An integrated approach to copper oxide removal and low-k remediation processes
By using a combination of reducing agent and ultraviolet light source in the process chamber to remove copper oxide and treat low dielectric constant films with recycled precursors, the problem of damage to low dielectric constant films after downstream processes was solved, achieving a reduction in dielectric constant and restoration of the film's hydrophobicity.
Patent Information
- Application Number
- CN202580027465.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-07-25
- Filing Date
- 2025-02-12
- Publication Date
- 2026-11-17
AI Technical Summary
As semiconductor devices shrink, low-dielectric-constant dielectric films are damaged by contamination in later processes, leading to resistance and capacitance delays and an increase in dielectric constant. Existing technologies struggle to effectively repair the integrity of copper and low-dielectric-constant films.
By combining reducing agents such as ammonia, hydrogen, carbon monoxide, ethanol, methane, or ethylene with an ultraviolet light source, copper oxides are removed and the dielectric constant is reduced using recycled precursors. The low dielectric constant film is then processed through a process chamber.
It restores the hydrophobicity of low dielectric constant films, reduces the dielectric constant value, and improves the reliability and integrity of dielectric films.
Smart Images

Figure CN123126093A_ABST
Abstract
Description
Background Technology
[0001] field
[0002] The embodiments described herein generally relate to processes for treating low dielectric constant (k) dielectric films. More specifically, the embodiments described herein relate to processes for repairing copper and low dielectric constant dielectric films.
[0003] Related technical descriptions
[0004] In semiconductor manufacturing, the dielectric constant (k) of dielectric films decreases continuously as device scaling continues. Minimizing integration defects on low-dielectric-constant (LDC) films is crucial for further feature size reduction. However, as feature sizes shrink, improving the resistance, capacitance, and reliability of dielectric films becomes a significant challenge.
[0005] Porous low-dielectric-constant dielectric films suffer severe damage after back-end-of-line (BEOL) integration due to contamination in the exposed pores, resulting in greater resistive-capacitive (RC) delays. To maintain the integrity of the low-dielectric-constant dielectric film and minimize oxidation on copper, a method for restoring both the copper and the low-dielectric-constant film is needed. Summary of the Invention
[0006] The embodiments described herein generally relate to processes for treating low-dielectric-constant dielectric films. More specifically, the embodiments described herein relate to processes for repairing copper and low-dielectric-constant dielectric films.
[0007] In one embodiment, a method for repairing copper and low-dielectric-constant dielectric films is provided. The method includes positioning a substrate within a process chamber and introducing a reducing agent into the process chamber to remove copper oxide from a copper layer on the substrate. After removing the copper oxide, the method further includes removing the reducing agent from the process chamber and introducing a recycled precursor into the process chamber to reduce the dielectric constant of the low-dielectric-constant film on the substrate.
[0008] In another embodiment, a method for repairing copper and low-dielectric-constant dielectric films is provided. The method includes positioning a substrate within a process chamber and introducing a reducing agent into the process chamber to remove copper oxide from a copper layer on the substrate. In some embodiments, the reducing agent includes ammonia (NH3), hydrogen (H2), carbon monoxide (CO), ethanol (C2H5OH), methane (CH4), or ethylene (C2H4). The method also includes turning on an ultraviolet light source to expose the substrate to ultraviolet light. After removing the copper oxide, the method further includes removing the reducing agent from the process chamber and introducing a recycled precursor into the process chamber to reduce the dielectric constant of the low-dielectric-constant film on the substrate.
[0009] In a further embodiment, a non-transitory computer-readable medium is provided. The non-transitory computer-readable medium includes instructions that, when executed by a processor, cause a computer system to perform the following steps: positioning a substrate within a process chamber; introducing a reducing agent into the process chamber to remove copper oxide from a copper layer on the substrate; removing the reducing agent from the process chamber; and introducing a recycled precursor into the process chamber to reduce the dielectric constant of a low-dielectric-constant film on the substrate.
[0010] Brief description of the attached figures
[0011] To gain a more detailed understanding of the features described above, a more specific description of the present disclosure can be obtained by referring to the embodiments, some of which are illustrated in the accompanying drawings. However, it should be noted that the drawings illustrate only typical embodiments of the present disclosure and should therefore not be considered as limiting its scope, as other equally effective embodiments are permissible.
[0012] Figure 1 This is a schematic cross-sectional view of a process chamber according to one or more embodiments.
[0013] Figure 2 This is a schematic block diagram of a substrate processing method according to one or more embodiments.
[0014] Figures 3A to 3C This is a molecular diagram of a low dielectric constant film during a method according to one or more embodiments.
[0015] Figures 4A to 4D This is a partial schematic side cross-sectional view of a semiconductor element during a method according to one or more embodiments. Detailed Implementation
[0016] The embodiments described herein generally relate to processes for treating low-dielectric-constant dielectric films. More specifically, the embodiments described herein relate to processes for repairing copper and low-dielectric-constant dielectric films.
[0017] During downstream processing operations, processing steps can damage the copper layer by oxidizing it. Furthermore, these steps can damage low-dielectric-constant dielectric films through carbon loss (leading to a higher dielectric constant) and the introduction of undesirable Si-OH bonds (making the low-dielectric-constant surface hydrophilic). Therefore, the technique described herein for repairing copper and low-dielectric-constant dielectric films reverses copper oxidation, reduces the k-dielectric constant on the low-dielectric-constant film, and increases the hydrophobicity of the low-dielectric-constant film.
[0018] Figure 1 This is a schematic cross-sectional view of a process chamber 100 according to one or more embodiments. The process chamber 100 may be a vapor deposition chamber including ultraviolet radiation for assisting the silanization reaction. In one or more embodiments, the process chamber 100 may be an ONYX material available from Applied Materials, Inc., Santa Clara, California. ® Or SILENA ® Process chamber. Process chamber 100 may include a chamber body 102 and a chamber cover 104 disposed on the chamber body 102. The chamber body 102 and the chamber cover 104 may form an internal volume 106. A substrate support assembly 108 may be disposed in the internal volume 106. The substrate support assembly 108 may receive and support a substrate 110 thereon for processing.
[0019] A first ultraviolet-transparent gas dispensing nozzle 116 is suspended in the internal volume 106 through the central opening 112 of the chamber cover 104 via an upper clamping member 118 and a lower clamping member 120. The ultraviolet-transparent gas dispensing nozzle 116 is positioned facing the substrate support assembly 108 to dispense one or more processing gases in a dispensing volume 122 located below the first ultraviolet-transparent gas dispensing nozzle 116. A second ultraviolet-transparent nozzle 124 is suspended in the internal volume 106 through the central opening 112 of the chamber cover 104 below the first ultraviolet-transparent gas dispensing nozzle 116. Each of the ultraviolet-transparent gas dispensing nozzles 116 and 124 can be disposed in a recess formed in the chamber cover 104. A first recess 126 can be an annular recess surrounding the inner surface of the chamber cover 104, and the first ultraviolet-transparent gas dispensing nozzle 116 is fitted into the first recess 126. Similarly, a second recess 128 can receive the second ultraviolet-transparent gas dispensing nozzle 124.
[0020] The ultraviolet transparent window 114 can be disposed above the first ultraviolet transparent gas distribution nozzle 116. The ultraviolet transparent window 114 can be positioned above the first ultraviolet transparent gas distribution nozzle 116, forming a gas volume 130 between the ultraviolet transparent window 114 and the first ultraviolet transparent gas distribution nozzle 116. The ultraviolet transparent window 114 can be fixed to the chamber cover 104 by any means (such as clamps, screws, bolts, etc.).
[0021] The ultraviolet transparent window 114 and the first and second ultraviolet transparent gas distribution nozzles 116 and 124 are at least partially transparent to thermal or radiant energy within the ultraviolet wavelength range. The ultraviolet transparent window 114 may be made of quartz or another ultraviolet transparent material, such as sapphire, CaF2, MgF2, AlON, silicon oxide, silicon oxynitride, or another transparent material.
[0022] An ultraviolet (UV) source 150 may be positioned above a UV-transparent window 114. The UV source 150 may be configured to generate UV energy and project it toward the substrate support assembly 108 through the UV-transparent window 114, a first UV-transparent gas distribution nozzle 116, and a second UV-transparent gas distribution nozzle 124, thereby exposing the substrate 110 on the substrate support assembly 108 to UV light. A cover (not shown) may be positioned above the UV source 150. In one or more embodiments, the cover may be shaped to facilitate the projection of UV energy from the UV source 150 toward the substrate support assembly.
[0023] In one or more embodiments, the ultraviolet source 150 may include one or more ultraviolet lights 152 to generate ultraviolet radiation. The ultraviolet light 152 may be a lamp, an LED emitter, or other ultraviolet emitter. In one or more embodiments, the ultraviolet light 152 may be an argon lamp discharging radiation at 126 nm, a krypton lamp discharging at 146 nm, a xenon lamp discharging at 172 nm, a krypton chloride lamp discharging at 222 nm, a xenon chloride lamp discharging at 308 nm, a mercury lamp discharging at 254 nm or 365 nm, a metal vapor lamp (such as a zinc lamp) discharging at 214 nm, or a rare-earth near-ultraviolet lamp (such as a europium-doped strontium borate or fluoroborate lamp) discharging at 368 nm to 371 nm, to name a few examples.
[0024] Process chamber 100 may include flow channels 132, 134, and 136 configured to supply one or more processing gases to substrate support assembly 108 for processing substrate 110 disposed thereon. First flow channel 132 provides a flow path for the gas into gas volume 130 and exposes it to ultraviolet radiation from ultraviolet source 150. Gas from gas volume 130 may flow through first ultraviolet-transparent gas distribution nozzle 116 into distribution volume 122. Second flow channel 134 provides a flow path for precursor compounds and gases to flow directly into distribution volume 122 without passing through first ultraviolet-transparent gas distribution nozzle 116, to mix with the gas previously exposed to ultraviolet radiation in gas volume 130. Before flowing through second ultraviolet-transparent gas distribution nozzle 124 into the space adjacent to substrate support assembly 108, the mixed gas in distribution volume 122 may be further exposed to ultraviolet radiation through first ultraviolet-transparent gas distribution nozzle 116. The gas near the substrate support assembly 108 and the substrate mounted on the substrate support assembly 108 are further exposed to ultraviolet radiation through the second ultraviolet transparent gas distribution nozzle 124. Purifying gas can be supplied through an opening 138 in the bottom of the process chamber 100, allowing the purifying gas to flow around the substrate support assembly 108 and preventing process gas from intruding into the space below the substrate support assembly 108. One or more gases can be discharged through the opening 138.
[0025] The first ultraviolet transparent gas distribution nozzle 116 may include a plurality of holes 140, which allow process gas to flow from the gas volume 130 to the distribution volume 122. The second ultraviolet transparent gas distribution nozzle 124 may also include a plurality of holes 142, which allow process gas to flow from the distribution volume 122 into the processing space adjacent to the substrate support assembly 108. The holes 140 and 142 in the first and second ultraviolet transparent gas distribution nozzles 116 and 124 may be uniformly distributed or irregularly spaced.
[0026] A purge gas or carrier gas source 154 can be coupled to the first flow channel 132 via a conduit 156. During substrate processing, purge gas from the purge gas source 154 can be supplied through the first flow channel 132 to prevent process gases from entering the gas volume 130. A cleaning gas source 174 can also be coupled to the first flow channel 132 via a conduit 156 to provide cleaning of the conduit 156, the first flow channel 132, the gas volume 130, and the rest of the chamber body 102 when the substrate is not being processed.
[0027] A process gas or precursor compound source 158 may be coupled to a second flow channel 134 via conduit 160 to supply a mixture to the chamber body 102 (as described above). The process gas source 158 may also be coupled to a third flow channel 136. Appropriate valves may allow selection of one or both of flow channels 134 and 136 for allowing the process gas mixture to flow into the chamber body 202.
[0028] The substrate temperature can be controlled by providing heating and cooling features in the substrate support assembly 108. A coolant conduit 164 can be coupled to a coolant source 170 to supply coolant to a cooling chamber 162 disposed in the substrate support assembly 108. One example of a coolant that can be used is a mixture of 50% ethylene glycol in water (by volume). The coolant flow is controlled to maintain the substrate temperature at or below a desired level to promote the deposition of UV-activated oligomers or fragments on the substrate. A heating element 166 can also be provided in the substrate support assembly 108. The heating element 166 can be a resistance heater and can be coupled to a heat source 172, such as a power supply, via a conduit 168. The heating element 166 can be used to heat the substrate during the aforementioned curing process.
[0029] Figure 2 This is a schematic block diagram of a substrate processing method 200 according to one or more embodiments. Figures 3A to 3C Molecular diagrams of low dielectric constant films 310a, 310b, 310c during method 200 according to one or more embodiments. Figures 4A to 4D This is a partial schematic side cross-sectional view of the interconnect structure 400 during method 200 according to one or more embodiments.
[0030] At operation 210, the substrate (such as...) Figure 4A The interconnect structure 400 shown is transferred to the process chamber. The process chamber can be a deposition process chamber, such as... Figure 1 The process chamber 100 is depicted in the image. At operation 210, according to some embodiments, the interconnect structure 400 is post-deposited. The interconnect structure 400 (e.g.) Figure 4A The method 200 may include a low-dielectric-constant film 310a on the etch stop layer 430, a metal barrier 432 between the etch stop layer 430 and the copper layer 420, a metal barrier 432 between the copper layer and the substrate 434, residue 422 on the copper layer 420, and residue 424 on the low-dielectric-constant film 310a. In some embodiments, interconnect structures 400 with different configurations may be used in method 200.
[0031] Figure 3A Molecular diagram of the low dielectric constant film 310a at position 210. Figure 3A In the middle, the low dielectric constant film 310a has Si-O bonds, Si-CH3 bonds and Si-H bonds.
[0032] In some embodiments, the metal barrier 432 may include tantalum nitride (TaN).
[0033] At operation 220, the interconnect structure 400 is processed in the process chamber 100. As a result of operation 220, the copper layer 420 of the interconnect structure 400 is damaged. Figure 4B As shown, copper oxide 426 can be formed on copper layer 420, and residues 422 on copper oxide 426 can be reduced. Operation 220 may also damage the low dielectric constant film 310b of interconnect structure 400. Figure 3B As shown, the total number of Si-CH3 bonds in the low dielectric constant film 310b may decrease, and Si-OH bonds may form. With the increase of Si-OH bonds, the low dielectric constant film 310b becomes more hydrophilic, which is undesirable. The reduction of Si-CH3 bonds in the low dielectric constant film 310b leads to an increase in the dielectric constant value of the low dielectric constant film 310b. In some embodiments, the processing operation of operation 220 may include etching, ashing, wet cleaning operations, or a combination thereof.
[0034] At operation 230, copper oxide 426 on interconnect structure 400 is removed from copper layer 420, as follows: Figure 4C As shown. Operation 230 can be performed in process chamber 100 using a reducing agent and ultraviolet light. In some embodiments, interconnect structure 400 may be exposed to ultraviolet light during operation 230. In some embodiments, the reducing agent may be a reducing gas, such as ammonia (NH3), hydrogen (H2), carbon monoxide (CO), ethanol (C2H5OH), methane (CH4), or ethylene (C2H4). Figure 4C As shown, the low dielectric constant film 310b may still be damaged after operation 230.
[0035] In some embodiments, operation 230 may be performed at a temperature between about 75°C and about 500°C. In some embodiments, operation 230 may be performed for a period ranging from about 1 minute to about 10 minutes. In some embodiments, operation 230 may be performed at a pressure between about 3 Torr and about 100 Torr. In some embodiments, operation 230 may be performed using a reducing gas flow rate ranging from about 100 sccm to about 2000 sccm. In some embodiments, operation 230 may be performed using an RF power ranging from 0 W to about 1000 W. In some embodiments, operation 230 may be performed using an ultraviolet power percentage between 0% and about 90%.
[0036] After operation 230 is completed, the reducing gas can be removed from the process chamber.
[0037] Table 1
[0038] Table 1 demonstrates the ability of ultraviolet light and NH3 to remove copper oxide 426 from copper layer 420. Copper reflectance was used as an indicator of the oxidation state of copper layer 420. As shown in Table 1, the pressure of NH3 has almost no effect on the recovery of copper layer 420. Furthermore, copper layer 420 can be completely recovered by utilizing ultraviolet light and NH3 in operation 230.
[0039] At operation 240, such as Figure 4D As shown, the low dielectric constant film 310c is repaired. Figure 3C As shown, the low dielectric constant film 310c is respectively compared to Figure 3A and Figure 3B The low dielectric constant films 310a and 310b shown have fewer or no Si-OH bonds and a higher percentage of Si-CH3 bonds.
[0040] In some embodiments, operation 240 may be performed using a recycled precursor. In some embodiments, operation 240 may also be performed using ultraviolet light; for example, interconnect structure 400 may be exposed to ultraviolet light during operation 240. In some embodiments, operation 240 may be performed by chemical reactions (1) and (2) as described below. Chemical reactions (1) and (2) illustrate the removal of Si-OH bonds and the formation of Si-CH3 bonds when the low dielectric constant film 310b is exposed to the recycled precursor.
[0041] R2N-Si-(CH3)3 + HO-Si (s) (CH3)3-Si-O-Si (s) + R2NH (g) (1)
[0042] HO-Si (s) + HO-Si (s) Si-O-Si (s) + H2O (g) (2)
[0043] Recycling precursors may include molecules selected from Group 1. In Group 1, R may be independently selected from Me, Et, iPr, tBu, and H. R' may be independently selected from alkanes, alkenes, and alkynes. R' may include between one and twenty carbon atoms.
[0044] Group 1
[0045] In one or more embodiments, the recovered precursor may be one of the molecules depicted in the examples of Group 1 below.
[0046] Group 1
[0047] Example
[0048] In some embodiments, the recovered precursor may include molecules selected from Group 2. In Group 2, R may be independently selected from Me, Et, iPr, and tBu. R' may be independently selected from alkanes, alkenes, and alkynes. R' may include between one and twenty carbon atoms.
[0049] Group 2
[0050] In some embodiments, the recovered precursor may include molecules selected from Group 3. In Group 3, X may be Cl, Br, or I. R' may be independently selected from alkanes, alkenes, and alkynes. R' may include between one and twenty carbon atoms.
[0051] Group 3
[0052] In some embodiments, the recovered precursor may include molecules selected from Group 4. In Group 4, R' may be independently selected from alkanes, alkenes, and alkynes. R' may include between one and twenty carbon atoms.
[0053] Group 4
[0054] In some embodiments, the recovered precursor may include molecules selected from Group 5. In Group 5, R and R' may be independently selected from hydrogen, alkanes, alkenes, alkynes, and aryl groups. In embodiments where R and / or R' contain carbon, R and R' may each comprise between one and twenty carbon atoms.
[0055] Group 5
[0056] In some embodiments, the recovered precursor may include molecules selected from Group 6. In Group 6, R, R', and R" may be independently selected from hydrogen, alkanes, alkenes, alkynes, and aryl groups. In embodiments where R, R', and / or R" contain carbon, R, R', and R" may each include between one and twenty carbon atoms.
[0057] Group 6
[0058] In some embodiments, operation 240 may be performed at a temperature between about 75°C and about 500°C. In some embodiments, operation 240 may be performed for a period of time ranging from about 1 minute to about 10 minutes. In some embodiments, operation 240 may be performed at a pressure between about 3 Torr and about 100 Torr. In some embodiments, operation 240 may be performed by a gas flow rate of the recovered precursor ranging from about 100 mgm to about 2000 mgm.
[0059] Performing operation 230 prior to operation 240 may be advantageous because the recovery precursor is readily reacted with copper oxide (CuO). x The removal of the silicon residue on the copper layer 420 leads to the formation of Si residue, which affects the via resistance.
[0060] The following non-limiting examples are provided to further illustrate the implementation methods described herein. However, these examples are not intended to be inclusive, nor are they intended to limit the scope of the implementation methods described herein.
[0061] Table 2
[0062] As shown in Table 2, after operation 240, the amount of silicon residue in the copper oxide increased compared to reduced copper. Furthermore, performing operation 240 without ultraviolet light may be desirable to minimize silicon residue on the copper surface.
[0063] Table 3
[0064] As shown in Table 3, the low dielectric constant film 310a has a high water contact angle and is therefore hydrophobic. After the damage in operation 220, the low dielectric constant film 310b has a low water contact angle and is therefore hydrophilic. Then, after operation 240, the low dielectric constant film 310c has an even higher water contact angle and is therefore hydrophobic. Operation 220 increases the dielectric constant value, but operation 240 subsequently partially restores the dielectric constant value. In some embodiments, UV exposure may be performed sequentially during operation 240 or after the recovery precursor process in operation 240. When UV exposure is performed after operation 240, the low dielectric constant film 310b has a lower water contact angle compared to operation 240 without UV exposure or operation 240 with UV exposure.
[0065] Although the foregoing embodiments relating to this disclosure are described, other and further embodiments of this disclosure may be designed without departing from its basic scope, the scope of which is defined by the foregoing claims.
Claims
1. A method, the method comprising: Position the substrate within the process chamber; A reducing agent is introduced into the process chamber to remove copper oxide from the copper layer on the substrate; Remove the reducing agent from the process chamber; and The recycled precursor is introduced into the process chamber to reduce the dielectric constant of the low dielectric constant film on the substrate.
2. The method of claim 1, further comprising: When the reducing agent is located in the process chamber, the substrate is exposed to ultraviolet light for at least a portion of the time.
3. The method of claim 2, wherein the reducing agent is ammonia.
4. The method of claim 1, further comprising: When the recycled precursor is located within the process chamber, the substrate is exposed to ultraviolet light for at least a portion of the time.
5. The method of claim 1, wherein the recovery precursor is introduced into the process chamber after the reducing agent is removed from the process chamber.
6. The method of claim 1, wherein the recovered precursor comprises molecules selected from the group consisting of: , and R is independently selected from Me, Et, iPr, tBu and H, and R' is an alkane, alkene or alkyne.
7. The method of claim 1, wherein the recovered precursor comprises molecules selected from the group consisting of... , , and .
8. The method of claim 1, wherein the recovered precursor comprises molecules selected from the group consisting of... , and , where R is independently selected from Me, Et, iPr and tBu, and R' is an alkane, alkene or alkyne.
9. The method of claim 1, wherein the recovered precursor comprises molecules selected from the group consisting of... , and , where X is Cl, Br or I, and R' is an alkane, alkene or alkyne.
10. The method of claim 1, wherein the recovered precursor comprises a molecule having the following formula: , where R' is an alkane, alkene, or alkyne.
11. The method of claim 1, wherein the recovered precursor comprises a molecule having the following formula: , where R is hydrogen, alkane, alkene, alkyne or aryl, and R' is hydrogen, alkane, alkene, alkyne or aryl.
12. The method of claim 1, wherein the recovered precursor comprises a molecule having the following formula: , where R is hydrogen, alkane, alkene, alkyne or aryl, and R' is hydrogen, alkane, alkene, alkyne or aryl, and R" is hydrogen, alkane, alkene, alkyne or aryl.
13. The method of claim 1, wherein the reducing agent comprises ammonia (NH3), hydrogen (H2), carbon monoxide (CO), ethanol (C2H5OH), methane (CH4) or ethylene (C2H4).
14. A method, the method comprising: Position the substrate within the process chamber; A reducing agent is introduced into the process chamber to remove copper oxide from the copper layer on the substrate, wherein the reducing agent includes ammonia (NH3), hydrogen (H2), carbon monoxide (CO), ethanol (C2H5OH), methane (CH4), or ethylene (C2H4). Turn on the ultraviolet light source to expose the substrate to ultraviolet light; Remove the reducing agent from the process chamber; as well as The recycled precursor is introduced into the process chamber to reduce the dielectric constant of the low dielectric constant film on the substrate.
15. The method of claim 14, further comprising: The ultraviolet light source is turned off before the recycled precursor is introduced into the process chamber.
16. A non-transitory computer-readable medium storing instructions, which, when executed by a processor, cause a computer system to perform the following steps: Position the substrate within the process chamber; A reducing agent is introduced into the process chamber to remove copper oxide from the copper layer on the substrate; Remove the reducing agent from the process chamber; and The recycled precursor is introduced into the process chamber to reduce the dielectric constant of the low dielectric constant film on the substrate.
17. The non-transitory computer-readable medium of claim 16, wherein the non-transitory computer-readable medium further comprises: Turn on the ultraviolet light source to expose the substrate to ultraviolet light.
18. The non-transitory computer-readable medium of claim 17, wherein the non-transitory computer-readable medium further comprises: The ultraviolet light source is turned off before the recycled precursor is introduced into the process chamber.
19. The non-transitory computer-readable medium of claim 16, wherein the non-transitory computer-readable medium further comprises: The flow rate of the recovered precursor was adjusted to be between 100 mgm and 2000 mgm.
20. The non-transitory computer-readable medium of claim 16, wherein the non-transitory computer-readable medium further comprises: Adjust the pressure inside the process chamber to between 3 Torr and 100 Torr; as well as The temperature inside the process chamber is adjusted to be between 75°C and 500°C.