to form an assembly; and diffusion bonding of the assembly at a low bonding temperature to form a sputtering target assembly.

[0019] In embodiment 14, according to the method described in embodiment 13, the powder metallurgy high-purity cobalt-titanium alloy sputtering target is composed of 10 atomic percent (atomic %) titanium to 20 atomic percent titanium.

[0020] In embodiment 15, the method according to embodiment 13 is wherein the bonding strength is at least 10 ksi (68.9 MPa).

[0021] In embodiment 16, the method according to embodiment 13 is wherein the sputtering target assembly is suitable for a high-power sputtering chamber.

[0022] In embodiment 17, according to the method of embodiment 13, the powder metallurgy high-purity cobalt-titanium alloy sputtering target has an average grain size of less than about 100 μm.

[0023] In embodiment 18, the method according to embodiment 13 is further comprising depositing a first copper layer on a powder metallurgy high-purity cobalt-titanium alloy sputtering target before diffusion bonding the powder metallurgy high-purity cobalt-titanium alloy sputtering target to the second copper layer, wherein diffusion bonding the powder metallurgy high-purity cobalt-titanium alloy sputtering target to the second copper layer comprises positioning the second copper layer adjacent to the first copper layer.

[0024] In embodiment 19, the method according to embodiment 13 is wherein the high binding temperature is from about 600°C to about 1000°C.

[0025] In embodiment 20, the method according to embodiment 13 is wherein the low binding temperature is from about 250°C to about 500°C.

[0026] While several embodiments have been disclosed, other embodiments of the invention will become apparent to those skilled in the art from the following detailed description illustrating and describing exemplary embodiments of the invention. Therefore, the drawings and detailed description should be considered illustrative rather than restrictive in nature. Attached Figure Description

[0027] Figure 1 This is a schematic diagram of a sputtering device.

[0028] Figure 2 This is a schematic cross-sectional view of an exemplary cobalt-titanium sputtering target assembly.

[0029] Figure 3 This is a block diagram for preparing cobalt-titanium sputtering target components.

[0030] Figure 4 This is a SEM image of a cobalt-titanium sputtering target.

[0031] Figure 5 This is an EBSD mapping of a cobalt-titanium sputtering target.

[0032] Figure 6 This is a bar chart of the grain size of the cobalt-titanium sputtering target.

[0033] Figure 7 This is an X-ray diffraction pattern of a cobalt-titanium sputtering target. Detailed Implementation

[0034] This paper discloses an improved cobalt-titanium sputtering target and its preparation method. Figure 2 This is a schematic cross-sectional view of a sputtering target assembly 100, which includes a backplate 102, a sputtering target 104, and an intermediate layer 106, which includes optional first layer 108, second layer 110, and third layer 112. The backplate 102 and the sputtering target 104 are joined by a diffusion joint.

[0035] The sputtering target 104 is a cobalt-titanium alloy, which may include unavoidable impurities. For example, the sputtering target 104 may consist of cobalt and titanium, along with unavoidable impurities. In some embodiments, the cobalt-titanium alloy may contain cobalt as the primary or base metal and titanium as the alloying metal. In some embodiments, the cobalt-titanium alloy contains about 0.5 atomic percent (atomic %) to about 24.9 atomic %, or about 10 atomic % to about 20 atomic % titanium, with the remainder being cobalt. The sputtering target 104 has a purity sufficient for, for example, forming a barrier layer in semiconductor manufacturing. In one example, the sputtering target 104 has a purity of at least about 99.95% or 3N5. In some embodiments, the sputtering target 104 is free of iron, unless it may be present as an impurity.

[0036] The sputtering target 104 has a sufficient average grain size for the interconnect material. For example, the sputtering target 104 may have an average grain size of less than about 100 micrometers (μm). In some examples, the sputtering target 104 may have an average grain size of less than about 50 μm. In some examples, the sputtering target 104 has an average grain size of less than about 10 μm. In some embodiments, the average grain size can be determined using electron backscatter diffraction (EBSD). In some embodiments, the grain size is measured using EBSD according to ASTM E2627-2013.

[0037] The sputtering target 104 has a density sufficient for PVD. In some examples, the sputtering target 104 has a density of at least 95%. In other examples, the sputtering target 104 has a density of at least 99% or at least 100%. In some embodiments, the density can be measured using the Archimedes method.

[0038] As described herein, the sputtering target 104 can be formed by powder metallurgy. For example, the sputtering target 104 can be formed by vacuum hot pressing cobalt in powder form and titanium in powder form.

[0039] Cobalt powder can be a high-purity powder. For example, cobalt powder can have a purity of about 3N5 to about 5N. Titanium powder can also be a high-purity powder. For example, titanium powder can have a purity of about 3N5 to about 5N.

[0040] The backplate 102 may be formed of a copper alloy, such as a copper-zinc alloy, a copper-chromium alloy, or a copper-chromium-nickel-silicon alloy. For example, the backplate 102 may be formed of C46400 (CuZn alloy), C18200 (Cu-1%Cr alloy), or C18000 (CuCrNiSi alloy). In some embodiments, the backplate 102 is a CuZn alloy. It has been found that insufficient bonding occurs between the backplate 102 and the sputtering target 104 when using low bonding temperatures (e.g., below 250°C). Higher bonding temperatures may induce thermal stress between the two components due to the difference in the coefficients of thermal expansion (CTE) between the sputtering target 104 and the backplate 102, which can lead to delamination or cracking of the sputtering target 104. For example, using mixture rules, the CTE of a standard CuZn backplate is about 20 μm / m·K, and the CTE of Co-15 atomic%Ti is about 12.4 μm / m·K.

[0041] Intermediate layer 106 improves the bonding between sputtering target 104 and backplane 102. Intermediate layer 106 includes a first layer 108 (optional), a second layer 110, and a third layer 112. The first layer 108 is a copper layer and, when present, is directly or immediately adjacent to the sputtering target 104. In some embodiments, the first layer 108 is composed of copper or is substantially composed of copper. The first layer 108 is a thin layer. For example, the first layer 108 may have a thickness of about 1 micrometer to about 10 micrometers.

[0042] When the first layer 108 is present, the second layer 110 is directly adjacent to the first layer 108 on the first side, and when the first layer 108 is absent, the second layer is directly adjacent to the sputtering target 104 on the first side. The second layer 110 is directly adjacent to the third layer 112 on the side opposite to the first side. The second layer 110 is formed of copper foil, such as oxygen-free copper, such as Cu-OFE (oxygen-free electronic grade). In some embodiments, the second layer 110 is formed of copper with an oxygen-free degree of up to 99.99%. The second layer 110 is a thin layer. For example, the second layer 110 may have a thickness of about 0.010 inches to about 0.100 inches (about 0.254 millimeters (mm) to about 2.54 mm). In some examples, the second layer 110 may be formed of copper foil with a thickness of about 0.025 inches.

[0043] The third layer 112 is directly adjacent to the second layer 110 on the first side and directly adjacent to the back plate 102 on the opposite side. The third layer 112 may also be formed of copper. For example, the third layer 112 may be formed of oxygen-free copper, such as Cu-OFE. In some embodiments, the third layer 112 is formed of copper with an oxygen-free degree of up to 99.99%. In some embodiments, the third layer 112 has a thickness of about 0.1 inches to about 0.3 inches (about 2.5 mm to about 7.62 mm).

[0044] The sputtering target 104 and the backing plate 102 are diffusely bonded to each other. In some embodiments, the sputtering target 104 and the backing plate 102 are bonded by hot isostatic pressing (HIP) or vacuum thermopressing. In some embodiments, the bond strength is at least 10 kpsi (68.9 MPa).

[0045] Thermal stress occurs at the bonding interface between sputtering target 104 and backplane 102 as the sputtering target assembly cools after diffusion bonding. Thermal stress may also occur at the bonding interface during the sputtering cycle. Thermal stress can cause peeling or cracking of the sputtering target 104. As described herein, the sputtering target 104, intermediate layer 106, and two-step diffusion bonding process produce a sputtering target assembly with suitable characteristics for use in high-power PVD chambers (i.e., 10 kW or higher) in semiconductor manufacturing, such as barrier layers for interconnects. For example, the sputtering target 104 may be able to withstand sputtering of 10 kW or higher without warping.

[0046] Figure 3This is a diagram of a method 200 for preparing a sputtering target assembly 100. In step 202, a sputtering target 104 is produced using powder metallurgy. For example, cobalt powder and titanium powder can be shaped into a sputtering target using vacuum hot pressing. For example, high-purity cobalt powder and high-purity titanium powder can be mixed to form a desired cobalt / titanium mixture and loaded into a mold of a vacuum hot press. In some embodiments, the cobalt powder is mixed with about 0.5 atomic% to about 24.9 atomic% of titanium powder. In some embodiments, the cobalt powder is mixed with about 5 atomic% to about 20 atomic%, or 10 atomic% to about 20 atomic% of titanium powder. In some embodiments, the cobalt powder may have a purity of at least 4N (99.99%) and / or a particle size of 200 mesh, and the titanium powder may have a purity of at least 4N and / or a particle size of 325 mesh.

[0047] The mixed powders are vacuum hot-pressed to form a cobalt-titanium alloy sputtering target. In some embodiments, the vacuum hot-pressing is performed at a temperature of about 800°C to about 1150°C, under hydraulic pressure of about 2 ksi (13.8 MPa) to about 5 ksi (34.5 MPa), and with a holding time of about 2 hours to about 5 hours. In some embodiments, the vacuum hot-pressing is performed at 1000°C to about 1150°C, at 2.5 ksi (17.2 MPa) to 4 ksi (27.6 MPa), and with a holding time of 2 hours to 4 hours. In some embodiments, the vacuum hot-pressing is performed at 1000°C to about 1150°C, at 3 ksi (20.7 MPa) to 4 ksi (27.6 MPa), and with a holding time of 2 hours to 4 hours. The sputtering target has a density of at least 95%. In some embodiments, the sputtering target has a density of at least 99% or at least 100%.

[0048] In step 204, optionally, the first layer is formed directly on the back surface of the sputtering target. As described herein, the first layer is a thin copper layer. In some embodiments, the first layer may be formed by electroplating, PVD processes, or ion plating. In some embodiments, the first layer may be about 1 micrometer to about 10 micrometers thick. The first layer acts as an adhesion layer and bonds the sputtering target to the second layer.

[0049] In step 206, a second layer is formed on the sputtering target. In embodiments where a first layer is present, the second layer can be formed by diffusion bonding the second layer to the first layer on the sputtering target. In embodiments where a first layer is absent, the second layer can be formed by direct diffusion bonding the second layer to the back surface of the sputtering target. In some embodiments, the second layer is an oxygen-free copper foil. The second layer can be bonded to the first layer (if present) or the back surface of the sputtering target by high-temperature diffusion bonding. For example, the assembly can be hot-pressed at about 600°C to about 1000°C. The second layer provides a bonding surface with the third layer. The copper in the second layer and the copper in the third layer provide copper-to-copper bonding for the assembly.

[0050] In step 208, a sputtering target having a first (optional) and a second layer is bonded to a backplate by diffusion bonding. In step 208, a third layer is placed adjacent to the second layer on the sputtering target, and the backplate is placed adjacent to the third layer. The assembly is bonded to form a composite material by cryogenic hot isostatic pressing (HIP). Figure 2 The sputtering target assembly 100. For example, the assembly can be bonded at a temperature of about 250°C to about 500°C.

[0051] The low bonding temperature in step 208 minimizes thermal stress between the sputtering target and the backing plate, preventing target cracking. The use of the second layer provides a CTE gradient between the sputtering target and the backing plate.

[0052] Example 1

[0053] Cobalt-titanium alloy samples (Co-15Ti alloy) containing 15 atomic% titanium were prepared by vacuum hot pressing a mixture of cobalt powder and titanium powder at 1200 °C and 3.5 ksi (24.1 MPa) for 2 hours.

[0054] The density of the sputtering target can be measured using the Archimedes method. The transverse fracture strength can be determined using ASTM B528-16. Figure 4 This is a scanning electron microscope (SEM) image of a cobalt-titanium alloy. The image shows that the alloy has a small grain size. Grain size can be measured using EBSD. Figure 5 This is the electron backscatter diffraction (EBSD) mapping of the alloy. The average grain size is 4.6 μm. Figure 6 It is a bar chart of grain size (diameter in micrometers).

[0055] The X-ray diffraction (XRD) pattern of the alloy is provided in Figure 7 Based on XRD analysis, the alloy is believed to have two phases: TiCo3 and α-Co. Phase concentrations are provided in Table 1.

[0056] Table 1 .

[0057]

[0058] Hypothetical Example 1

[0059] The cobalt-titanium alloy of Example 1 can be diffusely bonded to the copper-zinc alloy C46400. The bond can be analyzed by C-scan, and the bond strength can be determined using the RAM tensile test method as described in Zatorski, Z. (2007) Evaluation of Steel Clad Plate Weldability Using Ram Tensile Test Method. Engineering Transactions, 55(3), 229-238.

[0060] Various modifications and additions can be made to the exemplary embodiments discussed without departing from the scope of the invention. For example, while the above embodiments relate to specific features, the scope of the invention also includes embodiments with different combinations of features and embodiments that do not include all of the above features.

Claims

1. A method for manufacturing a cobalt-titanium sputtering target, the method comprising: Cobalt powder and titanium powder are combined to form a powder mixture containing 0.5 atomic percent (atomic %) titanium to 24.9 atomic percent titanium, and the remainder cobalt and impurities; and The powder mixture is vacuum hot-pressed at approximately 800°C to approximately 1150°C under hydraulic pressure of approximately 2,000 psi (ksi) (13.8 MPa) to approximately 5 ksi (34.5 MPa) for a holding time of approximately 2 hours to approximately 5 hours to form a cobalt-titanium sputtering target with a density of at least 95%.

2. The method according to claim 1, wherein the vacuum hot pressing is performed at about 1000°C to about 1150°C.

3. The method of claim 2, wherein the vacuum hot pressing is performed under hydraulic pressure of about 2.5 ksi (17.2 MPa) to about 4 ksi (27.6 MPa).

4. The method according to claim 1, wherein the density is at least 99%.

5. The method of claim 1, wherein the powder mixture contains 10 atomic percent (atomic %) titanium to 20 atomic percent titanium, and the remainder cobalt and impurities.

6. A sputtering target assembly, comprising: A powder metallurgical cobalt-titanium alloy sputtering target, wherein the cobalt-titanium alloy sputtering target has a density of at least 95%; A copper alloy backplate, wherein the copper alloy backplate is diffusely bonded to the sputtering target; and Intermediate layer, positioned between the sputtering target and the backplate, the intermediate layer comprising: An optional first layer, which is directly adjacent to the sputtering target and is composed of copper; The second layer, if the first layer exists, is directly adjacent to the first layer; or if the first layer does not exist, the second layer is directly adjacent to the sputtering target, wherein the second layer is composed of copper; and The third layer is directly adjacent to the second layer on the first side and directly adjacent to the back plate on the opposite side, wherein the third layer is composed of copper.

7. The sputtering target assembly of claim 6, wherein the powder metallurgy cobalt-titanium alloy sputtering target comprises 0.5 atomic percent (atomic %) titanium to 24.9 atomic percent titanium, with the remainder cobalt and impurities.

8. A method for forming a sputtering target assembly, the method comprising: At a high bonding temperature, a powder metallurgy cobalt-titanium alloy sputtering target is diffusely bonded to a second copper layer to form an intermediate plating sputtering target, wherein the powder metallurgy cobalt-titanium alloy sputtering target consists of 0.5 atomic percent (atomic %) titanium to 24.9 atomic percent titanium, as well as the remainder cobalt and impurities; The first side of the third copper layer is positioned adjacent to the backplate, and the side opposite to the first side of the third copper layer is positioned adjacent to the second layer to form an assembly; and The component is diffused and bonded at a low bonding temperature to form a sputtering target component.

9. The method of claim 8, further comprising: Before diffusion bonding the powder metallurgy cobalt-titanium alloy sputtering target to the second copper layer, a first copper layer is deposited on the powder metallurgy cobalt-titanium alloy sputtering target; and wherein diffusion bonding the powder metallurgy cobalt-titanium alloy sputtering target to the second copper layer includes positioning the second copper layer adjacent to the first copper layer.

10. The method of claim 8, wherein the high bonding temperature is from about 600°C to about 1000°C, and wherein the low bonding temperature is from about 250°C to about 500°C.