Liquid immersion cooling device
By configuring a second resin layer containing fluorinated resin and (meth)acrylic resin on the first resin layer of the electronic component, the problem of resin layer degradation due to coolant in liquid immersion cooling devices is solved, thereby achieving protection of the electronic component and improving cooling efficiency.
Patent Information
- Application Number
- CN202580029698.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-09-06
- Filing Date
- 2025-04-17
- Publication Date
- 2026-11-17
AI Technical Summary
In existing liquid immersion cooling devices, the resin layer of electronic components deteriorates due to the coolant, leading to damage to the electronic components.
A second resin layer comprising at least one selected from vinyl chloride resin, epoxy resin, polyimide resin, silicone resin, olefin resin, ethylene propylene diene rubber, ethylene vinyl acetate copolymer and polyester resin is disposed on the first resin layer of the electronic component. The second resin layer comprises fluorinated resin and (meth)acrylic resin and has a thickness of 50 nm to 100 μm, and is used to protect the first resin layer.
It effectively inhibits resin layer degradation caused by coolant, and improves the durability and cooling efficiency of electronic components.
Smart Images

Figure CN123125559A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a liquid immersion cooling device. Background Technology
[0002] As a cooling method for electronic components that make up servers, supercomputers, etc., air cooling and liquid immersion cooling are known. From the point of view of superior cooling efficiency, liquid immersion cooling has attracted attention in recent years.
[0003] Patent Document 1 discloses a method for cooling a substrate disposed within a container using a liquid immersion cooling device having a container containing a coolant, a pump unit having a heat exchanger and a liquid pump, and a cooling device having a fan.
[0004] Existing technical documents
[0005] Patent documents
[0006] Patent Document 1: Japanese Patent Application Publication No. 2023-000068 Summary of the Invention
[0007] The problem the invention aims to solve
[0008] The inventors have discovered that, when using the liquid immersion cooling device described in Patent Document 1, the resin layer of electronic components may deteriorate due to the coolant. Thus, if the resin layer of the electronic component deteriorates, it can sometimes lead to damage to the electronic component itself.
[0009] The present invention was made in view of the above-mentioned problems, and the problem is to provide a liquid immersion cooling device that suppresses the deterioration of the resin layer of electronic components caused by coolant.
[0010] Solution for solving the problem
[0011] The inventors conducted in-depth research on the above-mentioned issues and found that by configuring a second resin layer comprising at least one of the groups selected from fluorinated resins and (meth)acrylic resins on the first resin layer of the electronic component, the degradation of the resin layer of the electronic component caused by the coolant can be suppressed, thereby completing the present invention.
[0012] That is, the inventors discovered that the above-mentioned problems can be solved by the following configuration.
[0013] [1] A liquid immersion cooling device comprising: a coolant; a container having the coolant inside; and an electronic component that is in contact with the coolant at least in a portion of the container.
[0014] At least a portion of the surface of the aforementioned electronic component has a first resin layer, the first resin layer comprising at least one selected from the group consisting of vinyl chloride resin, epoxy resin, polyimide resin, silicone resin, olefin resin, ethylene propylene diene rubber, ethylene vinyl acetate copolymer, and polyester resin.
[0015] A second resin layer is disposed on at least a portion of the surface of the first resin layer, the second resin layer comprising at least one selected from the group consisting of fluorinated resins and (meth)acrylic resins.
[0016] [2] According to the liquid immersion cooling device of [1], the second resin layer comprises the fluorinated resin.
[0017] [3] According to the liquid immersion cooling device of [1] or [2], wherein the electronic component includes a component selected from the group consisting of a printed circuit board and a cable.
[0018] At least a portion of the surface of the aforementioned component is composed of the aforementioned first resin layer.
[0019] [4] The immersion cooling apparatus according to any one of [1] to [3], wherein the fluorinated resin comprises a fluoroolefin-based unit.
[0020] [5] The immersion cooling apparatus according to any one of [1] to [4], wherein the fluorinated resin comprises a trifluorochloroethylene-based unit and a vinyl ether-based unit.
[0021] [6] The liquid immersion cooling apparatus according to any one of [1] to [5], wherein the thickness of the second resin layer is 50 nm to 100 μm.
[0022] [7] The liquid immersion cooling apparatus according to any one of [1] to [6], wherein the standard boiling point of the coolant is 45 to 450°C.
[0023] [8] The liquid immersion cooling apparatus according to any one of [1] to [7], wherein the coolant is selected from at least one of the groups consisting of fluorinated compounds and hydrocarbon compounds.
[0024] [9] The liquid immersion cooling apparatus according to any one of [1] to [8], wherein the GWP of the coolant is 0 to 7500.
[0025] The effects of the invention
[0026] According to the present invention, a liquid immersion cooling device is provided that suppresses the deterioration of the resin layer of electronic components caused by coolant. Attached Figure Description
[0027] Figure 1This is a schematic diagram illustrating one aspect of the liquid immersion cooling apparatus of the present invention. Detailed Implementation
[0028] The meanings of the terms used in this invention are as follows.
[0029] The numerical range indicated by "~" refers to the range of values recorded before and after "~" as the lower and upper limits. Within the numerical ranges described in this specification, the upper or lower limit recorded in a particular numerical range can be replaced with the upper or lower limit of another numerical range described in another stage. Furthermore, within the numerical ranges described in this specification, the upper or lower limit recorded in a particular numerical range can also be replaced with the values shown in the embodiments.
[0030] In this specification, each component may be used alone with one equivalent substance, or with two or more substances used in combination. When two or more substances are used in combination for each component, the content of that component, unless otherwise specified, refers to the total content of the substances used in combination.
[0031] In this specification, a combination of two or more preferred methods is a more preferred method.
[0032] A unit refers to a group of atoms directly formed through the polymerization of monomers, based on one molecule of the aforementioned monomer, and the group of atoms obtained by chemical transformation of a portion of the aforementioned group of atoms. The content (molar percentage) of each unit relative to all units contained in the resin can be determined by analyzing the resin using nuclear magnetic resonance spectroscopy, or it can be determined by the amount of components used in the manufacture of the resin.
[0033] (Meth)acrylic resins are a general term for acrylic resins and methacrylic resins.
[0034] The thickness of the second resin layer was measured using a probe-type film thickness gauge (SANKO ELECTRONIC LABORATORY CO., LTD, SWT9300).
[0035] The liquid immersion cooling device of the present invention includes: a coolant; a container having the coolant inside; and an electronic component in the container, at least a portion of which is in contact with the coolant, wherein at least a portion of the surface of the electronic component has a first resin layer comprising at least one selected from the group consisting of vinyl chloride resin, epoxy resin, polyimide resin, silicone resin, olefin resin, ethylene propylene diene rubber, ethylene vinyl acetate copolymer, and polyester resin, and a second resin layer is disposed on the surface of at least a portion of the first resin layer, the second resin layer comprising at least one selected from the group consisting of fluorinated resin and (meth)acrylic resin.
[0036] The liquid immersion cooling apparatus according to the present invention can suppress the deterioration of the first resin layer of electronic components caused by the coolant. This is presumably because the first resin layer is protected by a second resin layer containing a specific resin.
[0037] The liquid immersion cooling apparatus of the present invention will be described with reference to the accompanying drawings.
[0038] Figure 1 This is a schematic diagram illustrating one aspect of the liquid immersion cooling apparatus of the present invention.
[0039] The liquid immersion cooling device 1 includes: a coolant L; a container 10 storing the coolant L inside; a plurality of electronic components 20 disposed inside the container 10 in such a manner as to be immersed in the coolant L; a heat exchange pump unit 30 connected to the container 10 via a coolant supply pipe 31 and a coolant return pipe 32; and a cooler 40 connected to the heat exchange pump unit 30 via a cold water supply pipe 41 and a cold water return pipe 42.
[0040] The container 10 has an openable and closable lid 10a at the top. The interior of the container 10 is filled with coolant L to a height to which at least a portion of the electronic components 20 are immersed.
[0041] Coolant L is used to cool electronic component 20. Preferred methods for using coolant L will be described later.
[0042] Multiple electronic components 20 are disposed inside the container 10, and the multiple electronic components 20 are arranged at predetermined intervals. Figure 1 In the example, nine electronic components 20 are shown arranged side by side, but the arrangement and number of electronic components 20 are not particularly limited.
[0043] The electronic component 20 has an electronic component body 20a and a cable 20b connected to the electronic component body 20a.
[0044] As a specific example of the main body of the electronic component 20a, a computing processing board (e.g., a motherboard) in a server or the like can be cited. The computing processing board, for example, has a printed circuit board and electronic components mounted on the printed circuit board (e.g., CPU, power supply unit, memory, hard disk or SSD (Solid State Drive) memory, communication unit, etc.).
[0045] Specific examples of cable 20b include power cables and communication cables.
[0046] exist Figure 1The image shows an example where the entire electronic component body 20a and at least a portion of the cable 20b are immersed in coolant, but this is not a limitation. For example, a portion of the electronic component body 20a may be immersed in coolant L, or the entire cable 11b may be immersed in coolant L.
[0047] At least a portion of the surface of the electronic component 20 is composed of a first resin layer (not shown).
[0048] The first resin layer comprises at least one selected from the group consisting of vinyl chloride resin, epoxy resin, polyimide resin, silicone resin, olefin resin (e.g., polyethylene resin, polypropylene resin), ethylene propylene diene rubber, ethylene vinyl acetate copolymer, and polyester resin. From the viewpoint of more significantly exerting the effects of the present invention, vinyl chloride resin, ethylene propylene diene rubber, ethylene vinyl acetate copolymer, or polyester resin is preferred, and vinyl chloride resin is more preferred.
[0049] The electronic component 20 preferably includes a component selected from the group consisting of a printed circuit board and a cable, wherein at least a portion of the surface of the component is formed by the first resin layer.
[0050] Here, the first resin layer of the cable, for example, in the case where the cable is composed of copper wires and a resin coating covering the copper wires, is equivalent to the first resin layer.
[0051] In addition, if a protective layer (e.g., a sealing resin) is disposed on the surface of the printed substrate, the first resin layer of the printed substrate is equivalent to the first resin layer.
[0052] When applying labels with printed text and symbols for identification and performance display to components such as cables and printed circuit boards, the label itself can be considered as the first resin layer. When the label is the first resin layer, by applying a second resin layer (described later) to the surface of the label, it is possible to prevent the label itself and the text and symbols printed on it from disappearing due to the coolant.
[0053] The first resin layer may contain components other than the resins mentioned above.
[0054] As a specific example of a component other than resin, plasticizers can be cited. There is no particular limitation on the type of plasticizer. For example, if the resin contained in the first resin layer is vinyl chloride resin, specific examples of plasticizers that may be included in the first resin layer include phthalates (bis(2-ethylhexyl) phthalate, diisononyl phthalate, diisodecyl phthalate, dibutyl phthalate, etc.), adipates (dioctyl adipate, diisononyl adipate, etc.), trimellitates (trioctyl trimellitate, etc.), polyesters, phosphate esters (tricresyl phosphate, etc.), citrate esters (acetyl tributyl citrate, etc.), epoxidized vegetable oils (epoxidized soybean oil, epoxidized linseed oil, etc.), sebacic acid esters, azelaic acid esters, maleic acid esters, benzoic acid esters, etc.
[0055] Here, when the first resin layer is in contact with the coolant, components such as plasticizers may sometimes leach from the first resin layer, causing it to deteriorate. Furthermore, the leached plasticizers may sometimes adhere to the substrate, causing malfunctions. Additionally, the leached resin may float or adhere within the liquid immersion cooling device, sometimes requiring more frequent filter replacements and causing other adverse conditions.
[0056] To address these issues, by depositing a second resin layer (described later) on the surface of the first resin layer of the electronic component 20, the leaching of components such as plasticizers can be suppressed, thereby suppressing the deterioration of the first resin layer.
[0057] A second resin layer (not shown) is disposed on at least a portion of the surface of the first resin layer. That is, the electronic component 20, the first resin layer, and the second resin layer are sequentially stacked.
[0058] Regarding the second resin layer, it is preferable that the second resin layer is disposed on a portion of the first resin layer that may come into contact with at least one coolant L selected from the group consisting of liquids and gases. Alternatively, the second resin layer may be disposed on the entire surface of the first resin layer.
[0059] In addition, other layers may be included between the first resin layer and the second resin layer.
[0060] At least a portion of the second resin layer on the surface of the first resin layer is in contact with the coolant. The coolant in contact with the second resin layer can be a liquid or a gas.
[0061] The preferred composition of the second resin layer and the preferred configuration of the second resin layer will be described later.
[0062] The heat exchange pump unit 30 is connected to the container 10 via a coolant supply pipe 31 and a coolant return pipe 32. Additionally, the heat exchange pump unit 30 internally includes a heat exchanger 34 and a liquid pump 35.
[0063] The upstream end 31b of the coolant supply pipe 31 is connected to the heat exchanger 34, and the downstream end 31a of the coolant supply pipe 31 is connected to the side wall of the container 10.
[0064] The upstream end 32a of the coolant return pipe 32 is connected to the side wall of the container 10, and the downstream end 32b of the coolant return pipe 32 is connected to the liquid pump 35.
[0065] The heat exchanger 34 allows the cold water supplied from the cooler 40 to exchange heat with the coolant L supplied from the liquid pump 35 via the coolant discharge pipe 33. As a result, the coolant L is cooled.
[0066] The liquid pump 35 may also be driven by an electric motor, and the discharge rate may be adjusted by a control unit (not shown).
[0067] The cooler 40 is connected to the heat exchange pump unit 30 via a cold water supply pipe 41 and a cold water return pipe 42. In addition, the cooler 40 has a fan 43.
[0068] Cooler 40 allows external air drawn in by fan 43 to exchange heat with cold water. As a result, the cold water is cooled.
[0069] The start-up, stop-up, and speed of fan 43 are controlled by a control unit (not shown).
[0070] Electronic component 20 is cooled by heat exchange with coolant L stored in container 10. The coolant L, heated by the heat dissipation of electronic component 20, is supplied to heat exchanger 34 via liquid pump 35 in heat exchange pump unit 30, where it exchanges heat with cold water or external gas supplied from cooler 40 to heat exchanger 34. The coolant L, cooled by heat exchange, is then supplied back into container 10.
[0071] Figure 1 The invention illustrates a so-called single-phase liquid immersion cooling device in which coolant L is used directly in a liquid state, but it is not limited to this. The liquid immersion cooling device of the present invention can also be a so-called two-phase liquid immersion cooling device that utilizes a cooling cycle of vaporization and liquefaction of coolant L.
[0072] In the case of using a two-phase liquid immersion cooling device, either the liquid coolant L is in contact with the second resin layer, or the volatile coolant L is in contact with the second resin layer.
[0073] Next, the preferred method for using coolant L will be explained.
[0074] The standard boiling point of coolant L is preferably 45~500℃, more preferably 50~450℃, and even more preferably 50~430℃. If the standard boiling point of solvent L is 45℃ or higher, then, especially in the case of a two-phase immersion cooling device, not only cold water but also external gas can be effectively utilized to cool coolant L, thus further reducing power consumption; the ability to effectively utilize heat of vaporization further reduces power consumption, both of which are excellent. If the standard boiling point of solvent L is 500℃ or lower, then, especially in the case of a single-phase immersion cooling device, the viscosity of coolant L will not increase, allowing for efficient circulation of coolant L, which is excellent.
[0075] It should be noted that the standard boiling point refers to the boiling point at 1 atmosphere.
[0076] The GWP of the coolant is preferably 0~7500, more preferably 0~5000, and even more preferably 0~150.
[0077] GWP refers to the global warming potential, which, unless otherwise specified, is set to the 100-year value from the Intergovernmental Panel on Climate Change (IPCC) Fourth Assessment Report (2007) related to climate change. It should be noted that when the coolant is a mixture of two or more components, the GWP is a weighted average based on the compositional mass of each component. A lower GWP indicates a coolant with a smaller impact on global warming.
[0078] From the viewpoint of increasing the heat exchange efficiency with electronic components 20, at least one of the following is preferably selected as the coolant L: a mixture of fluorinated compounds and hydrocarbon compounds. Two or more coolants may be used together.
[0079] From the viewpoint of non-flammability, fluorinated compounds are preferred. When used indoors, from the viewpoint of fire protection laws, non-flammability is preferred. Furthermore, from the viewpoint of easy desiccation and less stickiness, fluorinated compounds are preferred.
[0080] In particular, when the coolant L is a fluorinated compound and the second resin layer disposed on the first resin layer of the electronic component 20 contains a fluorinated resin, the coolant L has excellent wettability to the second resin layer, thus further improving the heat exchange efficiency.
[0081] From the perspective of low dielectric constant, hydrocarbon compounds are preferred. When CPUs and GPUs become highly efficient, the clock frequency increases and becomes high-frequency. At this time, if the dielectric constant of the coolant is low, it is less likely to cause malfunctions.
[0082] Fluorinated compounds can be commercially available, such as Opteon 2P50 (48.9°C, hydrofluoroolefin) from Chemours, Galden HT55 (55°C, perfluoropolyether) from Solvay, AMOLEA AS-300 (55°C, hydrochlorofluoroolefin) from AGC, ASAHIKLIN AE-3000 (56°C, hydrofluoroether), ASAHIKLIN AC-6000 (115°C, hydrofluorocarbon) from 3M, Novec 7100 (61°C, hydrofluoroether), FC-3284 (50°C, perfluorocarbon), FC-3283 (128°C, perfluorocarbon), Novec 7300 (98°C, hydrofluoroether), Novec 7700 (167°C, hydrofluoroether), Novec 7500 (128°C, hydrofluoroether), and Fluorinert from 3M. FC-40 (165℃, perfluorocarbon). It should be noted that the temperature in parentheses indicates the standard boiling point.
[0083] Among fluorinated compounds, fluorinated olefin compounds (such as hydrofluoroolefins and hydrochlorofluoroolefins) have low GWPs and are preferred from an environmental perspective, but they are easily decomposed and readily produce acidic components. Therefore, the first resin layer is easily corroded by acidic components, and its degradation can sometimes be significant compared to other types of coolants. However, by providing a second resin layer, even when using fluorinated olefin compounds as coolants, it is possible to balance reducing environmental impact and suppressing coolant-induced degradation of the resin layer of electronic components.
[0084] Hydrocarbon compounds can be commercially available, such as Synfluid PAO 8 manufactured by ChevronPhilips Chemical Company, HIGM P 100 manufactured by NEOS Company, and the ENEOS IX series.
[0085] The larger the molecular weight of a hydrocarbon compound, the less likely it is to cause resin layer deterioration when used as a coolant.
[0086] The components that may be included in the second resin layer disposed on the surface of the first resin layer, and the preferred manner of the second resin layer, are described.
[0087] The second resin layer comprises at least one selected from the group consisting of fluorinated resins and (meth)acrylic resins, and preferably comprises a fluorinated resin for better effects of the invention.
[0088] From the viewpoint of achieving better results in this invention, the fluorinated resin preferably has a fluoroolefin-based unit (hereinafter also referred to as "unit F-1").
[0089] Fluoroolefins are alkenes obtained by replacing one or more hydrogen atoms with fluorine atoms. One or more of the unsubstituted hydrogen atoms in a fluoroolefin may be replaced by a chlorine atom. The preferred carbon number of a fluoroolefin is 2 to 8, more preferably 2 to 4.
[0090] Specific examples of fluoroolefins include CF2=CF2 (TFE), CF2=CFCl (trifluorochloroethylene), CF2=CHF, CH2=CF2 (VDF), CF2=CFCF3, CF2=CHCF3, CF3CH=CHF, CF3CF=CH2, and CH2=CX. f1 (CF2) n1 Y f1 (where X) f1 and Y f1 The monomers shown are, in view of superior compatibility, CF2=CF2, CH2=CF2, CF2=CFCl, CF3CH=CHF, and CF3CF=CH2, more preferably CF2=CF2 or CF2=CFCl, and even more preferably CF2=CFCl.
[0091] Fluoroolefins can be used in combination with two or more types.
[0092] In the case where the fluorinated resin contains unit F-1, from the perspective of adhesion, the content of unit F-1 is preferably 20 to 100 mol% relative to all units contained in the fluorinated resin, more preferably 30 to 70 mol%, and even more preferably 40 to 60 mol%.
[0093] Fluorinated resins may contain units having at least one of an aliphatic hydrocarbon ring and an aromatic ring (hereinafter also referred to as "unit F-2").
[0094] Unit F-2 is preferably based on a monomer (hereinafter also referred to as "monomer f2") having at least one of an aliphatic hydrocarbon ring and an aromatic ring.
[0095] Unit F-2 is preferably a unit that does not have fluorine atoms.
[0096] Specific examples of aliphatic hydrocarbon rings include monocyclic aliphatic hydrocarbons such as cyclobutane, cyclopentane, cyclohexane, cycloheptane, and cyclooctane; polycyclic aliphatic hydrocarbons such as 4-cyclohexylcyclohexane and decahydronaphthalene; norbornene and aliphatic hydrocarbons with bridged ring structures such as 1-adamantyl; and aliphatic hydrocarbons with spirocyclic structures such as spiro[3.4]octyl.
[0097] Specific examples of aromatic rings include aromatic hydrocarbon rings such as benzene, toluene, xylene, naphthalene, phenol, and benzoic acid; and aromatic heterocycles such as furan, thiophene, pyrrole, and pyridine.
[0098] As monomer f2, it is preferably a vinyl ether, vinyl ester, allyl ether, allyl ester or (meth)acrylate having at least one of an aliphatic hydrocarbon ring and an aromatic ring.
[0099] Specific examples of monomer f2 include cyclohexyl (meth)acrylate, cyclohexyl vinyl ether, and cyclohexanediethanol monovinyl ether (CH2=CHO-CH2-cycloC6H). 10 -CH2OH), CH2=CHCH2O-CH2-cycloC6H 10 -CH2OH, CH2=CHO-CH2-cycloC6H 10 -CH2-(OCH2CH2) 15 OH, vinyl benzoate, tert-butylvinyl benzoate and benzyl (meth)acrylate.
[0100] It should be noted that "-cycloC6H" 10 - indicates subcyclohexyl group, "-cycloC6H" represents the group with the cyclohexyl group. 10 The bonding site of "-" is usually 1,4-.
[0101] Two or more monomers f2 can be used together.
[0102] When the fluorinated resin contains unit F-2, the content of unit F-2 is preferably 1 to 50 mol% relative to all units contained in the fluorinated resin, more preferably 5 to 45 mol%, and even more preferably 10 to 40 mol%.
[0103] Fluorinated resins may also not have either an aliphatic hydrocarbon ring or an aromatic ring, but instead contain a unit having at least one of a hydroxyl group and a carboxyl group (hereinafter also referred to as "unit F-3").
[0104] Unit F-3 is preferably a unit that does not have fluorine atoms.
[0105] Unit F-3 can be a unit based on a monomer having at least one of a hydroxyl group and a carboxyl group (hereinafter also referred to as "monomer f3"), or it can be a unit obtained by converting a fluorinated resin containing a unit having a group capable of being converted into a hydroxyl group or a carboxyl group into at least one of a hydroxyl group and a carboxyl group. As such a unit, an example is a unit obtained by reacting a fluorinated resin containing a unit having a hydroxyl group with a polycarboxylic acid, its anhydride, etc., to convert part or all of the hydroxyl group into a carboxyl group.
[0106] At least a portion of the hydroxyl or carboxyl groups in monomer f3 may crosslink with a curing agent (e.g., a compound having two or more isocyanate groups in one molecule, or a compound having two or more epoxy groups in one molecule), or may remain uncrosslinked with the curing agent.
[0107] Examples of monomers f3 containing hydroxyl groups include vinyl ethers, vinyl esters, allyl ethers, allyl esters, (meth)acrylates, and allyl alcohols.
[0108] Specific examples of monomers f3 having hydroxyl groups include CH2=CHOCH2CH2OH, CH2=CHCH2OCH2CH2OH, CH2=CHOCH2CH2CH2CH2OH and CH2=CHCH2OCH2CH2CH2CH2OH. From the viewpoint of copolymerization with fluoroolefins, CH2=CHCH2OCH2CH2OH or CH2=CHOCH2CH2CH2CH2OH are preferred.
[0109] Examples of monomers f3 containing a carboxyl group include unsaturated carboxylic acids, (meth)acrylic acid, and monomers obtained by reacting carboxylic anhydrides with the hydroxyl groups of the aforementioned monomers containing hydroxyl groups.
[0110] Specific examples of monomers f3 containing a carboxyl group include CH2=CHCOOH, CH(CH3)=CHCOOH, CH2=C(CH3)COOH, HOOCCH=CHCOOH, and CH2=CH(CH2). n11 COOH (where n11 is an integer from 1 to 10), CH2=CHO(CH2) n12 OC(O)CH2CH2COOH (where n12 is an integer from 1 to 10), from the perspective of copolymerization with fluoroolefins, CH2=CH(CH2) is preferred. n11 COOH or CH2=CHO(CH2) n12 OC(O)CH2CH2COOH.
[0111] Two or more monomers f3 can also be used together.
[0112] When the fluorinated resin contains unit F-3, the content of unit F-3 is preferably more than 0 mol% and less than 30 mol%, more preferably 1 to 15 mol%, and even more preferably 1.5 to 5 mol%.
[0113] Fluorinated resins may also contain units (hereinafter also referred to as unit F-4) based on monomers (hereinafter also referred to as monomer f4) that do not have either an aliphatic hydrocarbon ring or an aromatic ring and do not have hydroxyl or carboxyl groups.
[0114] Unit F-4 is preferably a unit that does not have fluorine atoms.
[0115] Unit F-4 may have crosslinking groups other than hydroxyl and carboxyl groups. Specific examples of such groups include amino, epoxy, oxetyl, and hydrolyzable silyl groups.
[0116] As monomer f4, one or more can be selected from the group consisting of olefins, vinyl ethers, vinyl esters, allyl ethers, allyl esters and (meth)acrylates. From the perspective of copolymerization with fluoroolefins and weather resistance of fluorinated resins, at least one of vinyl ethers and vinyl esters is preferred, and vinyl ethers are even more preferred.
[0117] Specific examples of monomer f4 include ethylene, propylene, 1-butene, ethyl vinyl ether, tert-butyl vinyl ether, 2-ethylhexyl vinyl ether, vinyl acetate, vinyl tertvalerate, vinyl neononanoate (manufactured by HEXION, trade name "Veova 9"), vinyl neodecanoate (manufactured by HEXION, trade name "Veova 10"), and tert-butyl (meth)acrylate.
[0118] Two or more monomers of f4 can be used together.
[0119] When the fluorinated resin contains unit F-4, the content of unit F-4 is preferably 10 to 40 mol% relative to all units contained in the fluorinated resin, and more preferably 20 to 30 mol%.
[0120] From the viewpoint of achieving better results with the present invention, it is preferable to have a fluoroolefin-based unit as the fluorinated resin, more preferably a trifluorochloroethylene-based unit, and even more preferably a trifluorochloroethylene-based unit and a vinyl ether-based unit.
[0121] Here, fluorinated resins having trifluorochloroethylene-based units and vinyl ether-based units exhibit excellent wettability for both fluorinated and hydrocarbon coolants. More specifically, for fluorinated compound coolants, the fluorinated resins having trifluorochloroethylene-based units and vinyl ether-based units exhibit excellent wettability because they are both fluorine-based; for hydrocarbon coolants, the fluorinated resins having trifluorochloroethylene-based units and vinyl ether-based units do not exhibit excessively high oil repellency, thus also exhibiting excellent wettability. Therefore, heat exchange efficiency is increased, and the cooling efficiency of coolant-based electronic components is further improved.
[0122] Fluorine-containing resins can be used in combination with two or more types.
[0123] When the second resin layer contains a fluorinated resin, the content of the fluorinated resin is preferably 50 to 90% by mass, more preferably 60 to 80% by mass, relative to the total mass of the second resin layer.
[0124] Fluorinated resins are manufactured using known methods.
[0125] For example, fluorinated resins are obtained by copolymerizing the monomers in the presence of a solvent and a free radical polymerization initiator. Examples of methods for manufacturing fluorinated resins include solution polymerization and emulsion polymerization. During or after the manufacture of fluorinated resins, polymerization stabilizers, polymerization inhibitors, and surfactants may be used as needed.
[0126] As fluorinated resins, commercially available products can be used, such as the "LUMIFLON" series (manufactured by AGC), the "Fluon" series (manufactured by AGC), the "Kynar" series (manufactured by ARKEMA), the "Zeffle" series (manufactured by Daikin Industries), the "Eterflon" series (manufactured by Eternal), and the "Zendura" series (manufactured by Honeywell).
[0127] (Meth)acrylic resins are polymers or crosslinks thereof that contain units based on (meth)acrylates.
[0128] Examples of (meth)acrylates include alkyl (meth)acrylates and aryl (meth)acrylates.
[0129] Specific examples of (meth)acrylates include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, n-hexyl (meth)acrylate, cyclohexyl (meth)acrylate, lauryl (meth)acrylate, 2-ethylhexyl (meth)acrylate, benzyl (meth)acrylate, and phenyl (meth)acrylate.
[0130] (Meth)acrylates can have reactive groups such as hydroxyl, carboxyl, amino, epoxy, oxetyl, and hydrolyzable silyl groups. These reactive groups may remain unreacted or be cross-linked through intramolecular cross-linking or through curing agents containing groups capable of reacting with the reactive groups.
[0131] As a (meth)acrylic resin, commercially available products can be used. For example, ACRYDIC A-801 (an acrylic resin with hydroxyl groups) manufactured by DIC Corporation can be cited.
[0132] (Meth)acrylic resins can be used in combination with two or more types.
[0133] When the second resin layer contains a (meth)acrylic resin, the content of the (meth)acrylic resin relative to the total mass of the second resin layer is preferably 20 to 90% by mass, more preferably 30 to 80% by mass.
[0134] The second resin layer may contain additives in the various resins mentioned above.
[0135] Examples of additives include curing agents, curing catalysts, ultraviolet absorbers, matting agents, leveling agents, surface conditioners, degassing agents, fillers, thickeners, dispersants, surfactants, antistatic agents, rust inhibitors, silane coupling agents, antifouling agents, low-pollution treatment agents, colorants, and plasticizers.
[0136] The second resin layer preferably includes a curing agent. When the second resin layer comprises a fluorinated resin having unit F-3 based on monomer f3 having hydroxyl groups and a curing agent, the molar amount of isocyanate groups in the curing agent relative to the molar amount of hydroxyl groups in the fluorinated resin is preferably 30% or more, more preferably 40% or more, further preferably 50% or more, and particularly preferably 90% or more. Furthermore, it is preferably 230% or less, more preferably 200% or less, further preferably 150% or less, and particularly preferably 105% or less. Additionally, it is preferably 30-230%, more preferably 40-200%, further preferably 40-150%, particularly preferably 50-150%, and most preferably 90-105%. If the proportion is at or above the lower limit mentioned above, the solvent resistance of the coating film is more excellent. If the proportion is below the upper limit mentioned above, the non-adhesiveness is more excellent. Here, the above proportions are calculated based on the amount of fluorinated resin and curing agent added.
[0137] The thickness of the second resin layer is preferably 50 nm to 100 μm, more preferably 100 nm to 80 μm, even more preferably 500 nm to 40 μm, and particularly preferably 800 nm to 20 μm. If the thickness of the second resin layer is 50 nm or more, the effect of the present invention is even better. If the thickness of the second resin layer is 100 μm or less, the flexibility of the electronic components will not be impaired, and the resistance to deterioration caused by coolant L is excellent.
[0138] There is no particular limitation on the method for forming the second resin layer. Examples include a method of attaching a coating composition to a first resin layer of an electronic component and forming a second resin layer on at least a portion of the surface of the first resin layer.
[0139] The coating composition is preferably a composition containing a resin.
[0140] As a resin, examples of resins that may be included in the second resin layer described above include at least one of fluorinated resins and (meth)acrylic resins.
[0141] In addition to resin, the coating composition may also contain various components and liquid media (e.g., water, organic solvents) that may be contained in the second resin layer.
[0142] The coating composition can be a coating composition in which resin is dissolved or dispersed in a liquid medium, or it can be a coating composition that does not substantially contain a liquid medium (e.g., powder coating composition).
[0143] Examples of liquid media include organic solvents and water. Examples of coating compositions dissolved or dispersed in liquid media include coating compositions dissolved in organic solvents (e.g., solvent-based coating compositions) and coating compositions dispersed in water (e.g., water-based coating compositions).
[0144] The coating composition is substantially free of liquid media, meaning that the content of liquid media is less than 0.1% by mass relative to the total mass of the coating composition.
[0145] Examples of organic solvents include ketone solvents, ester solvents, hydrocarbon solvents, alcohol solvents, glycol ether solvents, and glycol ester solvents.
[0146] Specific examples of ketone solvents include acetone, methyl ethyl ketone, methyl isobutyl ketone, diisobutyl ketone, and diacetone alcohol.
[0147] Specific examples of ester solvents include ethyl acetate and butyl acetate.
[0148] Specific examples of hydrocarbon solvents include hexane, heptane, cyclohexane, xylene, ethylbenzene, toluene, ExxonMobil Solvesso 100, ExxonMobil Solvesso 150, etc., as well as aromatic hydrocarbon solvents (such as mineral oil).
[0149] Butanol is a specific example of an alcohol-based solvent.
[0150] Specific examples of glycol ether solvents include ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, and propylene glycol monopropyl ether.
[0151] 1-Methoxypropyl-2-acetic acid ester is a specific example of a diol ester solvent.
[0152] When the coating composition contains a liquid medium, the content of the liquid medium relative to the total mass of the coating composition is preferably 10 to 95% by mass, more preferably 20 to 90% by mass.
[0153] The resin content is preferably 50-80% by mass, more preferably 60-80% by mass, relative to the total solids content of the coating composition.
[0154] When the coating composition is a water-based coating composition or a solvent-based coating composition, specific examples of coating methods include spraying, scraper coating, flow coating, bar coating, spin coating, dip coating, screen printing, gravure printing, stencil coating, inkjet coating, curtain coating, and methods using brushes and scrapers.
[0155] When the coating composition is a powder coating composition, specific examples of coating methods include electrostatic coating, electrostatic spraying, electrostatic impregnation, spraying, flow impregnation, spraying, spraying, plating, and plasma plating.
[0156] If required, it may also include a process to remove the solvent by drying it after coating.
[0157] The preferred drying temperature is 20~140℃, and the preferred drying time is 1 minute~60 minutes.
[0158] Example
[0159] The present invention will now be described in detail with examples. Examples 1 to 3 are embodiments, and Example 4 is a comparative example. However, the present invention is not limited to these examples.
[0160] [Abbreviations, etc.]
[0161] CTFE: Trifluorochloroethylene
[0162] CHVE: Cyclohexyl vinyl ether
[0163] EVE: Ethyl vinyl ether
[0164] HBVE: 4-Hydroxybutylvinyl ether
[0165] 2-EHVE: 2-Ethylhexylvinyl ether
[0166] Fluoropolymer F1: A fluoropolymer with a molar ratio of CTFE unit / CHVE unit / EVE unit / HBVE unit = 50 / 15 / 25 / 10.
[0167] Acrylic resin A1: ACRYDIC A-801 (manufactured by DIC Company)
[0168] Curing agent: CORONATE HX (trade name, manufactured by Tosoh Corporation, isocyanurate form of hexamethylene diisocyanate)
[0169] Curing catalyst: a 10,000-fold diluted solution of butyl acetate (manufactured by Kanto Chemical Co., Ltd.) for the use of dibutyltin dilaurate (DBTDL).
[0170] [Example 1]
[0171] The various components shown in Table 1 below are mixed to prepare coating composition 1. In coating composition 1, the molar amount of isocyanate groups in the curing agent is 52% relative to the molar amount of hydroxyl groups in the fluoropolymer.
[0172] Next, coating composition 1 was applied to the surface of a polyvinyl chloride film (product name "Achilles Flat", manufactured by Achilles Company) using a doctor blade to form a coating film. The resulting coating film was dried at 80°C for 30 minutes to obtain evaluation sample 1 with a second resin layer formed on the surface of the polyvinyl chloride film. The thickness of the second resin layer was 40 μm.
[0173] [Example 2]
[0174] The coating amount of coating composition 1 was adjusted so that the thickness of the second resin layer was 20 μm. Otherwise, the same procedure as in Example 1 was followed to obtain evaluation sample 2 with a second resin layer formed on the surface of the polyvinyl chloride film.
[0175] [Example 3]
[0176] The various components shown in Table 1 (described later) were mixed to prepare coating composition 2. In coating composition 2, the molar ratio of the isocyanate groups in the curing agent to the molar ratio of the hydroxyl groups in the fluoropolymer was 52%. Coating composition 2 was used instead of coating composition 1, and the procedure was the same as in Example 1 to obtain evaluation sample 3 with a second resin layer formed on the surface of a polyvinyl chloride film. The thickness of the second resin layer was 40 μm.
[0177] [Example 4]
[0178] A polyvinyl chloride film (product name "Achilles Flat", manufactured by Achilles Company) was used as the evaluation sample 4.
[0179] [Evaluation of Deterioration Status]
[0180] The coolant was dropped onto the surface of the evaluation sample using the drop method described in JIS K 5600-6-1 (2016). The deterioration state of the evaluation sample was visually confirmed after 24 hours, and the evaluation was conducted according to the following criteria. The results are shown in Table 1. It should be noted that an evaluation result of C or higher indicates that the sample is considered to be practically usable.
[0181] It should be noted that for evaluation samples 1 to 3, coolant was dropped onto the surface of the second resin layer, and for evaluation sample 4, coolant was dropped onto the surface of the polyvinyl chloride film.
[0182] In addition, ASAHIKLIN AE-3000 (manufactured by AGC), AMOLEA AS-300 (manufactured by AGC), and hexane were used as coolants added to the evaluation samples.
[0183] (Evaluation Criteria)
[0184] A: No changes can be seen on the surface.
[0185] B: Some roughness was observed on the surface.
[0186] C: Some deformation was observed on a portion of the surface.
[0187] D: Deformation was observed across the entire surface.
[0188] [Table 1]
[0189]
[0190] As shown in Table 1, when a component with a second resin layer comprising a fluorinated resin or a (meth)acrylic resin on its surface is used, it can be confirmed that the component located below the second resin layer is less prone to deterioration due to the coolant (Examples 1-3). Therefore, if the aforementioned second resin layer is disposed on the first resin layer of an electronic component in a liquid immersion cooling device, it can be said that deterioration of the first resin layer caused by the coolant is less likely to occur.
[0191] In addition, other embodiments of the present invention will be described with reference to examples.
[0192] <Preparation of Coating Composition 3 and Coating Composition 4>
[0193] A coating composition 3 was prepared by adding 21 parts by mass of Coronate HX to 100 parts by mass of LF200MEK (manufactured by AGC) containing fluoropolymers with a molar ratio of CTFE units / CHVE units / EVE units / HBVE units of 50 / 15 / 25 / 10. In coating composition 3, the molar amount of isocyanate groups in the curing agent relative to the molar amount of hydroxyl groups in the fluoropolymer is 150%.
[0194] A coating composition 4 was prepared by adding 14 parts by mass of Coronate HX to 100 parts by mass of LF800 (manufactured by AGC) of a fluoropolymer containing CTFE units / CHVE units / HBVE units / 2-EHVE units in a molar ratio of 50 / 26 / 9 / 15. In coating composition 4, the molar amount of isocyanate groups in the curing agent relative to the molar amount of hydroxyl groups in the fluoropolymer is 100%.
[0195] [Reference Example 1]
[0196] A 30cm section of a PanZone (product name) Cat6 cable assembly LAN cable (manufactured by Panduit Corporation) with a PVC coating was immersed in coating composition 3. After lifting, it was heated in a dryer for 10 minutes to coat the cable. It was confirmed that the coated portion of coating composition 3 was not sticky. Then, coating composition 4 was applied to a 30cm section from the opposite end in the same manner.
[0197] The LAN cable was immersed in the IX series (hydrocarbon compound manufactured by ENEOS) and left at room temperature for six months. Then, the LAN cable was removed and wiped with Kimwipe (manufactured by CRECIA, Nippon Paper) to check whether any changes had occurred in each part before and after immersion.
[0198] As a result, the portion coated with paint composition 3 or paint composition 4 does not bend into an acute angle even when bent, retains its flexibility, and the bent portion does not turn white. On the other hand, the portion not coated with paint composition 3 or paint composition 4 bends into an acute angle when bent, loses its flexibility, and the bent portion also turns white and deteriorates.
[0199] [Reference Example 2]
[0200] Affix two polyester film barcode labels to the surface of a 5cm square stainless steel plate. Apply coating composition 3 to the surface of one of the labels and heat it in a dryer for 5 minutes. Confirm that the coated area is not sticky.
[0201] The stainless steel plate was immersed in the IX series (hydrocarbon compounds produced by ENEOS) and left at room temperature for six months. Then, the stainless steel plate was removed and wiped with wiping paper to confirm whether any changes had occurred before and after immersion.
[0202] As a result, the ink on labels coated with paint composition 3 did not bleed even when rubbed with wiping paper, and the barcode could be read. On the other hand, the ink on labels not coated with paint composition 3 bleeded when wiped with Kimwipe, making the barcode unreadable.
[0203] [Reference Example 3]
[0204] Affix a PVC film barcode label to the surface of one end of a PanZone Cat6 cable assembly LAN cable (manufactured by Panduit Corporation Japan). Apply coating composition 3 to the surface of this label and heat it in a dryer for 5 minutes. Confirm that the coated area is not sticky. Meanwhile, affix only a PVC film barcode label to the surface of the other end of the LAN cable, without applying the coating composition.
[0205] The LAN cable was immersed in IX series (hydrocarbon compounds from ENEOS) and left at room temperature for six months. Then, the LAN cable was removed and wiped with wiping paper to confirm whether any changes had occurred in the various parts before and after immersion.
[0206] As a result, the ink on labels coated with paint composition 3 did not bleed even when rubbed with wiping paper, and the barcode could be read. On the other hand, the ink on labels not coated with paint composition 3 bleeded when rubbed with wiping paper, making the barcode unreadable, and the labels themselves also hardened and deteriorated slightly.
[0207] It should be noted that the entire contents of the description, claims, drawings and abstract of Japanese Patent Application No. 2024-072204, filed on April 26, 2024 and Japanese Patent Application No. 2024-154227, filed on September 6, 2024, are incorporated herein as a disclosure of the specification of this invention.
[0208] Explanation of reference numerals in the attached figures
[0209] 1. Liquid Immersion Cooling Device
[0210] 10 containers
[0211] 10a Cover
[0212] 20 Electronic components
[0213] 20a Electronic component body
[0214] 20b cable
[0215] 30 heat exchange pump units
[0216] 31 Coolant supply pipe
[0217] 31a Downstream end
[0218] 31b Upstream end
[0219] 32 Coolant return
[0220] 32a Upstream end
[0221] 32b Downstream end
[0222] 33 Coolant discharge pipe
[0223] 34 Heat Exchanger
[0224] 35 Liquid Pump
[0225] 40 Cooler
[0226] 41 Cold water supply Suga
[0227] 42 Cold water return to Suga
[0228] 43 Fans
[0229] L coolant
Claims
1. A liquid immersion cooling device, comprising: coolant; A container containing the coolant inside; And electronic components within the container that are at least partially in contact with the coolant. At least a portion of the surface of the electronic component has a first resin layer, the first resin layer comprising at least one selected from the group consisting of vinyl chloride resin, epoxy resin, polyimide resin, silicone resin, olefin resin, ethylene propylene diene rubber, ethylene vinyl acetate copolymer, and polyester resin. A second resin layer is disposed on at least a portion of the surface of the first resin layer, the second resin layer comprising at least one selected from the group consisting of fluorinated resins and (meth)acrylic resins.
2. The liquid immersion cooling device according to claim 1, wherein, The second resin layer comprises the fluorinated resin.
3. The liquid immersion cooling device according to claim 1 or 2, wherein, The electronic components include parts selected from the group consisting of printed circuit boards and cables. At least a portion of the surface of the component is composed of the first resin layer.
4. The liquid immersion cooling device according to claim 1 or 2, wherein, The fluorinated resin comprises fluoroolefin-based units.
5. The liquid immersion cooling device according to claim 1 or 2, wherein, The fluorinated resin comprises trifluorochloroethylene-based units and vinyl ether-based units.
6. The liquid immersion cooling device according to claim 1 or 2, wherein, The thickness of the second resin layer is 50nm~100μm.
7. The liquid immersion cooling device according to claim 1 or 2, wherein, The standard boiling point of the coolant is 45~450℃.
8. The liquid immersion cooling device according to claim 1 or 2, wherein, The coolant is selected from at least one of the groups consisting of fluorinated compounds and hydrocarbon compounds.
9. The liquid immersion cooling device according to claim 1 or 2, wherein, The GWP of the coolant is 0~7500.
Citation Information
Patent Citations
Immersion cooling device and control method thereof
JP2023000068A
Vehicular notification device, vehicular notification method and program
JP2024072204A
Pallet with runaway prevention
JP2024154227A