Photosensitive resin composition, resin-cured film and image display element
By using a photosensitive resin composition with a specific composition, the problems of insufficient developability and solvent resistance of resin-cured films in the prior art are solved, providing a resin-cured film with good developability, excellent solvent resistance and adhesion, suitable for color filters and image display elements of liquid crystal displays.
Patent Information
- Application Number
- CN202580029500.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2025-01-06
- Filing Date
- 2025-10-16
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies struggle to provide resin-cured films with good developability, solvent resistance, and excellent adhesion, thus affecting the performance of liquid crystal displays.
A photosensitive resin composition containing copolymer (A-1), copolymer (A-2), photopolymerization initiator (C) and solvent (D) is used. The copolymer (A-1) contains hydroxyl groups, blocked isocyanate groups and specific structural units. The resin is polymerized by light irradiation to form a resin-cured film.
It achieves resin-cured films with good developability, excellent solvent resistance and adhesion, suitable for color filters and image display elements of liquid crystal displays.
Smart Images

Figure SMS_3 
Figure SMS_4 
Figure SMS_5
Abstract
Description
Technical Field
[0001] This disclosure relates to photosensitive resin compositions, resin-cured films, and image display elements. Background Technology
[0002] In recent years, with the popularization of liquid crystal displays (LCDs), active research has been conducted on color filters used as components of LCDs, outer coatings applied to these color filters, and interlayer insulating films.
[0003] Existing technical documents
[0004] Patent documents
[0005] Patent Document 1: Japanese Patent Application Publication No. 2019-53266 Summary of the Invention
[0006] The problem that the invention aims to solve
[0007] This disclosure provides a photosensitive resin composition that exhibits good developability and yields a resin-cured film with excellent solvent resistance and adhesion. Furthermore, this disclosure provides a resin-cured film with excellent solvent resistance and adhesion, and an image display element having the resin-cured film.
[0008] Methods for solving problems
[0009] This disclosure includes the following schemes.
[0010] [1]
[0011] A photosensitive resin composition containing
[0012] copolymer (A-1), copolymer (A-2), Photopolymerization initiator (C), and Solvent (D), The above copolymer (A-1) contains hydroxyl, Structural units with blocked isocyanate groups (a) Structural unit (b) having a partial structure as shown in equation (1) below, and Structural units (c) containing acid groups, The unsaturated group equivalent of the above copolymer (A-2) is 30 to 3000 g / mol.
[0013]
[0014] (In equation (1), R) 1 (This is a divalent hydrocarbon group, where n1 represents an integer from 2 to 20.)
[0015] [2]
[0016] A photosensitive resin composition containing
[0017] copolymer (A-1), Reactive diluent (B), Photopolymerization initiator (C), and Solvent (D), The above copolymer (A-1) contains hydroxyl, Structural units with blocked isocyanate groups (a) Structural unit (b) having a partial structure as shown in equation (1) below, and Structural units with acid groups (c).
[0018]
[0019] (In equation (1), R) 1 (This is a divalent hydrocarbon group, where n1 represents an integer from 2 to 20.)
[0020] [3]
[0021] A photosensitive resin composition containing
[0022] copolymer (A-1), copolymer (A-2), Reactive diluent (B), Photopolymerization initiator (C), and Solvent (D), The above copolymer (A-1) contains hydroxyl, Structural units with blocked isocyanate groups (a) Structural unit (b) having a partial structure as shown in equation (1) below, and Structural units (c) containing acid groups, The unsaturated group equivalent of the above copolymer (A-2) is 30-3000 g / mol.
[0023] (In equation (1), R) 1 (This is a divalent hydrocarbon group, where n1 represents an integer from 2 to 20.)
[0024] [4]
[0025] According to any one of [1] to [3], R in the above formula (1) 1 It consists of hydrocarbon groups with 2 to 6 carbon atoms.
[0026] [5]
[0027] According to any one of [1] to [3], R in the above formula (1) 1 It is a hydrocarbon group with 2 or 3 carbon atoms, and n1 is an integer from 2 to 6.
[0028] [6]
[0029] According to any one of [1] to [5], the above structural unit (b) has a group represented by the following formula (2).
[0030] (In equation (2), R) 1 (This is a divalent hydrocarbon group, where n1 represents an integer from 2 to 20.)
[0031] [7]
[0032] According to any one of [1] to [6], the above-mentioned structural unit (a) is a structural unit having at least one of the groups shown in the following formula (3) and the following formula (4).
[0033]
[0034] (In equation (3), R) 2 and R 3 Each of n1 and n2 independently represents an alkyl group with 1 to 10 carbon atoms, and each of n3 independently represents an integer from 0 to 2. Indicates the connection point.
[0035] (In equation (4), R) 4 and R 5 Each of these characters independently represents an alkyl group with 1 to 10 carbon atoms, and n4 and n5 independently represent integers from 0 to 2. Indicates the connection point.
[0036] [8]
[0037] According to any one of [1] to [6], the blocking agent constituting the blocked isocyanate group of the above-mentioned structural unit (a) is at least one selected from pyrazole compounds, oxime compounds and phenolic compounds.
[0038] [9]
[0039] According to any one of [1] to [8], the above copolymer (A-1) further contains other structural units (d).
[0040]
[10]
[0041] According to any one of [1] to [9], the photosensitive resin composition has a blocked isocyanate equivalent of 200 to 3000 g / mol in the copolymer (A-1). Furthermore, its hydroxyl equivalent is 100–5000 g / mol.
[0042]
[11]
[0043] According to any one of [1] to
[10] , the photosensitive resin composition of the above copolymer (A-1) has an acid value of 5 to 400 KOH mg / g. Furthermore, its weight-average molecular weight is 3,000–50,000.
[0044]
[12]
[0045] According to any one of [1] to
[11] , in all structural units of the copolymer (A-1), The content of the above structural unit (a) is 1 to 50 mol%. The content of the above structural unit (b) is 1–70 mol%. The content of the above structural unit (c) is 1 to 70 moles.
[0046]
[13]
[0047] A photosensitive coloring composition comprising any one of the photosensitive resin compositions described in [1] to
[12] and a colorant (E).
[0048]
[14]
[0049] A resin-cured film, which is a cured product of the photosensitive resin composition described in any one of [1] to
[12] .
[0050]
[15]
[0051] A color filter having a color pattern as a cured product of the photosensitive coloring composition described in
[13] .
[0052]
[16]
[0053] An image display element having the color filter described in
[15] .
[0054] The effects of the invention
[0055] According to this disclosure, a photosensitive resin composition can be provided that exhibits good developability and yields a resin-cured film with excellent solvent resistance and adhesion. Furthermore, a resin-cured film with excellent solvent resistance and adhesion, and an image display element having the resin-cured film, can be provided. Detailed Implementation
[0056] The embodiments of the present invention will now be described in detail. However, the present invention is not limited to the embodiments shown below.
[0057] In this specification, when "~" is used to refer to a numerical range, the values at both ends are the upper and lower limits, respectively, and are included within the numerical range. When multiple upper or lower limits are specified, a numerical range can be created from all combinations of the upper and lower limits. Similarly, when multiple numerical ranges are specified, additional numerical ranges can be created by individually selecting and combining the upper and lower limits from these ranges.
[0058] In this specification, "(meth)acrylic acid" refers to methacrylic acid or acrylic acid, "(meth)acrylate" refers to acrylate or methacrylate, and "(meth)acryloyl" refers to acryloyl or methacryloyl. In this specification, "(poly)alkylene glycol" refers to alkylene glycol or polyalkylene glycol.
[0059] In this specification, "olefin unsaturated bond" refers to a double bond formed between carbon atoms other than the carbon atoms forming the aromatic ring, "olefin unsaturated group" refers to a group having olefin unsaturated bonds, and "olefin unsaturated compound" refers to a compound having olefin unsaturated bonds.
[0060] In this specification, the term "structural unit" refers to a unit derived from the polymeric compound itself used as a monomer, or a unit obtained by further modifying a unit derived from the polymeric compound itself used as a monomer after polymerization.
[0061] In this specification, the acid value of the copolymer is the acid value of the curable polymer as measured according to JIS K6901:2008 5.3.2. That is, the acid value refers to the number of mg of potassium hydroxide required to neutralize the acidic components contained in 1g of the copolymer.
[0062] In this specification, the term "blocked isocyanate equivalent" of a copolymer refers to the mass of the copolymer relative to 1 mole of blocked isocyanate groups in the copolymer. The blocked isocyanate equivalent can be determined by dividing the mass of the copolymer by the number of blocked isocyanate groups in the copolymer (g / mol). In this specification, the term "blocked isocyanate equivalent" of a copolymer is a theoretical value calculated from the amount of raw materials added during the manufacture of the copolymer.
[0063] In this specification, the hydroxyl equivalent of a copolymer is the mass of the copolymer relative to 1 mole of hydroxyl groups in the copolymer. The hydroxyl equivalent can be determined by dividing the mass of the copolymer by the number of hydroxyl groups in the copolymer (g / mol). In this specification, the hydroxyl equivalent of a copolymer is a theoretical value calculated from the amount of raw materials added during the manufacture of the copolymer.
[0064] In this specification, the term "unsaturated group equivalent" of a copolymer refers to the mass of the copolymer relative to 1 mole of olefinically unsaturated groups in the copolymer. The unsaturated group equivalent can be determined by dividing the mass of the copolymer by the number of olefinically unsaturated groups in the copolymer (g / mol). In this specification, the term "unsaturated group equivalent" of a copolymer is a theoretical value calculated from the amount of raw materials added during the manufacture of the copolymer.
[0065] In this specification, the weight-average molecular weight (Mw) and number-average molecular weight (Mn) are values obtained by gel permeation chromatography (GPC) under the following conditions using a standard polystyrene standard curve.
[0066] Column: Used by connecting two columns of Setontronix (trademark) LF-804 (Russell Co., Ltd.) in series.
[0067] Column temperature: 40℃
[0068] Sample: 0.2% (w / w) tetrahydrofuran solution of the analyte being tested
[0069] Developing solvent: Tetrahydrofuran
[0070] Detector: Differential refractometer (ショウデックス (trademark) RI-71S) (Ryosun Co., Ltd.)
[0071] Flow rate: 1 mL / min
[0072] <Photosensitive Resin Composition>
[0073] One embodiment of the photosensitive resin composition comprises copolymer (A-1), copolymer (A-2), photopolymerization initiator (C), and solvent (D), wherein the unsaturated group equivalent of copolymer (A-2) is 30 to 3000 g / mol. Another embodiment of the photosensitive resin composition comprises copolymer (A-1), reactive diluent (B), photopolymerization initiator (C), and solvent (D). Another embodiment of the photosensitive resin composition comprises copolymer (A-1), copolymer (A-2), reactive diluent (B), photopolymerization initiator (C), and solvent (D), wherein the unsaturated group equivalent of copolymer (A-2) is 30 to 3000 g / mol. The photosensitive resin composition polymerizes and cures upon light irradiation to form a cured resin film. The photosensitive resin composition exhibits good low-temperature curing properties and can form a cured resin film with sufficient hardness and solvent resistance. Furthermore, due to its excellent alkaline developability, the photosensitive resin composition can form fine patterns by developing it with an alkaline aqueous solution. Therefore, the photosensitive resin composition is suitable for use as, for example, a photoresist.
[0074] [Copolymer (A-1)]
[0075] The copolymer (A-1) has hydroxyl groups, structural units (a) having blocked isocyanate groups (hereinafter also referred to as "structural unit (a)"), structural units (b) having a partial structure as shown in formula (1) (hereinafter also referred to as "structural unit (b)"), and structural units (c) having acid groups (hereinafter also referred to as "structural unit (c)"). The copolymer (A-1) may, as needed, have other structural units (d) besides the above-mentioned structural units (a) to (c) (hereinafter also referred to as "structural unit (d)").
[0076]
[0077] (In equation (1), R) 1 (This is a divalent hydrocarbon group, where n1 represents an integer from 2 to 20.)
[0078] The weight-average molecular weight of the copolymer (A-1) is preferably 3,000 or more, more preferably 5,000 or more, further preferably 7,000 or more, and even more preferably 9,000 or more. The weight-average molecular weight of the copolymer (A-1) is preferably 50,000 or less, more preferably 30,000 or less, further preferably 20,000 or less, and even more preferably 15,000 or less. If the weight-average molecular weight of the copolymer (A-1) is 3,000 or more, the photosensitive resin composition or photosensitive coloring composition exhibits good curability, and the cured product has better solvent resistance. If the weight-average molecular weight of the copolymer (A-1) is 50,000 or less, the photosensitive resin composition or photosensitive coloring composition exhibits good storage stability.
[0079] The molecular weight distribution (Mw / Mn) of the copolymer (A-1) is preferably 1.1 or more, more preferably 1.3 or more, further preferably 1.5 or more, and even more preferably 1.7 or more. The molecular weight distribution (Mw / Mn) of the copolymer (A-1) is preferably 5 or less, more preferably 4 or less, further preferably 2.5 or less, and even more preferably 2.3 or less. If the molecular weight distribution (Mw / Mn) of the copolymer (A-1) is 1.1 or more, the reaction conditions during synthesis are easier to control. If the molecular weight distribution (Mw / Mn) of the copolymer (A-1) is 5 or less, the storage stability of the photosensitive resin composition or the photosensitive coloring composition, and the solvent resistance of its cured product, are better.
[0080] The blocked isocyanate group equivalent of copolymer (A-1) is preferably 200 g / mol or more, more preferably 300 g / mol or more, further preferably 400 g / mol or more, and even more preferably 500 g / mol or more. The blocked isocyanate group equivalent of copolymer (A-1) is preferably 3000 g / mol or less, more preferably 2000 g / mol or less, further preferably 1500 g / mol or less, and even more preferably 1000 g / mol or less. If the blocked isocyanate group equivalent of copolymer (A-1) is 200 g / mol or more, the photosensitive resin composition or photosensitive coloring composition exhibits good storage stability. If the blocked isocyanate group equivalent of copolymer (A-1) is 3000 g / mol or less, the cured photosensitive resin composition or photosensitive coloring composition exhibits better solvent resistance.
[0081] The hydroxyl equivalent of the copolymer (A-1) is preferably 100 g / mol or more, more preferably 200 g / mol or more, further preferably 300 g / mol or more, and even more preferably 400 g / mol or more. The hydroxyl equivalent of the copolymer (A-1) is preferably 5000 g / mol or less, more preferably 4000 g / mol or less, further preferably 3000 g / mol or less, and even more preferably 2000 g / mol or less. If the hydroxyl equivalent of the copolymer (A-1) is 100 g / mol or more, the photosensitive resin composition or photosensitive coloring composition exhibits good storage stability. If the hydroxyl equivalent of the copolymer (A-1) is 5000 g / mol or less, the cured photosensitive resin composition or photosensitive coloring composition exhibits even better solvent resistance.
[0082] The acid value of copolymer (A-1) is preferably 5 KOH mg / g or more, more preferably 10 KOH mg / g or more, further preferably 15 KOH mg / g or more, and even more preferably 20 KOH mg / g or more. The acid value of copolymer (A-1) is preferably 400 KOH mg / g or less, more preferably 300 KOH mg / g or less, further preferably 200 KOH mg / g or less, and even more preferably 100 KOH mg / g or less. If the acid value of copolymer (A-1) is 5 KOH mg / g or more, the photosensitive resin composition or photosensitive coloring composition exhibits good storage stability. If the acid value of copolymer (A-1) is 400 KOH mg / g or less, the cured photosensitive resin composition or photosensitive coloring composition exhibits better solvent resistance.
[0083] (Structural unit with blocked isocyanate group (a))
[0084] The structural unit (a) is not particularly limited as long as it has a structure in which the isocyanate group is blocked by the addition of a blocking agent. The structural unit (a) can be only one type or two or more types. The structural unit (a) is a structural unit derived from a monomer (ma) containing blocked isocyanate groups (hereinafter also simply referred to as "monomer (ma)"). By having structural unit (a) in the copolymer (A-1), crosslinking with reactive functional groups contained in the composition occurs when the photosensitive resin composition or photosensitive coloring composition is heated, forming a cured product with high crosslinking density. Therefore, the cured product also exhibits good solvent resistance under low-temperature curing conditions. Crosslinking is formed, for example, by reacting isocyanate groups generated by the dissociation of the blocking agent due to heating with reactive functional groups. Examples of reactive functional groups include, for example, hydroxyl groups, acid groups, and amino groups contained in the copolymer (A-1) as needed. Because the copolymer (A-1) has hydroxyl groups, crosslinking can be formed through transesterification even without the dissociation of the blocking agent when the blocking agent is a compound with an alkyloxy carbonyl group.
[0085] In one embodiment, the monomer (ma) has an olefinic unsaturated bond and a blocked isocyanate group. Examples of olefinic unsaturated groups include vinyl, (meth)acryloyloxy, etc.
[0086] Monomers (ma) can be manufactured, for example, by blocking the isocyanate groups of isocyanate compounds having olefinic unsaturated bonds with a blocking agent. The blocking reaction can be carried out in the presence or absence of a solvent. Organometallic salts containing metals such as tin, zinc, and lead, as well as tertiary amines, can be used as catalysts in the blocking reaction.
[0087] Examples of isocyanate compounds having olefinic unsaturated bonds include, for example, the compound shown in formula (5) below.
[0088]
[0089] (In equation (5), R) 6 Represents a hydrogen atom or a methyl group; R 7 Indicates -CO-, -COOR 8 -(Here, R) 8 It is an alkylene group having 1 to 6 carbon atoms. (or -COO-R) 9 O-CONH-R 10 -(Here, R) 9 R is an alkylene group having 2 to 6 carbon atoms. 10 It can be an alkylene group having 2 to 12 carbon atoms or an aryl group having 6 to 12 carbon atoms, which may have substituents.
[0090] In the isocyanate compound shown in formula (5), from the viewpoint of the good reactivity of the unsealed isocyanate group, R is preferred. 7 -COOR 8 -, better R 8 It is an alkylene group having 1 to 4 carbon atoms.
[0091] As an isocyanate compound having an olefinically unsaturated bond, the reaction product obtained by reacting a diisocyanate compound with a hydroxyalkyl methacrylate such as hydroxyethyl methacrylate or hydroxypropyl methacrylate in equimolar amounts (hydroxyalkyl methacrylate: diisocyanate compound = 1 mole: 1 mole) can be used.
[0092] Examples of the aforementioned diisocyanate compounds include, for example, 1,6-hexanediisocyanate, 2,4-(or 2,6-)toluenediisocyanate (TDI), 4,4'-diphenylmethanediisocyanate (MDI), 3,5,5-trimethyl-3-isocyanate-methylcyclohexyl isocyanate (IPDI), xylene m-(or p-)diisocyanate, 1,3-(or 1,4-)bis(isocyanate-methyl)cyclohexane, lysine diisocyanate, etc.
[0093] From the viewpoint of the low-temperature curability of the photosensitive resin composition or the photosensitive coloring composition, the structural unit (a) is preferably a structural unit derived from a (meth)acrylate containing a blocked isocyanate group that has been blocked from a (meth)acrylate containing an isocyanate group.
[0094] Examples of (meth)acrylates containing isocyanate groups include, for example, 2-isocyanate-ethyl (meth)acrylate, 2-isocyanate-propyl (meth)acrylate, 3-isocyanate-propyl (meth)acrylate, 2-isocyanate-1-methylethyl (meth)acrylate, 2-isocyanate-1,1-dimethylethyl (meth)acrylate, 4-isocyanate-cyclohexyl (meth)acrylate, 1,1-bis(acryloyloxymethyl)methyl isocyanate, 1,1-bis(acryloyloxymethyl)ethyl isocyanate, 1,1-bis(methacryloyloxymethyl)methyl isocyanate, and 1,1-bis(methacryloyloxymethyl)ethyl isocyanate. Among these, 2-isocyanate-ethyl (meth)acrylate, 2-isocyanate-propyl (meth)acrylate, and 1,1-bis(methacryloyloxymethyl)ethyl isocyanate are preferred.
[0095] Examples of blocking agents include, for instance, lactam compounds such as ε-caprolactam, δ-valerolactam, γ-butyrolactam, and β-propiolactam; alcohol compounds such as methanol, ethanol, propanol, 1-methoxy-2-propanol, butanol, ethylene glycol, methyl cellosolve, butyl cellosolve, methyl carbitol, benzyl alcohol, phenyl cellosolve, furfuryl alcohol, and cyclohexanol; phenol, 2,6-dimethylphenol, cresol, 3,5-xylenol, ethylphenol, o-isopropylphenol, p-tert-butylphenol, butylphenol, p-tert-octylphenol, nonylphenol, dinonylphenol, styrylated phenol, methyl 2-hydroxybenzoate, methyl 4-hydroxybenzoate, thymol, 1-naphthol, and p-nitrobenzene. Phenolic compounds such as phenol and p-chlorophenol; active methylene compounds such as dimethyl malonate, diethyl malonate, methyl acetoacetate, ethyl acetoacetate, and acetylacetone; thiols such as butyl mercaptan, thiophenol, and tert-dodecyl mercaptan; amine compounds such as diisopropylamine, diphenylamine, phenylnaphthylamine, aniline, and carbazole; acid amide compounds such as acetanilide, acetaminophen, acetamide, and benzamide; imide compounds such as succinimide and maleimide; imidazole compounds such as imidazole, 2-methylimidazole, and 2-ethylimidazole; pyrazole compounds such as pyrazole and 3,5-dimethylpyrazole; urea compounds such as urea, thiourea, and ethylidene urea; and phenyl N-phenylcarbamate, 2- Carbamic acid compounds such as azole ketones; imine compounds such as ethyleneimine and polyethyleneimine; oxime compounds such as formaldehyde oxime, acetaldehyde oxime, acetone oxime, methyl ethyl ketone oxime, methyl isobutyl ketone oxime, and cyclohexanone oxime; and bisulfite salts such as sodium bisulfite and potassium bisulfite. Sealing agents can be used alone or in combination of two or more.
[0096] In one embodiment, as a sealing agent, from the viewpoint of the low-temperature curability of the photosensitive resin composition or the photosensitive coloring composition, it is preferably selected from at least one of pyrazole compounds, oxime compounds and phenolic compounds, more preferably from at least one of 3,5-dimethylpyrazole, methyl 4-hydroxybenzoate and methyl ethyl ketone oxime.
[0097] In structural unit (a), the dissociation rate of the blocked isocyanate groups after heating at 100°C for 30 minutes is preferably 5–99%, more preferably 10–90%, and most preferably 15–80%. The dissociation rate can be, for example, 8–70%, 15–60%, or 30–50% as needed. If the dissociation rate is 99% or less, unintended crosslinking reactions caused by the regeneration of isocyanate groups in structural unit (a) can be suppressed during the synthesis of the copolymer (A-1) and during the storage of the photosensitive resin composition or photosensitive coloring composition. If the dissociation rate is 5% or more, good curability can be obtained even with a sufficiently low heating temperature for curing the photosensitive resin composition or photosensitive coloring composition, resulting in a cured product with superior solvent resistance.
[0098] From the viewpoint of the stability of the copolymer (A-1) and the low-temperature curability of the photosensitive resin composition or the photosensitive coloring composition, suitable blocking agents with the above-mentioned dissociation rate can be cited as examples, such as γ-butyrolactam, 1-methoxy-2-propanol, 2,6-dimethylphenol, diisopropylamine, methyl ethyl ketone oxime and 3,5-dimethylpyrazole, preferably 3,5-dimethylpyrazole and methyl ethyl ketone oxime.
[0099] The above-mentioned dissociation rate can be considered to be the same as the dissociation rate of the blocked isocyanate groups when the monomer (ma) containing blocked isocyanate groups is heated at 100°C for 30 minutes, and is calculated by the following method. Specifically, a 20% by mass solution of monomer (ma) in n-octanol is prepared. To the resulting n-octanol solution, 1% by mass of dibutyltin laurylate is added as a catalyst and 3% by mass of phenothiazine is added as a polymerization inhibitor, and the solution is heated at 100°C for 30 minutes. The heated n-octanol solution is analyzed by high-performance liquid chromatography (HPLC) to determine the mass of the monomer (ma) in the n-octanol solution. Using this result, the mass reduction percentage is calculated and determined as the dissociation rate after heating at 100°C for 30 minutes.
[0100] The dissociation temperature at which the dissociation rate of the blocked isocyanate groups in structural unit (a) reaches 80% or more within 30 minutes is preferably 80°C or higher, more preferably 90°C or higher, and even more preferably 100°C or higher. If the dissociation temperature is 80°C or higher, unintended crosslinking reactions caused by the regeneration of isocyanate groups in structural unit (a) can be suppressed during the synthesis of the copolymer (A-1) and during the storage of the photosensitive resin composition or photosensitive coloring composition. The dissociation temperature can be 160°C or lower. If the dissociation temperature is 160°C or lower, good curability can be obtained even with a sufficiently low heating temperature for curing the photosensitive resin composition or photosensitive coloring composition, resulting in a cured product with superior solvent resistance.
[0101] The dissociation temperature was calculated using the method described below. Specifically, a n-octanol solution with a monomer (ma) concentration of 20% by mass was prepared. To the resulting n-octanol solution, 1% by mass of dibutyltin laurylate was added as a catalyst, and 3% by mass of phenothiazine was added as a polymerization inhibitor. The solution was then heated for 30 minutes under various different temperatures. The n-octanol solutions heated at different temperatures were analyzed by high-performance liquid chromatography (HPLC) to determine the mass of the monomer (ma) in the n-octanol solution. Using this result, the temperature at which the extraction mass reduction ratio reached 80% or more was determined. The lowest of these temperatures was identified as the dissociation temperature at which the dissociation rate of the blocked isocyanate groups reached 80% or more after 30 minutes.
[0102] Specifically, structural unit (a) is preferably selected from at least one of the structural units derived from the compound shown in formula (6) below, in which acryloyloxyethyl isocyanate is blocked with 3,5-dimethylpyrazole (dissociation temperature at which the dissociation rate of the blocked isocyanate group reaches 80% or more after 30 minutes: 120°C, dissociation rate at 100°C for 30 minutes: 35%) and the compound shown in formula (7) below, in which methacryloyloxyethyl isocyanate is blocked with methyl ethyl ketone oxime (dissociation temperature at which the dissociation rate of the blocked isocyanate group reaches 80% or more after 30 minutes: 130°C, dissociation rate at 100°C for 30 minutes: 18%).
[0103]
[0104] In one embodiment, from the viewpoint of low-temperature curability of the photosensitive resin composition or photosensitive coloring composition, a compound having an alkyloxycarbonyl group is preferred as the sealing agent, and an active methylene compound having an alkyloxycarbonyl group is more preferred. When a compound having an alkyloxycarbonyl group is used as the sealing agent, the photosensitive resin composition or photosensitive coloring composition can obtain a cured film with excellent solvent resistance even when cured at low temperatures of 50°C to 150°C.
[0105] In this embodiment, the structural unit (a) preferably has at least one group selected from the group shown in formula (3) and the group shown in formula (4).
[0106]
[0107] (In equation (3), R) 2 and R 3 Each of n1 and n2 independently represents an alkyl group with 1 to 10 carbon atoms, and each of n3 independently represents an integer from 0 to 2. Indicates the connection point.
[0108] (In equation (4), R) 4 and R 5 Each of these characters independently represents an alkyl group with 1 to 10 carbon atoms, and n4 and n5 independently represent integers from 0 to 2. Indicates the connection point.
[0109] R in equation (3) above 2 and R 3 Preferably, each alkyl group is an alkyl group having 2 to 6 carbon atoms; more preferably, it is an alkyl group having 2 to 3 carbon atoms; and most preferably, R. 2 and R 3 Both are ethyl. In R 2 and R3 In the case of ethyl groups, if the photosensitive resin composition or photosensitive coloring composition is thermocured, ethanol is generated through transesterification. The generated ethanol is preferably removed by easy evaporation due to heating during thermocuring. Preferably, both n2 and n3 in the above formula (3) are 0.
[0110] R in equation (4) above 5 Preferably, it is an alkyl group having 2 to 6 carbon atoms, more preferably an alkyl group having 2 to 3 carbon atoms, and even more preferably an ethyl group. In R 5 In the case of ethyl groups, if the photosensitive resin composition or photosensitive coloring composition is thermocured, ethanol is generated through transesterification. The generated ethanol is preferably removed by easy evaporation due to heating during thermocuring. Preferably, both n4 and n5 in formula (4) above are 0.
[0111] In this embodiment, the modification rate of the blocked isocyanate group of the structural unit (a) having blocked isocyanate group after heating at 100°C for 30 minutes is set to be the same as the modification rate of the blocked isocyanate group of the monomer (ma) containing blocked isocyanate group after heating at 100°C for 30 minutes, and is calculated in the same manner as the method for calculating the dissociation rate described above. That is, a catalyst and a polymerization inhibitor are added to a n-octanol solution with a monomer (ma) concentration of 20% by mass, the solution is heated at 100°C for 30 minutes, the mass reduction ratio of the monomer (ma) caused thereby is calculated, and the modification rate after heating at 100°C for 30 minutes is determined. The modification rate of the blocked isocyanate group is preferably 5 to 99%, more preferably 10 to 90%, and most preferably 15 to 80%.
[0112] In the copolymer (A-1), the content of structural unit (a) is preferably 1 mol% or more, more preferably 3 mol% or more, further preferably 5 mol% or more, even more preferably 10 mol% or more, preferably 50 mol% or less, more preferably 40 mol% or less, even more preferably 30 mol% or less, and even more preferably 20 mol% or less. If the content of structural unit (a) is 1 mol% or more, the photosensitive resin composition or photosensitive coloring composition exhibits good low-temperature curability, and the cured product has better solvent resistance. If the content of structural unit (a) is 50 mol% or less, the content of structural units (b) and (c) can be sufficiently ensured, resulting in better developability of the photosensitive resin composition or photosensitive coloring composition.
[0113] (Structural unit (b) with the partial structure shown in equation (1))
[0114] There are no particular limitations on structural unit (b), as long as it does not have a blocked isocyanate group and has a partial structure as shown in formula (1) below. Structural unit (b) can be only one type or two or more types. Although not bound by any theory, structural unit (b) can improve the developability of photosensitive resin composition or photosensitive coloring composition by improving the adhesion to the substrate.
[0115]
[0116] (In equation (1), R) 1 (This is a divalent hydrocarbon group, where n1 represents an integer from 2 to 20.)
[0117] From the viewpoint of reactivity with structural unit (a), structural unit (b) preferably has the group shown in the following formula (2).
[0118]
[0119] (In equation (2), R) 1 (This is a divalent hydrocarbon group, where n1 represents an integer from 2 to 20.)
[0120] In equations (1) and (2), R 1 The number of carbon atoms is preferably 2 to 6, more preferably 2 to 4, and even more preferably 2 or 3. In formulas (1) and (2), R 1 Preferably, it is a saturated hydrocarbon group with 2 to 6 carbon atoms, more preferably a saturated hydrocarbon group with 2 to 4 carbon atoms, and even more preferably a saturated hydrocarbon group with 2 or 3 carbon atoms. A structural unit (b) contains multiple -(R) groups. 1 -O)- can be a single type or multiple types. In -(R 1 In the case of multiple types of -O), n1 refers to all types of -(R) 1 The total number of -O)-. n1 is preferably an integer from 2 to 10, more preferably an integer from 2 to 6.
[0121] Structural unit (b) is derived from a monomer (mb) (hereinafter also simply referred to as "monomer (mb)") that does not have a blocked isocyanate group and has a partial structure as shown in formula (1). Examples of monomers (mb) include compounds that do not have a blocked isocyanate group but have an olefinic unsaturated group and a partial structure as shown in formula (1). Examples of olefinic unsaturated groups include vinyl groups, (meth)acryloyloxy groups, etc.
[0122] Examples of monomers (mb) include, for instance, polyalkylene glycol mono(meth)acrylates such as polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, polybutylene glycol mono(meth)acrylate, polyethylene glycol polybutylene glycol mono(meth)acrylate, and propylene glycol polybutylene glycol mono(meth)acrylate; alkoxy polyalkylene glycol (meth)acrylates such as methoxy polyethylene glycol (meth)acrylate, ethoxy polyethylene glycol (meth)acrylate, and methoxy polypropylene glycol (meth)acrylate; and aryloxy polyalkylene glycol (meth)acrylates such as phenoxy polyethylene glycol (meth)acrylate and nonylphenoxy polyethylene glycol mono(meth)acrylate. These monomers (mb) can be used alone or in combination of two or more.
[0123] As monomers (mb), from the viewpoint of solvent resistance and fine-line adhesion of the resin-cured film, at least one of polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, and methoxy polyethylene glycol (meth)acrylate is preferred.
[0124] In the copolymer (A-1), the content of structural unit (b) is preferably 1 mol% or more, more preferably 3 mol% or more, further preferably 5 mol% or more, even more preferably 10 mol% or more, preferably 70 mol% or less, more preferably 60 mol% or less, even more preferably 50 mol% or less, and even more preferably 30 mol% or less. If the content of structural unit (b) is 1 mol% or more, the developability, solvent resistance of the cured resin film, and fine-line adhesion are better. If the content of structural unit (b) is 70 mol% or less, the content of structural unit (a) can be sufficiently ensured, and the amount of crosslinking obtained by thermosetting can be sufficiently ensured, thus resulting in better solvent resistance. If the content of structural unit (b) is 70 mol% or less, the storage stability of the photosensitive resin composition or photosensitive coloring composition is good.
[0125] (Structural unit with acid group (c))
[0126] The structural unit (c) having an acid group is not particularly limited as long as it does not have a closed isocyanate group and the partial structure shown in formula (1). Examples of acid groups include carboxyl, sulfonyl, and phosphonoyl (-P(=O)(OH)2). Among these acid groups, carboxyl is preferred from the perspective of ease of acquisition. The structural unit (c) can be only one type or two or more types. By having the structural unit (c) in the copolymer (A-1), the photosensitive resin composition or photosensitive coloring composition has good developability.
[0127] Structural unit (c) is derived from a monomer (mc) containing an acid group (hereinafter also simply referred to as "monomer (mc)"). The monomer (mc) containing an acid group is a monomer that does not have a closed isocyanate group and the partial structure shown in formula (1) and has an acid group. Examples of monomers (mc) include, for example, unsaturated carboxylic acids or their anhydrides, unsaturated sulfonic acids, unsaturated phosphonic acids, etc.
[0128] Specifically, monomers (mc) include unsaturated carboxylic acids or their anhydrides such as (meth)acrylic acid, α-bromo(meth)acrylic acid, β-furanyl(meth)acrylic acid, crotonic acid, propynic acid, cinnamic acid, α-cyanocinonic acid, maleic acid, maleic anhydride, monomethyl maleate, monoethyl maleate, monoisopropyl maleate, fumaric acid, itaconic acid, itaconic anhydride, citraconic acid, citraconic anhydride, and 2-(meth)acryloyloxyethyl succinic acid; unsaturated sulfonic acids such as 2-acrylamido-2-methylpropanesulfonic acid, tert-butylacrylamidosulfonic acid, and p-styrenesulfonic acid; and unsaturated phosphonic acids such as vinylphosphonic acid. These monomers (mc) can be used alone or in combination of two or more.
[0129] Of all the structural units in the copolymer (A-1), the content of structural unit (c) is preferably 1 mol% or more, more preferably 3 mol% or more, and even more preferably 5 mol% or more. From the viewpoint of the adhesion of the cured product, it is preferably 70 mol% or less, more preferably 60 mol% or less, and even more preferably 50 mol% or less. From the viewpoint of the solvent resistance of the cured product, it is preferably 60 mol% or less, more preferably 50 mol% or less, and even more preferably 30 mol% or less. If the content of structural unit (c) is 1 mol% or more, the developability is better. If the content of structural unit (c) is 70 mol% or less, the content of structural unit (b) can be sufficiently ensured, and the solvent resistance and fine-line adhesion of the resin cured film are better. If the content of structural unit (c) is 70 mol% or less, the storage stability of the photosensitive resin composition or the photosensitive coloring composition is good.
[0130] (Other structural units (d))
[0131] There are no special restrictions on structural unit (d) as long as it is not equivalent to structural units (a) to (c). Structural unit (d) can be of only one type or more types.
[0132] Structural unit (d) is a structural unit derived from other monomers (md) (hereinafter also simply referred to as "monomer (md)") that are capable of copolymerizing with monomers (ma) to (mc) without having a closed isocyanate group, a partial structure shown in formula (1), and an acid group. Specific examples of monomers (md) include olefinic unsaturated compounds containing hydroxyl groups, aromatic vinyl compounds, cyclic olefins having a norbornene structure, conjugated dienes, (meth)acrylates, (meth)acrylamides, vinyl compounds, unsaturated dicarboxylic acid diesters, monomaleimides, olefinic unsaturated compounds containing epoxy groups, (meth)acrylamide, (meth)acrylonitrile, acrolein, etc. From the viewpoint of improving low-temperature curability by crosslinking with structural unit (a), an olefinic unsaturated compound containing hydroxyl groups is preferred; from the viewpoint of heat resistance, at least one of aromatic vinyl compounds, cyclic olefins having a norbornene structure, and (meth)acrylates having a cyclic structure is preferred; and from the viewpoint of fine-line adhesion, at least one of aromatic vinyl compounds and compounds containing phenyl groups is preferred.
[0133] Examples of hydroxyl-containing olefinic unsaturated compounds include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 2,3-dihydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and other hydroxyalkyl (meth)acrylates; 2-hydroxy-3-phenoxypropyl (meth)acrylate, etc. From the viewpoint of reactivity during the synthesis of copolymer (A-1), low-temperature curability of the photosensitive resin composition or photosensitive coloring composition, and ease of acquisition, hydroxyalkyl (meth)acrylates are preferred, and 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate are more preferred.
[0134] Examples of aromatic vinyl compounds include styrene, α-methylstyrene, o-vinyltoluene, p-vinyltoluene, o-chlorostyrene, m-chlorostyrene, methoxystyrene, p-nitrostyrene, p-cyanostrene, p-acetaminostyrene, and vinylpyridine.
[0135] Examples of cyclic olefins with a norbornene structure include norbornene (bicyclo[2.2.1]hept-2-ene), 5-methylbicyclo[2.2.1]hept-2-ene, and tetracyclo[4.4.0.1]. 2,5 .1 7,10 [Dodecyl-3-ene, 8-ethyltetracyclo[4.4.0.1]] 2, 5 .1 7,10 [Dodecyl-3-ene, dicyclopentadiene, tricyclo[5.2.1.0]] 2,6[Dec-8-ene, tricyclic [4.4.0.1]] 2,5 Undec-3-ene, tricyclic [6.2.1.0] 1,8 Undec-9-ene, tetracyclic [4.4.0.1] 2,5 .1 7,10 .0 1,6 [Dodecyl-3-ene, 8-ethylidene tetracyclo[4.4.0.1]] 2,5 .1 7,12 [Dodecyl-3-ene, pentacyclic [6.5.1.1]] 3,6 .0 2,7 .0 9,13 [Pentadec-4-ene, etc.]
[0136] Examples of conjugated dienes include butadiene, isoprene, and chloroprene.
[0137] Examples of (meth)acrylates include methyl methacrylate, ethyl methacrylate, isopropyl methacrylate, tert-butyl methacrylate, amyl methacrylate, benzyl methacrylate, isoamyl methacrylate, 2-ethylhexyl methacrylate, dodecyl methacrylate, cyclohexyl methacrylate, methylcyclohexyl methacrylate, rosin (meth)acrylate, norbornyl methacrylate, 5-ethylnorbornyl (meth)acrylate, dicyclopentenyl (meth)acrylate, and dicyclopentenyloxy (meth)acrylate. Ethyl acrylate, isobornyl acrylate, adamantyl acrylate, tetrahydrofurfuryl acrylate, 1,1,1-trifluoroethyl acrylate, perfluoroethyl acrylate, perfluoro-n-propyl acrylate, 3-(N,N-dimethylamino)propyl (meth)acrylate, triphenylmethyl acrylate, phenyl acrylate, cumyl acrylate, 4-phenoxyphenyl acrylate, phenoxyethyl acrylate, biphenoxyethyl acrylate, naphthyl acrylate, anthracene acrylate, etc.
[0138] Examples of (meth)acrylamide compounds include (meth)acrylamide, N,N-dimethyl (meth)acrylamide, N,N-diisopropyl (meth)acrylamide, and anthracene (meth)acrylamide.
[0139] Examples of vinyl compounds include vinyl chloride, 1,1-dichloroethylene, vinyl fluoride, 1,1-difluoroethylene, N-vinylpyrrolidone, and vinyl acetate.
[0140] Examples of unsaturated dicarboxylic acid diesters include diethyl citrate, diethyl maleate, diethyl fumarate, and diethyl itaconic acid.
[0141] Examples of monomaleimides include N-phenylmaleimide, N-cyclohexylmaleimide, N-laurylmaleimide, and N-(4-hydroxyphenyl)maleimide.
[0142] Examples of epoxy-containing olefinic unsaturated compounds include, for example, epoxyalkyl(meth)acrylate, glycidyl(meth)acrylate, 2-methylglycidyl(meth)acrylate, 2-ethylglycidyl(meth)acrylate, 2-epoxyalkylethyl(meth)acrylate, 2-glycidyloxyethyl(meth)acrylate, 3-glycidyloxypropyl(meth)acrylate, glycidyloxyphenyl(meth)acrylate, 4-hydroxybutyl(meth)acrylate glycidyl ether, and other (meth)acrylate derivatives containing epoxy groups. And 3,4-epoxycyclohexyl(meth)acrylate, 3,4-epoxycyclohexylmeth(meth)acrylate, 2-(3,4-epoxycyclohexyl)ethyl(meth)acrylate, 2-(3,4-epoxycyclohexylmethoxy)ethyl(meth)acrylate, 3-(3,4-epoxycyclohexylmethoxy)propyl(meth)acrylate and other (meth)acrylate derivatives containing an epoxy group such as an alicyclic carbocyclic ring containing an epoxy group; vinyl ether compounds containing an epoxy group; and allyl ether compounds containing an epoxy group.
[0143] In all structural units of the copolymer (A-1), the content of structural unit (d) is preferably 1 mol% or more, more preferably 5 mol% or more, further preferably 10 mol% or more, preferably 90 mol% or less, more preferably 80 mol% or less, and even more preferably 60 mol% or less. If the content of structural unit (d) is 1 mol% or more, the desired function can be imparted. If the content of structural unit (d) is 90 mol% or less, the content of structural units (a) to (c) can be sufficiently ensured, and the amount of crosslinking obtained by thermosetting can be sufficiently ensured, thus resulting in better solvent resistance. Furthermore, the developability of the photosensitive resin composition or photosensitive coloring composition is better.
[0144] [Copolymer (A-2)]
[0145] The copolymer (A-2) is a copolymer that is not equivalent to copolymer (A-1), and its unsaturated group equivalent is 30 to 3000 g / mol. There is no particular limitation on the copolymer (A-2), but resins such as (meth)acrylic resins, epoxy resins containing (meth)acryloyl groups, and vinyl ester resins, which are generally used in negative photoresists, are preferred. Resins containing olefinic unsaturated groups such as vinyl and (meth)acryloyl groups, and substituents such as carboxyl, phosphate, and sulfonyl groups that contribute to alkali solubility, are also preferred. By using such a resin, photosensitive resin compositions and photosensitive coloring compositions with superior fine-line adhesion and developability can be provided. In this disclosure, the (meth)acrylic resin is a polymer containing at least one structural unit derived from a monomer having a (meth)acryloyloxy group. The proportion of monomers having a (meth)acryloyloxy group in the raw monomers of the (meth)acrylic resin can, for example, be more than 50% by mass, more than 70% by mass, or more than 90% by mass, or less than 100% by mass or less than 99% by mass.
[0146] Among these resins, from the viewpoint of resins that can readily provide a particularly wide range of properties, (meth)acrylic resins having (meth)acryloyl and carboxyl groups are preferred. This resin can be synthesized, for example, by polymerizing a monomer containing (meth)acryloyl groups and other polymerizable monomers as needed using a known free radical polymerization method to obtain a base polymer, and then introducing (meth)acryloyl and carboxyl groups into the base polymer.
[0147] As a method for introducing (meth)acryloyl groups, examples include polymerizing a base polymer using polymerizable monomers having reactive groups such as hydroxyl, amino, carboxyl, epoxy, and isocyanate groups, adding an inhibitor and a catalyst, and then adding a compound containing (meth)acryloyl groups with functional groups capable of reacting with these reactive groups, and reacting the mixture at 50–150°C. As a method for adding carboxyl groups, examples include reacting a polybasic acid or its anhydride with a base polymer having hydroxyl groups, reacting a compound containing epoxy and (meth)acryloyl groups with a base polymer having carboxyl groups followed by reacting the polybasic acid or its anhydride, and reacting a compound containing carboxyl and (meth)acryloyl groups with a base polymer having epoxy groups followed by reacting the polybasic acid or its anhydride. Alternatively, the carboxyl group in the base polymer may remain. Examples of polybasic acids or their anhydrides include succinic anhydride.
[0148] The weight-average molecular weight of copolymer (A-2) is preferably 3,000 or more, more preferably 4,000 or more, further preferably 5,000 or more, and even more preferably 6,000 or more. The weight-average molecular weight of copolymer (A-2) is preferably 50,000 or less, more preferably 30,000 or less, further preferably 20,000 or less, and even more preferably 15,000 or less. If the weight-average molecular weight of copolymer (A-2) is 3,000 or more, the photosensitive resin composition or photosensitive coloring composition exhibits good curability, and the cured product has better solvent resistance. If the weight-average molecular weight of copolymer (A-2) is 50,000 or less, the photosensitive resin composition or photosensitive coloring composition exhibits good storage stability.
[0149] The acid value of copolymer (A-2) is preferably 5 KOH mg / g or more, more preferably 10 KOH mg / g or more, further preferably 25 KOH mg / g or more, and even more preferably 30 KOH mg / g or less. The acid value of copolymer (A-2) is preferably 300 KOH mg / g or less, more preferably 200 KOH mg / g or less, further preferably 150 KOH mg / g or less, and even more preferably 100 KOH mg / g or less. If the acid value of copolymer (A-2) is 5 KOH mg / g or more, the cured photosensitive resin composition or photosensitive coloring composition exhibits better solvent resistance. If the acid value of copolymer (A-2) is 300 KOH mg / g or less, the photosensitive resin composition or photosensitive coloring composition exhibits good storage stability.
[0150] The copolymer (A-2) has an unsaturated group equivalent of 30 g / mol or more, preferably 100 g / mol or more, more preferably 200 g / mol or more, and even more preferably 300 g / mol or more. The copolymer (A-2) has an unsaturated group equivalent of 3000 g / mol or less, preferably 2000 g / mol or less, more preferably 1500 g / mol or less, and even more preferably 1000 g / mol or less. If the copolymer (A-2) has an unsaturated group equivalent of 30 g / mol or more, the photosensitive resin composition or photosensitive coloring composition exhibits good storage stability. If the copolymer (A-2) has an unsaturated group equivalent of 3000 g / mol or less, it exhibits good compatibility with the copolymer (A-1) and the reactive diluent (B), and sufficient photocurability can be obtained.
[0151] In a preferred embodiment, the copolymer (A-2) is a copolymer obtained by adding at least a portion of the epoxy group of a copolymer precursor containing an epoxy group to an olefinic unsaturated compound having a functional group reactive with the epoxy group, and then adding a polybasic acid or its anhydride to the hydroxyl group generated by ring-opening the epoxy group. The copolymer precursor may contain structural units other than those having an epoxy group. Suitable examples of other structural units include structural units without epoxy groups in the above-described structural unit (d).
[0152] The structural unit having an epoxy group is derived from the structural unit of a monomer containing an epoxy group. Specific examples of monomers containing epoxy groups include compounds similar to the aforementioned olefinic unsaturated compounds containing epoxy groups.
[0153] Examples of olefinic unsaturated compounds having functional groups reactive with epoxy groups include, for example, (meth)acrylic acid, 2-methacryloyloxyethyl succinic acid, 2-acryloyloxyethyl succinic acid, α-bromo(meth)acrylic acid, β-furanyl(meth)acrylic acid, crotonic acid, cinnamic acid, α-cyanocinonic acid, maleic acid, monomethyl maleate, monoethyl maleate, monoisopropyl maleate, fumaric acid, itaconic acid, citraconic acid, and other unsaturated carboxylic acids. Among these, (meth)acrylic acid is preferred.
[0154] Examples of polybasic acids include adipic acid, itaconic acid, succinic acid, oxalic acid, malonic acid, phthalic acid, fumaric acid, maleic acid, glutaric acid, tartaric acid, glutamic acid, and sebacic acid. Examples of polybasic anhydrides include tetrahydrophthalic anhydride, hexahydrophthalic anhydride, 4-methylhexahydrophthalic anhydride, maleic anhydride, itaconic anhydride, ethylmaleic anhydride, methylitaconic anhydride, chloromaleic anhydride, citraconic anhydride, 2-norbornene-5,6-dicarboxylic anhydride, 4-[2-(methacryloyloxy)ethoxycarbonyl]phthalic anhydride, succinic anhydride, and cyclohexanetricarboxylic anhydride.
[0155] In a preferred embodiment, copolymer (A-2) is a copolymer in which a portion of the acid group of a copolymer precursor containing an acid group has been added to an olefinically unsaturated compound having a functional group reactive with the acid group. Specific and suitable examples of the acid-containing structural unit are the same as those for structural unit (c) described above. The copolymer precursor may contain other structural units besides the acid-containing structural unit. As a suitable example of other structural units, structural unit (d) described above can be cited.
[0156] Examples of olefinic unsaturated compounds that are functional groups that are reactive with acid groups include, for example, olefinic unsaturated compounds containing epoxy groups.
[0157] [Reactive diluent (B)]
[0158] As the reactive diluent (B), any low molecular weight compound having at least one olefin unsaturated group is acceptable, and there is no particular limitation. In this disclosure, a low molecular weight compound is defined as a compound with a molecular weight of less than 1,000. Examples of olefin unsaturated groups include, for example, vinyl, allyl, and (meth)acryloyloxy groups. From the viewpoint of improving reactivity, reactive diluents having multiple olefin unsaturated groups (also called multifunctional reactive diluents) are preferred. Specific examples of reactive diluents (B) include aromatic vinyl compounds; aromatic allyl compounds such as diallyl phthalate and diallyl phenylphosphonate; vinyl carboxylic acid esters such as vinyl acetate and vinyl adipate; monofunctional (meth)acrylates; polyfunctional (meth)acrylates; and triallyl cyanurate.
[0159] Specific examples of aromatic vinyl compounds include styrene, α-methylstyrene, α-chloromethylstyrene, vinyltoluene, and divinylbenzene.
[0160] Specific examples of monofunctional (meth)acrylates include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, β-hydroxyethyl (meth)acrylate, and hydroxypropyl (meth)acrylate.
[0161] Specific examples of polyfunctional (meth)acrylates include ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, ethylene glycol di(meth)acrylate, trimethylolpropane di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and tri(meth)acrylate of tri(hydroxyethyl)isocyanurate.
[0162] Among them, as a reactive diluent (B), from the viewpoint of improving reactivity, polyfunctional (meth)acrylates are preferred, and more preferably at least one selected from pentaerythritol penta(meth)acrylate and pentaerythritol hexa(meth)acrylate.
[0163] Reactive diluent (B) can be used alone or in combination of two or more.
[0164] [Photopolymerization initiator (C)]
[0165] As a photopolymerization initiator (C), there are no particular limitations on any compound that generates free radicals through light irradiation. Examples of photopolymerization initiators (C) include, for instance, benzoin, benzoin methyl ether, benzoin ethyl ether, and other benzoin and their alkyl ethers; acetophenone, 2,2-dimethoxy-2-phenylacetophenone, 1,1-dichloroacetophenone, 4-(1-tert-butyldioxy-1-methylethyl)acetophenone, 1-hydroxycyclohexylphenyl ketone, 2-hydroxy-2-methyl-1-phenylpropane-1-one, and other alkyl acetones; anthraquinone compounds such as 2-methylanthraquinone, 2-pentylanthraquinone, 2-tert-butylanthraquinone, and 1-chloroanthraquinone; thioxanthone compounds such as 2,4-dimethylthioxanthone, 2,4-diisopropylthioxanthone, and 2-chlorothioxanthone; ketal compounds such as acetophenone dimethyl ketal and benzoyl dimethyl ketal; benzophenone, 4-(1- Benzophenone compounds such as tert-butyldioxy-1-methylethyl)benzophenone and 3,3',4,4'-tetra(tert-butyldioxycarbonyl)benzophenone; oxime esters such as 1,2-octanedione, 1-[4-(phenylthio)phenyl]-,2-(o-benzoyl oxime), acetone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl],1-(o-acetyl oxime); 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propane-1-one; 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone-1; acylphosphine oxides such as 2,4,6-trimethylbenzoyl diphenylphosphine oxide and bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide; Tonketone, etc. Photopolymerization initiators (C) can be used alone or in combination of two or more.
[0166] [Solvent (D)]
[0167] The solvent (D) is not particularly limited, but when the copolymer (A-1) is a (meth)acrylic acid copolymer, a glycol ether is preferred from the viewpoint of solubility. Specific examples include ethylene glycol monomethyl ether, diethylene glycol monomethyl ether, polyethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monoisopropyl ether, diethylene glycol monobutyl ether, ethylene glycol monoisobutyl ether, ethylene glycol monohexyl ether, ethylene glycol mono-2-ethylhexyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, 3-methoxy-1-butanol, 1,3-propanediol monoalkyl ether, 1,3-butanediol monoalkyl ether, 1,4-butanediol monoalkyl ether, etc. (poly(meth)acrylic acid) Alkylene glycol monoalkyl ethers; propylene glycol monoaryl ethers such as ethylene glycol monophenyl ether, ethylene glycol monobenzyl ether, and propylene glycol monophenyl ether; ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol methyl ethyl ether, diethylene glycol dibutyl ether, and dipropylene glycol dimethyl ether; and (poly)alkylene glycol monoalkyl ether acetates such as ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether acetate, and propylene glycol monoethyl ether acetate. Among these, from the viewpoint of ease of acquisition and reactivity, at least one selected from propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, and 3-methoxy-1-butanol is preferred, and more preferably at least one selected from propylene glycol monomethyl ether and propylene glycol monomethyl ether acetate. Solvent (D) can be used alone or in combination with two or more solvents.
[0168] Other specific examples of solvent (D) include monohydric alcohols other than (poly)alkylene glycol monoalkyl ethers. Specific examples of monohydric alcohols include primary alcohols such as propanol, butanol, pentanol, hexanol, octanol, nonanol, decanol, and dodecanol; secondary alcohols such as benzyl alcohol; and tertiary alcohols such as tert-butanol and diacetone alcohol.
[0169] Other specific examples of solvents (D) include other ethers such as tetrahydrofuran; ketones such as methyl ethyl ketone, cyclohexanone, 2-heptanone, and 3-heptanone; methyl 2-hydroxypropionate, ethyl 2-hydroxypropionate, methyl 2-hydroxy-2-methylpropionate, ethyl 2-hydroxy-2-methylpropionate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, ethyl ethoxypropionate, ethyl hydroxypropionate, methyl 2-hydroxy-3-methylbutyrate, and methyl 3-methyl-3-methoxybutylacetic acid ester. Esters such as 3-methyl-3-methoxybutylpropionate, ethyl acetate, n-butyl acetate, n-propyl acetate, isopropyl acetate, isobutyl acetate, n-pentyl acetate, isopentyl acetate, n-butyl propionate, ethyl butyrate, n-propyl butyrate, isopropyl butyrate, n-butyl butyrate, methyl pyruvate, ethyl pyruvate, n-propyl pyruvate, methyl acetoacetate, ethyl acetoacetate, ethyl 2-oxobutyrate; aromatic hydrocarbons such as toluene and xylene; and carboxylic amides such as N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide.
[0170] <Photosensitive Coloring Composition>
[0171] The photosensitive coloring composition comprises the above-described photosensitive resin composition and a colorant (E).
[0172] [Coloring agent (E)]
[0173] As the colorant (E), at least one selected from known dyes and pigments can be used. In the case of a color filter, from the viewpoint of color reproduction, a dye is preferred as the colorant (E). If a dye is used as the colorant (E), compared with the case of using a pigment, it tends to obtain a color pattern with higher brightness and a photosensitive coloring composition exhibiting good alkaline developability.
[0174] As dyes, considering factors such as solubility in solvents (D) and alkaline developing solutions, interaction with other components in the photosensitive coloring composition, and heat resistance, acid dyes having acidic groups such as carboxyl groups, salts of acid dyes and nitrogen compounds, and sulfonamide adducts of acid dyes are preferred. Examples of such dyes include, for instance, Acid Alizarin Violet N; Acid Black 1, 2, 24, 48; Acid Blue 1, 7, 9, 25, 29, 40, 45, 62, 70, 74, 80, 83, 90, 92, 112, 113, 120, 129, 147; and Solvent Blue 38, 44 (VALIFAST). BLUE 2620); Acid Chrome Violet K; Acid Magenta; Acid Green 1, 3, 5, 25, 27, 50; Acid Orange 6, 7, 8, 0, 12, 50, 51, 52, 56, 63, 74, 95; Acid Red 1, 4, 8, 14, 17, 18, 26, 27, 29, 31, 34, 35, 37, 42, 44, 50, 51, 52, 57, 69, 73, 80, 87, 88, 91, 92, 94, 97, 103, 111, 114, 129, 133, 134 138, 143, 145, 150, 151, 158, 176, 183, 198, 211, 215, 216, 217, 249, 252, 257, 260, 266, 274; Acid Violet 6B, 7, 9, 17, 19; Acid Yellow 1, 3, 9, 11, 17, 23, 25, 29, 34, 36, 42, 54, 72, 73, 76, 79, 98, 99, 111, 112, 114, 116; Food Yellow 3; Solvent Yellow 82 and their derivatives, etc. Among them, azo dyes are preferred. Acid dyes based on tonnes, anthraquinones, or phthalocyanines. Depending on the color of the target pixel, dyes can be used alone or in combination of two or more.
[0175] Examples of CI pigments include: Yellow (1, 3, 12, 13, 14, 15, 16, 17, 20, 24, 31, 53, 83, 86, 93, 94, 109, 110, 117, 125, 128, 137, 138, 139, 147, 148, 150, 153, 154, 166, 173, 194, 214); Orange (13, 31, 36, 38, 40, 42, 43, 51, 55, 59, 61, 64, 65, 71, 73); and Red (9, 97, 10). CI pigments include: 5, 122, 123, 144, 149, 166, 168, 176, 177, 180, 192, 209, 215, 216, 224, 242, 254, 255, 264, and 265 (red pigments); CI pigments include: 15, 15:3, 15:4, 15:6, and 60 (blue pigments); CI pigments include: 1, 19, 23, 29, 32, 36, and 38 (purple pigments); CI pigments include: 7, 36, and 58 (green pigments); CI pigments include: 23 and 25 (brown pigments); and CI pigments include: 1, 7 (black pigments), carbon black, titanium black, and iron oxide pigments. Pigments can be used individually or in combination of two or more, depending on the color of the target pixel.
[0176] When using pigments as colorants (E), from the viewpoint of improving the dispersibility of the pigments, known dispersants can be incorporated into the photosensitive coloring composition. As a dispersant, a polymeric dispersant with excellent dispersion stability over time is preferred. Examples of polymeric dispersants include, for instance, urethane-based dispersants, polyethyleneimine-based dispersants, polyoxyethylene alkyl ether-based dispersants, polyoxyethylene glycol diester-based dispersants, sorbitol aliphatic ester-based dispersants, and aliphatic modified ester-based dispersants. Such polymeric dispersants can be commercially available under trade names such as EFKA (EFKA Corporation), Disperbyk (Disperbyk Corporation), Disperon (Kusumoto Chemical Co., Ltd.), and SOLSPERSE (Loulizore Corporation). The content of the dispersant can be appropriately set according to the type and amount of pigment used as a colorant (E).
[0177] The content of colorant (E) in the photosensitive coloring composition is preferably 0.1 parts by mass or more, more preferably 3 parts by mass or more, further preferably 5 parts by mass or more, and even more preferably 10 parts by mass or more, relative to the total of 100 parts by mass of copolymer (A-1), copolymer (A-2), and reactive diluent (B). The content of colorant (E) in the photosensitive coloring composition is preferably 80 parts by mass or less, more preferably 70 parts by mass or less, and further preferably 60 parts by mass or less, relative to the total of 100 parts by mass of copolymer (A-1), copolymer (A-2), and reactive diluent (B). If the content of colorant (E) is 0.1 parts by mass or more, the effect of containing colorant (E) becomes significant, and a photosensitive coloring composition suitable as a coloring pattern for a color filter can be obtained. If the content of colorant (E) is 80 parts by mass or less, the colorant (E) does not hinder the curability of the photosensitive coloring composition, and a photosensitive coloring composition with good low-temperature curability can be obtained.
[0178] The content of solvent (D) in the photosensitive coloring composition is preferably 30 parts by mass or more, more preferably 50 parts by mass or more, even more preferably 100 parts by mass or more, preferably 1000 parts by mass or less, more preferably 700 parts by mass or less, and even more preferably 500 parts by mass or less, relative to 100 parts by mass of the total components other than solvent (D).
[0179] [Other additives]
[0180] The photosensitive resin composition or photosensitive coloring composition may contain one or more known additives such as leveling agents, heat-resistant polymerization inhibitors, and sensitizers, as needed. The content of the additives is not particularly limited, as long as it does not hinder the effects of the present invention.
[0181] <Content of each component in the photosensitive resin composition>
[0182] The content of copolymer (A-1) relative to the total of copolymer (A-1), copolymer (A-2) and reactive diluent (B) is preferably 10% by mass or more, more preferably 20% by mass or more, even more preferably 30% by mass or more, preferably 90% by mass or less, more preferably 80% by mass or less, and even more preferably 70% by mass or less.
[0183] The content of copolymer (A-1) relative to the total of 100 parts by mass of the components excluding solvent (D) is preferably 10 parts by mass or more, more preferably 20 parts by mass or more, even more preferably 25 parts by mass or more, preferably 70 parts by mass or less, more preferably 60 parts by mass or less, and even more preferably 50 parts by mass or less.
[0184] When the photosensitive resin composition contains copolymer (A-2), the content of copolymer (A-2) relative to the total of copolymer (A-1), copolymer (A-2) and reactive diluent (B) is preferably 10% by mass or more, more preferably 20% by mass or more, even more preferably 30% by mass or more, preferably 90% by mass or less, more preferably 80% by mass or less, and even more preferably 70% by mass or less.
[0185] When the photosensitive resin composition contains copolymer (A-2), the mass ratio of copolymer (A-1) to copolymer (A-2) is preferably 10:90 to 90:10, more preferably 20:80 to 80:20, and even more preferably 30:70 to 70:30.
[0186] When the photosensitive resin composition contains a reactive diluent (B), the content of the reactive diluent (B) relative to the total of copolymer (A-1), copolymer (A-2) and reactive diluent (B) is preferably 10% by mass or more, more preferably 20% by mass or more, even more preferably 30% by mass or more, preferably 90% by mass or less, more preferably 80% by mass or less, and even more preferably 70% by mass or less.
[0187] The content of photopolymerization initiator (C) relative to the total of 100 parts by mass of copolymer (A-1), copolymer (A-2) and reactive diluent (B) is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, even more preferably 1 part by mass or more, preferably 20 parts by mass or less, more preferably 10 parts by mass or less, and even more preferably 5 parts by mass or less.
[0188] The content of solvent (D) is preferably 30 parts by mass or more, more preferably 50 parts by mass or more, even more preferably 100 parts by mass or more, preferably 1000 parts by mass or less, more preferably 700 parts by mass or less, and even more preferably 500 parts by mass or less, relative to 100 parts by mass of the total components excluding solvent (D).
[0189] <Method for manufacturing copolymer (A-1)>
[0190] The copolymerization reaction of the synthetic copolymer (A-1) can be carried out in the presence or absence of a polymerization solvent according to free radical polymerization methods known in this art. For example, the polymerization reaction can be carried out at 40–100°C for 1–20 hours by dissolving the monomer in a solvent, adding a polymerization initiator to the solution, and then performing the polymerization reaction.
[0191] Examples of polymerization initiators suitable for this copolymerization reaction include azo-based thermal polymerization initiators such as azobisisobutyronitrile, azobisisovalerate, and 2,2'-azobis(2,4-dimethylvalerate); and peroxide-based thermal polymerization initiators such as benzoyl peroxide and tert-butyl peroxide. Polymerization initiators can be used alone or in combination of two or more.
[0192] When the total amount of monomer added is set to 100 parts by mass, the amount of polymerization initiator used is generally 0.5 to 30 parts by mass, preferably 1 to 25 parts by mass, and more preferably 5 to 20 parts by mass.
[0193] As a solvent for the copolymerization reaction, the same substance as solvent (D) described above can be used. Other examples include glycerol monoalkyl ethers, glycerol dialkyl ethers, methanol, ethanol, C5-6 cycloalkanediols, C5-6 cycloalkanediethanols, and ethyl lactate. Furthermore, "C5-6 cycloalkane" refers to a cycloalkyl group having 5 to 6 carbon atoms. The solvent can be used alone or in combination of two or more.
[0194] <Method for manufacturing photosensitive resin compositions and photosensitive coloring compositions>
[0195] The photosensitive resin composition and the photosensitive coloring composition can be manufactured by mixing the components using a known mixing apparatus.
[0196] When manufacturing a photosensitive resin composition or a photosensitive coloring composition, the reaction solution obtained during the manufacture of the copolymer (A-1) can be used directly as a raw material. In this case, the solvent (D) contained in the reaction solution can be used as part or all of the solvent (D) contained in the photosensitive resin composition or the photosensitive coloring composition. When manufacturing a photosensitive resin composition or a photosensitive coloring composition, the copolymer (A-1) obtained by separation from the reaction solution containing the copolymer (A-1) using a known method can be used as a raw material. In this case, regardless of the type and amount of solvent used in the manufacture of the copolymer (A-1), the type and content of the solvent (D) can be appropriately selected according to the type of copolymer (A-1), the intended use of the photosensitive resin composition or the photosensitive coloring composition, etc.
[0197] The photosensitive resin composition and photosensitive coloring composition exhibit excellent low-temperature curability because they contain copolymers (A-1) with structural units (a) containing hydroxyl groups and blocked isocyanate groups. Therefore, when a cured product is formed using the photosensitive resin composition or photosensitive coloring composition, curing can be achieved at a lower temperature compared to the case of using conventional resin compositions. Thus, when the photosensitive resin composition or photosensitive coloring composition, for example, is baked after exposure of a coating film formed on a substrate, the crosslinking reaction proceeds sufficiently even at a low baking temperature, thereby forming a cured product with excellent solvent resistance and hardness.
[0198] Therefore, when a cured product is formed using a photosensitive resin composition or a photosensitive coloring composition, the energy required for heating during curing is minimal. Furthermore, by using a photosensitive resin composition or a photosensitive coloring composition, a cured product can be formed on substrates with low heat resistance, such as resin substrates, without hindering the substrate. Moreover, even when using a substance with low heat resistance as the colorant (E), a cured product that exhibits the inherent properties of the colorant (E) can be formed.
[0199] Regarding photosensitive coloring compositions, even with low baking temperatures, cured products exhibiting excellent solvent resistance and hardness can be obtained, thus preventing the colorant (E) from leaching out of the cured product. Therefore, it is also possible to produce photosensitive coloring compositions with a high content of colorant (E). For example, when used as a material for coloring patterns in a color filter, a color filter with excellent color reproduction can be formed.
[0200] The copolymer (A-1) contained in the photosensitive resin composition or photosensitive coloring composition has good alkaline developability because it has structural units (c) with acid groups. Due to its excellent alkaline developability, such a photosensitive resin composition or photosensitive coloring composition can be formed, for example, by coating it onto a substrate to form a coated film, exposing it through a photomask corresponding to a predetermined pattern shape, developing the unexposed areas with an alkaline aqueous solution, and then baking it at a sufficiently low temperature, thereby forming a cured product with excellent solvent resistance and a predetermined pattern shape.
[0201] Based on these circumstances, photosensitive resin compositions and photosensitive coloring compositions are extremely useful as materials for components of image display elements such as pixels, black matrices, color filter protective films, light spacers, protrusions for liquid crystal alignment, microlenses, and insulating films for touch panels.
[0202] <Resin Cured Film>
[0203] One embodiment of the resin-cured film is a cured product of a photosensitive resin composition or a photosensitive coloring composition.
[0204] Resin-cured films can be manufactured, for example, by coating a substrate with a photosensitive resin composition or a photosensitive coloring composition, allowing the solvent (D) to evaporate and be removed, forming a coated film, exposing the coated film for photocuring, and then baking it. Resin-cured films can be manufactured using baking methods at low temperatures and exhibit excellent solvent resistance.
[0205] When forming a resin-cured film with a predetermined pattern shape, the following method can be used, for example. Specifically, a photosensitive resin composition or a photosensitive coloring composition is coated onto a substrate, and the solvent (D) is evaporated and removed to form a coated film. Next, the coated film is exposed to a photomask with a predetermined pattern shape to photocur the exposed portions. Then, the unexposed portions of the coated film are developed with an alkaline aqueous solution. Finally, the developed coated film is baked to form a resin-cured film with a predetermined pattern shape.
[0206] Known methods can be used for coating methods, exposure methods, and development methods of the photosensitive resin composition or photosensitive coloring composition used in manufacturing resin-cured films.
[0207] The baking conditions performed during the manufacture of the resin-cured film can be appropriately determined based on the composition of the photosensitive resin composition or photosensitive coloring composition, the film thickness of the coating film, the material of the substrate, etc. The baking process can be carried out, for example, at a temperature of 70°C to 250°C. If the baking temperature is 70°C or higher, the blocked isocyanate groups contained in the copolymer (A-1) are fully dissociated. This generates isocyanate groups, which undergo a crosslinking reaction with reactive functional groups. In the case where structural unit (a) has an alkyloxy carbonyl group, crosslinking occurs through transesterification. As a result, good curing degree is obtained, and a cured product with excellent solvent resistance and hardness can be obtained. In the case where structural unit (a) has an alkyloxy carbonyl group, both the deblocking reaction and the transesterification reaction can occur; by adjusting the baking temperature, either reaction can be preferentially carried out. The baking temperature is preferably 75°C or higher, more preferably 80°C or higher. If the baking temperature is below 250°C, it is a condition that materials with low heat resistance can tolerate, and discoloration of the photosensitive resin composition or photosensitive coloring composition can be suppressed, therefore this is preferred. The photosensitive resin composition and the photosensitive coloring composition have good low-temperature curing properties. Therefore, depending on the heat resistance of the substrate on which the resin-cured film is formed, the baking temperature can be below 160°C. For example, when using a resin substrate as the substrate, it can be below 150°C, below 120°C, or below 100°C.
[0208] The baking process performed during the manufacture of the resin-cured film can be, for example, 10 minutes to 4 hours, preferably 20 minutes to 2 hours, and can be appropriately determined according to the composition of the photosensitive resin composition or the photosensitive coloring composition, the baking temperature, the film thickness of the coating film, etc.
[0209] Resin-cured films are preferably used as components of transparent films, protective films, insulating films, outer coatings, light spacers, black matrices, black columnar spacers, and color filters.
[0210] <Color Filter>
[0211] One embodiment of the color filter includes a color pattern as a cured product of a photosensitive coloring composition. Preferably, the color filter includes a color pattern as a cured product of the photosensitive coloring composition, wherein the photosensitive coloring composition contains, relative to the total amount of copolymer (A-1), copolymer (A-2), and reactive diluent (B), 10 to 100% by mass of copolymer (A-1), more than 0% by mass and less than 90% by mass of reactive diluent (B), more than 0% by mass and less than 90% by mass of copolymer (A-2), 0.1 to 20 parts by mass of photopolymerization initiator (C), 3 to 80 parts by mass of colorant (E) relative to the total amount of copolymer (A-1), copolymer (A-2), and reactive diluent (B), and 30 to 1,000 parts by mass of solvent (D) relative to the total amount of components other than solvent (D).
[0212] A color filter may include, for example, a substrate, RGB pixels formed thereon, a black matrix formed at the boundaries of each pixel, and a protective film formed on the pixels and the black matrix.
[0213] In the color filter, at least a portion of the pixels and the black matrix is a color pattern that is a cured product of the aforementioned photosensitive coloring composition. In the color filter, the components other than the materials of the pixels and the black matrix can employ known configurations.
[0214] There are no particular limitations on the substrate used for color filters. Depending on the application, glass substrates, silicon substrates, polycarbonate substrates, polyester substrates, polyamide substrates, polyamide-imide substrates, polyimide substrates, aluminum substrates, printed wiring substrates, array substrates, etc., may be used.
[0215] <Method for Manufacturing Color Filters>
[0216] Next, the manufacturing method of an example color filter will be described. First, a color pattern is formed on a substrate. Specifically, a color pattern that forms a black matrix at the boundaries of each pixel and a color pattern that forms RGB pixels are sequentially formed on the substrate using the method shown below.
[0217] Colored patterns can be formed using photolithography. Specifically, a photosensitive coloring composition is coated onto a substrate to form a coating film. Then, the coating film is exposed to a photomask with a predetermined pattern shape to photocur the exposed portions. Next, the unexposed portions of the coating film are developed with an alkaline aqueous solution. Finally, the developed coating film is baked to form a colored pattern with a predetermined pattern shape.
[0218] There are no particular limitations on the coating method of the photosensitive coloring composition. Known methods such as screen printing, roller coating, curtain coating, spraying, and spin coating can be used.
[0219] Furthermore, after coating the substrate with a photosensitive coloring composition, the substrate can be heated using a circulating oven, infrared heater, hot plate, or other heating method as needed, thereby causing the solvent (D) contained in the coating film to evaporate and be removed. The conditions for heating the substrate to remove the solvent (D) are not particularly limited, and can be appropriately set according to the substrate material, the composition of the photosensitive coloring composition, and the thickness of the coating film. For example, the substrate can be heated at a temperature of 50°C to 120°C for 30 seconds to 30 minutes.
[0220] Next, the coated film formed in this way is partially exposed to active energy rays such as ultraviolet light or excimer laser through a negative photomask, and the exposed portion is photocured. The amount of active energy rays irradiating the coated film can be appropriately selected according to the composition of the photosensitive coloring composition, for example, it can be 30 to 2000 mJ / cm. 2 There are no particular limitations on the light source used for exposure; low-pressure mercury lamps, medium-pressure mercury lamps, high-pressure mercury lamps, xenon lamps, metal halide lamps, etc., can be used.
[0221] The alkaline aqueous solution used for developing the coated film is not particularly limited. It can be aqueous solutions of inorganic alkaline compounds such as sodium carbonate, potassium carbonate, calcium carbonate, sodium hydroxide, and potassium hydroxide; aqueous solutions of amine compounds such as ethylamine, diethylamine, and dimethylethanolamine; aqueous solutions of quaternary ammonium salts such as tetramethylammonium sulfate, hydrochloride, or p-toluenesulfonate; aqueous solutions of aniline compounds and their salts, such as 3-methyl-4-amino-N,N-diethylaniline, 3-methyl-4-amino-N-ethyl-N-β-hydroxyethylaniline, 3-methyl-4-amino-N-ethyl-N-β-methanesulfonamide ethylaniline, 3-methyl-4-amino-N-ethyl-N-β-methoxyethylaniline and their sulfates, hydrochlorides, or p-toluenesulfonates; and aqueous solutions of p-phenylenediamine compounds and their salts. Additionally, additives such as defoamers and surfactants can be added to the alkaline aqueous solution as needed.
[0222] Preferably, after developing the coated film using the above-mentioned alkaline aqueous solution, the coated film is washed with water and then dried.
[0223] The baking conditions performed during the manufacture of the color filter can be appropriately determined based on the composition of the photosensitive coloring composition, the film thickness of the coating film, the material of the substrate, etc. The baking temperature can be, for example, 70°C to 210°C. If the baking temperature is 70°C or higher, there is a tendency to obtain a cured product with good curability and excellent solvent resistance and hardness. The baking temperature is preferably 75°C or higher, more preferably 80°C or higher. If the baking temperature is 210°C or lower, materials with low heat resistance, such as substrates with low heat resistance, can be used as the material for the color filter, which is therefore preferred.
[0224] When using conventional photosensitive resin compositions to form color patterns for color filters, the hardness of the color pattern is insufficient if the baking temperature is below 200°C. In contrast, the photosensitive coloring composition of one embodiment has excellent low-temperature curing properties, thus ensuring the hardness of the color pattern, and allowing for a lower baking temperature compared to conventional photosensitive resin compositions. Specifically, depending on the heat resistance of the substrate forming the resin-cured film, the baking temperature can be below 160°C; for example, when using a resin substrate as the substrate to form the color pattern, it can be below 150°C, below 120°C, or below 100°C.
[0225] The baking process performed during the manufacture of the color filter can be, for example, 10 minutes to 4 hours, preferably 20 minutes to 2 hours, and can be appropriately determined according to the composition of the photosensitive coloring composition, the baking temperature, the film thickness of the coating film, etc.
[0226] The photosensitive coloring composition exhibits excellent photocurability and low-temperature curability. Therefore, when forming a coloring pattern using the photosensitive coloring composition of one embodiment, the baking time can be shortened and the color filter can be formed efficiently if the baking temperature is the same as that used when forming a coloring pattern using a conventional photosensitive resin composition.
[0227] After forming RGB pixels and a black matrix formed on the boundaries of each pixel using the above-described method for manufacturing RGB patterns, a protective film is formed on the RGB pixels and the black matrix.
[0228] The method of manufacturing the protective film is not particularly limited. It can be formed using the photosensitive resin composition or photosensitive coloring composition of one embodiment, or it can be formed using known materials and known methods.
[0229] The color filter is obtained through the above process.
[0230] The color filter has a color pattern that is a cured product of the aforementioned photosensitive coloring composition. Therefore, the color pattern in the color filter can be formed by baking at a low temperature. Thus, the energy required for the baking process can be reduced.
[0231] Furthermore, the colorant (E) contained in the photosensitive coloring composition used as the material for the color filter can be a substance with low heat resistance. Therefore, a wider selection of colorants (E) can be used. Thus, for example, a color filter can be formed that contains a colorant (E) with low heat resistance and has a coloring pattern that exhibits the inherent properties of the colorant (E) with low heat resistance.
[0232] Furthermore, the color patterns in the color filter can be formed on substrates with low heat resistance, such as resin substrates, without hindering the substrate. Therefore, a wider range of substrate options can be used. Specifically, for example, since the color filter can be formed on substrates with low heat resistance, such as resin substrates, the flexibility of the display is possible. In addition, the color patterns in the color filter exhibit excellent solvent resistance and hardness, resulting in minimal color variation.
[0233] Here, an example is given of a case in which a color pattern is created by using a photosensitive coloring composition containing a photopolymerization initiator (C) and photocuring the photosensitive coloring composition. However, for example, a color pattern can also be formed as a cured product of a photosensitive coloring composition containing a copolymer (A-1) by using a photosensitive coloring composition containing a curing accelerator and a known epoxy resin instead of the photopolymerization initiator (C) contained in the photosensitive coloring composition, applying it to a substrate by inkjet printing and then heating it.
[0234] <Image display element>
[0235] One embodiment of the image display element includes a color filter. In the image display element, known configurations can be used as components other than the color filter. Specific examples of image display elements include solid-state imaging elements such as liquid crystal display elements, organic EL display elements, CCD elements, and CMOS elements.
[0236] The components of an image display element, excluding the color filter, can be manufactured using known methods. For example, when manufacturing a liquid crystal display element as an image display element, the following method can be used. First, a color filter is formed on a substrate using the method described above. Then, electrodes, spacers, etc., are sequentially formed on the substrate having the color filter. Next, electrodes, etc., are formed on another substrate, and they are arranged opposite to and bonded to the substrate having the color filter. Then, a predetermined amount of liquid crystal is injected between the opposing substrates for sealing.
[0237] Image display elements exhibit minimal color variation due to their color filters, which possess excellent solvent resistance and hardness.
[0238] Example
[0239] The present invention will be further described in detail below through examples and comparative examples, but the present invention is not limited to the following examples.
[0240] <Determination of Acid Value>
[0241] According to JIS K6901:2008 5.3.2, the number of mg of potassium hydroxide required to neutralize the acidic components contained in 1g of the copolymer was determined.
[0242] Measuring instrument: 776 Dosimat (Metrohm)
[0243] Mixed indicator: A mixed indicator of bromothymol blue and phenol red.
[0244] The following shows an example of the synthesis of copolymer (A-1).
[0245] [Synthesis example 1]
[0246] 124.4 g of propylene glycol monomethyl ether as solvent (D) was added to a flask equipped with a stirring device, dropping funnel, condenser, thermometer and gas inlet tube. The mixture was stirred while being purged with nitrogen and heated to 78 °C.
[0247] Next, 32.7 g (16 mol%) of AOI-DEM as monomer (ma), 18.9 g (16 mol%) of PE-90 as monomer (mb), 6.4 g (11 mol%) of methacrylic acid as monomer (mc), 68.1 g (57 mol%) of benzyl methacrylate as monomer (md), 15.3 g (12.1 parts by mass relative to the total of 100 parts by mass of the above monomer components) of V-65 (Fuji Film Wako Pure Medicine Co., Ltd.) as polymerization initiator, and 80.8 g of propylene glycol monomethyl ether acetate and 41.6 g of propylene glycol monomethyl ether as solvent (D) were mixed to prepare a raw material monomer solution.
[0248] The entire volume of the prepared monomer solution was added dropwise over 1 hour using a dropping funnel to solvent (D) in a flask under a nitrogen atmosphere at atmospheric pressure. After the addition was complete, the solution in the flask was stirred and polymerized at 78°C for 3 hours to obtain a reaction solution containing copolymer (A-1) and solvent (D). Propylene glycol monomethyl ether acetate, excluding the solvent, was added to the reaction solution obtained in this manner as solvent (D) at a concentration of 35% by mass to obtain the liquid containing copolymer (A-1) of Synthesis Example 1.
[0249] [Synthetic Examples 2-29, Comparative Synthetic Examples 1-3]
[0250] Using the monomers, solvent (D), and polymerization initiator and their mixing amounts as described in Table 1, except that the same procedures were followed as in Synthesis Example 1, to obtain the liquids containing copolymer (A-1) of Synthesis Examples 2-29 and the liquids containing copolymer (cA-1) of Comparative Synthesis Examples 1-3. Furthermore, the amount of polymerization initiator added was adjusted according to the desired weight-average molecular weight.
[0251] The weight-average molecular weight, molecular weight distribution, blocked isocyanate equivalent, hydroxyl equivalent, and acid value of the copolymers (A-1) of Synthetic Examples 1-29 and the copolymers (cA-1) of Comparative Synthetic Examples 1-3 are shown in Table 1.
[0252] [Table 1-1]
[0253] [Table 1-2]
[0254] [Table 1-3]
[0255] [Table 1-4]
[0256] [Table 1-5]
[0257] [Table 1-6]
[0258] The following shows an example of the synthesis of copolymer (A-2).
[0259] [Synthesis Example 30]
[0260] 260.1 g of propylene glycol monomethyl ether acetate as solvent (D) was added to a flask equipped with a stirring device, dropping funnel, condenser, thermometer and gas inlet tube. The mixture was stirred while being purged with nitrogen and heated to 118 °C.
[0261] Next, 228.3 g (80 mol%) of glycidyl methacrylate, 44.2 g (10 mol%) of dicyclopentyl methacrylate, 35.4 g (10 mol%) of benzyl methacrylate, 16.8 g of TBO (tert-butyl peroxide, polymerization initiator) (5.5 parts by mass relative to the total 100 parts by mass of the above monomer components) and 141.7 g of propylene glycol monomethyl ether acetate as solvent (D) were mixed to prepare a raw material monomer solution.
[0262] The entire volume of the prepared raw material monomer solution was added dropwise over 1 hour using a dropping funnel to solvent (D) in a flask under a nitrogen atmosphere at atmospheric pressure. After the addition was complete, the solution in the flask was stirred and polymerized at 120°C for 2 hours to obtain a liquid containing the copolymer precursor and solvent (D).
[0263] In a flask containing the copolymer precursor and solvent (D) under atmospheric pressure and an atmosphere of 6 mol% oxygen, 1.3 g (0.3 parts by mass relative to 100 parts by mass of the monomer content of the copolymer precursor and acrylic acid) of hydroquinone monomethyl ether (MEHQ) as an inhibitor, 1.3 g (0.3 parts by mass relative to 100 parts by mass of the monomer content of the copolymer precursor and acrylic acid) of tri-p-tolylphosphine (Hokuko Sangyo Co., Ltd.) and 112.3 g (80 mol relative to 100 mol relative to the monomer content of the copolymer precursor) of acrylic acid as a catalyst were added, and the mixture was stirred and kept at 120°C for 720 minutes. Next, 64.3 g (32 mol relative to 100 mol relative to the monomer content of the copolymer precursor) of succinic anhydride was added, and the mixture was stirred and kept at 115°C for 120 minutes to obtain a reaction solution containing copolymer (A-2) and solvent (D).
[0264] In the reaction solution containing copolymer (A) and solvent (D) obtained by such operation, propylene glycol monomethyl ether acetate (Tokyo Chemical Industry Co., Ltd.) as solvent (D) was added in such a way that the components other than solvent were 45% by mass, and the liquid containing copolymer (A-2) of Synthesis Example 30 was obtained.
[0265] [Synthesis Example 31]
[0266] Using the raw materials and their mixing amounts listed in Table 2, except that the same procedure was followed as in Synthesis Example 30, the liquid containing copolymer (A-2) of Synthesis Example 31 was obtained.
[0267] [Synthesis Example 32]
[0268] 229.1 g of propylene glycol monomethyl ether acetate as solvent (D) was added to a flask equipped with a stirring device, dropping funnel, condenser, thermometer and gas inlet tube. The mixture was stirred while being purged with nitrogen and heated to 118 °C.
[0269] Next, 52.6 g (10 mol%) of dicyclopentyl methacrylate, 176.7 g (42 mol%) of benzyl methacrylate, 98.7 g (48 mol%) of methacrylic acid, 19.7 g of TBO (tert-butyl peroxide, polymerization initiator) (6.0 parts by mass relative to the total 100 parts by mass of the above monomer components) and 105.0 g of propylene glycol monomethyl ether acetate as solvent (D) were mixed to prepare a raw material monomer solution.
[0270] The entire volume of the prepared raw material monomer solution was added dropwise over 1 hour using a dropping funnel to solvent (D) in a flask under a nitrogen atmosphere at atmospheric pressure. After the addition was complete, the solution in the flask was stirred and polymerized at 120°C for 2 hours to obtain a liquid containing the copolymer precursor and solvent (D).
[0271] In a flask containing the copolymer precursor and solvent (D) under atmospheric pressure and an atmosphere of 6 mol% oxygen, 1.1 g (0.3 parts by mass relative to 100 parts by mass of monomeric components of the copolymer precursor and glycidyl methacrylate) of hydroquinone monomethyl ether (MEHQ) as an inhibitor, 1.1 g (0.3 parts by mass relative to 100 parts by mass of monomeric components of the copolymer precursor and glycidyl methacrylate) of tri-p-tolylphosphine (Hokuko Sangyo Co., Ltd.) and 52.3 g (15 mol relative to 100 mol of monomeric components of the copolymer precursor) of glycidyl methacrylate as a catalyst were added, and the mixture was stirred and kept at 120°C for 300 minutes.
[0272] In the reaction solution containing copolymer (A-2) and solvent (D) obtained by such operation, propylene glycol monomethyl ether acetate (Tokyo Chemical Industry Co., Ltd.) as solvent (D) was added in such a way that the components other than solvent were 40% by mass, and the liquid containing copolymer (A-2) of Synthesis Example 32 was obtained.
[0273] [Synthesis Example 33]
[0274] Using the raw materials and their mixing amounts listed in Table 2, except that the same procedure was followed as in Synthesis Example 32, the liquid containing copolymer (A-2) of Synthesis Example 33 was obtained.
[0275] The weight-average molecular weight, acid value, and unsaturated group equivalent of the copolymers (A-2) of Synthetic Examples 30-33 are shown in Table 2.
[0276] [Table 2]
[0277] The following substances were used as compounds listed in Tables 1 and 2, respectively.
[0278] AOI-DEM: The product of the reaction between CARENZ (trademark) AOI (2-isocyanate ethyl acrylate, Rezonack Co., Ltd.) and diethyl malonate (malonate-2-[[[[2-[1-oxo-2-propenyl]oxy]ethyl]amino]carbonyl]-1,3-diethyl ester)
[0279] MOI-DEM: A product of the reaction between CARENZ (trademark) MOI (2-isocyanate-ethyl methacrylate, Rezonack Co., Ltd.) and diethyl malonate (malonate-2-[[[[2-[2-methyl-1-oxo-2-propenyl]oxy]ethyl]amino]carbonyl]-1,3-diethyl malonate).
[0280] AOI-DMM: CARENZ (trademark) AOI (2-isocyanate ethyl acrylate, Rezonack Co., Ltd.) reacts with dimethyl malonate, (malonate-2-[[[[2-[1-oxo-2-propenyl]oxy]ethyl]amino]carbonyl]-1,3-dimethyl ester)
[0281] AOI-BP: CARENZ (trademark) AOI (2-isocyanate-based ethyl acrylate, Rezonack Co., Ltd.) reacts with 3,5-dimethylpyrazole to form (2-[(3,5-dimethylpyrazole)carbonylamino]ethyl acrylate).
[0282] AOI-AM: CARENZ (trademark) AOI (2-isocyanate ethyl acrylate, Rezonack Co., Ltd.) reacts with methyl 4-hydroxybenzoate to form (4-[[[[[(1-oxo-2-propen-1-yl)oxy]ethyl]amino]carbonyl]oxy]-methyl benzoate)
[0283] PE-90: Polyethylene glycol monomethacrylate, product name Bremmer PE-90, EO units: approx. 2, Nippon Oil Co., Ltd.
[0284] PE-200: Polyethylene glycol monomethacrylate, product name Bremmer PE-200, EO unit: approx. 4.5, Nippon Oil Co., Ltd.
[0285] PE-350: Polyethylene glycol monomethacrylate, product name Bremmer PE-350, EO units: approx. 8, Nippon Oil Co., Ltd.
[0286] AE-200: Polyethylene glycol monoacrylate, product name Bremmer AE-200, EO unit: approx. 4.5, Nippon Oil Co., Ltd.
[0287] AP-400D: Polypropylene glycol monoacrylate, product name: Bream AP-400D, PO unit: approx. 6, Nippon Oil Co., Ltd.
[0288] PP-1000: Polypropylene glycol monomethacrylate, product name Bremmer PP-1000, PO unit: approx. 4-6, Nippon Oil Co., Ltd.
[0289] 10PPB-500B: Propylene glycol polybutylene glycol monomethacrylate, product name Bremmer-10PPB-500B, BO unit: approx. 6, Nippon Oil Co., Ltd.
[0290] 55PET-800: Polyethylene glycol-1,4-butanediol-monomethacrylate, product name Bremmer 55PET-800, EO units: approx. 10, BO units: approx. 5, Nippon Oil Co., Ltd.
[0291] PME-200: Methoxylated polyethylene glycol methacrylate, product name Bremmill PME-200, EO units: approx. 4, Nippon Oil Co., Ltd.
[0292] HEMA: 2-Hydroxyethyl methacrylate, Tokyo Chemical Industry Co., Ltd.
[0293] 4HBA: 4-Hydroxybutyl acrylate, Tokyo Chemical Industry Co., Ltd.
[0294] MAA: Methacrylic acid, Tokyo Chemical Industry Co., Ltd.
[0295] AA: Acrylic acid, Tokyo Chemical Industry Co., Ltd.
[0296] HOMS(N): 2-Methylacryloyloxyethylsuccinic acid, product name Light Ester HO-MS(N), Kyoei Chemical Co., Ltd.
[0297] BZMA: Benzyl methacrylate, Tokyo Chemical Industry Co., Ltd.
[0298] 2EHA: 2-Ethylhexyl acrylate, Tokyo Chemical Industry Co., Ltd.
[0299] MMA: Methyl methacrylate, Tokyo Chemical Industry Co., Ltd.
[0300] SM: Styrene
[0301] TCDMA: Dicyclopentyl methacrylate, Tokyo Chemical Industry Co., Ltd.
[0302] GMA: Glycidyl methacrylate
[0303] PhMI: Phenyl maleimide, Tokyo Chemical Industry Co., Ltd.
[0304] PGMEA: Propylene glycol monomethyl ether acetate, Tokyo Chemical Industry Co., Ltd.
[0305] PGME: Propylene glycol monomethyl ether, Tokyo Chemical Industry Co., Ltd.
[0306] MB: 3-Methoxy-1-Butanol, Tokyo Chemical Industry Co., Ltd.
[0307] V-65: 2,2'-azobis(2,4-dimethylvaleronitrile) (Fuji Fiber Wako Junyu Co., Ltd.)
[0308] SA: Succinic anhydride (Tokyo Chemical Industry Co., Ltd.)
[0309] <Preparation of Photosensitive Coloring Compositions>
[0310] [Examples 1-34, Comparative Examples 1-3]
[0311] The copolymers of Synthetic Examples 1-29 (A-1), or the copolymers of Comparative Synthetic Examples 1-3 (cA-1), and the copolymers of Synthetic Examples 30-33 (A-2), dipentaerythritol pentaacrylate (Toa Synthetic Co., Ltd.) as reactive diluent (B), and acetone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl-]-,-1-(O-acetyl oxime)(chiba) as photopolymerization initiator (C) were used. A mixture of propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, or 3-methoxy-1-butanol (338 parts by mass and 257 parts by mass, respectively) as solvent (D), and Valifast Blue 2620 (phthalocyanine dye, Original Chemical Industries, Ltd.) as colorant (E) was mixed in the proportions shown in Table 3 to prepare the photosensitive coloring compositions of Examples 1-34 and Comparative Examples 1-3. The amounts of copolymer (A-1) or (cA-1) and copolymer (A-2) mixed in Table 3 do not include the amount of solvent. The amount of solvent (D) mixed in Table 3 is the total amount of solvent contained in the liquid containing copolymer (A-1) or copolymer (cA) obtained in the synthetic examples or comparative synthetic examples, the solvent contained in the liquid containing copolymer (A-2), and the solvent added when preparing the photosensitive coloring compositions.
[0312] [Table 3-1]
[0313] [Table 3-2]
[0314] [Table 3-3]
[0315] [Table 3-4]
[0316] <Evaluation of Photosensitive Coloring Compositions>
[0317] The photosensitive coloring compositions of Examples 1-34 and Comparative Examples 1-3 were evaluated using the methods shown below.
[0318] [Evaluation of solvent resistance]
[0319] Solvent resistance was evaluated using residual film yield.
[0320] (residual film rate)
[0321] The photosensitive coloring compositions of Examples 1-34 and Comparative Examples 1-3 were each spin-coated onto a 5cm x 5cm square alkali-free glass substrate to form a coating film with a thickness of 2.5μm after exposure. The coating film was then heated at 100°C for 3 minutes to evaporate and remove the solvent (D) from the coating film.
[0322] Next, with an energy radiation dose of 100 mJ / cm 2 The coated film was exposed to ultraviolet light with a wavelength of 365 nm for photocuring. Then, it was baked at 85°C for 30 minutes to cure the coating film, thus forming a cured film. The thickness of the cured film was measured using a profilometer. This thickness is designated as X.
[0323] The prepared cured film was then immersed in 20g of propylene glycol monomethyl ether acetate (PGMEA) at 23°C for 15 minutes. After vacuum drying the cured film at 40°C for 30 minutes, the thickness of the cured film was measured using a step meter. This thickness is denoted as Y.
[0324] The solvent resistance of the cured film was evaluated by calculating the residual film rate as the ratio of the thickness Y of the cured film after PGMEA impregnation to the thickness X of the cured film before PGMEA impregnation. That is, the closer the residual film rate is to 100%, the better the solvent resistance of the cured film. As an evaluation criterion, a residual film rate of 70% or higher was set as the passing grade. The residual film rates of the cured films are shown in Table 3.
[0325] Residual film rate = (Y / X) × 100 (%)
[0326] As shown in Table 3, the residual film rate (%) of the cured film of the photosensitive coloring compositions of Examples 1 to 34 after PGMEA impregnation is more than 70%, and the solvent resistance is good even at a low temperature of 85°C during baking treatment.
[0327] [Evaluation of radioactivity]
[0328] The developability was evaluated by the solubility and adhesion of the cured film.
[0329] (Solubility)
[0330] The photosensitive coloring compositions prepared in Examples 1-34 and Comparative Examples 1-3 were coated onto 5 cm square alkali-free glass substrates using a spin coating method to achieve a thickness of 1.5 μm after exposure (coating process). The coated glass substrates were then heated at 100°C for 3 minutes to evaporate the solvent and dry the coating film (pre-baking process).
[0331] Next, an ultra-high pressure mercury lamp was used to apply 100 mJ / cm 2 Light was irradiated onto the surface of the dried coated film via a photomask (exposure process). The photomask was positioned 100 μm away from the coated film during the exposure process. A material with a line and gap pattern of 3–100 μm width was used as the photomask. Next, Semiclean DL-A10 developer (Yokohama Yushi Kogyo Co., Ltd.) (300-fold dilution) was sprayed onto the surface of the coated film for 60 seconds at 23°C and 0.1 MPa to remove unexposed areas (development process). The dissolution morphology of the coated film after spraying the developer was observed, and the solubility was evaluated using the following criteria. The results are shown in Table 3.
[0332] 1. No residue was found in the unexposed areas, no powder was observed in the developer, and the pattern shape was good.
[0333] 2: Although there was no residue in the unexposed area, powder was observed in the developer, and the pattern shape was relatively good.
[0334] 3: Residues remain in the unexposed areas, and there are defects in the pattern shape.
[0335] 4: No pattern remains in the exposure section.
[0336] (Seamless fit)
[0337] A colored pattern was obtained by placing a glass substrate with a coated film after the development process in a dryer at 100°C for 30 minutes to thermally cure the coated film (post-baking process). The colored pattern obtained in this way was observed under a microscope, and the adhesion was evaluated by the minimum developable linewidth, i.e., the minimum developable size (μm). The results are shown in Table 3. Comparative Examples 1-3 were not evaluated because no pattern remained.
[0338] [Storage stability of photosensitive coloring compositions]
[0339] The storage stability of the photosensitive coloring compositions of Examples 1-34 and Comparative Examples 1-3 was evaluated according to the following method. 10g of each of the photosensitive coloring compositions of Examples 1-34 and Comparative Examples 1-3 were weighed into 20mL glass containers, and the viscosity was measured to determine the viscosity before storage. The viscosity was measured using an E-type viscometer (RE-80, rotor 1°34'×R24, Toki Sangyo Co., Ltd.) at 25°C and 20rpm. Each sample was then stored in a thermostat maintained at 12°C for 3 months. The viscosity was then measured again using the same method described above to determine the viscosity after storage. The thickening rate was calculated using the viscosity before and after storage using the following formula, and evaluated according to the criteria shown below. The results are shown in Table 3.
[0340] Thickening rate (%) = (([viscosity after storage] - [viscosity before storage]) / [viscosity before storage]) × 100
[0341] (Evaluation criteria for thickening rate)
[0342] Excellent: Thickening rate less than 10%
[0343] Good: Thickening rate 10-20%
[0344] Undesirable: Thickening rate exceeds 20%.
Claims
1. A photosensitive resin composition containing copolymer (A-1), copolymer (A-2), Photopolymerization initiator (C), and Solvent (D), The copolymer (A-1) contains hydroxyl, Structural units with blocked isocyanate groups (a) Structural unit (b) having a partial structure as shown in equation (1) below, and Structural units (c) containing acid groups, The copolymer (A-2) has an unsaturated group equivalent of 30–3000 g / mol. In equation (1), R 1 It is a divalent hydrocarbon group, and n1 represents an integer from 2 to 20.
2. A photosensitive resin composition containing copolymer (A-1), Reactive diluent (B), Photopolymerization initiator (C), and Solvent (D), The copolymer (A-1) contains hydroxyl, Structural units with blocked isocyanate groups (a) Structural unit (b) having a partial structure as shown in equation (1) below, and Structural units (c) containing acid groups, In equation (1), R 1 It is a divalent hydrocarbon group, and n1 represents an integer from 2 to 20.
3. A photosensitive resin composition containing copolymer (A-1), copolymer (A-2), Reactive diluent (B), Photopolymerization initiator (C), and Solvent (D), The copolymer (A-1) contains hydroxyl, Structural units with blocked isocyanate groups (a) Structural unit (b) having a partial structure as shown in equation (1) below, and Structural units (c) containing acid groups, The copolymer (A-2) has an unsaturated group equivalent of 30–3000 g / mol. In equation (1), R 1 It is a divalent hydrocarbon group, and n1 represents an integer from 2 to 20.
4. The photosensitive resin composition according to any one of claims 1 to 3, wherein R in formula (1) 1 It consists of hydrocarbon groups with 2 to 6 carbon atoms.
5. The photosensitive resin composition according to any one of claims 1 to 3, wherein R in formula (1) 1 It is a hydrocarbon group with 2 or 3 carbon atoms, and n1 is an integer from 2 to 6.
6. The photosensitive resin composition according to any one of claims 1 to 3, wherein the structural unit (b) has a group represented by the following formula (2), In equation (2), R 1 It is a divalent hydrocarbon group, and n1 represents an integer from 2 to 20.
7. The photosensitive resin composition according to any one of claims 1 to 3, wherein the structural unit (a) is a structural unit having at least one group selected from the groups shown in formula (3) and formula (4) below. In equation (3), R 2 and R 3 Each of n1 and n2 independently represents an alkyl group with 1 to 10 carbon atoms, and each of n3 independently represents an integer from 0 to 2. Indicates the connection point. In equation (4), R 4 and R 5 Each of these characters independently represents an alkyl group with 1 to 10 carbon atoms, and n4 and n5 independently represent integers from 0 to 2. Indicates the connection point.
8. The photosensitive resin composition according to any one of claims 1 to 3, wherein the blocking agent constituting the blocked isocyanate group of the structural unit (a) is selected from at least one of pyrazole compounds, oxime compounds and phenolic compounds.
9. The photosensitive resin composition according to any one of claims 1 to 3, wherein the copolymer (A-1) further contains other structural units (d).
10. The photosensitive resin composition according to any one of claims 1 to 3, wherein the equivalent of blocked isocyanate groups in the copolymer (A-1) is 200 to 3000 g / mol. Furthermore, its hydroxyl equivalent is 100–5000 g / mol.
11. The photosensitive resin composition according to any one of claims 1 to 3, wherein the copolymer (A-1) has an acid value of 5 to 400 KOH mg / g. Furthermore, its weight-average molecular weight is 3,000–50,000.
12. The photosensitive resin composition according to any one of claims 1 to 3, wherein in all structural units of the copolymer (A-1), The content of the structural unit (a) is 1 to 50 mol%. The content of the structural unit (b) is 1–70 mol%. The content of the structural unit (c) is 1 to 70 moles.
13. A photosensitive coloring composition comprising the photosensitive resin composition according to any one of claims 1 to 3 and a colorant (E).
14. A resin-cured film, which is a cured product of the photosensitive resin composition according to any one of claims 1 to 3.
15. A color filter having a color pattern as a cured product of the photosensitive coloring composition of claim 13.
16. An image display element comprising the color filter of claim 15.
Citation Information
Patent Citations
Photosensitive resin composition, cured film, and method for producing the same
JP2019053266A