Inductively emitting linear compositions, patterns and methods thereof for forming gate insulating films; hardened films for gate insulating films; semiconductor devices; organic electrochemical transistors; organic EL display devices; liquid crystal display devices; micro LED display devices; quantum dot light-emitting display devices; wearable devices; electronic skin devices; biosensors; and neuromorphic devices.
By using a gate insulating film formed with a specific composition, the problems of material stretching and pattern formation in flexible devices are solved, achieving a gate insulating film with low voltage drive and high capacitance, suppressing ionic liquid leakage, and improving the performance of the display device.
Patent Information
- Application Number
- CN202580029031.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-07-19
- Filing Date
- 2025-07-18
- Publication Date
- 2026-11-17
AI Technical Summary
In the prior art, the gate insulating film material used in flexible devices lacks elasticity, leading to breakage. At the same time, low molecular weight ionic liquids are prone to seeping out in photosensitive compositions or becoming cloudy during development, making it difficult to form high-capacitance patterns.
A grid insulating film with elasticity and high capacitance is formed by using a grid-linked composition comprising a polymer with a specific structure, a radiosensitive linear compound, and a low glass transition temperature polymerized ionic liquid, and by patterning through coating, radiation irradiation, and development.
A low-voltage driven, stretchable gate insulating film with excellent patterning and capacitance was achieved, and ionic liquid leakage was effectively suppressed, improving the quality of semiconductor devices and display devices.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_4
Abstract
Description
Technical Field
[0001] This invention relates to a radioactive linear composition for forming a gate insulating film, a pattern thereof and a method for manufacturing the same, a hardened film for a gate insulating film, a semiconductor element, an organic electrochemical transistor, an organic EL display device, a liquid crystal display device, a micro LED display device, a quantum dot light-emitting display device, a wearable device, an electronic skin device, a biosensor, and a neuromorphic device. Background Technology
[0002] Thin-film transistors (TFTs) and other field-effect transistors are widely used as unit electronic components in semiconductor memory integrated circuits, high-frequency signal amplification components, and liquid crystal driving components. In various display devices, such as liquid crystal displays (LCDs) and organic electroluminescent (EL) displays, they are mostly used as switching elements to apply driving voltages to the display elements, thereby driving the display device.
[0003] The thin-film transistor typically includes a semiconductor layer, a gate electrode, a source electrode, and a drain electrode. A voltage is applied from the gate electrode to the source and drain electrodes via a gate insulating film to control the current flowing through the semiconductor layer. Previously, silicon oxide (SiO2) or silicon nitride (SiN), as inorganic materials, were used in the formation of the gate insulating film.
[0004] In recent years, flexible devices such as flexible displays have been actively developed. To adapt to such flexible devices, transistors such as TFTs are required to be flexible, and naturally, the gate insulating film is also required to be flexible. However, the gate insulating film formed from the aforementioned inorganic materials sometimes lacks flexibility and breaks.
[0005] Regarding flexible transistors, organic thin-film transistors (OTFTs), whose structural components are made of organic materials, have attracted much attention and have been the subject of extensive research and development in recent years. Furthermore, ion gels are known as organic materials for forming the gate insulating film. These ion gels are formed by mixing an ionic liquid with a positive photoresist containing a cresol phenolic varnish with naphthoquinone diazide added as a photosensitizer (see, for example, Patent Document 1).
[0006] Existing technical documents
[0007] Patent documents
[0008] Patent Document 1: Japanese Patent Application Publication No. 2016-80998 Summary of the Invention
[0009] The problem that the invention aims to solve
[0010] In recent years, there has been a demand for developing transistors that are flexible and have low drive voltages, suitable for flexible devices. This also requires the gate insulating film used in such transistors to be flexible, and consequently, to have good patterning properties and high capacitance.
[0011] In addition, when a low molecular weight ionic liquid is added to the photosensitive composition, there is a possibility that the low molecular weight ionic liquid may seep out onto the surface of the hardened film or become cloudy during development, making it difficult to pattern.
[0012] Therefore, the object of the present invention is to provide a linearly oriented composition capable of forming a gate insulating film with stretchability and sufficient patterning ability and capacitance, thereby suppressing exudation; a pattern (hardened film) formed by the linearly oriented composition and a method for manufacturing the same; a hardened film for a gate insulating film; a semiconductor element including the hardened film; an organic electrochemical transistor; an organic EL display device; a liquid crystal display device; a light-emitting diode (LED) display device; a quantum dot light-emitting display device; a wearable device; an electronic skin device; a biosensor; and a neuromorphic device.
[0013] Methods for solving problems
[0014] Through repeated research efforts to solve this problem, the inventors discovered that the objective can be achieved by incorporating a polymer (A) with a specific structure, a radiosensitive linear compound (B), and a polymerized ionic liquid (C) with a glass transition temperature below 5°C into the radiosensitive linear composition, thus completing the present invention.
[0015] In one embodiment, the present invention relates to an inductively linearized composition for forming a gate insulating film, comprising:
[0016] At least one polymer (A) selected from the group consisting of polymers (A1) containing structural units (I) having acid groups, siloxane polymers (A2), and polyamic acids or polyamic esters (A3).
[0017] Radiosensitive linear compound (B), and
[0018] Polymerized ionic liquids with a glass transition temperature below 5°C (C).
[0019] In another embodiment of the present invention, therein lies a method for manufacturing a pattern and a pattern obtained by the method, the method comprising:
[0020] The process of forming the gate insulating film by coating a substrate with an inductively linearized composition;
[0021] The process of irradiating at least a portion of the coating with radiation; and
[0022] A process of developing the coating film irradiated with said radiation to form a pattern.
[0023] In another embodiment of the present invention, there is a hardened film for a gate insulating film formed using the aforementioned gate insulating film forming radiometric linear composition, a semiconductor element including the hardened film, an organic electrochemical transistor, an organic EL display device, a liquid crystal display device, a micro LED display device, a quantum dot light-emitting display device, a wearable device, an electronic skin device, a biosensor, and a neuromorphic device.
[0024] The effects of the invention
[0025] The inductively linear composition for forming a gate insulating film of the present invention enables the construction of a pattern (hardened film) with excellent patterning properties, superior capacitance, and suppressed leakage. Transistors having this pattern (hardened film) as a gate insulating film can be driven at low voltages and also exhibit stretchability. This is because the inductively linear composition for forming a gate insulating film contains a polymerized ionic liquid (C). If the pattern (hardened film) obtained from this composition is used as the gate insulating film, an electrical double layer can be formed, thereby reducing the driving voltage of the transistor. Furthermore, compared to gate insulating films containing inorganic materials, it exhibits superior stretchability. Additionally, the polymerized ionic liquid (C) has a large molecular weight, thus enabling the formation of a pattern (hardened film) with suppressed leakage.
[0026] In the pattern manufacturing method of the present invention, since the radiosensitive linear composition capable of forming patterns (hardened films) with excellent pattern-forming properties, capacitance, and exudation suppression is used, high-quality patterns (hardened films) can be formed efficiently. The patterns (hardened films) of the present invention exhibit excellent pattern-forming properties, capacitance, and exudation suppression due to the use of the radiosensitive linear composition.
[0027] The semiconductor elements, organic electrochemical transistors, organic EL display devices, liquid crystal display devices, micro LED display devices, quantum dot light-emitting display devices, wearable devices, electronic skin devices, biosensors, and neuromorphic devices of the present invention are of high quality due to the inclusion of patterns (hardened films) with excellent patterning properties, capacitance, and chemical resistance. Detailed Implementation
[0028] The embodiments of the present invention will be described in detail below, but the present invention is not limited to these embodiments.
[0029] The following provides a detailed description of matters related to the implementation method. Furthermore, in this specification, the numerical range indicated by “~” means the values before and after the “~” are considered as lower and upper limits. A “structural unit” refers to a unit that primarily constitutes the main chain structure, and is one of at least two units contained within the main chain structure.
[0030] In this specification, "hydrocarbon group" encompasses chain-like hydrocarbon groups, alicyclic hydrocarbon groups, and aromatic hydrocarbon groups. "Chain-like hydrocarbon group" refers to a straight-chain hydrocarbon group or branched hydrocarbon group that contains only a chain structure in its main chain and no cyclic structure. It can be saturated or unsaturated. "Alicyclic hydrocarbon group" refers to a hydrocarbon group that contains only an alicyclic hydrocarbon structure as its ring structure and does not contain an aromatic ring structure. It is not necessary to contain only an alicyclic hydrocarbon structure; it may also include those with a chain structure in a portion of their structure. "Aromatic hydrocarbon group" refers to a hydrocarbon group that contains an aromatic ring structure as its ring structure. It is not necessary to contain only an aromatic ring structure; it may also contain a chain structure or an alicyclic hydrocarbon structure in a portion of its structure. Furthermore, the ring structure of alicyclic hydrocarbon groups and aromatic hydrocarbon groups may also have substituents containing hydrocarbon structures. "Cyclic hydrocarbon group" encompasses both alicyclic hydrocarbon groups and aromatic hydrocarbon groups.
[0031] In this specification, "(meth)acryloyl" means including both "acryloyl" and "methacryloyl", "(meth)acrylate" means including both "acrylate" and "methacrylate", and "(meth)acrylate" means including both "acrylate" and "methacrylate".
[0032] Radioactive linear compositions
[0033] The radiosensitive linear composition of this embodiment (hereinafter also simply referred to as the "composition") contains at least one polymer (A) selected from the group consisting of a polymer (A1) comprising a structural unit (I) having an acid group, a siloxane polymer (A2), and a polyamic acid or polyamic ester (A3).
[0034] The radioactive linear composition of the present invention is suitable for use in the formation of gate insulating films because it can form patterns (hardened films) with good patterning properties, excellent capacitance and suppressed leakage.
[0035] <Polymer (A)>
[0036] The polymer (A) is selected from at least one of the group consisting of polymers (A1) containing structural units (I) having acid groups, siloxane polymers (A2), and polyamic acids or polyamic esters (A3).
[0037] (Polymer (A1))
[0038] The polymer (A1) is an aggregate of polymers containing structural units (I) having acid groups (hereinafter, the aggregate is also referred to as the "base polymer"). The structural unit (I) need only be contained in at least one polymer constituting the base polymer. The polymer (A1) may also contain structural units other than structural units (I). The structural units contained in the polymer (A1) will be described below.
[0039] [Structural Unit (I)]
[0040] The polymer (A1) can improve its solubility (alkali solubility) in alkaline developing solutions or enhance its curing reactivity by having structural units (I) with acid groups. Furthermore, in this specification, "alkali solubility" means that it can dissolve or swell in alkaline aqueous solutions such as a 2.38% by mass solution of tetramethylammonium hydroxide.
[0041] The structural unit (I) is not particularly limited as long as it has an acid group, but is preferably selected from at least one of the group consisting of structural units having a carboxyl group, structural units having a sulfonic acid group, structural units having a phenolic hydroxyl group, and maleimide units. In addition, in this specification, the term "phenolic hydroxyl group" refers to a hydroxyl group that is directly bonded to an aromatic ring (e.g., a benzene ring, a naphthalene ring, an anthracene ring, etc.).
[0042] Structural unit (I) is preferably derived from an unsaturated monomer having an acid group. Specific examples of unsaturated monomers having acid groups are provided below.
[0043] As monosaccharides that constitute structural units with carboxyl groups, examples include unsaturated monocarboxylic acids such as (meth)acrylic acid, crotonic acid, and 4-vinylbenzoic acid; and unsaturated dicarboxylic acids such as maleic acid, fumaric acid, citraconic acid, medoconic acid, and itaconic acid.
[0044] Examples of monosemblables that constitute structural units having sulfonic acid groups include vinyl sulfonic acid, (meth)allyl sulfonic acid, styrene sulfonic acid, and (meth)acryloyloxyethyl sulfonic acid.
[0045] Examples of monomorphs that constitute structural units with phenolic hydroxyl groups include 4-hydroxystyrene, o-isopropenylphenol, m-isopropenylphenol, p-isopropenylphenol, and hydroxyphenyl methacrylate.
[0046] In addition, maleimide can also be used as a monolith that constitutes structural unit (I).
[0047] Among these, unsaturated monocarboxylic acids and maleimides are preferred, and (meth)acrylic acid and maleimides are more preferred.
[0048] The basic polymer may contain one structural unit (I) or a combination of two or more structural units (I).
[0049] The lower limit of the content ratio (total content ratio in the case of multiple structural units) of structural unit (I) relative to all structural units constituting the base polymer is preferably 1% by mass, more preferably 2% by mass, and even more preferably 5% by mass. Furthermore, the upper limit of the content ratio is preferably 40% by mass, more preferably 35% by mass, even more preferably 30% by mass, and particularly preferably 20% by mass. By setting the content ratio of structural unit (I) within the aforementioned range, good solubility in alkaline developing solutions is imparted, and therefore preferred.
[0050] [Structural Unit (II)]
[0051] The polymer (A1) may contain structural units (II) having one or more groups selected from the group consisting of oxetyl and oxetylpropyl. The inclusion of structural units (II) in the polymer (A1) further improves the resolution or adhesion of the film, and is therefore preferred. Furthermore, by utilizing the epoxy group as a crosslinking group, a pattern (hardened film) with high heat resistance and long-term degradation suppression can be formed. Structural units (II) are preferably derived from unsaturated monomers having epoxy groups, and more specifically, are preferably structural units represented by the following formula (a1).
[0052] [Chemistry 1]
[0053]
[0054] (In formula (a1),
[0055] R 21 It is a monovalent group having an oxetine propyl or oxetine butyl group;
[0056] R α It can be a hydrogen atom, methyl, hydroxymethyl, cyano, or trifluoromethyl;
[0057] X 1 (For single-bond or divalent linkages)
[0058] In the above equation (a1), R is... 21 Examples include: oxetyl propyl, oxetyl butyl, 3,4-epoxycyclohexyl, 3,4-epoxytricyclic [5.2.1.0] 2,6 Decyl, 3-methyloxetyl, 3-ethyloxetyl, etc.
[0059] As X 1 The divalent linker is preferably a alkyl dimethyl group, such as methylene, ethylene, or 1,3-propanediyl.
[0060] Specific examples of monoliths providing structural unit (II) represented by formula (a1) include: glycidyl (meth)acrylate, 3,4-epoxycyclohexyl (meth)acrylate, methyl (meth)acrylate, 2-(3,4-epoxycyclohexyl)ethyl (meth)acrylate, and 3,4-epoxytricyclo(meth)acrylate [5.2.1.0]. 2,6 [Methyl methyl methacrylate, 3-methyloxetane-3-yl methacrylate, 3-ethyloxetane-3-yl methacrylate, methyl methacrylate, 3-ethyloxetane-3-yl methacrylate, etc. Among these, glycidyl methacrylate, 3,4-epoxycyclohexyl methacrylate, and 3-ethyloxetane-3-yl methacrylate are preferred.]
[0061] The base polymer may contain one structural unit (II) or a combination of two or more structural units (II).
[0062] When the polymer (A1) contains structural unit (II), the lower limit of the content ratio (total content ratio in the case of multiple structural units) of structural unit (II) relative to all structural units constituting the base polymer is preferably 5% by mass, more preferably 15% by mass, and even more preferably 25% by mass. Furthermore, the upper limit of the content ratio is preferably 90% by mass, more preferably 85% by mass, and even more preferably 80% by mass. By setting the content ratio of structural unit (II) within the aforementioned range, the coating film exhibits better resolution, and the heat resistance of the obtained pattern (hardened film) can be sufficiently improved, which is preferable in this respect.
[0063] [Structural Unit (III)]
[0064] In the case that the radiosensitive linear composition of the present invention is a chemically amplified composition (hereinafter referred to as the "third composition"), from the viewpoint that a coating with excellent development adhesion can be formed, it is preferable that the polymer (A1) further comprises a structural unit (III) having one or more groups selected from the group consisting of groups represented by the following formula (a2) and acid-dissociable groups.
[0065] [Chemistry 2]
[0066]
[0067] (in formula (a2),
[0068] R 1 R 2 and R 3Each of the following is independently a hydrogen atom, a halogen atom, a hydroxyl group, an alkoxy group having 1 to 6 carbon atoms, or an alkyl or phenyl group having 1 to 10 carbon atoms; wherein, R 1 R 2 and R 3 At least one of them is an alkoxy group having 1 to 6 carbon atoms;
[0069] “ "Indicates a bond"
[0070] As R 1 ~R 3 Alkoxy groups with 1 to 6 carbon atoms include: methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, tert-butoxy, etc. Among these, R... 1 ~R 3 The alkoxy group is preferably methoxy or ethoxy.
[0071] R 1 ~R 3 The alkyl group having 1 to 10 carbon atoms can be either straight-chain or branched. Examples of alkyl groups having 1 to 10 carbon atoms include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, etc. Among these, methyl, ethyl, or propyl is preferred.
[0072] From the perspective of obtaining a heat-resistant hardened film by forming a cross-linked structure and improving the storage stability of the radiosensitive linear composition, R is preferred. 1 ~R 3 At least one of them is an alkoxy group having 1 to 6 carbon atoms, more preferably two or more are alkoxy groups, and particularly preferably all of them are alkoxy groups.
[0073] In the above, R 1 Preferably, it is an alkoxy group having 1 to 6 carbon atoms, more preferably an alkoxy group having 1 to 3 carbon atoms, and even more preferably a methoxy or ethoxy group. 2 and R 3 Preferably, it is a hydroxyl group, an alkoxy group with 1 to 6 carbon atoms, an alkyl group with 1 to 10 carbon atoms, or a phenyl group; more preferably, it is a hydroxyl group, an alkoxy group with 1 to 3 carbon atoms, or an alkyl group with 1 to 3 carbon atoms.
[0074] In structural unit (III), the group represented by formula (a2) is preferably bonded to an aromatic ring group or a chain hydrocarbon group. Furthermore, in this specification, "aromatic ring group" refers to a group formed by removing n (n is an integer) hydrogen atoms from the ring portion of an aromatic ring. Examples of such aromatic rings include benzene rings, naphthalene rings, and anthracene rings. The ring may have substituents such as alkyl groups. Examples of chain hydrocarbon groups bonded to the group represented by formula (a2) include alkyldiyl groups and alkenediyl groups.
[0075] In this embodiment, the group represented by formula (a2) is preferably bonded to a benzene ring, a naphthalene ring, or an alkyl chain. That is, structural unit (III) preferably has at least one group selected from the group represented by formula (i), formula (ii), and formula (iii).
[0076] [Chemistry 3]
[0077]
[0078] (In equations (i), (ii) and (iii),
[0079] A 1 and A 2 Each is independently a halogen atom, a hydroxyl group, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms;
[0080] n1 is an integer from 0 to 4;
[0081] n2 is an integer from 0 to 6; where n1 is 2 or more, multiple A's 1 They are either identical or different bases; when n² is greater than 2, multiple A's are... 2 The bases are either identical or different.
[0082] R 31 It is an alkyl diol;
[0083] R 1 R 2 and R 3 It has the same meaning as the above formula (a2);
[0084] “ "Indicates a bond"
[0085] As A 1 and A 2 The alkoxy group having 1 to 6 carbon atoms can be suitably represented by R of formula (a2). 1 ~R 3 Examples include alkoxy groups having 1 to 6 carbon atoms. Additionally, as A... 1 and A 2 Alkyl groups having 1 to 6 carbon atoms may suitably employ R of formula (a2). 1 ~R 3 The alkyl group having 1 to 10 carbon atoms that corresponds to the group having 1 to 6 carbon atoms.
[0086] The group "-SiR" bonded to the aromatic ring 1 R 2 R 3 The position of " relative to A" 1 and A 2Other bases can be in any position. For example, in the case of equation (i), the base "-SiR" 1 R 2 R 3 The position of “” can be any of the adjacent, intermediate, or opposite positions, with the opposite position being preferred.
[0087] n1 is preferably 0 or 1, more preferably 0. n2 is preferably 0 to 2, more preferably 0.
[0088] In equation (iii), R 31 Preferably, it is linear. From the viewpoint of improving the heat resistance of the obtained hardened film, R 31 Preferably, it has 1 to 6 carbon atoms, more preferably 1 to 4 carbon atoms.
[0089] In equations (i) to (iii), the structural unit (III) is preferably at least one of the groups selected from the bases represented by equation (i) and the bases represented by equation (ii). Additionally, in the base "-SiR..." 1 R 2 R 3 "When directly bonded to an aromatic ring, the silanol group generated in the presence of water can be stabilized. This improves the solubility of the exposure section in alkaline developer and allows for the formation of good patterns, which is preferable in this respect. Among these, structural unit (III) is particularly preferred to be a structural unit having the base represented by formula (i)."
[0090] The structural unit (III) is preferably a structural unit derived from a monolith having polymeric carbon-carbon unsaturated bonds (hereinafter also referred to as "unsaturated monolith"), and more specifically, preferably at least one selected from the group consisting of the structural unit represented by the following formula (2a-1) and the structural unit represented by the following formula (2a-2).
[0091] [Chemistry 4]
[0092]
[0093] (In equations (2a-1) and (2a-2),
[0094] R α1 It can be a hydrogen atom, methyl, hydroxymethyl, cyano, or trifluoromethyl;
[0095] R 32 and R 33 Each is independently a divalent aromatic cyclic group or a chain hydrocarbon group;
[0096] R 1 R 2 and R 3 (This has the same meaning as the above formula (a2))
[0097] In equations (2a-1) and (2a-2), R 32 R 33 The divalent aromatic cyclic group is preferably a substituted or unsubstituted phenylene or a substituted or unsubstituted naphthylene. The divalent chain hydrocarbon group is preferably an alkyldiyl group having 1 to 6 carbon atoms, more preferably an alkyldiyl group having 1 to 4 carbon atoms.
[0098] Regarding the aspects of obtaining patterns (hardened films) with higher heat resistance and hardness, and improving the solubility of the exposure section in alkaline developing solutions, R... 32 R 33 Preferably, it is a divalent aromatic cyclic group, and particularly preferably a substituted or unsubstituted phenylene group.
[0099] As specific examples of the structural unit represented by equation (2a-1), structural units represented by equations (2a-1-1) and (2a-1-2) can be listed below. Furthermore, as specific examples of the structural unit represented by equation (2a-2), structural units represented by equations (2a-2-1) and (2a-2-2) can be listed below.
[0100] [Chemistry 5]
[0101]
[0102] (In equations (2a-1-1), (2a-1-2), (2a-2-1), and (2a-2-2),)
[0103] R 34 and R 35 Each is independently an alkyl group having 1 to 4 carbon atoms;
[0104] R 36 It is an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, or a hydroxyl group;
[0105] n3 is an integer from 1 to 4;
[0106] A 1 A 2 n1 and n2 have the same meaning as equations (i) and (ii);
[0107] R α1 (This has the same meaning as equations (2a-1) and (2a-2) mentioned above)
[0108] Specific examples of monomorphs constituting structural unit (III) include: styryltrimethoxysilane, styryltriethoxysilane, styrylmethyldimethoxysilane, styrylethyldiethoxysilane, styryldimethoxyhydroxysilane, styryldiethoxyhydroxysilane, (meth)acrylate oxyphenyltrimethoxysilane, (meth)acrylate oxyphenyltriethoxysilane, (meth)acrylate oxyphenylmethoxydimethoxysilane, (meth)acrylate oxyphenylethyldiethoxysilane, etc.; trimethoxy (4 -vinylnaphthyl)silane, triethoxy(4-vinylnaphthyl)silane, methyldimethoxy(4-vinylnaphthyl)silane, ethyldiethoxy(4-vinylnaphthyl)silane, (meth)acrylateoxynaphthyltrimethoxysilane, etc.; 3-(meth)acrylateoxypropyltrimethoxysilane, 3-(meth)acrylateoxypropyltriethoxysilane, 3-(meth)acrylateoxypropylmethyldimethoxysilane, 3-(meth)acrylateoxypropylmethyldiethoxysilane, 4-(meth)acrylateoxybutyltrimethoxysilane, etc.
[0109] The term "acid-dissociable group" refers to a group that substitutes for hydrogen atoms in acidic functional groups such as phenolic hydroxyl groups, carboxyl groups, and sulfonic acid groups, and specifically to a group that dissociates under the action of an acid. For example, the acid generated from a photoacid generator during exposure causes the acid-dissociable group to dissociate and generate a carboxyl group, etc. This creates a difference in the solubility of the developer between the exposed and unexposed areas of the coating, enabling pattern formation.
[0110] The acid dissociative group is preferably a group represented by formula (3a-1) or a group represented by formula (3a-2).
[0111] [Chemistry 6]
[0112]
[0113] (In formula (3a-1),
[0114] R 4 and R 5 Each group is independently composed of a hydrogen atom, a hydrocarbon group having 1 to 30 carbon atoms, or a group formed by substituting at least a portion of the hydrogen atoms in the hydrocarbon group with a hydroxyl group, a halogen atom, or a cyano group; wherein, R is absent. 4 and R 5 The case where both are hydrogen atoms;
[0115] R 6 It is a hydrocarbon group having 1 to 30 carbon atoms, a group having an oxygen atom or a sulfur atom at the carbon-carbon inter-carbon or bond side end of the hydrocarbon group, or a group having at least a portion of the hydrogen atoms of these groups substituted by a hydroxyl group, a halogen atom or a cyano group.
[0116] R 7 It consists of carbon atoms or silicon atoms;
[0117] In equation (3a-2),
[0118] R 8 ~R 14 Each is an independent hydrogen atom or a hydrocarbon group having 1 to 12 carbon atoms;
[0119] m is 1 or 2; when m is 2, multiple R 11 and R 12 They can be the same or different;
[0120] In equations (3a-1) and (3a-2), " (This indicates the bonding location)
[0121] As R 4 ~R 6 Hydrocarbon groups with 1 to 30 carbon atoms can be listed as follows: chain hydrocarbon groups with 1 to 30 carbon atoms, alicyclic hydrocarbon groups with 3 to 30 carbon atoms, and aromatic hydrocarbon groups with 6 to 30 carbon atoms.
[0122] Examples of chain-like hydrocarbon groups having 1 to 30 carbon atoms include straight-chain or branched saturated hydrocarbon groups having 1 to 30 carbon atoms, and straight-chain or branched unsaturated hydrocarbon groups having 2 to 20 carbon atoms. Examples of straight-chain or branched saturated hydrocarbon groups having 1 to 30 carbon atoms include alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, 2-methylpropyl, 1-methylpropyl, tert-butyl, n-pentyl, isopentyl, neopentyl, n-hexyl, 2-hexyl, 3-hexyl, n-octyl, n-dodecyl, n-tetradecyl, and n-octadecyl. Examples of monovalent straight-chain or branched unsaturated hydrocarbon groups having 2 to 20 carbon atoms include alkenyl groups such as vinyl, propynyl, and butenyl; and alkynyl groups such as ethynyl, propynyl, and butynyl.
[0123] Examples of alicyclic hydrocarbon groups with 3 to 30 carbon atoms include monocyclic or polycyclic saturated hydrocarbon groups and monocyclic or polycyclic unsaturated hydrocarbon groups. Examples of monocyclic saturated hydrocarbon groups include cyclopropyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, and other cycloalkyl groups. Examples of polycyclic saturated hydrocarbon groups include borneol, norborneol, adamantyl, tricyclic decyl, tetracyclic dodecyl, and other bridged alicyclic hydrocarbon groups. Examples of monocyclic unsaturated hydrocarbon groups include cyclopropenyl, cyclobutenyl, cyclopentenyl, cyclohexenyl, and other monocyclic cycloalkenyl groups. Examples of polycyclic unsaturated hydrocarbon groups include norbornel, tricyclic decenyl, tetracyclic dodecenyl, and other polycyclic cycloalkenyl groups. Furthermore, a bridged alicyclic hydrocarbon group refers to a polycyclic alicyclic hydrocarbon group in which two non-adjacent carbon atoms constituting the alicyclic ring are bonded together by a linker containing one or more carbon atoms.
[0124] The aromatic hydrocarbon group having 6 to 30 carbon atoms can be a structure formed by a single ring, a condensed ring, or a structure formed by an aromatic ring and an aliphatic hydrocarbon group. Examples of aromatic hydrocarbon groups include aryl groups such as phenyl, tolyl, xylyl, naphthyl, and anthracene; and aralkyl groups such as benzyl, phenethyl, and naphthylmethyl.
[0125] R as in equation (3-1) 4 ~R 6 Each of the alkyl groups is preferably an alkyl group having 1 to 30 carbon atoms, more preferably an alkyl group having 1 to 20 carbon atoms, and even more preferably an alkyl group having 1 to 10 carbon atoms, and particularly preferably an alkyl group having 1 to 5 carbon atoms.
[0126] As R 8 ~R 14 Hydrocarbon groups with 1 to 12 carbon atoms can be appropriately used with the aforementioned R. 4 ~R 6 The groups in hydrocarbon groups with 1 to 30 carbon atoms that correspond to the groups with 1 to 12 carbon atoms.
[0127] m is 1 or 2. When m is 2, multiple R... 11 and R 12 They can be the same or different.
[0128] As a structural unit having the acid dissociative group, the structural unit represented by the following formulas (3a-1-1) and (3a-1-2) is preferred, for example.
[0129] [Chemistry 7]
[0130]
[0131] In equations (3a-1-1) and (3a-1-2), m1 is either 0 or 1. R α1 R in equations (2a-1) and (2a-2) α1 They have the same meaning. R 4 ~R 14 R in equations (3a-1) and (3a-2) 4 ~R 14 They have the same meaning.
[0132] L in equations (3a-1-1) and (3a-1-2) 1 L 2 They are independent single-bond and divalent linkage groups, respectively.
[0133] As the L 1 L 2 Divalent linkages in alkyl groups can be listed as: alkyldiyl, cycloalkyldiyl, alkenyl, and aryldiyl.
[0134] As the alkyl diene, examples include X in formula (a1). 1 The same as the divalent linkage base.
[0135] Examples of cycloalkyl dimethyl groups include monocyclic cycloalkyl dimethyl groups such as cyclopentanediyl and cyclohexanediyl, and polycyclic cycloalkyl dimethyl groups such as norbornenediyl and adamantanediyl.
[0136] Examples of the alkenyl groups include: ethylenediyl, propylenediyl, butenediyl, etc.
[0137] Examples of the aryl dimethyl group include phenylene, methylphenylene, and naphthylene. Preferably, the aryl dimethyl group has 6 to 15 carbon atoms.
[0138] The base polymer may contain one structural unit (III) or a combination of two or more structural units (III).
[0139] When the polymer (A1) contains structural unit (III), the lower limit of the content ratio of structural unit (III) (or the total content ratio in the case of multiple structural units) relative to all structural units constituting the base polymer is preferably 5% by mass, more preferably 10% by mass, and even more preferably 15% by mass. Furthermore, the upper limit of the content ratio is preferably 50% by mass, more preferably 40% by mass, and even more preferably 30% by mass. By setting the content ratio of structural unit (III) within the aforementioned range, the coating film exhibits better resolution, which is preferable in this respect.
[0140] [Structural Unit (IV)]
[0141] The polymer (A) may further comprise structural units (IV), namely structural units (IV) derived from at least one monotony of a group consisting of alkyl (meth)acrylates, (meth)acrylates having an alicyclic structure, (meth)acrylates having an aromatic ring structure, aromatic vinyl compounds, N-substituted maleimide compounds, vinyl compounds having a heterocyclic structure, conjugated diene compounds, nitrogen-containing vinyl compounds, and dialkyl dicarboxylic acid ester compounds. Introducing these structural units (IV) into the polymer allows for adjustment of the glass transition temperature of the polymer (A1) composition and improves the pattern shape of the obtained cured film, which is preferred in this respect.
[0142] Examples of alkyl methacrylates include: methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, butyl methacrylate, 2-ethylhexyl methacrylate, lauryl methacrylate, and stearyl methacrylate.
[0143] Examples of (meth)acrylates having an alicyclic structure include: cyclohexyl (meth)acrylate, 2-methylcyclohexyl (meth)acrylate, and tricyclohexyl (meth)acrylate [5.2.1.0]. 2,6 ] Decane-8-yl ester, (meth)acrylate tricyclic [5.2.1.0] 2,5 Decane-8-yloxyethyl ester, isobornyl acrylate, etc.
[0144] Examples of (meth)acrylates having an aromatic ring structure include phenyl (meth)acrylate and benzyl (meth)acrylate.
[0145] Examples of such aromatic vinyl compounds include: styrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, α-methylstyrene, 2,4-dimethylstyrene, 2,4-diisopropylstyrene, 5-tert-butyl-2-methylstyrene, divinylbenzene, trivinylbenzene, tert-butoxystyrene, vinylbenzyldimethylamine, (4-vinylbenzyl)dimethylaminoethyl ether, N,N-dimethylaminoethylstyrene, N,N-dimethylaminomethylstyrene, 2-ethylstyrene, 3-ethylstyrene, 4-ethylstyrene, 2-tert-butylstyrene, 3-tert-butylstyrene, 4-tert-butylstyrene, diphenylethylene, vinylnaphthalene, vinylpyridine, etc.
[0146] Examples of the N-substituted maleimide compounds include: N-cyclohexylmaleimide, N-cyclopentylmaleimide, N-(2-methylcyclohexyl)maleimide, N-(4-methylcyclohexyl)maleimide, N-(4-ethylcyclohexyl)maleimide, N-(2,6-dimethylcyclohexyl)maleimide, N-norbornylmaleimide, N-tricyclodecylmaleimide, N-adamantylmaleimide, N-phenylmaleimide, N-(2-methylphenyl)maleimide, N-(4-methylphenyl)maleimide, N-(4-ethylphenyl)maleimide, N-(2,6-dimethylphenyl)maleimide, N-benzylmaleimide, N-naphthylmaleimide, etc.
[0147] Examples of vinyl compounds having heterocyclic structures include: tetrahydrofurfuryl (meth)acrylate, tetrahydropyran acrylate, 5-ethyl-1,3-dioxane-5-yl methyl acrylate, 5-methyl-1,3-dioxane-5-yl methyl acrylate, (2-methyl-2-ethyl-1,3-dioxane-4-yl)methyl acrylate, 2-(meth)acrylateoxymethyl-1,4,6-trioxaspiro[4,6]undecane, (γ-butyrolactone-2-yl) acrylate, (meth)acrylate glyceryl carbonate, (γ-lactam-2-yl) acrylate, N-(meth)acrylateoxyethylhexahydrophthalimide, etc.
[0148] Examples of conjugated diene compounds include 1,3-butadiene and isoprene; examples of nitrogen-containing vinyl compounds include (meth)acrylonitrile and (meth)acrylamide; and examples of unsaturated dialkyl dicarboxylic acid esters include diethyl itaconic acid. In addition, examples of monomers constituting other structural units include vinyl chloride, vinylidene chloride, and vinyl acetate.
[0149] As a monolithic entity providing the structural unit (IV), it is preferably composed of at least one selected from the group consisting of alkyl (meth)acrylates, aromatic vinyl compounds and N-substituted maleimide compounds, more preferably at least one selected from the group consisting of methyl (meth)acrylates and styrene.
[0150] The base polymer may contain one structural unit (IV) or a combination of two or more structural units (IV).
[0151] When the polymer (A1) contains structural units (IV), the lower limit of the content ratio of structural units (IV) (or the total content ratio when multiple structural units are included) relative to all structural units constituting the base polymer is preferably 1% by mass, more preferably 3% by mass, and even more preferably 5% by mass. Furthermore, the upper limit of the content ratio is preferably 60% by mass, more preferably 50% by mass. By setting the content ratio of structural units (IV) within the aforementioned range, the glass transition temperature of the polymer (A1) can be appropriately increased, which is preferable in this respect.
[0152] (Synthesis method of polymer (A1))
[0153] The polymer (A1) can be manufactured, for example, using an unsaturated monomer capable of incorporating the structural units, in a suitable solvent, in the presence of a polymerization initiator, by known methods such as free radical polymerization.
[0154] Examples of azo compounds that can be used as polymerization initiators include 2,2'-azobis(isobutyronitrile), 2,2'-azobis(2,4-dimethylpentanonitrile), and dimethyl 2,2'-azobis(isobutyric acid) ester. The preferred proportion of the polymerization initiator used is 0.01 to 30 parts by mass relative to 100 parts by mass of the total monomer used in the reaction.
[0155] Examples of polymerization solvents include alcohols, ethers, ketones, esters, and hydrocarbons. The amount of polymerization solvent used is preferably set to be 0.1% to 60% by mass of the total amount of the monomers used in the reaction relative to the total amount of the reaction solution.
[0156] In polymerization, the reaction temperature is typically 30°C to 180°C. The reaction time varies depending on the type of polymerization initiator and monomer, or the reaction temperature, and is typically 0.5 hours to 10 hours. The polymer obtained through polymerization can be used directly in the reaction solution for the preparation of radiosensitive linear compositions, or it can be used after separation from the reaction solution. Polymer separation can be carried out using known methods such as injecting the reaction solution into a large volume of undesirable solvent and drying the resulting precipitate under reduced pressure, or removing the precipitate by vacuum distillation using an evaporator.
[0157] The weight-average molecular weight (Mw) of the polymer contained in the polymer component, converted from polystyrene by gel permeation chromatography (GPC), is preferably 2,000 or more. If Mw is 2,000 or more, a hardened film with sufficiently high heat resistance or chemical resistance and good developability can be obtained, which is preferable in this respect. The Mw of the polymer is more preferably 5,000 or more, even more preferably 6,000 or more, and particularly preferably 7,000 or more. Furthermore, from the viewpoint of achieving good film-forming properties, Mw is preferably 50,000 or less, more preferably 30,000 or less, even more preferably 20,000 or less, and particularly preferably 15,000 or less.
[0158] Furthermore, the molecular weight distribution (Mw / Mn) represented by the ratio of weight average molecular weight Mw to number average molecular weight Mn is preferably 4.0 or less, more preferably 3.0 or less, and even more preferably 2.5 or less. In addition, when the base polymer comprises two or more polymers, it is preferable that the Mw and Mw / Mn of each polymer respectively satisfy the aforementioned range.
[0159] (Siloxane polymer (A2))
[0160] The siloxane polymer (A2) is not particularly limited as long as it can form a hardened film through hydrolysis and condensation. The siloxane polymer (A2) is preferably a polymer obtained by hydrolyzing a hydrolytic silane compound represented by the following formula (4a).
[0161] (R 51 ) r Si(OR 52 ) 4-r (4a)
[0162] (In formula (4a),
[0163] R 51 It is a non-hydrolyzable monovalent group;
[0164] R 52 It is an alkyl group having 1 to 4 carbon atoms, an aromatic group having 6 to 12 carbon atoms, or an arylalkyl group having 7 to 20 carbon atoms;
[0165] r is an integer from 0 to 3; where, when r is 2 or 3, the multiple R values in the formula are... 51 They may be identical or different; when r is 0 to 2, the multiple R in the formula 52 (Same or different)
[0166] As R 51 Examples include: alkyl groups with 1 to 20 carbon atoms, alkenyl groups with 2 to 20 carbon atoms, aryl groups with 6 to 20 carbon atoms, aralkyl groups with 7 to 20 carbon atoms, groups having (meth)acryloyl groups, and groups having epoxy groups.
[0167] As R 52 Examples include: methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, etc. Among these, R... 52 Methyl or ethyl is preferred.
[0168] r is preferably 0 to 2, more preferably 0 or 1, and even more preferably 1.
[0169] Specific examples of the monomers constituting siloxane polymers,
[0170] Examples of silane compounds having four hydrolyzable groups include tetramethoxysilane, tetraethoxysilane, triethoxymethoxysilane, tetrabutoxysilane, tetraphenoxysilane, tetrabenzoxysilane, and tetran-propoxysilane.
[0171] Examples of silane compounds having three hydrolyzable groups include methyltrimethoxysilane, methyltriethoxysilane, methyltriisopropoxysilane, methyltributoxysilane, phenyltrimethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, ethyltriisopropoxysilane, ethyltributoxysilane, butyltrimethoxysilane, 3-glycidyloxypropyltrimethoxysilane, 3-glycidyloxypropyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-(meth)acrylateoxypropyltrimethoxysilane, and 3-(meth)acrylateoxypropyltriethoxysilane.
[0172] Examples of silane compounds having two hydrolyzable groups include dimethyldimethoxysilane and diphenyldimethoxysilane.
[0173] Examples of silane compounds having a hydrolyzable group include trimethylmethoxysilane and trimethylethoxysilane.
[0174] Siloxane polymers can be obtained by hydrolyzing or condensing one or more hydrolyzable silane compounds with water, preferably in the presence of a suitable catalyst and an organic solvent. During the hydrolysis or condensation reaction, the hydrolytic group (-OR) of the hydrolyzable silane compound is... 52 The total amount of water used is 1 mole, and the preferred proportion of water is 0.1 mole to 3 moles, more preferably 0.2 moles to 2 moles, and even more preferably 0.5 moles to 1.5 moles. By using this amount of water, the reaction rate of hydrolysis and condensation can be optimized.
[0175] Catalysts used in hydrolysis and condensation reactions include, for example, acids, alkali metal compounds, organic bases, titanium compounds, zirconium compounds, etc. The amount of catalyst used varies depending on the type of catalyst, reaction conditions such as temperature, etc., and can be set appropriately. It is preferably 0.0001 mol to 0.2 mol relative to 1 mol of hydrolyzable silane compound, and more preferably 0.0005 mol to 0.1 mol.
[0176] Examples of organic solvents used in the hydrolysis and condensation reactions include hydrocarbons, ketones, esters, ethers, and alcohols. Among these, non-water-soluble or poorly water-soluble organic solvents are preferred, such as ethylene glycol monoalkyl ether acetates, diethylene glycol dialkyl ethers, propylene glycol monoalkyl ethers, propylene glycol monoalkyl ether acetates, and propionate esters. The proportion of organic solvent used is preferably 10 to 10,000 parts by mass relative to a total of 100 parts by mass of the hydrolyzable silane compound used in the reaction, more preferably 50 to 1,000 parts by mass.
[0177] During the hydrolysis and condensation reactions, it is preferable to set the reaction temperature to below 130°C, more preferably to 40°C to 100°C. The reaction time is preferably 0.5 hours to 24 hours, more preferably 1 hour to 12 hours. During the reaction, the mixture can be stirred or placed under reflux. Alternatively, after the hydrolysis and condensation reactions, a dehydrating agent can be added to the reaction solution, followed by evaporation, thereby removing water and the generated alcohol from the reaction system.
[0178] For siloxane polymers, the weight-average molecular weight (Mw) of the polystyrene obtained by GPC is preferably 500 or more. If Mw is 500 or more, a pattern (hardened film) exhibiting sufficiently high heat resistance or solvent resistance and good developability can be obtained, which is preferable in this respect. Mw is more preferably 1000 or more. Furthermore, from the viewpoint of good film-forming properties and suppression of reduced radioactive linearity, Mw is preferably 10000 or less, more preferably 5000 or less. Additionally, the molecular weight distribution (Mw / Mn) is preferably 4.0 or less, more preferably 3.0 or less, and even more preferably 2.5 or less.
[0179] (Polyamic acid or polyamic acid ester (A3))
[0180] The polyamic acid can be obtained, for example, by reacting a tetracarboxylic dianhydride with a diamine.
[0181] Examples of tetracarboxylic dianhydrides include, for example, aliphatic tetracarboxylic dianhydrides, alicyclic tetracarboxylic dianhydrides, and aromatic tetracarboxylic dianhydrides. Specific examples of these include...
[0182] Examples of aliphatic tetracarboxylic dianhydrides include 1,2,3,4-butanetetracarboxylic dianhydrides.
[0183] Examples of alicyclic tetracarboxylic dianhydrides include 1,2,3,4-cyclobutanetetracarboxylic dianhydride, 1,3-dimethyl-1,2,3,4-cyclobutanetetracarboxylic dianhydride, 2,3,5-tricarboxylated cyclopentylacetic dianhydride, 5-(2,5-dioxotetrahydrofuran-3-yl)-3a,4,5,9b-tetrahydronaphtho[1,2-c]furan-1,3-dione, 5-(2,5-dioxotetrahydrofuran-3-yl)-8-methyl-3a,4,5,9b-tetrahydronaphtho[1,2-c]furan-1,3-dione, 2,4,6,8-tetracarboxylated bicyclo[3.3.0]octane-2:4,6:8-dianhydride, cyclopentanetetracarboxylic dianhydride, and cyclohexanetetracarboxylic dianhydride.
[0184] Examples of aromatic tetracarboxylic dianhydrides include pyromellitic dianhydride, 4,4'-(hexafluoroisopropylidene)phthalic anhydride, ethylene glycol bis(triphenylene)phthalic anhydride ester, 4,4'-carbonyl phthalic anhydride, 4,4'-oxyphthalic anhydride, and propane-1,3-dimethylbis(1,3-dioxo-1,3-dihydroisobenzofuran-5-carboxylic acid ester). In addition, the tetracarboxylic dianhydride described in Japanese Patent Application Publication No. 2010-97188 may also be used. One or more of these tetracarboxylic dianhydrides may be used alone or in combination.
[0185] Among these, the tetracarboxylic dianhydride is preferably an aromatic tetracarboxylic dianhydride, and more preferably a 4,4'-oxydiphthalic anhydride.
[0186] There are no particular limitations on the diamines mentioned above, and examples include: aliphatic diamines, alicyclic diamines, aromatic diamines, and diamino organosiloxanes.
[0187] Examples of aliphatic diamines include: m-phenylenediamine, 1,3-propanediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, etc.
[0188] Examples of alicyclic diamines include 1,4-diaminocyclohexane and 4,4'-methylenebis(cyclohexylamine).
[0189] Examples of aromatic diamines include p-phenylenediamine, 4,4'-diaminodiphenylmethane, 4-aminophenyl-4-aminobenzoate, 4,4'-diaminoazobenzene, 1,5-bis(4-aminophenoxy)pentane, 1,2-bis(4-aminophenoxy)ethane, 1,6-bis(4-aminophenoxy)hexane, bis[2-(4-aminophenyl)ethyl]adipic acid, 2,6-diaminopyridine, 1,4-bis-(4-aminophenyl)piperazine, 2,2'-dimethyl-4,4'-diaminobiphenyl, and 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl. 4,4'-Diaminodiphenyl ether, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,2-bis(4-aminophenyl)hexafluoropropane, 4,4'-(phenylene diisopropylidene)bisaniline, 1,4-bis(4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, 4,4'-[4,4'-propane-1,3-diylbis(piperidine-1,4-diyl)]diphenylamine, 4,4'-diaminobenzoylaniline, 4,4'-diaminostilbene, 1,4-bis(4-aminophenyl)-piperazine, and other main-chain diamines of the following formula (S-1);
[0190] [Chemistry 8]
[0191]
[0192] (In formula (S-1),
[0193] X can be -O-, -S-, -CO-, -SO2-, -CH2-, -C(CH3)2-, -C(CH3)(C2H5)-, or -C(CF3)2-.
[0194] Dodecyloxy-2,4-diaminobenzene, pentadecyloxy-2,4-diaminobenzene, hexadecyloxy-2,4-diaminobenzene, octadecyloxy-2,4-diaminobenzene, pentadecyloxy-2,5-diaminobenzene, octadecyloxy-2,5-diaminobenzene, cholesteryloxy-3,5-diaminobenzene, cholesteryloxy-3,5-diaminobenzene, cholesteryloxy-2,4-diaminobenzene, cholesteryloxy-2,4-diaminobenzene, 3,5-diaminobenzoic acid cholesteryl ester, 3,5-di Cholesterol aminobenzoate, lanostane 3,5-diaminobenzoate, 3,6-bis(4-aminobenzoyloxy)cholestan, 3,6-bis(4-aminophenoxy)cholestan, 4-(4'-trifluoromethoxybenzoyloxy)cyclohexyl-3,5-diaminobenzoate, 1,1-bis(4-((aminophenyl)methyl)phenyl)-4-butylcyclohexane, 3,5-diaminobenzoic acid=5ξ-cholestan-3-yl, and other side-chain diamines represented by the following formula (S-2);
[0195] [Chemistry 9]
[0196]
[0197] (In formula (S-2),
[0198] X I and X II Each is independently a single bond, -O-, -COO- or -OCO- (where, " "Indicates with X" I (the bond of the bond).
[0199] R I It is an alkyldiyl group with 1 to 3 carbon atoms;
[0200] R II It is a single bond or an alkyl dienyllium with 1 to 3 carbon atoms;
[0201] R III It is an alkyl, alkoxy, fluoroalkyl, or fluoroalkoxy group having 1 to 20 carbon atoms;
[0202] a is 0 or 1;
[0203] b is an integer between 0 and 3;
[0204] c is an integer from 0 to 2;
[0205] d is 0 or 1; where 1 ≦ a + b + c ≦ 3)
[0206] Examples of diamino organosiloxanes include 1,3-bis(3-aminopropyl)-tetramethyldisiloxane. In addition to these, the diamine described in Japanese Patent Application Publication No. 2010-97188 may also be used.
[0207] Among these, the diamine is preferably an aromatic diamine or a diamino organosiloxane, more preferably a compound represented by formula (S-1) or 1,3-bis(3-aminopropyl)-tetramethyldisiloxane.
[0208] The diamine can be used alone or in combination of two or more.
[0209] Polyamic acid can be obtained by reacting the tetracarboxylic dianhydride with a diamine and, as needed, a molecular weight adjuster. The preferred ratio of tetracarboxylic dianhydride to diamine used in the synthesis reaction of polyamic acid is 0.2 to 2 equivalents relative to the amino group of the diamine and the anhydride group of the tetracarboxylic dianhydride. Examples of molecular weight adjusters include: maleic anhydride, phthalic anhydride, itaconic anhydride, and other monoanhydrides; monoamine compounds such as aniline, cyclohexylamine, and n-butylamine; and monoisocyanate compounds such as phenyl isocyanate and naphthyl isocyanate. The preferred ratio of the molecular weight adjuster is 20 parts by mass or less, relative to a total of 100 parts by mass of the tetracarboxylic dianhydride and diamine used.
[0210] The synthesis reaction of polyamic acid is preferably carried out in an organic solvent. The preferred reaction temperature is -20°C to 150°C, and the preferred reaction time is 0.1 hours to 24 hours. Examples of organic solvents used in the reaction include: aprotic polar solvents, phenolic solvents, alcohols, ketones, esters, ethers, halogenated hydrocarbons, and hydrocarbons. Particularly preferred organic solvents are one or more selected from the group consisting of N-methyl-2-pyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, dimethyl sulfoxide, γ-butyrolactone, tetramethylurea, hexamethylphosphoric triamine, m-cresol, xylenol, and halogenated phenols, or a mixture of one or more of these with other organic solvents (e.g., butyl cellosolve, diethylene glycol diethyl ether, etc.). The amount (a) of the organic solvent used is preferably set to be 0.1% to 50% by mass relative to the total amount (a+b) of the tetracarboxylic dianhydride and diamine.
[0211] A reaction solution obtained by dissolving polyamic acid is obtained in the manner described. The reaction solution can be used directly for the preparation of the radiosensitive linear composition, or it can be used for the preparation of the radiosensitive linear composition after separating the polyamic acid contained in the reaction solution.
[0212] The polyamic acid ester can be obtained, for example, by methods such as: [I] reacting the polyamic acid obtained by the synthesis reaction with an esterifying agent; [II] reacting a tetracarboxylic acid diester with a diamine; [III] reacting a tetracarboxylic acid diester dihalide with a diamine. The polyamic acid ester contained in the radiosensitive linear composition of the present invention may have only an amide ester structure, or it may be a partial esterification containing both an amide acid structure and an amide ester structure. The reaction solution obtained by dissolving the polyamic acid ester can be used directly for the preparation of the radiosensitive linear composition, or it can be used for the preparation of the radiosensitive linear composition after separating the polyamic acid ester contained in the reaction solution.
[0213] The content of polymer (A) is preferably 20% by mass or more, more preferably 30% by mass or more, and even more preferably 50% by mass or more, relative to the total amount of solid components contained in the radiosensitive linear composition (i.e., the total mass of components other than the solvent in the radiosensitive linear composition). Furthermore, the content of polymer (A) is preferably 99% by mass or less, more preferably 95% by mass or less, relative to the total amount of solid components contained in the radiosensitive linear composition. By setting the content of polymer (A) within the aforementioned range, pattern formation properties and substrate adhesion can be sufficiently improved.
[0214] <Radiosensitive linear compound (B)>
[0215] The radiosensitive linear composition (B) comprises the polymer (A) and the radiosensitive linear compound (B). By irradiating the radiosensitive linear composition (B) with radiation (visible light, ultraviolet light, far ultraviolet light, etc.), positive or negative patterns can be formed. Examples of radiosensitive linear compounds (B) include photoacid generators, photopolymerization initiators, and photoalkali generators. Preferably, at least one of the group consisting of quinone diazide compound (B-1), photopolymerization initiator (B-2), and photoacid generator (B-3) is used as the radiosensitive linear compound (B).
[0216] Here, when using a photoacid generator or a photoalkali generator as a radiosensitive linear compound, positive or negative patterns can be formed by changing the solubility of the exposed portion in the developer. Alternatively, when the photoacid generator or photoalkali generator functions as a curing catalyst, the solubility of the exposed portion in the developer decreases as curing of the exposed portion is promoted, thereby also forming a negative pattern. On the other hand, when using a photopolymerization initiator as a radiosensitive linear compound, for example, by reacting with a compound having a vinyl or (meth)acryloyl group to promote curing of the exposed portion, the solubility of the exposed portion in the developer decreases, thereby forming a negative pattern.
[0217] Specific examples of the radiosensitive linear composition of the present invention can be cited as follows:
[0218] A radiosensitive linear composition (first composition) comprises the polymer (A), a quinone diazide compound (B-1) as a radiosensitive linear compound (B), and a polymerized ionic liquid (C).
[0219] A negative-type radiosensitive linear composition (second composition) comprises the polymer (A), a photopolymerization initiator (B-2) as a radiosensitive linear compound (B), a polymerizable monomer (X1), and a solvent (C);
[0220] A chemically amplified radiosensitive linear composition (third composition) comprises the polymer (A), a photoacid generator (B-3) as a radiosensitive linear compound (B), and a polymerized ionic liquid (C).
[0221] The first to third radioactive linear compositions will be described below.
[0222] (First Composition)
[0223] The first composition is a radiosensitive composition comprising a quinone diazide compound (B-1) as a radiosensitive linear compound (B).
[0224] (quinone diazide compound (B-1))
[0225] The quinone diazide compound (B-1) is a compound that produces a carboxylic acid by irradiation with radiation. Examples of quinone diazide compounds (B-1) include condensates of phenolic or alcoholic compounds (hereinafter also referred to as "cores") with o-naphthoquinone diazide compounds. Among these, the quinone diazide compound used is preferably a condensate of a compound having a phenolic hydroxyl group as the core and an o-naphthoquinone diazide compound. Specific examples of cores include the compounds described in paragraphs
[0065] to
[0070] of Japanese Patent Application Publication No. 2014-186300.
[0226] Specific examples of quinone diazide compounds (B-1) include compounds containing phenolic hydroxyl groups selected from 4,4'-dihydroxydiphenylmethane, 2,3,4,2',4'-pentahydroxybenzophenone, tris(p-hydroxyphenyl)methane, 1,1,1-tris(p-hydroxyphenyl)ethane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 1,3-bis[1-(4-hydroxyphenyl)-1-methylethyl]benzene, 1,4-bis[1-(4-hydroxyphenyl)-1-methylethyl]benzene, 4,6-bis[1-(4-hydroxyphenyl)-1-methylethyl]-1,3-dihydroxybenzene and 4,4'-[1-[4-[1-[4-[4-hydroxyphenyl]-1-methylethyl]phenyl]ethylidene]bisphenol, and ester compounds with 1,2-naphthoquinone diazide-4-sulfonyl chloride or 1,2-naphthoquinone diazide-5-sulfonyl chloride. Among these, the preferred condensate of 4,4'-[1-[4-[1-[4-[4-hydroxyphenyl]-1-methylethyl]phenyl]ethylidene]bisphenol with 1,2-naphthoquinone diazide-5-sulfonyl chloride is the quinone diazide-5-sulfonyl chloride.
[0227] These quinone diazide compounds (B-1) can be used alone or in combination of two or more. The lower limit of the content of quinone diazide compound (B-1) relative to 100 parts by mass of polymer (A) formulated in the first composition is preferably 1 part by mass, more preferably 10 parts by mass, and even more preferably 15 parts by mass. Furthermore, the upper limit of the content of quinone diazide compound (B-1) relative to 100 parts by mass of polymer (A) formulated in the first composition is preferably 50 parts by mass, more preferably 30 parts by mass. If the content of quinone diazide compound (B-1) is set to 5 parts by mass or more, the carboxylic acid is sufficiently generated by irradiating the first composition with radiation, which sufficiently increases the difference in solubility of the irradiated and unirradiated portions in the developer, allowing for good patterning; this is preferable in this respect. In addition, increasing the amount of carboxylic acid participating in the reaction with the polymer components sufficiently ensures heat resistance and chemical resistance; this is preferable in this respect. On the other hand, by setting the content of quinone diazide compound to 50 parts by mass or less, the amount of unreacted quinone diazide compound after exposure can be sufficiently reduced, and the decrease in developability caused by the residue of quinone diazide compound can be suppressed, which is preferable in this respect.
[0228] (Second Composition)
[0229] The second composition is a negatively radiosensitive linear composition comprising a photopolymerization initiator (B-2) as a radiosensitive linear compound (B) and comprising a polymerizable monomer (X1).
[0230] (Photopolymerization initiator (B-2))
[0231] As the photopolymerization initiator (B-2), a compound that senses and initiates and promotes the polymerization of the polymerizable monomer (X1) with a wavelength of 300 nm or higher (preferably 300 nm to 450 nm) is preferably used. When using a photopolymerization initiator (B-2) that does not directly sense photochemical rays with a wavelength of 300 nm or higher, it can also sense and initiate and promote the polymerization of the polymerizable monomer (X1) with a wavelength of 300 nm or higher by using it in conjunction with a sensitizer.
[0232] Known compounds can be used as photopolymerization initiators (B-2). Specific examples include: oxime ester compounds, organohalogenated compounds, oxydiazole compounds, carbonyl compounds, ketal compounds, benzoin compounds, acridine compounds, organoperoxide compounds, azo compounds, coumarin compounds, azide compounds, metallocene compounds, hexaarylbiimidazole compounds, organoboronic acid compounds, disulfonic acid compounds, α-aminoketone compounds, onium salt compounds, acylphosphine (oxide) compounds, etc. In terms of further improving the sensitivity of the second composition, at least one of these is preferably selected from the group consisting of oxime ester compounds, α-aminoketone compounds, and hexaarylbiimidazole compounds, more preferably oxime ester compounds or α-aminoketone compounds. Furthermore, commercially available products can also be used as photopolymerization initiators (B-2), such as IRGACURE OXE01 and IRGACURE OXE02 (both manufactured by BASF).
[0233] These photopolymerization initiators (B-2) can be used alone or in combination of two or more. The lower limit of the content of photopolymerization initiator (B-2) relative to 100 parts by mass of the polymerizable monomer (X1) contained in the second composition is preferably 1 part by mass, more preferably 5 parts by mass, and even more preferably 10 parts by mass. Furthermore, the upper limit of the content of photopolymerization initiator (B-2) relative to 100 parts by mass of the polymerizable monomer (X1) is preferably 45 parts by mass, more preferably 35 parts by mass, and even more preferably 25 parts by mass.
[0234] (Polymerized monolith (X1))
[0235] The second composition contains a polymerizable monomer (X1). The polymerizable monomer (X1) contained in the second composition is a compound having one or more polymerizable groups, preferably two or more. Examples of polymerizable groups include: vinyl unsaturated groups, oxetyl, oxetyl, N-alkoxymethylamino, etc. Among these, vinyl unsaturated groups and N-alkoxymethylamino are preferred in terms of high polymerizability, and vinyl-containing groups such as (meth)acryloyl, vinyl, and vinylphenyl are preferred.
[0236] Specifically, as a polymerizable monomer (X1), it is preferably a compound having two or more (meth)acryloyl groups or a compound having two or more N-alkoxymethylamino groups, and particularly preferably a compound having two or more (meth)acryloyl groups. The number of polymerizable groups in one molecule of polymerizable monomer (X1) is preferably two to ten, more preferably two to eight.
[0237] Specific examples of polymerizable monomers (X1) that are compounds having two or more (meth)acryloyl groups include: polyfunctional (meth)acrylates obtained by reacting trivalent or higher aliphatic polyhydroxy compounds with (meth)acrylic acid; polyfunctional (meth)acrylates modified with caprolactone; polyfunctional (meth)acrylates modified with epoxide; polyfunctional urethane (meth)acrylates obtained by reacting hydroxyl-containing (meth)acrylates with polyfunctional isocyanates; and polyfunctional (meth)acrylates with carboxyl groups obtained by reacting hydroxyl-containing (meth)acrylates with acid anhydrides.
[0238] Compounds having two or more N-alkoxymethyl amino groups include, for example, compounds with melamine, benzoguanamine, or urea structures. Furthermore, the terms melamine or benzoguanamine structures refer to chemical structures having one or more triazine rings or phenyl-substituted triazine rings as the basic skeleton, and also include melamine, benzoguanamine, or their condensates. Specific examples of compounds having two or more N-alkoxymethyl amino groups include: N,N,N',N',N'',N''-hexa(alkoxymethyl)melamine, N,N,N',N'-tetra(alkoxymethyl)benzoguanamine, and N,N,N',N'-tetra(alkoxymethyl)glycourea.
[0239] As a polymerizable monomer (X1), the preferred options are polyfunctional (meth)acrylates obtained by reacting trivalent or higher aliphatic polyhydroxy compounds with (meth)acrylate, caprolactone-modified polyfunctional (meth)acrylates, polyfunctional urethane (meth)acrylates, polyfunctional (meth)acrylates having carboxyl groups, N,N,N',N',N'',N''-hexa(alkoxymethyl)melamine, and N,N,N',N'-tetra(alkoxymethyl)benzoguanidine. More preferably, polyfunctional (meth)acrylates, polyfunctional urethane (meth)acrylates, and polyfunctional (meth)acrylates having carboxyl groups are obtained by reacting trivalent or higher aliphatic polyhydroxy compounds with (meth)acrylate. Even more preferably, polyfunctional (meth)acrylates are obtained by reacting trivalent or higher aliphatic polyhydroxy compounds with (meth)acrylate.
[0240] Specific examples of polyfunctional (meth)acrylates obtained by reacting trivalent or higher aliphatic polyhydroxy compounds with (meth)acrylic acid include: pentaerythritol tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol tri(meth)acrylate, dipentaerythritol di(meth)acrylate, dipentaerythritol hexa(meth)acrylate, trimethylolpropane di(meth)acrylate, and dipentaerythritol polyacrylate. Among these, pentaerythritol triacrylate, dipentaerythritol pentaacrylate, dipentaerythritol hexaacrylate, and dipentaerythritol polyacrylate are particularly preferred in terms of increasing the density of intermolecular or intramolecular crosslinking and further improving the curability of the film through low-temperature calcination.
[0241] These polymeric monomers (X1) can be used alone or in combination of two or more. The lower limit of the content of polymeric monomer (X1) relative to 100 parts by weight of polymer (A) contained in the second composition is preferably 20 parts by weight, more preferably 25 parts by weight, and even more preferably 30 parts by weight. Furthermore, the upper limit of the content of polymeric monomer (X1) relative to 100 parts by weight of polymer (A) is preferably 300 parts by weight, more preferably 200 parts by weight, and even more preferably 100 parts by weight. If the content ratio of polymeric monomer (X1) is within the aforementioned range, sufficient curability and sufficient alkaline developability as a curing film can be ensured, and the generation of scale, film residue, etc., on the unexposed substrate or the light-shielding layer can be sufficiently suppressed; therefore, this is preferable.
[0242] (Third Composition)
[0243] The third composition is a chemically amplified radioactive linear composition comprising a photoacid generator (B-3) as a radioactive linear compound (B). The polymer (A) in the third composition is a polymer (A1) comprising a structural unit (III) having one or more groups selected from the group represented by the formula (a2) and acid-dissociable groups.
[0244] (Photoacid generator (B-3))
[0245] Photoacid generators (B-3) are any compounds that generate acid in response to radiation (i.e., radiosensitive acid generators), and there are no particular limitations. Examples of photoacid generators (B-3) include: oxime sulfonates, onium salts, sulfonylimide compounds, halogen-containing compounds, diazomethane compounds, sulfone compounds, sulfonate compounds, and carboxylic acid ester compounds.
[0246] Specific examples of oxime sulfonate compounds, onium salts, sulfonylimide compounds, halogen-containing compounds, diazomethane compounds, sulfone compounds, sulfonate compounds, and carboxylic acid ester compounds include, for example, compounds described in paragraphs
[0078] to
[0106] of Japanese Patent Application Publication No. 2014-157252, and compounds described in International Publication No. 2016 / 124493. As a photoacid generator, from the viewpoint of radiation sensitivity, at least one selected from the group consisting of oxime sulfonate compounds and sulfonylimide compounds is preferably used.
[0247] The oxime sulfonate compound is preferably a compound having a sulfonate group represented by the following formula (t1).
[0248] [Chemistry 10]
[0249]
[0250] (In formula (t1),
[0251] R 40 It is a monovalent hydrocarbon group, or a monovalent group formed by substituting some or all of the hydrogen atoms in the hydrocarbon group with substituents;
[0252] “ "Indicates a bond"
[0253] In the above equation (t1), R is... 40 Monovalent hydrocarbon groups, such as alkyl groups having 1 to 20 carbon atoms, cycloalkyl groups having 4 to 12 carbon atoms, and aryl groups having 6 to 20 carbon atoms, can be used as substituents, such as alkyl groups having 1 to 5 carbon atoms, alkoxy groups having 1 to 5 carbon atoms, side oxygen groups, and halogen atoms.
[0254] If oxime sulfonate compounds are to be exemplified, the following can be listed: (5-propylsulfonyloxyimino-5H-thiophen-2-ylidene)-(2-methylphenyl)acetonitrile, (5-octylsulfonyloxyimino-5H-thiophen-2-ylidene)-(2-methylphenyl)acetonitrile, (camphorsulfonyloxyimino-5H-thiophen-2-ylidene)-(2-methylphenyl)acetonitrile, (5-p-toluenesulfonyloxyimino-5H-thiophen-2-ylidene)-(2-methylphenyl)acetonitrile, (2-[2-(4-methylphenylsulfonyloxyimino)])-2,3-dihydrothiophen-3-ylidene]-2-(2-methylphenyl)acetonitrile, 2-(octylsulfonyloxyimino)-2-(4-methoxyphenyl)acetonitrile, and the compounds described in International Publication No. 2016 / 124493, etc. Commercially available oxime sulfonate compounds include Irgacure PAG121 manufactured by BASF.
[0255] If sulfonylimide compounds are to be exemplified, the following can be listed: N-(trifluoromethylsulfonyloxy)succinimide, N-(camphorsulfonyloxy)succinimide, N-(4-methylphenylsulfonyloxy)succinimide, N-(2-trifluoromethylphenylsulfonyloxy)succinimide, N-(4-fluorophenylsulfonyloxy)succinimide, N-(trifluoromethylsulfonyloxy)phthalimide, N-(camphor ... N-(2-trifluoromethylphenylsulfonyloxy)phthalimide, N-(2-fluorophenylsulfonyloxy)phthalimide, N-(trifluoromethylsulfonyloxy)diphenylmaleimide, N-(camphorsulfonyloxy)diphenylmaleimide, (4-methylphenylsulfonyloxy)diphenylmaleimide, trifluoromethanesulfonic acid-1,8-naphthalenediamide.
[0256] These photoacid generating agents (B-3) can be used alone or in combination of two or more. The lower limit of the content of the photoacid generating agent (B-3) relative to 100 parts by mass of polymer (A) formulated in the third composition is preferably 0.01 parts by mass, more preferably 0.1 parts by mass, and even more preferably 2 parts by mass. Furthermore, the upper limit of the content of the photoacid generating agent (B-3) relative to 100 parts by mass of polymer (A) formulated in the third composition is preferably 30 parts by mass, more preferably 20 parts by mass, and even more preferably 10 parts by mass. Setting the content of the photoacid generating agent (B-3) to 1 part by mass or more allows for good patterning and ensures sufficient heat resistance, which is advantageous in this respect. Furthermore, setting the content of the photoacid generating agent (B-3) to 30 parts by mass or less sufficiently reduces the amount of unreacted photoacid generating agent after exposure, suppressing the decrease in developability caused by the residue of the photoacid generating agent, which is advantageous in this respect.
[0257] <Polymerized Ionic Liquids (C)>
[0258] Polymerized ionic liquids (C) are polymers comprising anionic and cationic portions constituting the ionic liquid, preferably polymers in which the anionic and cationic portions constituting the ionic liquid are included as side chain portions. "Included as side chain portions" means that the anionic or cationic portion is bonded (covalently bonded) to the main chain as a side chain structure of the polymer. In the case of polymers with three-dimensional bonding, such as polysiloxanes, where the main chain cannot be clearly identified, the groups bonded to Si, except for Si-O bonds, are designated as side chain portions. When the anionic portion is bonded to the main chain as a side chain structure of the polymer, the cationic portion, as the opposite ion of the anionic portion, forms an ionic bond with the anionic portion to form a salt. Conversely, when the cationic portion is bonded to the main chain as a side chain structure of the polymer, the anionic portion, as the opposite ion of the cationic portion, forms an ionic bond with the cationic portion to form a salt.
[0259] The polymerized ionic liquid (C) is also sometimes described as "poly(ionicliquid) block copolymers" (ACS Applied Polymer Materials, ACS Appl. Polym. Mater. 2023, 5, 2639-2653), "polymerized ionic liquids" (Journal of Physical Chemistry B, J. Phys. Chem. B 2017, 121, 11511-11519), "polymeric ionic liquids" (Polymer 55 (2014) 3385-3396), etc.
[0260] The glass transition temperature of the polymeric ionic liquid (C) is below 5°C, preferably below 0°C, more preferably below -10°C, even more preferably below -20°C, and further preferably below -30°C. Furthermore, the lower limit of the glass transition temperature is not particularly limited, but a lower value is preferred, typically around -100°C. By ensuring the glass transition temperature is within this range, although it is a polymer, ionic conductivity can be guaranteed.
[0261] The lower limit of the weight average molecular weight (Mw) of the polymerized ionic liquid (C) is preferably 1,000, more preferably 5,000, further preferably 10,000, and particularly preferably 50,000. The upper limit of the weight average molecular weight (Mw) is not particularly limited, but is preferably 1,000,000, more preferably 500,000. The weight average molecular weight (Mw) is a value converted from polystyrene obtained by gel permeation chromatography (hereinafter referred to as GPC).
[0262] The polymer having the anionic and cationic portions constituting the ionic liquid as side chain portions of the polymer is preferably an acrylic polymer or a polysiloxane polymer, more preferably an acrylic polymer.
[0263] As the polymerized ionic liquid (C), the polymer in which the anionic portion is bonded to the main chain as a side chain structure of the polymer and the cation portion is ionicly bonded to the anionic portion bonded to the main chain as a relative ion to form a salt is preferably a partial structure (C1) comprising one or more of the group consisting of the following formulas (C1-1) and (C1-2).
[0264] [Chemistry 11]
[0265]
[0266] (In equations (C1-1) and (C1-2),)
[0267] Rc 11 It consists of halogen atoms or substituted or unsubstituted chain hydrocarbon groups;
[0268] X m+ It is a proton or onium cation;
[0269] m is an integer from 1 to 3;
[0270] For bonding with other structures in polymerized ionic liquids (C)
[0271] As the R c11 The halogen atom represented can be fluorine, chlorine, bromine, or iodine, with fluorine being the preferred one.
[0272] As the R c11 The chain-like hydrocarbon group represented may suitably be R of formula (3a-1). 4 ~R 6 The chain hydrocarbon group having 1 to 30 carbon atoms. Additionally, groups formed by substituting some or all of the hydrogen atoms in the chain hydrocarbon group with substituents can be listed. Substituents (T) described later can be listed as examples of substituents.
[0273] Among these, as R c11 Preferably, it is a halogenated chain hydrocarbon group formed by substituting a halogen atom or a halogen atom for part or all of the hydrogen atoms in the chain hydrocarbon group, more preferably a halogen atom or a monovalent halogenated chain hydrocarbon group having 1 to 10 carbon atoms, and even more preferably a fluorine atom or a fluorinated alkyl group having 1 to 5 carbon atoms, and particularly preferably a fluorine atom or a trifluoromethyl atom.
[0274] As the X m+ Examples of onion cations include: ammonium cations, phosphonium cations, sulfonium cations, imidazole onion cations, pyrrolidine onion cations, and diazo onion cations.
[0275] As the ammonium cation, an organic ammonium cation is preferred, such as tetramethylammonium, tetraethylammonium, monostearinyltrimethylammonium, distearyldimethylammonium, tripearin monomethylammonium, cetyltrimethylammonium, trioctylmethylammonium, dioctyldimethylammonium, monolauryltrimethylammonium, dilauryldimethylammonium, trilaurylmethylammonium, tripentylbenzylammonium, trihexylbenzylammonium, trioctylbenzylammonium, trilaurylbenzylammonium, benzyldimethylstearinammonium, benzyldimethyloctylammonium, dialkyl (alkyl group is C14-C18) dimethylammonium, etc. Among these, tetramethylammonium and tetraethylammonium are preferred.
[0276] The preferred phosphonium cation is an organophosphonium cation, such as: tetraalkylphosphonium (e.g., methyltrioctylphosphonium, methyltripropylphosphonium, octyltributylphosphonium, dodecyltributylphosphonium, hexadecyltributylphosphonium, dihexyldioctylphosphonium); aryltrialkylphosphonium (e.g., benzyltributylphosphonium); dialkyldiarylphosphonium (e.g., dibutyldiphenylphosphonium); alkyltriphenylphosphonium (e.g., butyltriphenylphosphonium); tetraarylphosphonium (e.g., benzyltriphenylphosphonium). Among these, methyltripropylphosphonium is preferred.
[0277] Examples of imidazolium cations include: N-methylimidazolium cation, N-ethylimidazolium cation, 1,3-dimethylimidazolium cation, 1,3-diethylimidazolium cation, 1-ethyl-3-methylimidazolium cation, 1-propyl-3-methylimidazolium cation, 1-butyl-3-methylimidazolium cation, 1-propen-3-methylimidazolium cation, 1-hexyl-3-methylimidazolium cation, 1,2,3-trimethylimidazolium cation, and 1,2 ,3,4-Tetramethylimidazolium cation, 1-allyl-3-methylimidazolium cation, N-propylpyridinium cation, N-butylpyridinium cation, 1,4-dimethylpyridinium cation, 1-butyl-4-methylpyridinium cation, 1-butyl-2,4-dimethylpyridinium cation, trimethylammonium cation, ethyldimethylammonium cation, diethylmethylammonium cation, triethylammonium cation, tetramethylammonium cation, triethylmethylammonium cation, tetraethylammonium cation, etc. Among these, the preferred choices are dialkylimidazolium cations such as 1,3-dimethylimidazolium cation, 1,3-diethylimidazolium cation, 1-ethyl-3-methylimidazolium cation, 1-propyl-3-methylimidazolium cation, 1-butyl-3-methylimidazolium cation, 1-hexyl-3-methylimidazolium cation, or 1-propene-3-methylimidazolium cation.
[0278] Examples of pyrrolidone cations include N,N-dimethylpyrrolidone, N-ethyl-N-methylpyrrolidone, N,N-diethylpyrrolidone, N-propyl-N-methylpyrrolidone, N-butyl-N-methylpyrrolidone, N-pentyl-N-methylpyrrolidone, and N-hexyl-N-methylpyrrolidone.
[0279] As the sulfonium cation, the cation described in paragraph
[0063] of Japanese Patent Application Publication No. 2009-073871 can be cited. As the diazoonium cation, the cation described in paragraph
[0374] of Japanese Patent Application Publication No. 2002-332271 can be cited.
[0280] As a polymerized ionic liquid (C1) having the aforementioned partial structure (C1), it is preferably a polymer having a structural unit (X) represented by the following formula (1) or formula (2).
[0281] [Chemistry 12]
[0282]
[0283] (In equations (1) and (2),
[0284] R c1 It can be a hydrogen atom, a methyl group, or a trifluoromethyl group;
[0285] R c2 It is a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, or a fluorinated alkyl group having 1 to 10 carbon atoms, or it can be bonded to a silicon atom of a different structural unit to form a siloxane bond;
[0286] L c11 L c12 It is a single bond or a divalent linker;
[0287] R c12 R c13 R c14 It is a single bond or a divalent organic group with 1 to 20 carbon atoms;
[0288] D is the partial structure (C1) represented by the formula (C1-1) or formula (C1-2).
[0289] As the R c12 R c13 R c14 The divalent organic groups with 1 to 20 carbon atoms can be adapted to be formed by removing one hydrogen atom from a monovalent organic group with 1 to 20 carbon atoms.
[0290] Examples of monovalent organic groups having 1 to 20 carbon atoms include: monovalent hydrocarbon groups having 1 to 20 carbon atoms, groups (α) having divalent heteroatoms between carbon atoms or at the end of the hydrocarbon group, groups (β) formed by substituting some or all of the hydrogen atoms of the hydrocarbon group or the group (α) with a monovalent heteroatom, or combinations thereof.
[0291] As the monovalent hydrocarbon group having 1 to 20 carbon atoms, R of formula (3a-1) can be suitably adopted. 4 ~R 6 The hydrocarbon group representing the number of carbon atoms from 1 to 30 corresponds to the number of carbon atoms.
[0292] Examples of heteroatoms constituting the monovalent or divalent heteroatom-containing bases include: oxygen, nitrogen, sulfur, phosphorus, silicon, and halogen atoms. Examples of halogen atoms include: fluorine, chlorine, bromine, and iodine atoms.
[0293] Examples of monovalent heteroatom-containing groups include: hydroxyl, carboxyl, hydrogen sulfide, cyano, nitro, halogen atom, etc.
[0294] Examples of divalent heteroatom-containing groups include: -CO-, -C(=O)O-, -CS-, -NR'-, -O-, -S-, -SO2-, or combinations thereof. R' is a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms.
[0295] Among these, as the R c12 R c13 R c14 Preferably, it is an alkyldiyl such as methanediyl, ethanediyl, propanediyl, butanediyl, pentanediyl, or hexanediyl, or an aromatic diyl such as phenyldiyl, toluenediyl, xylenediyl, or naphthyl, and more preferably an alkyldiyl.
[0296] As the R c1 Preferably, it is a hydrogen atom or a methyl group, more preferably a methyl group.
[0297] As the R c2 The alkyl group having 1 to 10 carbon atoms can suitably be represented by R of formula (a2). 1 ~R 3 Alkyl groups with 1 to 10 carbon atoms.
[0298] As the R c2 The fluorinated alkyl group having 1 to 10 carbon atoms may be suitably formed by substituting some or all of the hydrogen atoms of the alkyl group having 1 to 10 carbon atoms with fluorine atoms.
[0299] The R c2 It can form siloxane bonds by bonding with silicon atoms of different structural units. Through bonding with silicon atoms of different structural units, siloxane bonds can be formed, enabling three-dimensional bond formation. In this case, R c2 Depend on -O-(Si(R t1 (R) t2 )-O) t - Represented by R. In the formula, R... t1 R t2 They are either hydrogen atoms or organic groups with 1 to 20 carbon atoms. This indicates the bond between Si and the given equation (2). This represents the bond between silicon atoms in different structural units. t is an integer from 0 to 10. As a divalent organic group with 1 to 20 carbon atoms, R of the above formulas (1) and (2) can be suitably adopted. c12 R c13 R c14Divalent organic groups with 1 to 20 carbon atoms.
[0300] As the L c11 L c12 Examples of divalent ligands include: -O-, -S-, -CO-, -COO-, -CONH-, -SO2-, etc. Among these, the L-... c1 Preferably, it is a single bond or -COO-, more preferably -COO-. As L c12 Preferably, it is a single bond or -S-.
[0301] The D is a partial structure (C1) represented by the formula (C1-1) or formula (C1-2), preferably a partial structure (C1) represented by the formula (C1-1).
[0302] The structural unit represented by equation (1) is preferably the structural unit represented by equation (1-1) and equation (1-2) below, and the structural unit represented by equation (2) is preferably the structural unit represented by equation (2-1) and equation (2-2) below.
[0303] [Chemistry 13]
[0304]
[0305] (In equations (1-1), (1-2), (2-1), and (2-2),)
[0306] R c121 R c123 R c131 R c141 R c142 Each is independently a substituted or unsubstituted divalent hydrocarbon group with 1 to 10 carbon atoms;
[0307] R c122 R c143 Each is independently a divalent chain hydrocarbon group having 1 to 5 carbon atoms;
[0308] m11 and m12 are independent integers from 1 to 10;
[0309] R c1 R c2 L c11 L c12 D has the same meaning as equations (1) and (2).
[0310] As the R c121 R c123 R c131 R c141 R c142The divalent hydrocarbon groups representing carbons 1 to 10 can be suitably represented by R from formula (3a-1). 4 ~R 6 The hydrocarbon group represented by carbon numbers 1 to 30 is formed by removing one hydrogen atom from the corresponding carbon number. The hydrocarbon group may have substituents. Examples of such substituents include halogen atoms such as fluorine, chlorine, bromine, and iodine; hydroxyl groups; carboxyl groups; cyano groups; nitro groups; alkyl groups, alkoxy groups, alkoxycarbonyl groups, alkoxycarbonyloxy groups, acyl groups, acyloxy groups, or groups formed by substituting hydrogen atoms of these groups using halogen atoms; and side oxygen groups (=O), etc. (T).
[0311] Among these, as R c121 R c123 R c131 R c141 R c142 Preferably, it is an alkyldiyl group with 1 to 5 carbon atoms.
[0312] As the R c122 R c143 The divalent chain hydrocarbon group representing 1 to 5 carbon atoms can be suitably represented by R from formula (3a-1). 4 ~R 6 A group formed by removing one hydrogen atom from a chain hydrocarbon group having 1 to 30 carbon atoms. Among these, R... c122 R c143 Preferably, it is ethanediyl or propanediyl, and more preferably ethanediyl.
[0313] The m11 and m12 are integers from 1 to 10, preferably integers from 1 to 5.
[0314] The structural unit (X) is preferably a polyepoxyalkane chain, more preferably a polyepoxyethylene chain.
[0315] The following structures can be listed as anion portions of the structural unit (X).
[0316] [Chemistry 14]
[0317]
[0318] (where R) c1 Equation (1) has the same meaning; p1 is an integer from 1 to 5; p is an integer from 1 to 5.
[0319] [Chemistry 15]
[0320]
[0321] (where R) c2(This has the same meaning as equation (2); q1 is an integer from 1 to 10; r is an integer from 1 to 5)
[0322] As a single entity providing the structural unit (X), all combinations of the anion and the cation can be suitably used, among which 1-butyl-3-methylimidazolium-1-[3-(methacryloyloxy)propylsulfonyl]-1-(trifluoromethanesulfonyl)imide is preferred.
[0323] Relative to all structural units constituting the polymerized ionic liquid (C), the lower limit of the content ratio (total content ratio in the case of multiple components) of the structural unit (X) is preferably 2% by mass, more preferably 6% by mass, and even more preferably 10% by mass. Furthermore, the upper limit of the content ratio is preferably 100% by mass, more preferably 90% by mass, and even more preferably 80% by mass. By setting the content ratio of the structural unit (X) within the aforementioned range, the effect as an ionic liquid can be efficiently and effectively achieved.
[0324] In the polymerized ionic liquid (C), the polymer in which the cation portion is bonded to the main chain as a side chain structure of the polymer and the anion portion is ionically bonded to the cation portion bonded to the main chain as a relative ion to form a salt is preferably a polymer having one or more partial structures (C2) selected from the group consisting of the following formulas (C2-1), (C2-2), (C2-3), (C2-4) and (C2-5).
[0325] [Chemistry 16]
[0326]
[0327] (In equations (C2-1) to (C2-5),
[0328] R c22 R c23 R c24 R c25 R c26 R c28 R c30 R c31 R c32 Each is independently a substituted or unsubstituted hydrocarbon group having 1 to 20 carbon atoms, or a hydrocarbon group having -O-, -CO- or -COO- between carbon atoms;
[0329] R c21 R c27 R c29Each of the following is independently a halogen atom, a substituted or unsubstituted hydrocarbon group having 1 to 20 carbon atoms, or a group containing -O-, -CO- or -COO- between carbon atoms in the hydrocarbon group having 1 to 20 carbon atoms;
[0330] s1 is 0 or 1;
[0331] Y - It is an anion;
[0332] For bonding with other structures in polymerized ionic liquids (C)
[0333] As R c22 R c23 R c24 R c25 R c26 R c28 R c30 R c31 R c32 R c21 R c27 R c29 The hydrocarbon group in the formula (3a-1) can be suitably represented by R. 4 ~R 6 The hydrocarbon group having 1 to 30 carbon atoms corresponds to the number of carbon atoms in the hydrocarbon group. The hydrocarbon group may have substituents. Examples of such substituents include the substituent (T). It is also suitable to use groups whose carbon-carbon intercarbon contains -O-, -CO-, or -COO-, for example, groups having a polyoxyalkylene chain. Among these, R... c22 R c23 R c24 R c25 R c26 R c28 R c30 R c31 R c32 R c21 R c27 R c29 Preferably, it is a chain hydrocarbon group having 1 to 10 carbon atoms, and more preferably an alkyl group having 1 to 5 carbon atoms.
[0334] As the Y - The anions referred to include, for example, halogen anions, boron anions, phosphorus anions, organic sulfonate anions, and sulfonyl imide anions, preferably anions having at least one electron-withdrawing group selected from the group consisting of a halogen group (preferably a fluorine group) and a cyano group. Specifically, for example, (FSO₂)₂N - (CF3SO2)2N - (CF3CF2SO2)2N- (CF3SO2)3C - ,Br - AlCl4 - Al2Cl7 - NO3 - BF4 - PF6 - CH3COO - CF3COO - CF3CF2CF2COO - CF3SO3 - CF3(CF2)3SO3 - AsF6 - SbF6 - CH3CH2OSO3 - CH3(CH2)7OSO3 - N(CN)2 - C(CN)3 - Cl - I - PF3(C2F5)3 - P3(CF3)3 - BF2(CF)2 - BF3 (CF3) - B(CN)4 - Among these, (FSO2)2N is preferred. - (CF3SO2)2N - BF4 - PF6 - .
[0335] As the polymerized ionic liquid (C2) having the aforementioned partial structure (C2), it is preferably a polymer having the structural unit (XI) represented by the following formula (3) or formula (4).
[0336] [Chemistry 17]
[0337]
[0338] (In equations (3) and (4),)
[0339] R c1 It can be a hydrogen atom, a methyl group, or a trifluoromethyl group;
[0340] R c2 It is a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, or a fluorinated alkyl group having 1 to 10 carbon atoms;
[0341] L c21 L c22 It is a single bond or a divalent linker;
[0342] R c33 R c34 R c35 It is a single bond or a divalent organic group with 1 to 20 carbon atoms;
[0343] A is the partial structure (C2) represented by equation (C2-1), equation (C2-2), equation (C2-3), equation (C2-4), or equation (C2-5).
[0344] The R c1 R c2 R in equations (1) and (2) c1 R c2 They have the same meaning.
[0345] As L c21 L c22 The divalent linker in the formula (1) can be suitably represented by L. c11 The divalent linker in [the group]. Among these, [the group] is a divalent linker in [the group]. c21 Preferably, it is a single bond or -COO-, more preferably -COO-. As L c22 Preferably, it is a single bond or -S-.
[0346] As the R c33 R c34 R c35 The divalent organic groups with carbon numbers 1 to 20 in the formula can be appropriately represented by R in formulas (1) and (2). c12 R c13 R c14 The divalent organogroups with 1 to 20 carbon atoms. Among these, as the R... c33 R c34 R c35 Preferably, it is an alkyldiyl such as methanediyl, ethanediyl, propanediyl, butanediyl, pentanediyl, or hexanediyl, or an aromatic diyl such as phenyldiyl, toluenediyl, xylenediyl, or naphthyl, and more preferably an alkyldiyl.
[0347] A is a partial structure (C2) represented by formula (C2-1), formula (C2-2), formula (C2-3), formula (C2-4) or formula (C2-5), among which the partial structure represented by formula (C2-1) is preferred.
[0348] The structural unit represented by equation (3) is preferably the structural unit represented by equation (3-1) and equation (3-2) below, and the structural unit represented by equation (4) is preferably the structural unit represented by equation (4-1) and equation (4-2) below.
[0349] [Chemistry 18]
[0350]
[0351] (In equations (3-1), (3-2), (4-1), and (4-2),)
[0352] R c331 R c333 R c341 R c351 R c352 Each is independently a substituted or unsubstituted divalent hydrocarbon group with 1 to 10 carbon atoms;
[0353] R c332 R c353 Each is independently a divalent chain hydrocarbon group having 1 to 5 carbon atoms;
[0354] m21 and m22 are independent integers from 1 to 10;
[0355] R c1 R c2 L c21 L c22 A has the same meaning as equations (3) and (4).
[0356] As the R c331 R c333 R c341 R c351 R c352 The divalent hydrocarbon groups representing carbons 1 to 10 can be suitably represented by R from formula (3a-1). 4 ~R 6 The group is formed by removing one hydrogen atom from the corresponding carbon number of a hydrocarbon group representing 1 to 30 carbon atoms. The hydrocarbon group may have substituents. Examples of substituents include the substituent (T).
[0357] Among these, as R c331 R c333 R c341 R c351 R c352 Preferably, it is an alkyldiyl group with 1 to 5 carbon atoms.
[0358] As the R c332 R c353 The divalent chain hydrocarbon group representing 1 to 5 carbon atoms can be suitably represented by R from formula (3a-1). 4 ~R 6 A group formed by removing one hydrogen atom from a chain hydrocarbon group having 1 to 30 carbon atoms. Among these, R... c332 R c353 Preferably, it is ethanediyl or propanediyl, and more preferably ethanediyl.
[0359] The m21 and m22 are integers from 1 to 10, preferably integers from 1 to 5.
[0360] The structural unit (XI) is preferably a polyepoxyalkylene chain, more preferably a polyepoxyethylene chain.
[0361] The following structures can be listed as the cationic portion of the structural unit (XI).
[0362] [Chemistry 19]
[0363]
[0364] (where R) c1 This has the same meaning as equation (3); p is an integer from 1 to 5; p1 is an integer from 1 to 5.
[0365] [Chemistry 20]
[0366]
[0367] (where R) c2 (This has the same meaning as equation (4); q1 is an integer from 1 to 10; r is an integer from 1 to 5)
[0368] As a single entity providing the structural unit (XI), all combinations of the anion and the cation can be suitably used, among which 1-[2-(2-(methacryloyloxy)ethoxy)ethoxy]ethyl]-N-methylpyrrolidone bis(trifluoromethylsulfonyl)imide is preferred.
[0369] Relative to all structural units constituting the polymerized ionic liquid (C), the lower limit of the content ratio (total content ratio in the case of multiple components) of the structural unit (XI) is preferably 2% by mass, more preferably 6% by mass, and even more preferably 10% by mass. Furthermore, the upper limit of the content ratio is preferably 100% by mass, more preferably 90% by mass, and even more preferably 80% by mass. By setting the content ratio of the structural unit (XI) within the aforementioned range, the effect as an ionic liquid can be efficiently and effectively achieved.
[0370] <Other structural units>
[0371] The polymerized ionic liquid (C) may contain structural units other than the aforementioned structural unit (X) or structural unit (XI). Examples of other structural units include structural units (XII) derived from an vinyl unsaturated monomer having one or more carboxyl groups (hereinafter also referred to as unsaturated monomer (d1)) and structural units (XIII) derived from an vinyl unsaturated monomer without carboxyl groups (hereinafter also referred to as unsaturated monomer (d2)).
[0372] Examples of unsaturated monomers (d1) include: (meth)acrylic acid, maleic acid, maleic anhydride, succinic acid mono[2-(meth)acryloyloxyethyl], ω-carboxylated polycaprolactone mono(meth)acrylate, p-vinylbenzoic acid, etc. Two or more unsaturated monomers (d1) may be used alone or in combination.
[0373] Furthermore, examples of unsaturated monomasks (d2) can be cited as follows:
[0374] N-substituted maleimides such as N-phenylmaleimide and N-cyclohexylmaleimide;
[0375] Aromatic vinyl compounds such as styrene, α-methylstyrene, p-hydroxystyrene, p-hydroxy-α-methylstyrene, p-vinylbenzyl glycidyl ether, and acenaphthylene;
[0376] Methyl methacrylate, n-butyl methacrylate, 2-ethylhexyl methacrylate, 2-hydroxyethyl methacrylate, 2-phenylethyl methacrylate, allyl methacrylate, benzyl methacrylate, polyethylene glycol (degree of polymerization 2-10) methyl ether (meth)acrylate, polypropylene glycol (degree of polymerization 2-10) methyl ether (meth)acrylate, polyethylene glycol (degree of polymerization 2-10) mono(meth)acrylate, polypropylene glycol (degree of polymerization 2-10) mono(meth)acrylate, cyclohexyl methacrylate, isobornyl methacrylate, tricyclohexyl methacrylate [5.2.1.0] 2,6 Decane-8-yl ester, dicyclopentenyl (meth)acrylate, glycerol mono(meth)acrylate, 4-hydroxyphenyl (meth)acrylate, ethylene oxide-modified (meth)acrylate of p-cumylphenol, glycidyl (meth)acrylate, 3,4-epoxycyclohexyl methyl (meth)acrylate, 3-[(meth)acryloyloxymethyl]oxetane, 3-[(meth)acryloyloxymethyl]-3-ethyloxetane, etc. (meth)acrylates;
[0377] Cyclohexyl vinyl ether, isobornyl vinyl ether, tricyclo[5.2.1.0] 2,6 Decane-8-yl vinyl ether, pentacyclic pentadecyl vinyl ether, 3-(vinyloxymethyl)-3-ethyloxetane and other vinyl ethers;
[0378] Polystyrene, poly(methyl methacrylate), poly(n-butyl methacrylate), polysiloxane, and other macromonomers with mono(meth)acryloyl groups at the ends of their polymer molecular chains are examples of such macromonomers.
[0379] The unsaturated monolith (d2) can be used alone or in combination of two or more.
[0380] As the unsaturated monomer (d2), (meth)acrylate is preferred, and more preferably polyethylene glycol (degree of polymerization 2-10) methyl ether (meth)acrylate or 2-phenylethyl (meth)acrylate.
[0381] When the polymerized ionic liquid (C) contains the other structural units (XII) or (XIII), the lower limit of the content ratio (total content ratio in the case of multiple structural units) of structural unit (XII) or structural unit (XIII) relative to all structural units constituting the polymerized ionic liquid (C) is preferably 0% by mass, more preferably 10% by mass, and even more preferably 20% by mass. Furthermore, the upper limit of the content ratio is preferably 98% by mass, more preferably 94% by mass, and even more preferably 90% by mass. By setting the content ratio of structural unit (XII) or structural unit (XIII) within the aforementioned range, the effects as an ionic liquid can be efficiently and effectively exhibited.
[0382] The polymerization method for the polymerized ionic liquid (C) can utilize the same method as that for the polymer (A).
[0383] The polymerized ionic liquid (C) can be used alone or in combination with two or more. The lower limit of the content of the polymerized ionic liquid (C) relative to 100 parts by mass of polymer (A) is preferably 80 parts by mass, more preferably 100 parts by mass, further preferably 150 parts by mass, further preferably 200 parts by mass, and particularly preferably 250 parts by mass. Furthermore, the upper limit of the content of the polymerized ionic liquid (C) relative to 100 parts by mass of polymer (A) is preferably 600 parts by mass, more preferably 500 parts by mass, and further preferably 450 parts by mass. Setting the content of the polymerized ionic liquid (C) to 80 parts by mass or more provides good capacitance, which is advantageous in this respect. Additionally, setting the content of the polymerized ionic liquid (C) to 600 parts by mass or less is advantageous in terms of shape stability or substrate adhesion during patterning.
[0384] <Close Contact Additive (D)>
[0385] The radiosensitive linear composition of the present invention may contain a bonding aid (D). The bonding aid is a component that improves the adhesion between the pattern (hardened film) formed using the radiosensitive linear composition and the substrate. Preferably, a functionalized silane coupling agent having a reactive functional group is used as the bonding aid. Examples of reactive functional groups that can be found in a functionalized silane coupling agent include: carboxyl, (meth)acryloyl, epoxy, vinyl, isocyanate, etc.
[0386] Specific examples of functional silane coupling agents include: trimethoxysilylbenzoic acid, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-(meth)acrylateoxypropyltrimethoxysilane, 3-(meth)acrylateoxypropyltriethoxysilane, vinyltriacetoxysilane, vinyltrimethoxysilane, 3-isocyanopropyltriethoxysilane, etc.
[0387] When the bonding agent (D) is incorporated into the radiosensitive linear composition, the lower limit of its content relative to 100 parts by weight of polymer (A) is preferably 0.01 parts by weight, more preferably 1 part by weight, and even more preferably 3 parts by weight. Furthermore, the upper limit of its content is preferably 30 parts by weight, more preferably 20 parts by weight, and even more preferably 10 parts by weight.
[0388] <Acid Diffusion Control Agent>
[0389] In the radiosensitive linear composition of the present invention, the third composition may contain an acid diffusion control agent. The acid diffusion control agent is a component that controls the diffusion length of acid generated from the photoacid generator (B-3) through exposure. By incorporating the acid diffusion control agent into the third composition, the diffusion length of the acid can be appropriately controlled, resulting in good pattern development. Furthermore, by incorporating the acid diffusion control agent, improved development adhesion and chemical resistance can be achieved, which is preferable in this respect.
[0390] As an acid diffusion control agent, any basic compound used in chemically amplified resists can be selected. Examples of basic compounds include fatty acid amines, aromatic amines, heterocyclic amines, quaternary ammonium hydroxide, and quaternary ammonium salts of carboxylic acids. Specific examples of basic compounds include compounds described in paragraphs
[0128] to
[0147] of Japanese Patent Application Publication No. 2011-232632. As an acid diffusion control agent, at least one selected from the group consisting of aromatic amines and heterocyclic amines is preferably used.
[0391] Examples of aromatic amines and heterocyclic amines include: aniline, N-methylaniline, N-ethylaniline, N-propylaniline, N,N-dimethylaniline, 2-methylaniline, 3-methylaniline, 4-methylaniline, ethylaniline, propylaniline, trimethylaniline, 2-nitroaniline, 3-nitroaniline, 4-nitroaniline, 2,4-dinitroaniline, 2,6-dinitroaniline, 3,5-dinitroaniline, N,N-dimethyltoluidine, and other aniline derivatives; imidazoles, 4-methylimidazolium, 4-methyl-2-phenylimidazolium, benzimidazole, 2-phenylbenzimidazole, triphenylimidazolium, and other imidazole derivatives; and pyrroles, 2H-pyrrole, 1-methylpyrrole, 2,4-dimethylpyrrole, 2,5-diphenylimidazolium, etc. Pyrrole derivatives such as methylpyrrole and N-methylpyrrole; pyridine, methylpyridine, ethylpyridine, propylpyridine, butylpyridine, 4-(1-butylpentyl)pyridine, dimethylpyridine, trimethylpyridine, triethylpyridine, phenylpyridine, 3-methyl-2-phenylpyridine, 3-methyl-4-phenylpyridine, 4-tert-butylpyridine, diphenylpyridine, benzylpyridine, methoxypyridine, butoxypyridine, dimethoxypyridine, 1-methyl-2-pyridone, 4-pyrrolidinylpyridine, 1-methyl-4-phenylpyridine, 2-(1-ethylpropyl)pyridine, aminopyridine, dimethylaminopyridine, nicotine, and other pyridine derivatives, as well as compounds described in Japanese Patent Application Publication No. 2011-232632.
[0392] From the viewpoint of fully obtaining the improved drug resistance effect brought about by the formulation of the acid diffusion control agent when it is incorporated into the radiosensitive linear composition, the lower limit of its content relative to 100 parts by weight of polymer (A) incorporated in the third composition is preferably 0.005 parts by weight, more preferably 0.01 parts by weight. Furthermore, the upper limit of the content of the acid diffusion control agent relative to 100 parts by weight of polymer (A) is preferably 10 parts by weight, more preferably 5 parts by weight.
[0393] <Other Ingredients>
[0394] The radiosensitive linear composition of the present invention may contain components other than those described above (other components). Examples of other components include: curing accelerators, multifunctional polymerizable compounds (multifunctional (meth)acrylates, etc.), surfactants (fluorinated surfactants, silicone surfactants, nonionic surfactants, etc.), polymerization inhibitors, antioxidants, chain transfer agents, etc. The proportions of these components may be appropriately selected according to each component without impairing the effects of the present disclosure.
[0395] <Solvent (E)>
[0396] The radiosensitive linear composition of the present invention preferably contains a solvent (E). As the solvent (E), it is preferably an organic solvent that dissolves each component formulated in the radiosensitive linear composition and does not react with each component.
[0397] Specific examples of solvents include: alcohols such as methanol, ethanol, isopropanol, butanol, octanol, and 1-methoxy-2-propanol; esters such as ethyl acetate, butyl acetate, ethyl lactate, γ-butyrolactone, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, methyl 3-methoxypropionate, and ethyl 3-ethoxypropionate; ethers such as ethylene glycol monobutyl ether, propylene glycol monomethyl ether, ethylene diethylene glycol monomethyl ether, ethylene diethylene glycol ethyl methyl ether, dimethylene glycol dimethyl ether, and diethylene glycol ethyl methyl ether; amides such as dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; and aromatic hydrocarbons such as benzene, toluene, xylene, and ethylbenzene. Among these, the solvent is preferably at least one selected from the group consisting of ethers and esters, more preferably at least one selected from the group consisting of ethylene glycol alkyl ether acetates, diethylene glycols, propylene glycol monoalkyl ethers and propylene glycol monoalkyl ether acetates.
[0398] <Preparation Method of Radiosensitive Linear Composition>
[0399] The radiosensitive linear composition can be prepared, for example, by mixing a polymer (A), a radiosensitive linear compound (B), a polymerized ionic liquid (C), and any other components as needed, in a predetermined ratio. The radiosensitive linear composition is preferably filtered after mixing using, for example, a filter with a pore size of approximately 0.05 μm to 0.4 μm. The solids concentration of the radiosensitive linear composition (the proportion of the total mass of components other than the solvent in the total mass of the radiosensitive linear composition) can be appropriately selected considering viscosity or volatility. The solids concentration of the radiosensitive linear composition is preferably in the range of 5% to 60% by mass, more preferably 10% to 55% by mass, and even more preferably 12% to 50% by mass. If the solids concentration is 5% by mass or more, sufficient film thickness can be ensured when coating the radiosensitive linear composition onto a substrate. Furthermore, if the solids concentration is 60% by mass or less, the film thickness will not become excessive, thereby moderately increasing the viscosity of the radiosensitive linear composition and ensuring good coatability.
[0400] Patterns (hardened films) and their manufacturing methods
[0401] The pattern (hardened film) of the present invention can be formed from the aforementioned radiosensitive linear composition. The radiosensitive linear composition has high radiation sensitivity and good pattern-forming properties. Furthermore, by using the aforementioned radiosensitive linear composition, a pattern (hardened film) that exhibits high adhesion to the substrate after development, has high capacitance, and good chemical resistance can be formed.
[0402] When manufacturing a pattern (hardening film), a positive or negative hardening film can be formed depending on the type of radiosensitive linear compound (B) by using the aforementioned radiosensitive linear composition. The pattern (hardening film) can be manufactured using the aforementioned radiosensitive linear composition, for example by a method comprising steps 1 to 4 below.
[0403] (Step 1) Step of forming a gate insulating film by coating a linearly inductive composition onto a substrate.
[0404] (Step 2) The step of irradiating at least a portion of the coating with radiation.
[0405] (Step 3) The step of developing the coating film irradiated with the radiation to form a pattern.
[0406] The following is a detailed description of each process.
[0407] [Process 1: Coating Process]
[0408] In this process, the radiosensitive linear composition is coated onto the surface on which the film is formed (hereinafter also referred to as the "film-forming surface"). Preferably, the solvent is removed by heat treatment (pre-baking), thereby forming a coating on the film-forming surface. The material of the film-forming surface is not particularly limited. In this invention, in order to form a gate insulating film, a coating is formed on a substrate containing glass or resin, on a substrate on which gate electrodes (scan signal lines) are formed.
[0409] Examples of coating methods for the radiosensitive linear composition include spraying, roller coating, spin coating, slot die coating, rod coating, and inkjet coating. Spin coating, slot die coating, or rod coating are preferred. Pre-baking conditions vary depending on the type and proportion of each component in the radiosensitive linear composition; for example, baking at 60°C to 130°C for 0.5 to 10 minutes. The film thickness formed (i.e., the film thickness after pre-baking) is preferably 0.1 μm to 12 μm. For the radiosensitive linear composition coated on the film-forming surface, vacuum drying (VCD) can also be performed before pre-baking.
[0410] [Process 2: Exposure Process]
[0411] In this process, at least a portion of the coating film formed in step 1 is irradiated with radiation. At this time, the coating film is irradiated with radiation through a mask having a predetermined pattern, thereby forming a patterned hardened film. The pattern of the mask corresponds to the pattern of the gate insulating film. Examples of radiation include ultraviolet light, far ultraviolet light, visible light, X-rays, and charged particle beams such as electron beams. Among these, ultraviolet light is preferred, such as gamma rays (wavelength 436 nm) and i-rays (wavelength 365 nm). The exposure dose of the radiation is preferably 0.1 J / m². 2 ~20,000 J / m 2 .
[0412] [Process 3: Developing Process]
[0413] In this process, the coating film irradiated with radiation in step 2 is developed. Specifically, the coating film irradiated with radiation in step 2 is subjected to positive development, which removes the irradiated portion by developing with a developing solution, or negative development, which removes the unirradiated portion by developing with a developing solution. Examples of developing solutions include aqueous solutions of alkalis (alkaline compounds). Examples of alkalis include sodium hydroxide, tetramethylammonium hydroxide, and the alkalis exemplified in paragraph
[0127] of Japanese Patent Application Publication No. 2016-145913. The alkali concentration of the aqueous solution is preferably 0.1% to 5% by mass from the viewpoint of obtaining adequate developability. Suitable developing methods include, for example, the immersion method, the shaking immersion method, and the spraying method. The developing time also varies depending on the composition of the composition, for example, from 30 seconds to 120 seconds. Furthermore, it is preferable to perform a rinsing treatment based on running water rinsing on the patterned coating film after the developing process.
[0414] [Process 4: Heating Process]
[0415] In this process, the developed coating from step 3 is heated (post-baking). Post-baking can be performed using a heating device such as an oven or a hot plate. Regarding the post-baking conditions, the heating temperature is, for example, 120°C to 250°C. For example, when heating is performed on a hot plate, the heating time is 5 minutes to 40 minutes; when heating is performed in an oven, the heating time is 10 minutes to 80 minutes. Performing this process as described above allows a hardened film with the desired pattern to be formed on the substrate. Furthermore, in this process, to prevent degradation of the gate electrode, heating can also be performed in an inert gas environment such as nitrogen or argon.
[0416] Semiconductor Components
[0417] The pattern (hardened film) formed using the aforementioned linearly induced emission composition can be used in semiconductor devices. The pattern (hardened film) can suitably serve as a gate insulating film disposed between the semiconductor layer and the gate electrode in a semiconductor device having a semiconductor layer and a gate electrode. Besides using the pattern (hardened film) formed by the linearly induced emission composition of the present invention as a gate insulating film, the semiconductor device can also be manufactured using known methods. Examples of semiconductor devices include transistors such as organic electrochemical transistors (OECT), integrated circuits (ICs), and large-scale integrated circuits (LSIs). Furthermore, the pattern (hardened film) can also be used as an interlayer insulating film, protective film, planarization film, etc., of semiconductor devices.
[0418] Display Devices
[0419] The semiconductor element of the present invention can be suitably used in display devices. That is, the pattern (hardening film) of the present invention can be suitably used in display devices. Examples of such display devices include: liquid crystal display devices, organic EL display devices, light-emitting diode (LED) display devices, quantum dot light-emitting display devices, etc.
[0420] Wearable devices
[0421] The semiconductor element of the present invention is suitable for use in wearable devices such as external devices, surface devices, and internal devices. That is, the pattern (hardening film) of the present invention is suitable for use in wearable devices. Furthermore, specifically, the pattern (hardening film) of the present invention can be used in wearable devices for flexible wiring, flexible substrates, frames, cover components, cables, sensors, etc.
[0422] Electronic Skin Devices
[0423] Electronic skin devices are soft and flexible devices that mimic the functions of human skin and can be suitably used in medical implants, robotic sensor skin, and wearable devices.
[0424] Biosensors
[0425] The semiconductor element of this invention is suitable for use in biosensors. That is, the pattern (hardened film) of this invention is suitable for use in biosensors. A biosensor is a sensor that detects the activities of living organisms, particularly animals. More specifically, examples include sensors that convert information such as body temperature, electrocardiogram, electromyogram, blood pressure, heart rate, cardiac output, blood glucose level, blood oxygen concentration, respiratory rate, and vein shape of humans and other animals into electrical or optical signals. Examples of biosensors include non-contact, touch-sensitive, patch, and wearable types.
[0426] Neuromorphic Devices
[0427] The semiconductor element of this invention can be used as a neuromorphic device and is highly suitable as an artificial synapse. That is, the pattern (hardening membrane) of this invention is suitable for use in neuromorphic devices. A neuromorphic device is a component that mimics the human brain (artificially mimicking the relationship between neurons and synapses in the human brain) through a neural network.
[0428] Example
[0429] The present invention will be specifically described below through examples, but the present invention is not limited to these examples. Unless otherwise specified, "parts" and "%" in the following examples refer to mass.
[0430] [Weight-average molecular weight (Mw) and number-average molecular weight (Mn)]
[0431] The Mw and Mn of the polymer were determined by the following method.
[0432] • Determination method: Gel permeation chromatography (GPC)
[0433] • Device: GPC-101 manufactured by Showa Denko Co., Ltd.
[0434] • GPC tubing: Combining GPC-KF-801, GPC-KF-802, GPC-KF-803 and GPC-KF-804 manufactured by Shimadzu GLC (stock).
[0435] • Mobile phase: Tetrahydrofuran
[0436] • Column temperature: 40℃
[0437] • Flow rate: 1.0 mL / min
[0438] • Sample concentration: 1.0% by mass
[0439] • Sample injection volume: 100 μL
[0440] • Detector: Differential refractometer
[0441] • Standard reference material: Monodisperse polystyrene
[0442] [Glass transition temperature (Tg)]
[0443] The glass transition temperature (Tg) is determined by the following method.
[0444] • Measurement method: Differential Scanning Calorimetry (DSC)
[0445] • Device: TAQ2000 manufactured by TA Instruments
[0446] • Sample tray: aluminum
[0447] • Measurement method: After placing the sample, equilibrate it at 383 K for 30 minutes, then cool it to 183 K and heat it to 453 K. Repeat this heating and cooling cycle three times at a rate of 10 K / min. The glass transition temperature (Tg) is set as the midpoint of the specific heat step during cooling.
[0448] <Monomers constituting polymer (A)>
[0449] The monomers used in the synthesis of polymer (A) are described below.
[0450] (Provide a single volume of structural unit (I))
[0451] MI: Maleimide
[0452] MA: Methacrylic acid
[0453] (Provide a single volume of structural unit (II))
[0454] GMA: Glycidyl methacrylate
[0455] ·OXMA: OXE-30 (manufactured by Osaka Organic Chemicals Co., Ltd.), methyl methacrylate (3-ethyloxetane-3-yl)
[0456] M100: 3,4-epoxycyclohexyl methyl methacrylate
[0457] (Provide a single volume of structural unit (III))
[0458] STMS: Styrene-trimethoxysilane
[0459] (Provide a single volume of structural unit (IV))
[0460] ST: Styrene
[0461] MMA: Methyl methacrylate
[0462] AM-1:
[0463] [Chemistry 21]
[0464]
[0465] <Synthesis of monomers constituting polymerized ionic liquid (C)>
[0466] [Synthetic Example C1] ILMC: Synthesis of 1-[2-(2-(methacryloyloxy)ethoxy)ethoxy]ethyl]-3-methylimidazolium bis(trifluoromethylsulfonyl)imide
[0467] 23.7 g of 2-[2-(chloroethoxy)-ethoxy]ethanol (manufactured by Tokyo Chemical Industry Co., Ltd.) was added dropwise to 60 mL of anhydrous methanol. The resulting solution was then added dropwise to a solution obtained by dissolving 10.0 g of N-methylimidazolium (manufactured by Tokyo Chemical Industry Co., Ltd.) in 25 mL of methanol at 0-1°C. The reaction mixture was stirred at 0-1°C for 1 hour, at 20°C for 12 hours, at 40°C for 24 hours, and finally at 55°C for 30 hours. The solvent was removed at 50°C under reduced pressure, and the remaining viscous liquid was extracted with anhydrous acetonitrile (3 times × 50 mL) while vigorous stirring. The product was dried at 50°C / 1 mmHg for 6 hours. A small amount of yellow, viscous liquid 1-[2-(2-(2-hydroxyethoxy)ethoxy)ethyl]-3-methylimidazolium chloride was obtained.
[0468] Next, 6.25 g of distilled methacryloyl chloride (manufactured by Tokyo Chemical Industry Co., Ltd.) was dissolved in 10 mL of anhydrous acetonitrile and placed in a round-bottom flask, which was then cooled to 0°C to 1°C using an ice bath. A solution of 10.0 g of 1-[2-(2-(2-hydroxyethoxy)ethoxy)ethyl]-3-methylimidazolium chloride dissolved in 20 mL of acetonitrile was slowly added dropwise to the cooled methacryloyl chloride solution, and the mixture was stirred at 0°C to 1°C for 1.5 hours while gently mixing. The ice bath was then removed, and the reaction mixture was allowed to react at 20°C for 5 hours, and finally at 40°C for 12 hours. The resulting solution was washed with diethyl ether (5 times × 15 mL) to remove excess methacryloyl chloride. After evaporating the residual ether, the reaction mixture was dissolved in dichloromethane and precipitated in ethyl acetate. The product of 4-methoxyphenol with added catalyst was then dried at 25°C / 14 mmHg for 2 hours, and then dried at 25°C / 1-2 mmHg for 2 hours to obtain 1-[2-(2-(2-(methacryloyloxy)ethoxy)ethoxy)ethyl]-3-methylimidazolium chloride. 9.04 g of lithium bis(trifluoromethanesulfonyl)imide (manufactured by Tokyo Chemical Industry Co., Ltd.) was dissolved in 10 mL of distilled water and added dropwise to a solution of 9.09 g of 1-[2-(2-(2-(methacryloyloxy)ethoxy)ethoxy)ethyl]-3-methylimidazolium chloride in 15 mL of water. The mixture was stirred at 25°C for 2 hours to obtain an oily precipitate. The upper aqueous layer was removed, and the oily precipitate was dissolved again in 90 mL of dichloromethane. The dichloromethane solution was washed three times with 30 mL of water and dried with anhydrous MgSO4. Magnesium sulfate was filtered to remove the dichloromethane under reduced pressure at -30°C, followed by drying at 30°C / 1 mmHg for 2 hours. A small amount of amber-colored, transparent liquid was obtained as the final product (yield: 60%).
[0469] [Synthetic Example C2] ILMA: Synthesis of 1-Butyl-3-methylimidazolium-1-[3-(methacryloyloxy)propylsulfonyl]-1-(trifluoromethanesulfonyl)imide
[0470] Potassium 3-(methacryloyloxy)propane-1-sulfonate (1) (manufactured by Tokyo Chemical Industry Co., Ltd.) 15.0 g was suspended in 25 mL of anhydrous tetrahydrofuran under environmental protection. 1.7 mL of N,N-dimethylformamide was injected as a catalyst using a syringe. The reaction flask was cooled to 0-1°C, and excess thionyl sulfate (manufactured by Tokyo Chemical Industry Co., Ltd.) 39.9 g was added dropwise while stirring. The reaction was carried out at 0-1°C for 1 hour, then at room temperature for 12 hours. The resulting suspension was carefully injected into 200 mL of ice water. The upper aqueous layer was removed, and the lower oily organic layer was diluted with 80 mL of dichloromethane. The dichloromethane solution was washed with water 6 times × 25 mL, and then dried with anhydrous magnesium sulfate. MgSO4 was filtered, and the dichloromethane was evaporated under reduced pressure and below 30°C. Finally, the obtained yellow transparent liquid was dried at 25℃ / 12 mmHg for 2 hours, and then dried at 25℃ / 1-2 mmHg for 8 hours to obtain chlorosulfonyl propyl methacrylate.
[0471] 7.3 g of trifluoromethanesulfonamide (manufactured by Tokyo Chemical Industry Co., Ltd.) was placed in a flask, and 10.9 g of distilled anhydrous triethylamine (manufactured by Tokyo Chemical Industry Co., Ltd.) was added while stirring. The reaction mixture was then diluted with 40 mL of anhydrous tetrahydrofuran, and the resulting colorless solution was cooled to 0°C using an ice bath. 11.1 g of chlorosulfonyl methacrylate was added dropwise to the cooled tetrahydrofuran solution relative to the trifluoromethanesulfonamide and triethylamine in the anhydrous tetrahydrofuran solution. The reaction was carried out at 0°C for 1 hour, and then at room temperature for 1 hour. The precipitate was removed by filtration, and the filtrate was gently evaporated at room temperature. The remaining yellow, transparent liquid was redissolved in 90 mL of dichloromethane. The dichloromethane solution was washed four times with 35 mL of water, and dried over anhydrous magnesium sulfate. Anhydrous magnesium sulfate was filtered, and 4-methoxyphenol was added as a catalyst to evaporate dichloromethane under reduced pressure and below 30°C. The remaining yellow transparent liquid was then dried under vacuum at 35°C / 12 mmHg for 1 hour using phosphorus pentoxide placed in a special flask, followed by further drying under vacuum at 35°C / 1-2 mmHg for 3 hours to obtain triethylammonium 1-[3-(methacryloyloxy)propylsulfonyl]-1-(trifluoromethanesulfonyl)imide.
[0472] 30.0 g of triethylammonium 1-[3-(methacryloyloxy)propylsulfonyl]-1-(trifluoromethanesulfonyl)imide was dissolved in 45 mL of anhydrous tetrahydrofuran (THF) and stirred at room temperature under an inert gas atmosphere. 1.3 g of lithium hydride (manufactured by Sigma-Aldrich) was added in a single batch, and the resulting suspension was stirred overnight at 30°C. Unreacted lithium hydride was then removed by filtration, and the solution was concentrated under reduced pressure to obtain a yellow viscous liquid. The product was washed with hexane (3 times × 40 mL), dried at 25°C / 15 mmHg, and finally crystallized in anhydrous dichloromethane (DCM) to obtain a white crystalline powder. The powder was filtered under an inert gas environment and dried overnight at 25°C / 1 mmHg to obtain lithium 1-[3-(methacryloyloxy)propylsulfonyl]-1-(trifluoromethanesulfonyl)imide.
[0473] 32.50 g of lithium 1-[3-(methacryloyloxy)propylsulfonyl]-1-(trifluoromethanesulfonyl)imide was added dropwise to 150 mL of Milli-Q water, and simultaneously stirred at room temperature with 60 mL of an aqueous solution of 21.10 g of 1-butyl-3-methylimidazolium bromide (manufactured by Tokyo Chemical Industry Co., Ltd.). The resulting emulsion was stirred continuously at room temperature for 2 hours. The organic solvent was extracted from the reaction mixture using dichloromethane. The mixture was washed with water (4 times × 30 mL) and dried with anhydrous magnesium sulfate. The anhydrous magnesium sulfate was filtered, a catalyst amount of 4-methoxyphenol was added, dichloromethane was removed at room temperature under reduced pressure, and the mixture was dried at 25 °C / 0.08 mmHg for 8 hours. A pale yellow, transparent liquid was obtained as the final product (yield: 30%).
[0474] <Synthesis of Polymer (A)>
[0475] [Synthesis Example 1] Synthesis of Polymer (A-1)
[0476] Ten parts of 2,2'-azobis(2,4-dimethylpentanonitrile) (ADVN) and 200 parts of propylene glycol monomethyl ether acetate were charged into a flask including a cooling tube and a stirrer. Then, 20 parts of MA, 30 parts of GMA, 20 parts of OXMA, and 30 parts of ST were added. After nitrogen purging, the temperature of the solution was raised to 70°C while stirring slowly, and this temperature was maintained for 5 hours, thereby obtaining a polymer solution containing polymer (A-1). The solid content concentration of the polymer solution was 34% by mass, the Mw of polymer (A-1) was 10,500, and the molecular weight distribution (Mw / Mn) was 2.2.
[0477] [Synthesis Examples 2-6] Synthesis of Polymers (A-2) to (A-6)
[0478] Using the types and proportions (parts by mass) of each component shown in Table 1, except that polymer solutions containing polymers (A-2) to (A-6) having the same solid component concentration as polymer (A-1) were obtained using the same method as in Synthesis Example 1. Furthermore, in Table 1, "-" indicates that the corresponding component was not used.
[0479] [Table 1]
[0480]
[0481] [Synthesis Example 7] Synthesis of Polymer (A-7)
[0482] 24 parts of propylene glycol monomethyl ether were added to a flask including a cooling tube and a stirrer, followed by 39 parts of methyltrimethoxysilane and 18 parts of 3-methacryloyloxypropyltrimethoxysilane. The mixture was heated until the solution temperature reached 60°C. After reaching 60°C, 0.1 parts of formic acid and 19 parts of water were added, and the solution temperature was raised to 75°C while stirring slowly. This temperature was maintained for 2 hours. After cooling to 45°C, 28 parts by mass of trimethyl orthoformate were added as a dehydrating agent, and the mixture was stirred for 1 hour. The solution temperature was then lowered to 40°C, and evaporation was carried out while maintaining the temperature to remove water and methanol produced during hydrolysis and condensation, thereby obtaining a polymer solution containing polymer (A-7). The solid content concentration of the polymer solution was 35% by mass, and the weight average molecular weight (Mw) of polymer (A-7) was 1,800, with a molecular weight distribution (Mw / Mn) of 2.2.
[0483] [Synthesis Example 8] Synthesis of Polymer (A-8)
[0484] Under a dry nitrogen atmosphere, 80 moles of compound (AM-1), 5 moles of 1,3-bis(3-aminopropyl)tetramethyldisiloxane, and 100 moles of 4,4'-oxyphthalic anhydride were dissolved in dehydrated N-methyl-2-pyrrolidone (NMP) and reacted at 40°C for 1 hour. A solution of 30 moles of 3-aminophenol as a capping agent was prepared in NMP and added to the solution, and the reaction was carried out at 40°C for 2 hours. Subsequently, 200 moles of N,N-dimethylformamide dimethyl acetal were added relative to the amount of tetracarboxylic acid dianhydride added, and the reaction was carried out at 40°C for 6 hours. After cooling the reaction solution to room temperature, the solution was added to a large volume of distilled water, and the precipitate was recovered by filtration. After washing three times with water, the solution was vacuum dried at 80°C for 20 hours to obtain polymer (A-8) powder.
[0485] <Synthesis of Polymerized Ionic Liquids (C)>
[0486] [Synthesis Example 9] Synthesis of Polymerized Ionic Liquid (C-1)
[0487] 1.02 g of poly(ethylene glycol) methyl ether methacrylate (Mn=500 g / mol) (manufactured by Sigma-Aldrich) and 0.23 g of ILMA were dissolved in 3.00 g of anhydrous N,N-dimethylformamide (manufactured by Tokyo Chemical Industry Co., Ltd.). 0.87 mg of 2,2'-azobis(isobutyronitrile) (manufactured by Tokyo Chemical Industry Co., Ltd.) and 7.40 mg of 4-cyano-4-(phenylcarbonothioylthio)pentanoic acid (Sigma-Aldrich) were added, and the mixture was stirred while mixing until the solution became clear. The solution was then purged with argon in a three-necked flask equipped with a stir bar and heated at 60°C for 15 hours. The obtained viscous solution was cooled to room temperature (RT) and diluted with N,N-dimethylformamide to precipitate it in excess diethyl ether. The copolymer was redissolved in ultrapure water and dialyzed against water for 2 days. 40 mg of 4-methoxyphenol was added to the resulting aqueous solution, and the mixture was dried in an oven filled with phosphorus pentoxide at 50 °C / 0.08 mmHg for 12 hours to obtain a pink viscous liquid.
[0488] 0.50 g of a pink viscous liquid, 0.46 g of 2-phenylethyl methacrylate (manufactured by Tokyo Chemical Industry Co., Ltd.), and 0.40 mg of 2,2'-azobis(isobutyronitrile) were dissolved in 2.87 g of anhydrous N,N-dimethylformamide. The mixture was purged with argon gas in a three-necked flask with a stir bar and heated at 60 °C for 15 hours. The reaction was then stopped by rapid cooling with liquid nitrogen. The resulting viscous solution was diluted with dichloromethane, precipitated in excess diethyl ether, and dried at 25 °C / 0.1 mbar for 24 hours. Subsequently, it was dried in an oven filled with phosphorus pentoxide at 50 °C / 0.1 mbar for 24 hours to obtain a white, waxy solid (C-1) (yield: 40%, weight average molecular weight: 100,000, glass transition temperature: -51 °C). The poly(ethylene glycol) methyl ether methacrylate, ILMA and 2-phenylethyl methacrylate used in the polymerized ionic liquid (C-1) are in a mass ratio of 42:10:48.
[0489] [Synthesis Example 10] Synthesis of Polymerized Ionic Liquid (C-2)
[0490] 1.02 g of poly(ethylene glycol) methyl ether methacrylate (Mn = 500 g / mol) and 0.23 g of ILMC were dissolved in 3.00 g of anhydrous N,N-dimethylformamide. 0.87 mg of 2,2'-azobis(isobutyronitrile) and 7.40 mg of 4-cyano-4-(phenylthiocarbamoylthio)valerate were added, and the mixture was stirred continuously until the solution became clear. The solution was then purged with argon in a three-necked flask with a stir bar and heated at 60 °C for 15 hours. The resulting viscous solution was cooled to RT and diluted with N,N-dimethylformamide to precipitate it in excess diethyl ether. The copolymer was redissolved in ultrapure water and dialyzed against water for 2 days. 40 mg of 4-methoxyphenol was added to the resulting aqueous solution, and the mixture was dried in an oven filled with phosphorus pentoxide at 50 °C / 0.1 mbar for 12 hours to obtain a pink viscous liquid.
[0491] 0.50 g of a pink viscous liquid, 0.46 g of 2-phenylethyl methacrylate, and 0.40 mg of 2,2'-azobis(isobutyronitrile) were dissolved in 2.87 g of anhydrous N,N-dimethylformamide. The solution was purged with argon in a three-necked flask with a stir bar and heated at 60 °C for 15 hours. The reaction was then stopped by rapid cooling with liquid nitrogen. The resulting viscous solution was diluted with dichloromethane, precipitated in excess diethyl ether, and dried at 25 °C / 0.1 mbar for 24 hours. Subsequently, it was dried in an oven filled with phosphorus pentoxide at 50 °C / 0.1 mbar for 24 hours to obtain a pink, waxy solid (C-2) (yield: 40%, weight average molecular weight: 100,000, glass transition temperature: -53 °C). The poly(ethylene glycol) methyl ether methacrylate, ILMC and 2-phenylethyl methacrylate used in the polymerized ionic liquid (C-2) are in a mass ratio of 42:10:48.
[0492] [Synthetic Example 11] Synthesis of Polymerized Ionic Liquid (C-3)
[0493] 1.02 g of poly(ethylene glycol) methyl ether methacrylate (Mn = 500 g / mol), 0.23 g of ILMC, and 1.2 g of 2-phenylethyl methacrylate were dissolved in 8.00 g of anhydrous N,N-dimethylformamide. 8.05 mg of 2,2'-azobis(isobutyronitrile) was added, and the mixture was stirred continuously until the solution became clear. After purging with argon in a three-necked flask with a stir bar, the solution was heated at 60 °C for 15 hours. The resulting viscous solution was cooled to room temperature and diluted with N,N-dimethylformamide to precipitate it in excess diethyl ether. The copolymer was then redissolved in ultrapure water and dialyzed against water for 2 days. 40 mg of 4-methoxyphenol was added to the obtained aqueous solution, and the mixture was dried in an oven filled with phosphorus pentoxide at 50 °C / 0.1 mbar for 12 hours to obtain a pink viscous liquid (C-3) (yield: 60%, weight average molecular weight: 100,000, glass transition temperature: -45 °C). The poly(ethylene glycol) methyl ether methacrylate, ILMC, and 2-phenylethyl methacrylate used in the polymerized ionic liquid (C-3) were in a mass ratio of 42:10:48.
[0494] [Synthesis Example 12] Synthesis of Polymerized Ionic Liquid (C-4)
[0495] 0.23 g of ILMC and 1.2 g of 2-phenylethyl methacrylate were dissolved in 8.00 g of anhydrous N,N-dimethylformamide. 7.75 mg of 2,2'-azobis(isobutyronitrile) was added, and the mixture was stirred continuously until the solution became clear. After purging with argon in a three-necked flask with a stir bar, the solution was heated at 60 °C for 15 hours. The resulting viscous solution was cooled to room temperature and diluted with N,N-dimethylformamide to precipitate in excess diethyl ether. The copolymer was redissolved in ultrapure water and dialyzed against water for 2 days. 40 mg of 4-methoxyphenol was added to the resulting aqueous solution, and the mixture was dried in an oven filled with phosphorus pentoxide at 50 °C / 0.1 mbar for 12 hours to obtain a pink viscous liquid (C-4) (yield: 60%, weight average molecular weight: 100,000, glass transition temperature: 5 °C). The polymerized ionic liquid (C-4) used has an ILMC to 2-phenylethyl methacrylate ratio of 16:84 (mass ratio).
[0496] [Synthetic Example 13] Synthesis of Polymerized Ionic Liquid (C-5)
[0497] 2.0 g of poly(methylhydrosiloxane) (manufactured by Sigma-Aldrich) and 5.0 g of 5-bromo-1-pentene (manufactured by Tokyo Chemical Industry Co., Ltd.) were added to a three-necked flask equipped with a stirrer. The reaction vessel was flushed with argon for 20 minutes, and 30 μL of a platinum (O)-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex solution (manufactured by Sigma-Aldrich) was added. The reaction mixture was stirred at 60 °C for 15 hours. After the reaction was complete, the solvent was removed, and the mixture was allowed to precipitate in the remaining methanol to obtain a brown, oily poly(methylhydrosiloxane)-grafted 5-bromo-1-pentene.
[0498] A solution obtained by adding 30 mL of dichloromethane to 2.4 g of polymethylhydrosiloxane-grafted-5-bromo-1-pentene, along with 1.03 g of 1-methylimidazole (manufactured by Tokyo Chemical Industry Co., Ltd.), was added to a two-necked round-bottom flask equipped with a stirrer. The reaction was stirred at 70°C for 72 hours. After the reaction was complete, the solvent was removed under reduced pressure, the mixture was washed three times with dichloromethane, and then vacuum dried at 40°C to obtain polymethylhydrosiloxane-grafted-5-imidazolium-1-pentene bromide.
[0499] In a round-bottom flask with a stirrer, a solution was prepared by adding 20 mL of ultrapure water to 1.0 g of polymethylhydrosiloxane-grafted-5-imidazolium-1-pentene bromide, and then adding 1.3 g of lithium bis(trifluoromethanesulfonyl)imide (manufactured by Tokyo Chemical Industry Co., Ltd.). The mixture was stirred at room temperature for 7 days. The precipitate was then washed three times with ultrapure water and vacuum dried at 40°C to obtain a viscous liquid (C-5) (weight average molecular weight: 3,000, Tg: -40°C).
[0500] [Synthesis Example 14] Synthesis of Polymer (CC-1)
[0501] 0.23 g of ILMC and 3.9 g of phenyl methacrylate (manufactured by Tokyo Chemical Industry Co., Ltd.) were dissolved in 8.00 g of anhydrous N,N-dimethylformamide. 7.75 mg of 2,2'-azobis(isobutyronitrile) was added, and the mixture was stirred continuously until the solution became clear. Argon purging was performed in a three-necked flask with a stir bar, and the solution was heated at 60 °C for 15 hours. The resulting viscous solution was cooled to room temperature and diluted with N,N-dimethylformamide to precipitate in excess diethyl ether. The copolymer was redissolved in ultrapure water and dialyzed against water for 2 days. 40 mg of 4-methoxyphenol was added to the resulting aqueous solution, and the mixture was dried in an oven filled with phosphorus pentoxide at 50 °C / 0.1 mbar for 12 hours to obtain a pink viscous liquid (CC-1) (yield: 60%, weight average molecular weight: 100,000, glass transition temperature: 45 °C).
[0502] <Preparation of Radiosensitive Linear Compositions>
[0503] The following shows the polymer (A), the radiosensitive linear compound (B), the polymerized ionic liquid (C), the bonding agent (D), and the polymeric monomer (X1) used in the preparation of the radiosensitive linear composition.
[0504] (Polymer (A))
[0505] A1~A8: Polymers (A-1) to (A-8) synthesized in Synthetic Examples 1 to 8.
[0506] (Radiosensitive linear compound (B))
[0507] B-1: A condensation product of 4,4'-[1-[4-[1-[4-hydroxyphenyl]-1-methylethyl]phenyl]ethylidene]bisphenol (1.0 mol) and 1,2-naphthoquinone diazido-5-sulfonyl chloride (2.0 mol).
[0508] B-2: Irgacure PAG121 (manufactured by BASF)
[0509] B-3: Irgacure OXE-01 (manufactured by BASF)
[0510] (Polymerized ionic liquid (C))
[0511] C-1 to C-5: Polymerized ionic liquids (C-1) to (C-5) synthesized in Synthetic Examples 9 to 13.
[0512] CC-1: The polymer synthesized in Example 14 (CC-1)
[0513] (Close contact agent (D))
[0514] D-1: 3-Glycidoxypropyltrimethoxysilane
[0515] (Polymerized monolith (X1))
[0516] X-1: Kayarad DPHA (manufactured by Nippon Kayaku Co., Ltd.)
[0517] <Preparation of Radiosensitive Linear Compositions>
[0518] [Example 1]
[0519] A mixture of 20 parts of a radiosensitive linear compound (B-1), 100 parts of a polymerized ionic liquid (C-1), and 5 parts of a bonding agent (D-1) was dissolved in propylene glycol monomethyl ether acetate as a solvent, with a solid content concentration of 20% by mass, relative to 100 parts of polymer (A-1) (solid component). The mixture was then filtered using a 0.2 μm membrane filter to prepare the radiosensitive linear composition.
[0520] [Examples 2-14, Comparative Example 1]
[0521] The radiosensitive linear composition was prepared using the same method as in Example 1, except that the components shown in Table 2 and their proportions (parts by mass) were used. In Table 2, "-" indicates that the corresponding component was not used.
[0522] The prepared radiosensitive linear composition was evaluated as follows.
[0523] [Evaluation of Pattern Formation]
[0524] Using a spinner, the radiosensitive linear composition was coated onto a silicon substrate treated with hexamethyl disilazane (HMDS) at 60°C for 60 seconds, followed by pre-baking at 110°C for 2 minutes on a hot plate to form a coating with an average thickness of 1.0 μm. A mask of arbitrary size with a line-to-space pattern of 1:1 spacing was used to irradiate the coating with a mercury lamp at 100 J / m². 2 The ultraviolet light was then applied. Following this, a 60-second development treatment was performed using a 2.38% (w / w) aqueous solution of tetramethylammonium hydroxide at 25°C, followed by a 1-minute rinse with ultrapure water. The width of the lines and spatial patterns that could be formed was then measured. Values less than 5 μm were rated "A", values greater than 5 μm were rated "B", and no patterns could be formed, resulting in a "C".
[0525] [Evaluation of capacitor Cp]
[0526] The radiosensitive linear composition was coated onto a glass substrate that had been deposited with indium tin oxide (ITO) to a thickness of 100 nm and calcined at 230°C for 30 minutes. The substrate was then pre-baked at 110°C for 2 minutes to form a 3.0 μm thick coating (formation of the coated substrate). A 5 mm ϕ Al electrode pattern was formed on the coating (gate insulating film) by vapor deposition to create a sample for dielectric constant measurement. For the substrate with the electrode pattern, the capacitance Cp was measured at a frequency of 10 kHz using an HP16451B electrode manufactured by Yokogawa-Hewlett-Packard and an HP4284A precision inductance-capacitance-resistance (LCR) meter via the capacitance voltage (CV) method. The value was set to 1 × 10⁻⁶. -9 Cases above F are designated as "A", while cases less than 1×10 are designated as "A". -9 F is 3×10 -9 F and above are designated as "B", and those less than 3×10 are designated as "B". -9 F is set to "C". In case A, the capacitance is excellent; in case B, it is rated as good; and in case C, it is rated as poor.
[0527] [Evaluation of Leakage]
[0528] Using a spinner, the radioactive linear composition was applied to a silicon substrate that had been treated with hexamethyldisilazane (HMDS) at 60°C for 60 seconds. After pre-baking at 110°C for 2 minutes on a hot plate, the substrate was visually inspected for any liquid leakage. No leakage was rated as "none," and leakage was rated as "yes."
[0529] [Table 2]
[0530]
[0531] As shown in Table 2, the radiosensitive linear compositions of Examples 1 to 14 exhibited good patterning properties. The hardened films obtained from these compositions showed good patterning and capacitance, and no exudation was observed. In contrast, Comparative Example 1 showed poor capacitance.
Claims
1. An inductively linearized composition for forming a gate insulating film, comprising: At least one polymer (A) selected from the group consisting of polymers (A1) containing structural units (I) having acid groups, siloxane polymers (A2), and polyamic acids or polyamic esters (A3). Radiosensitive linear compound (B), and Polymerized ionic liquids with a glass transition temperature below 5°C (C).
2. The inductively linearized composition for forming a gate insulating film according to claim 1, wherein, The polymerized ionic liquid (C) is a polymer having both anionic and cationic portions. The polymer is an acrylic polymer or a polysiloxane polymer.
3. The inductively linearized composition for forming a gate insulating film according to claim 1, wherein, The polymerized ionic liquid (C) comprises one or more partial structures (C1) selected from the group consisting of the following formulas (C1-1) and (C1-2). [Chemistry 1] (In equations (C1-1) and (C1-2),) Rc 11 It consists of halogen atoms or substituted or unsubstituted chain hydrocarbon groups; X m+ It is a proton or onium cation; m is an integer from 1 to 3; For bonding with other structures in polymerized ionic liquids (C).
4. The inductively linearized composition for forming a gate insulating film according to claim 3, wherein, The polymerized ionic liquid (C) is a polymer having a structural unit (X) represented by the following formula (1) or formula (2); [Chemistry 2] (In equations (1) and (2), R c1 It can be a hydrogen atom, a methyl group, or a trifluoromethyl group; R c2 It is a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, or a fluorinated alkyl group having 1 to 10 carbon atoms, or it can be bonded to a silicon atom of a different structural unit to form a siloxane bond; L c11 L c12 It is a single bond or a divalent linker; R c12 R c13 R c14 It is a single bond or a divalent organic group with 1 to 20 carbon atoms; D is the partial structure (C1) represented by the formula (C1-1) or formula (C1-2).
5. The inductively linearized composition for forming a gate insulating film according to claim 1, wherein, The polymerized ionic liquid (C) comprises one or more partial structures (C2) selected from the group consisting of the following formulas (C2-1), (C2-2), (C2-3), (C2-4) and (C2-5). [Chemistry 3] (In equations (C2-1) to (C2-5), R c22 R c23 R c24 R c25 R c26 R c28 R c30 R c31 R c32 Each is independently a substituted or unsubstituted hydrocarbon group having 1 to 20 carbon atoms, or a hydrocarbon group having -O-, -CO- or -COO- between carbon atoms; R c21 R c27 R c29 Each of the following is independently a halogen atom, a substituted or unsubstituted hydrocarbon group having 1 to 20 carbon atoms, or a group containing -O-, -CO- or -COO- between carbon atoms in the hydrocarbon group having 1 to 20 carbon atoms; s1 is 0 or 1; Y - It is an anion; For bonding with other structures in polymerized ionic liquids (C).
6. The inductively linearized composition for forming a gate insulating film according to claim 5, wherein, The polymerized ionic liquid (C) is a polymer having a structural unit (XI) represented by the following formula (3) or formula (4); [Chemistry 4] (In equations (3) and (4),) R c1 It can be a hydrogen atom, a methyl group, or a trifluoromethyl group; R c2 It is a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, or a fluorinated alkyl group having 1 to 10 carbon atoms; L c21 L c22 It is a single bond or a divalent linker; R c33 R c34 R c35 It is a single bond or a divalent organic group with 1 to 20 carbon atoms; A is a partial structure (C2) represented by the formula (C2-1), formula (C2-2), formula (C2-3), formula (C2-4) or formula (C2-5).
7. The inductively linearized composition for forming a gate insulating film according to claim 1, wherein, The polymerized ionic liquid (C) has a polyepoxide chain.
8. The inductively linearized composition for forming a gate insulating film according to claim 1, wherein, The radiosensitive linear compound (B) comprises a quinone diazide compound (B-1).
9. The inductively linearized composition for forming a gate insulating film according to claim 1, wherein, The radiosensitive linear compound (B) contains a photopolymerization initiator (B-2). The inductively linearized composition for forming the gate insulating film comprises a polymeric monomer (X).
10. The inductively linearized composition for forming a gate insulating film according to claim 1, wherein, The polymer (A1) further comprises structural units (III) having one or more groups selected from the group consisting of groups represented by the following formula (a2) and acid-dissociable groups. The radiosensitive linear compound (B) contains a photoacid generator (B-3); [Chemistry 5] (in formula (a2), R 1 R 2 and R 3 Each of the following is independently a hydrogen atom, a halogen atom, a hydroxyl group, an alkoxy group having 1 to 6 carbon atoms, or an alkyl or phenyl group having 1 to 10 carbon atoms; wherein, R 1 R 2 and R 3 At least one of them is an alkoxy group having 1 to 6 carbon atoms; " "Indicates a bond".
11. A method for manufacturing a pattern, comprising: The process of forming a coating by coating a grid insulating film with a grid-inductive linear composition according to any one of claims 1 to 10 onto a substrate; The process of irradiating at least a portion of the coating with radiation; and A process of developing the coating film irradiated with said radiation to form a pattern.
12. The method for manufacturing a pattern according to claim 11, further comprising a step of heating the pattern after the step of forming the pattern.
13. A pattern obtained by the pattern manufacturing method according to claim 11.
14. A hardened film for a gate insulating film, obtained from a gate insulating film forming inductively linearized composition according to any one of claims 1 to 10.
15. A semiconductor device comprising the hardened film according to claim 14.
16. An organic electrochemical transistor comprising the hardened film according to claim 14.
17. An organic electroluminescent display device comprising the hardened film according to claim 14.
18. A liquid crystal display device comprising the hardened film according to claim 14.
19. A micro-light-emitting diode display device, comprising the hardened film according to claim 14.
20. A quantum dot light-emitting display device, comprising the hardened film according to claim 14.
21. A wearable device comprising the hardened film according to claim 14.
22. An electronic skin device comprising the hardening membrane according to claim 14.
23. A biosensor comprising the hardened membrane according to claim 14.
24. A neuromorphic device comprising the sclerotherapy membrane according to claim 14.
Citation Information
Patent Citations
Novel color developer and recording material
JP2002332271A
Thermosetting resin composition, method for forming protective film of color filter, and protective film of color filter
JP2009073871A
Liquid crystal aligning agent and liquid crystal display element
JP2010097188A
Positive radiation-sensitive composition, interlayer insulation film and method for producing the same
JP2011232632A
Radiation-sensitive resin composition, cured film, method for forming the same, and display element
JP2014157252A