Cu@mn-cu organic framework catalyst and preparation method and application thereof

By preparing Cu@Mn-Cu organic framework catalysts, the problems of insufficient reactivity and stability of manganese-based Fenton catalysts were solved by utilizing the flexible release of copper ions and synergistic redox reactions, thus achieving efficient organic wastewater treatment.

CN123148992APending Publication Date: 2026-11-24CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202510669023.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-23
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing manganese-based Fenton catalysts have insufficient reactivity and stability, and their metal loading rate and cycling performance need to be improved, making it difficult to effectively address the differences in degradation rates of different pollutants.

Method used

A Cu@Mn-Cu organic framework catalyst was prepared by forming a rough, plate-like structure through hydrothermal reaction and vacuum activation. The Cu to Mn elemental ratio was 1~2:1. Combined with SiO₂ as a heterogeneous seed crystal and template agent, an ordered structure was formed, which enabled the flexible release of copper ions and synergistic redox reactions, thereby improving catalytic activity and cycle performance.

Benefits of technology

It achieves efficient catalyst regeneration and improved recycling performance at room temperature, significantly accelerates Fenton-like reaction rates, and is suitable for rapid oxidation treatment of various organic wastewaters.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123148992A_ABST
    Figure CN123148992A_ABST
Patent Text Reader

Abstract

This invention discloses a Cu@Mn-Cu organic framework catalyst, its preparation method, and its application. The Cu@Mn-Cu organic framework catalyst has a rough, sheet-like structure with a size of 100~200 nm. The Cu to Mn element ratio in the bulk catalyst phase is 1~2:1, and the Cu to Mn element ratio on the catalyst surface is 0.8~1.3:1. The preparation method includes the following: (1) Dissolving the organic ligand 2,5-dihydroxy-1,4-benzoquinone and manganese salt in deionized water and carrying out a hydrothermal reaction. The hydrothermal reaction product is separated into solid and liquid phases, and the solid phase is activated under vacuum to obtain Mn-dhbq seed crystals; (2) Adding Mn-dhbq seed crystals and benzoic acid to a mixture containing silicon source, copper source, and template agent and mixing them evenly to carry out a crystallization reaction. After the reaction is completed, the crystallization product is separated into solid and liquid phases, and the solid phase is dried to obtain a Cu@Mn-Cu bimetallic Fenton catalyst. The catalyst prepared by the method of this invention has a stable structure and efficient Fenton-like catalytic ability, and has broad application prospects in the field of organic wastewater oxidation treatment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of metal-organic framework catalysis technology, specifically relating to a bimetallic organic framework catalyst, its preparation method, and its application. Background Technology

[0002] Fenton-like technology is a common method for degrading organic pollutants in water bodies. It has the advantages of fast reaction speed, no secondary pollution, and low cost. Manganese-based compounds, as a new type of Fenton-like catalyst, can remove recalcitrant organic matter in wastewater through catalytic oxidation. However, there is still room for improvement in their Fenton-like reaction activity and stability. How to improve the regeneration rate of metal ions to ensure the continuous progress of the reaction is also one of the key issues.

[0003] Metal-organic frameworks (MOFs), with their stable porous structure, highly controllable pore size and surface chemistry, and strong functionalization capabilities, have demonstrated excellent performance in energy conversion, pollution control, and drug therapy, making them an ideal platform for catalyst development. Publication CN119076060A discloses the application of copper-manganese bimetallic MOFs in the catalytic degradation of sulfonamide antibiotics. Mn is doped into a two-dimensional MOF composed of Cu clusters and terephthalate ester linkages to prepare a highly efficient CuMn-BDC heterogeneous Fenton-like catalyst, thus solving the problem of low efficiency in existing water treatment catalysts. However, the degradation rate of this material varies significantly for different pollutants, and the metal loading rate and recycling performance need further investigation. Therefore, developing a flexible bimetallic organic framework with good recycling performance and regenerable active sites for the treatment of organic wastewater is of great significance. Summary of the Invention

[0004] To address the shortcomings of existing technologies, this invention provides a Cu@Mn-Cu organic framework catalyst, its preparation method, and its applications. The catalyst prepared by this invention possesses a stable structure and highly efficient Fenton-like catalytic activity. The preparation method is simple, and the solvent is environmentally friendly, showing broad application prospects in fields such as the oxidation treatment of organic wastewater.

[0005] The Cu@Mn-Cu organic framework catalyst of the present invention has a rough, sheet-like structure with a size of 100-200 nm. The Cu to Mn element ratio in the bulk catalyst phase is 1-2:1, and the Cu to Mn element ratio on the catalyst surface is 0.8-1.3:1.

[0006] The preparation method of the Cu@Mn-Cu organic framework catalyst of the present invention includes the following steps: (1) The organic ligand 2,5-dihydroxy-1,4-benzoquinone and manganese salt were dissolved in deionized water and subjected to hydrothermal reaction. The hydrothermal reaction product was separated into solid and liquid phases and the solid phase was activated under vacuum to obtain Mn-dhbq seed crystals. (2) Add Mn-dhbq seed crystals and benzoic acid to a mixture containing silicon source, copper source and template agent, mix evenly, carry out crystallization reaction, and after the reaction is completed, separate the solid and liquid of the crystallization product, and dry the solid phase to obtain the catalyst.

[0007] In the method of the present invention, the manganese salt mentioned in step (1) is manganese acetate; the molar ratio of manganese salt, organic ligand 2,5-dihydroxy-1,4-benzoquinone and deionized water is 1:(3~5):(300~800).

[0008] In the method of the present invention, the dissolution process in step (1) is preferably carried out by ultrasonic dispersion, with a temperature of 15~30℃, an ultrasonic time of 1~90 min, and an ultrasonic power of 100~600 W.

[0009] In the method of the present invention, the hydrothermal reaction conditions in step (1) are: temperature of 25~100℃, reaction time of 6~48 h; the hydrothermal reaction is carried out in a high-pressure reactor, and the reaction pressure is autogenous pressure.

[0010] In the method of this invention, the solid-liquid separation process described in steps (1) and (2) is carried out in a manner well known in the art, such as centrifugation or filtration. During the solid-liquid separation process, the solid phase is washed multiple times with deionized water. The centrifugation speed is 3000~10000 r / min, and the centrifugation time is 3~20 min.

[0011] In the method of the present invention, step (1) uses a vacuum drying oven for vacuum activation, the vacuum activation temperature is 100~200℃, and the vacuum activation time is 6~36 h.

[0012] In step (2) of the method of the present invention, the silicon source is silicon dioxide; the copper source is one or more of copper nitrate, copper chloride and copper sulfate; the template agent is one or more of P123, lauric acid, F127 and F108; the mass ratio of copper source, template agent, silicon source and deionized water is 1: (1~3): (3~6): (50~100).

[0013] In the method of the present invention, the mass ratio of Mn-dhbq seed crystal, benzoic acid and the mixed solution containing silicon source, copper source and template agent in step (2) is 1:8:(50~150).

[0014] In the method of the present invention, the drying temperature in step (5) is 100~200℃ and the drying time is 6~36 h.

[0015] This invention relates to the application of the Cu@Mn-Cu organic framework catalyst in the Fenton-like oxidation treatment of organic wastewater. The specific application conditions are as follows: the Cu@Mn-Cu organic framework catalyst is added to a pollutant solution containing H2O2. Initially, the reaction temperature is 20-30°C, and the reaction time is 5-15 min. Then, the reaction system is heated to 45-60°C, and the reaction continues for 10-15 min, thereby achieving a temperature-controlled Fenton-like degradation reaction and realizing rapid oxidation treatment of organic wastewater. The pollutants mentioned in this invention include one or more of chloroquine phosphate, bisphenol A, and methylene blue; the concentration of the pollutants is 10-50 mg / L; the concentration of the bimetallic organic framework catalyst is 0.05-1 g / L; and the concentration of H2O2 is 2-10 mM.

[0016] Compared with the prior art, the beneficial effects of the present invention are: (1) The present invention is based on the flexible framework structure of Mn-dhbq, and the copper-doped Mn-dhbq bimetallic organic framework skeleton and skeleton surface grown in situ are in a closed state at room temperature during the Fenton-like reaction process, and only the copper ions adsorbed on the skeleton surface interact with the manganese metal sites; when the temperature rises, the flexible framework flexibly releases the copper ions in the skeleton, and the copper ions adsorbed on the surface and the copper ions released in the skeleton work together, and more copper ions react with the manganese metal sites to achieve efficient regeneration of Mn(II), thereby greatly accelerating the Fenton-like reaction rate. By introducing copper ions into the manganese-based metal organic framework, and through cation doping and the construction of composite structures, the electronic structure of the composite material can be optimized and more catalytic active sites can be provided. The specific regeneration process of Mn(II) is as follows: In the Fenton-like reaction, a chain reaction occurs between Mn(II) and H2O2 to catalyze the generation of hydroxyl radicals. Mn(II) is oxidized to Mn(III), and Cu(II) is reduced to Cu(I) by H2O2. The generated Cu(I) and Mn(III) undergo a rapid redox reaction to generate Mn(II). The synergistic effect of the Mn-Cu dual sites in the Fenton-like reaction achieves the regeneration of Mn(II), and the overall framework of the composite structure remains unchanged.

[0017] (2) The method of the present invention uses SiO2 as a heterogeneous seed crystal, which adsorbs metal ions through surface functional groups (-OH, -COOH) to induce the growth of MOFs and the storage of copper ions; the template agent containing carboxylic acid groups coordinates with copper ions to form an ordered structure; at the same time, the cycling performance of the bimetallic organic framework is greatly improved at a certain temperature. Attached Figure Description

[0018] Figure 1 The images show the XRD patterns of the products obtained in Example 1, Comparative Example 1, and Comparative Example 2.

[0019] Figure 2SEM images of the products obtained in Example 1, Comparative Example 1, and Comparative Example 2.

[0020] Figure 3 XPS images of the products obtained in Experimental Example 1 and Comparative Example 1.

[0021] Figure 4 The degradation curves of CQ by the product obtained in Example 1 at different temperatures are shown.

[0022] Figure 5 The degradation curves of CQ by the products obtained in Example 1, Comparative Example 1, and Comparative Example 2 are shown.

[0023] Figure 6 Cyclic stability tests were conducted on the products obtained in Example 1 and Comparative Example 2.

[0024] Figure 7 The removal rate of the product obtained in Example 1 for three organic wastewater simulants is shown. Detailed Implementation

[0025] The present invention is further illustrated by the following embodiments: The present invention can be better understood from the following embodiments. However, those skilled in the art will readily understand that the specific material ratios, process conditions, and results described in the embodiments are for illustrative purposes only and should not, and will not, limit the present invention as described in detail in the claims.

[0026] Comparative Example 1 0.50 g of (CH3COO)2Mn·4H2O and 0.88 g of 2,5-dihydroxy-1,4-benzoquinone were added to 15 mL of deionized water and dissolved by sonication at 25 °C for 10 min. The solution was then transferred to a reaction vessel for hydrothermal reaction at 75 °C for 24 h. After the reaction, the reaction vessel was allowed to cool naturally, and the product was centrifuged at 4000 r / min for 10 min. The product was washed three times with deionized water until the supernatant was clear and transparent. The precipitate was collected and activated under vacuum at 150 °C for 24 h to obtain Mn-dhbq MOFs material.

[0027] Comparative Example 2 Based on Comparative Example 1, 0.85 g Cu(NO3)2·3H2O, 1 g Mn-dhbq, and 8 g benzoic acid were dissolved in 42.5 mL of deionized water, ultrasonically dispersed, and then the temperature was programmed to rise to 80°C at a rate of 5°C / h and held for 24 h. The mixture was then allowed to cool naturally to room temperature. The resulting reactants were separated into solid and liquid phases, washed repeatedly with deionized water, and the precipitate was collected and dried at 150°C for 24 h to obtain the powdered product Cu@Mn-dhbq.

[0028] Comparative Example 3 The preparation process was the same as that of Comparative Example 2, except that 1.70 g P123 and 0.85 g Cu(NO3)2·3H2O were dissolved in 42.5 mL of deionized water, and then 1 g Mn-dhbq and 8 g benzoic acid were added. The resulting product was denoted as Cu@Mn-1. Example 1

[0029] The preparation process was the same as that of Comparative Example 3, except that 1.70 g P123, 3.40 g SiO2 and 0.85 g Cu(NO3)2·3H2O were dissolved in 42.5 mL of deionized water, and the resulting product was denoted as Cu@Mn-Cu. Example 2

[0030] The preparation process was the same as that of Comparative Example 3, except that Cu(NO3)2·3H2O was replaced with CuCl2·2H2O and the amount of CuCl2·2H2O added was 0.57 g. The resulting product was denoted as Cu@Mn-Cu1. Example 3

[0031] The preparation process was the same as in Example 1, except that the amount of P123 added was 0.85 g and the amount of SiO2 added was 2.55 g. The resulting product was denoted as Cu@Mn-Cu2.

[0032] The XRD patterns of the products obtained in Example 1, Comparative Example 1, and Comparative Example 2 are shown below. Figure 1 As shown, by Figure 1 It can be seen that the main diffraction peak angles of Cu@Mn-Cu and Cu@Mn-dhbq are consistent with those of Mn-dhbq, and the diffraction peaks of the Cu complex phase also appear. However, the diffraction peak intensity of the Cu complex in Cu@Mn-dhbq is stronger, indicating that more Cu active sites in Cu@Mn-dhbq are adsorbed on the framework surface. The results show that copper doping does not significantly change the crystal structure of the composite material.

[0033] SEM images of the products obtained in Example 1, Comparative Example 1, and Comparative Example 2 are shown below. Figure 2 As shown in the figure, (a), (b), and (c) are SEM images of Mn-dhbq, Cu@Mn-dhbq, and Cu@Mn-Cu, respectively. Figure 2 It can be seen that Mn-dhbq exhibits a smooth plate-like structure. After the introduction of copper, the plate-like structures of Cu@Mn-dhbq and Cu@Mn-Cu can still be observed, with rough surfaces and irregular morphologies, proving the introduction of Cu active sites. Moreover, the morphological size of Cu@Mn-Cu is significantly reduced, with a size of 100~200 nm, which is beneficial to accelerating the Fenton-like reaction rate.

[0034] XPS plots of the products obtained in Experimental Example 1 and Comparative Example 1 are shown below. Figure 3 As shown, by Figure 3 It can be seen that Cu@Mn-Cu mainly contains C, O, Mn, and Cu elements, and the peaks near 951 and 931 eV correspond to Cu 2p, respectively. 1 / 2 and Cu 2p 3 / 2 The binding energy was determined, and XPS semi-quantitative results showed that the Cu to Mn elemental ratio on the Cu@Mn-Cu surface was 1.02:1, further verifying the successful preparation of the composite material. XRF determination of the elemental composition and content in the Cu@Mn-Cu bulk phase showed that the Cu to Mn elemental ratio in the Cu@Mn-Cu composite material was 1.37:1, thus inferring the chemical formula of Cu@Mn-Cu as Cu. 1.02 @Mn-Cu 0.35 This result confirms that Cu in Cu@Mn-Cu is not only adsorbed on the framework surface, but also exists inside the framework.

[0035] The copper and manganese elements in the surface and bulk phases of the products obtained in Examples 2, 3, and Comparative Example 3 were analyzed by XRF and XPS. The standard-free semi-quantitative XRF results showed that the Cu:Mn ratio in the bulk phase of Example 2 was 1.05:1, in Example 3 it was 1.86:1, and in Comparative Example 3 it was 0.65:1, indicating that the addition of SiO2 resulted in a large retention of copper ions in the MOFs. The semi-quantitative XPS results showed that the Cu:Mn ratio on the surface of Example 2 was 0.82:1, in Example 3 it was 1.27:1, and in Comparative Example 3 it was 0.62:1, suggesting that the chemical formula of the product obtained in Example 2 is Cu. 0.82 @Mn-Cu 0.23 The chemical formula of the product obtained in Example 3 is Cu. 1.27 @Mn-Cu 0.59 The bulk and surface Cu-Mn elemental ratios of the product obtained in Comparative Example 3 were not significantly different, indicating that copper ions only existed on the framework surface. The degradation performance of the products from Examples 1, 1, and 2 on organic wastewater simulants was analyzed using the following specific experimental methods: Chloroquine phosphate (CQ) was used as a simulant for organic wastewater to study the Fenton-like degradation performance of the catalytic material. 5 mg of the product prepared in Example 1 was added to 50 mL of a mixed solution of 20 mg / L CQ and 5 mM H₂O₂. The solutions were stirred continuously at 25 °C and 50 °C for 20 min, respectively. During this period, 1 mL samples were taken at intervals and filtered through a membrane. The absorbance was measured using a UV-Vis spectrophotometer. The removal rate of CQ by the product was calculated based on the absorbance changes. Simultaneously, the absorbance changes of 50 mL of the mixed solution of 20 mg / L chloroquine phosphate (CQ) and 5 mM H₂O₂ without the addition of the catalytic material were measured at 25 °C and 50 °C.

[0036] Take 5 mg of the products obtained in Example 1, Comparative Example 1 and Comparative Example 2 respectively, and add them to 50 mL of a mixed solution of 20 mg / L chloroquine phosphate (CQ) and 5 mM H2O2. After stirring continuously at 25℃ for 10 min, quickly transfer the solution to a 50℃ constant temperature water bath. Take 1 mL of sample at regular intervals and filter it through a filter membrane. Measure the absorbance using a UV-Vis spectrophotometer. Calculate the removal rate of CQ by the product based on the change in absorbance.

[0037] The removal rates of CQ by the product prepared in Example 1 at constant temperatures of 25°C and 50°C are as follows: Figure 4 As shown, after 20 min, Cu@Mn-Cu achieved removal rates of 92.37% and 99.86% of CQ under isothermal conditions of 25℃ and 50℃, respectively. When no catalytic material was added to the reaction system, CQ hardly degraded, so temperature had little effect on the degradation effect of CQ. However, Cu@Mn-Cu showed a more significant degradation effect on CQ at 50℃, indicating that Cu@Mn-Cu prepared in Example 1 is highly sensitive to temperature and exhibits a superior degradation effect on CQ at 50℃.

[0038] The removal rates of CQ by the products prepared in Examples 1, 1, and 2 are as follows: Figure 5 As shown, under constant temperature conditions of 25℃, the removal rates of CQ by Mn-dhbq, Cu@Mn-dhbq, and Cu@Mn-Cu were 10.37%, 80.31%, and 85.33%, respectively, after 10 min. After further reaction at a constant temperature of 50℃ for another 10 min, the final removal rate of CQ by Cu@Mn-dhbq after heating was 88.74%, while Cu@Mn-Cu showed a more significant degradation effect on CQ, reaching 99.83% after 20 min. This indicates that, compared to Comparative Examples 1 and 2, the temperature-sensitive Cu@Mn-Cu prepared in Example 1 exhibits a superior degradation effect on CQ.

[0039] The cyclic stability tests of the products obtained in Example 1 and Comparative Example 2 under Fenton-like degradation of CQ at a constant temperature of 50°C are as follows: Figure 6 As shown, after five cycles of Fenton-like degradation of organic wastewater simulants at a constant temperature of 50℃, Cu@Mn-Cu exhibits better cycle stability and reusability than Cu@Mn-dhbq.

[0040] The removal rates of the product prepared in Example 1 for three organic wastewater simulants CQ, bisphenol A (BPA), and methylene blue (MB) at a constant temperature of 50°C are as follows: Figure 7 As shown, the Cu@Mn-Cu prepared in Example 1 almost completely degraded CQ, BPA and MB within 20 min, indicating that this type of Fenton catalyst is suitable for degrading organic wastewater containing multiple pollutants.

Claims

1. A Cu@Mn-Cu organic framework catalyst, characterized in that: The microstructure is a rough, sheet-like structure with a size of 100-200 nm. The Cu to Mn ratio in the bulk catalyst phase is 1-2:1, while the Cu to Mn ratio on the framework surface is 0.8-1.3:

1.

2. A method for preparing the Cu@Mn-Cu organic framework catalyst according to claim 1, characterized in that... The following contents are included: (1) Dissolve the organic ligand 2,5-dihydroxy-1,4-benzoquinone and manganese salt in deionized water and carry out a hydrothermal reaction. The hydrothermal reaction product is separated into solid and liquid phases, and the solid phase is activated under vacuum to obtain Mn-dhbq seed crystals; (2) Add Mn-dhbq seed crystals and benzoic acid to a mixture containing silicon source, copper source and template agent, mix evenly, and carry out a crystallization reaction. After the reaction is completed, the crystallization product is separated into solid and liquid phases, and the solid phase is dried to obtain a catalyst.

3. The method according to claim 2, characterized in that: The manganese salt mentioned in step (1) is manganese acetate; the molar ratio of manganese salt, organic ligand 2,5-dihydroxy-1,4-benzoquinone and deionized water is 1:(3~5):(300~800).

4. The method according to claim 2, characterized in that: The dissolution process in step (1) is carried out by ultrasonic dispersion at a temperature of 15~30℃, an ultrasonic time of 1~90 min, and an ultrasonic power of 100~600 W.

5. The method according to claim 2, characterized in that: The hydrothermal reaction conditions for step (1) are: temperature 25~100℃, reaction time 6~48 h; the hydrothermal reaction is carried out in a high-pressure reactor, and the reaction pressure is autogenous pressure.

6. The method according to claim 2, characterized in that: Step (1) The vacuum activation temperature is 100~200℃ and the vacuum activation time is 6~36.

7. The method according to claim 2, characterized in that: In step (2), the silicon source is silicon dioxide; the copper source is one or more of copper nitrate, copper chloride and copper sulfate; and the template agent is one or more of P123, lauric acid, F127 and F108.

8. The method according to claim 2, characterized in that: The mass ratio of copper source, template agent, silicon source and deionized water is 1:(1~3):(3~6):(50~100).

9. The method according to claim 2, characterized in that: In step (2), the mass ratio of Mn-dhbq seed crystals, benzoic acid and a mixture solution containing silicon source, copper source and template agent is 1:8:(50~150).

10. The application of the Cu@Mn-Cu organic framework catalyst according to claim 1 in the Fenton-like oxidation treatment of organic wastewater.

11. The application according to claim 10, characterized in that: The specific application conditions are as follows: the Cu@Mn-Cu organic framework catalyst is added to the pollutant solution containing H2O2. The initial reaction temperature is 20~30℃, and the reaction is carried out for 5~15 min. Then the reaction system is heated to 45~60℃ and the reaction is continued for 10~15 min.

12. The application according to claim 11, characterized in that: The contaminants include one or more of chloroquine phosphate, bisphenol A, and methylene blue; the concentration of the contaminants is 10-50 mg / L.

13. The application according to claim 11, characterized in that: The concentration of the bimetallic organic framework catalyst is 0.05~1 g / L; the concentration of H2O2 is 2~10 mM.

Citation Information

Patent Citations

  • Application of copper-manganese bimetal MOFs in catalytic degradation of sulfonamide antibiotics