Preparation method of alkali-resistant organic silicon emulsion
A water-in-oil type high-content, low-viscosity silicone emulsion was prepared by condensation reaction of polyether-modified polysiloxane and silicone defoaming composition. This solved the problem of poor stability of silicone emulsion under alkaline conditions and improved its dispersibility and functional performance in alkaline systems.
Patent Information
- Application Number
- CN202510663283.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-22
- Publication Date
- 2026-11-24
AI Technical Summary
Existing silicone emulsions exhibit poor stability in application systems, especially under alkaline conditions, resulting in poor functional performance and difficulty in forming a dense microparticle layer.
A water-in-oil type high-content, low-viscosity silicone emulsion is prepared by condensing the active silanium-hydrogen bonds on polyether-modified polysiloxane with the active groups in the silicone defoaming composition under the action of an alkaline catalyst. Polyether is used to help disperse the emulsion, and the use of surfactants, stabilizers and preservatives ensures the stability of the emulsion in an alkaline system.
This study achieved good stability and dispersibility of silicone emulsions in alkaline systems, improving their overall performance in applications, especially their defoaming speed and foam suppression function.
Smart Images

Figure BDA0005414428950000021 
Figure BDA0005414428950000022 
Figure BDA0005414428950000051
Abstract
Description
Technical Field
[0001] This invention relates to a method for preparing an alkali-resistant organosilicon emulsion, and more precisely, to a method for preparing an alkali-resistant, high-content, low-viscosity organosilicon emulsion, belonging to the field of fine chemical formulation technology. Background Technology
[0002] Organosilicon emulsions have a wide range of applications, including textile finishing agents, fabric softeners, antiperspirants, defoamers, mold release agents, and waterproofing agents. The key technologies for these products are still largely controlled by foreign companies. Many domestic enterprises are imitating and improving upon these technologies, but their performance consistently lags behind foreign products. The fundamental reason for this is that as these emulsions function, the particle size gradually increases. For example, the particle size of waterproofing agents is a crucial factor in evaluating their effectiveness. If the emulsion particles are small, a dense microparticle layer can form on the substrate surface; conversely, if the particles are large, a dense microparticle layer will not form. Similarly, for defoamers, domestic defoamers are characterized by fast defoaming speed, while foreign defoamers exhibit strong foam suppression and good compatibility. This is because the defoaming particles maintain a good particle size distribution in the working fluid for a longer period, making them less prone to aggregation and precipitation, thus demonstrating superior overall performance. Therefore, the stability of the emulsion is extremely important for it to fully perform its functions.
[0003] Improving the stability of silicone emulsions is a problem that many scholars and researchers are dedicated to studying: CN201010584419.8 uses strong shearing of various devices to prepare emulsions; CN200810124771.6 uses low-viscosity polysiloxanes to dilute high-viscosity silicone compositions, thereby dispersing the high-viscosity silicone compositions in water to finally obtain silicone emulsions; US4853474 improves the low-temperature resistance of emulsions through cross-linked silicone polyethers, but this method is difficult to control the degree of cross-linking of the silicone polyethers themselves, so it is difficult to ensure the consistency of emulsion stability; CN1807512 introduces that the function of silicone emulsions is related to many properties of the emulsions themselves, such as the temperature stability, shear resistance, dilution stability and storage stability of the emulsions; US5451692 introduces the application of alkyl silicone polyethers in the preparation of water-in-oil emulsions, which improves the compatibility with oil phase components through the introduction of alkyl groups. EP-A-163541, in its research on defoamers, noted that the preparation of emulsions of high-viscosity polysiloxanes is difficult, costly, and ineffective.
[0004] The inventors used the active hydrogen on polyether-modified polysiloxane to undergo a condensation reaction with the active groups in the organosilicon defoaming composition under the action of an alkaline catalyst, and used polyether to help disperse the mixture, to obtain a high-content, low-viscosity emulsion in water, which also has good stability in alkaline systems. Summary of the Invention
[0005] This invention discloses a method for preparing an alkali-resistant silicone emulsion, which can prepare a high-content, low-viscosity silicone emulsion and also solves the dispersibility problem of silicone emulsion in application systems.
[0006] Technical solution:
[0007] A method for preparing an alkali-resistant silicone emulsion is characterized in that the active silane-hydrogen bonds on polyether-modified polysiloxane undergo a condensation reaction with the active groups in the silicone defoaming composition under the action of an alkaline catalyst, and the polyether is used to help disperse the emulsion, thereby obtaining a water-in-oil type high-content silicone emulsion. This emulsion has a low viscosity, is easy to disperse in the system, and also has good stability in the alkaline system.
[0008] The raw materials for preparing the organosilicon emulsion include: organosilicon composition A, polyether-modified polysiloxane B, polyether C, alkaline catalyst D, surfactant E, water F, stabilizer G, and preservative H.
[0009] The silicone emulsion can be prepared by diluting it with water and a stabilizer in any proportion; taking the preparation of a silicone emulsion with a solid content of 50% as an example, the required mass percentages of each component are as follows:
[0010]
[0011] The sum of the mass percentages of the above components is 100%.
[0012] A. Organosilicon composition
[0013] The raw materials for preparing the organosilicon composition include: polyorganosiloxane (A-1), hydrogen-containing polyorganosiloxane (A-2), vinyl-containing polyorganosiloxane (A-3), hydrophobic silica (A4), vinyl silicone resin (A-5), and platinum catalyst (A-6);
[0014] The mass percentages of the components in the organosilicon composition are as follows:
[0015]
[0016] The sum of the mass percentages of the above components is 100%;
[0017] The method for preparing the organosilicon composition is as follows:
[0018] Polyorganosiloxane, hydrophobic silica, and vinyl silicone resin are added to a container, the temperature is raised to 80-180℃, the stirring is turned on and the speed is maintained at 1000-5000 rpm, and finally the mixture is processed by a homogenizer to make the particle size D50 of the hydrophobic silica and vinyl silicone resin less than 10μm, and then cooled to room temperature to obtain the "polyorganosiloxane dispersion".
[0019] At room temperature, hydrogen-containing polyorganosiloxane and vinyl-containing polyorganosiloxane are added to the above "polyorganosiloxane dispersion". The rotation speed is 500-2000 rpm, the temperature is increased to 60-90℃, and platinum catalyst is slowly added dropwise to the mixture. Then the temperature is increased to 100-150℃ and the reaction is maintained for 1-5 hours. After cooling to room temperature, the organosilicon composition is obtained.
[0020] (A-1) Polyorganosiloxane
[0021] The general structural formula of polyorganosiloxanes is as follows:
[0022] (R 1 (CH3)2SiO 1 / 2 ) a ((CH3)2SiO 2 / 2 ) b (R(CH3)SiO 2 / 2 ) c (I)
[0023] In formula (I), a, b, and c are the degrees of polymerization of the three repeating units in formula (I), and their values determine the viscosity of the polyorganosiloxane, which ranges from 0.65 to 1,000,000 mPa·s.
[0024] R and R 1 These substituents can be the same or different, including:
[0025] (1) Alkyl groups having 1 to 30 carbon atoms, including methyl, ethyl, n-propyl, isopropyl, butyl, pentyl, hexyl, octyl, decyl, dodecyl, tetradecyl, hexadecyl, octadecyl, eicosyl, dodecyl, tetradecyl, hexadecyl, octadecyl, eicosyl, dodecyl, tetradecyl, hexadecyl, octadecyl, and triadecyl.
[0026] (2) Aryl, including α-methylphenethyl and phenethyl;
[0027] (3) Hydroxyl group.
[0028] (A-2) Hydrogen-containing polyorganosiloxane
[0029] The general structural formula of hydrogen-containing polyorganosiloxanes is as follows:
[0030] (R2 (CH3)2SiO 1 / 2 ) d ((CH3)2SiO 2 / 2 ) e (H(CH3)SiO 2 / 2 ) f (II)
[0031] In formula (II), d, e and f are the degrees of polymerization of the three repeating units in formula (II), and their values determine the viscosity of the polyorganosiloxane. The dynamic viscosity at 25°C is 5 to 200 mPa·s, and the hydrogen content is 0.1 to 1.0%.
[0032] R 2 Substituents that are the same or different include:
[0033] (1) Alkyl groups having 1 to 6 carbon atoms, including methyl, ethyl, n-propyl, isopropyl, butyl, pentyl, and hexyl.
[0034] (2) Hydrogen atom.
[0035] (A-3) Contains vinyl polyorganosiloxane
[0036] The general structural formula of vinyl-containing polyorganosiloxanes is as follows:
[0037] (R 3 (CH3)2SiO 1 / 2 ) g ((CH3)2SiO 2 / 2 ) h (R 4 (CH3)SiO 2 / 2 ) i (SiO 4 / 2 ) j (III)
[0038] In formula (Ⅲ), g, h, i and j are the degrees of polymerization of the four repeating units in formula (Ⅲ), and their values determine the viscosity of the polyorganosiloxane. The dynamic viscosity at 25℃ is 100 to 10,000 mPa·s.
[0039] R 3 and R 4 These substituents can be the same or different, including:
[0040] (1) Alkyl groups having 1 to 6 carbon atoms, including methyl, ethyl, n-propyl, isopropyl, butyl, pentyl, and hexyl;
[0041] (2) Vinyl.
[0042] (A-4) Hydrophobic silica
[0043] The hydrophobic silica mentioned is hydrophobic silica produced by precipitation or vapor phase methods, with a specific surface area of 50–500 m². 2 / g; The hydrophobic treatment of hydrophobic silica is obtained by heating and stirring hydrophilic silica and a hydrophobic agent in a reaction vessel; the hydrophobic agent is selected from low viscosity trimethylsiloxy-terminated polydimethylsiloxane, low viscosity hydroxyl-terminated polydimethylsiloxane, hexamethyldisilazane, hexamethyldisilazane, dimethyldiethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, trimethylchlorosilane, dimethyldichlorosilane, methyltrichlorosilane, tetrachlorosilane, stearic acid, tetradecyl alcohol, hexadecyl alcohol, octadecyl alcohol, stearyl alcohol, octamethylcyclotetrasiloxane, tetramethylcyclotetrasiloxane, and hexamethylcyclotrisiloxane.
[0044] (A-5) Vinyl silicone resin
[0045] The vinyl silicone resin is composed of M-links and Q-links, with a molar ratio of 0.5 to 0.8; the vinyl content on the surface of the vinyl silicone resin is 0.2% to 0.5% by mass.
[0046] (A-6) Platinum catalyst
[0047] The platinum catalyst is one or more of the following: platinum-alcohol complex, platinum-olefin complex, platinum-alkoxide complex, platinum-ether complex, platinum-ketone complex, isopropanol chloroplatinate solution, or platinum-vinyl complex.
[0048] B. Polyether-modified polysiloxane
[0049] The structural formula of the polyether-modified polysiloxane is as follows:
[0050]
[0051] In formula (Ⅳ), the subscripts k, l and m are the degrees of polymerization of the three repeating units of formula (Ⅳ), where l is 2 to 5; the subscripts p and q are the degrees of polymerization of ethylene oxide EO and propylene oxide PO, and the values of p and q are 0 or 5 to 30, but cannot be 0 at the same time.
[0052] The hydrogen-containing polysiloxane used to prepare polyether-modified polysiloxane of formula (IV) has a hydrogen content of 0.1-0.5% and a dynamic viscosity of 50-2,000 mPa·s at 25°C.
[0053] The preparation method of polyether-modified polysiloxane of formula (Ⅳ) is to obtain hydrogen-containing polyorganosiloxane and allyl polyether by hydrosilylation reaction under the action of platinum metal. This method can be found in general organosilicon literature.
[0054] C. Alkaline catalyst
[0055] The alkaline catalyst is one or more of sodium hydroxide, potassium hydroxide, cesium hydroxide, and tetramethylammonium hydroxide.
[0056] D. Polyether
[0057] The structural formula of the polyether is as follows:
[0058] R 5 {M(EO) s (PO) t H} w (V)
[0059] In formula (V),
[0060] R 5 The functional groups in the initiator of polyether are selected from:
[0061] (1) Alkyl groups having 1 to 30 carbon atoms, including methyl, ethyl, n-propyl, isopropyl, butyl, pentyl, hexyl, octyl, decyl, dodecyl, tetradecyl, hexadecyl, octadecyl, eicosyl, dodecyl, tetradecyl, hexadecyl, octadecyl, eicosyl, dodecyl, tetradecyl, hexadecyl, octadecyl, and triadecyl.
[0062] (2) Hydrogen atom;
[0063] M is a linking group, including: -O-, -NH-;
[0064] The subscripts s and t represent the degree of polymerization of EO and PO, respectively, with s having an average value of 1–40 and t having an average value of 1–80.
[0065] The subscript w represents the functionality of the initiator, which is an integer from 1 to 4.
[0066] E. Surfactants
[0067] Surfactants include anionic surfactants, cationic surfactants, and nonionic surfactants.
[0068] The nonionic surfactants mentioned are nonylphenol polyoxyethylene ether, octylphenol polyoxyethylene ether, lauric acid polyoxyethylene ether, oleic acid polyoxyethylene ether, lauryl alcohol polyoxyethylene ether, cetyl alcohol polyoxyethylene ether, octadecyl alcohol polyoxyethylene ether, sorbitan monolaurate, sorbitan monopalmitate, sorbitan monostearate, sorbitan monooleate, sorbitan tristearate, sorbitan trioleate, polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate, polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan monooleate, polyoxyethylene sorbitan monooleate, polyoxyethylene sorbitan tristearate, polyoxyethylene sorbitan trioleate, long-chain fatty alcohol polyoxyethylene ethers, and surfactants like these.
[0069] The anionic surfactant is nonylphenol polyoxyethylene ether sulfate, octylphenol polyoxyethylene ether sulfate, alkyl phosphate, and similar surfactants.
[0070] The cationic surfactant is an alkyl benzyl ammonium salt, imidazoline laurylate, oleoyl imidazoline, a salt of hexadecylamine, and other similar surfactants.
[0071] The amphoteric surfactants mentioned are alkyltrimethylammonium caprolactone type and phosphate ester type amphoteric surfactants.
[0072] The surfactant is a nonionic surfactant, and the nonionic surfactant used is one or more combinations thereof.
[0073] F. Water
[0074] The water is the continuous phase of the emulsion, including tap water, process water, purified water, and ice in solid form.
[0075] G. Stabilizer
[0076] Generally, stabilizers can be added depending on the required emulsion viscosity. Stabilizers include polyacrylamide, carbomer, xanthan gum, polyacrylate, and cellulose ethers.
[0077] H. Preservatives
[0078] Preservatives such as methylisothiazolinone, benzisothiazolinone, octylisothiazolinone, and potassium sorbate are required for long-term storage.
[0079] The preparation method of alkali-resistant silicone emulsion is as follows:
[0080] Add polyether-modified polysiloxane, organosilicon composition and alkaline catalyst to a container, start stirring, raise the temperature to 60-120℃, and mix at 500-2000 rpm for 0.5-3 hours. When the viscosity rises to 2-5 times that before the reaction, add polyether, control the temperature at 80-100℃ and stir at 1000-2000 rpm for 0.5-1 hours to ensure that the above components are fully mixed. Then add surfactant and mix at 80-100℃ for 20-60 minutes to obtain an oil phase component mixture.
[0081] Under conditions of maintaining a temperature of 50–80℃ and a rotation speed of 800–2000 rpm, a stabilizer is added to the above oil phase component mixture, followed by the first portion of water. The water addition time is controlled at 20–60 minutes. After the water is added, the pH value is adjusted to 6.5–7.5, and the rotation speed is increased to 3000–5000 rpm and stirred for 10–60 minutes. The mixture is then ground 1–2 times using a colloid mill to ensure that the particles are fully dispersed, at which point an emulsion with a solid content of 65–70% is obtained. Finally, the above emulsion is diluted with the second portion of water and the stabilizer mixture, and a preservative is added and stirred evenly to obtain an emulsion with a solid content of about 50%.
[0082] Without changing the type, ratio, and process conditions of the raw materials, any product with an even lower solid content obtained by adding water and stabilizer to the above-mentioned oil-in-water emulsion with a solid content of 50% falls within the scope of protection of this patent. Detailed Implementation
[0083] Example 1:
[0084] Preparation of organosilicon composition A1
[0085] 65 parts of polyorganosiloxane (with a dynamic viscosity of 1000 mPa·s at 25°C, substituent R being methyl, substituent R being...) were used. 1 (Phenylethyl), 3 parts of fumed hydrophobic silica (specific surface area of 110 m²) 2 / g, the hydrophobic treatment agent is hexamethyldisilazane), 1 part of vinyl silicone resin (the molar ratio of M-unit to Q-unit is 0.5, and the vinyl content is 0.5%) is added to a container, the temperature is raised to 80℃, the stirring is turned on and the speed is maintained at 3000rpm, and finally the mixture is processed by a homogenizer to make the particle size D50 of the hydrophobic silica and vinyl silicone resin 5μm. After cooling to room temperature, the "polyorganosiloxane dispersion" is obtained.
[0086] Add 1 part of hydrogen-containing polyorganosiloxane (with a dynamic viscosity of 5.7 mPa·s at 25°C and substituent R) to the above "polyorganosiloxane dispersion" at room temperature. 2 Methyl group (containing 0.45% hydrogen) and 30 parts of vinyl-containing polyorganosiloxane (with a dynamic viscosity of 2700 mPa·s at 25°C, substituent R) 3 Methyl, substituent R 4 (For vinyl groups), at a rotation speed of 1000 rpm and a temperature of 70°C, 10 ppm of platinum-ketone complex catalyst (calculated as platinum) was slowly added dropwise to the above mixture, and then the temperature was increased to 120°C. After reacting at this temperature for 2 hours, the mixture was cooled to room temperature to obtain organosilicon composition A1.
[0087] Example 2:
[0088] Preparation of organosilicon composition A2
[0089] 45 parts of polyorganosiloxane (with a dynamic viscosity of 1000,000 mPa·s at 25°C, substituent R being α-methylphenylethyl, substituent R...) were mixed. 1 Methyl), 6 parts of precipitated hydrophobic silica (specific surface area of 50 m²) 2 / g, the hydrophobic treatment agent is hexamethyldisilazane), 5 parts of vinyl silicone resin (the molar ratio of M-unit to Q-unit is 0.8, and the vinyl content is 0.2%) are added to a container, the temperature is raised to 180℃, the stirring is turned on and the speed is maintained at 1000rpm, and finally the mixture is processed by a homogenizer to make the particle size D50 of the hydrophobic silica and vinyl silicone resin 6.9μm. After cooling to room temperature, the "polyorganosiloxane dispersion" is obtained.
[0090] At room temperature, 10 parts of hydrogen-containing polyorganosiloxane (with a dynamic viscosity of 200 mPa·s at 25°C and substituent R) were added to the above "polyorganosiloxane dispersion". 2 (Hexyl group, hydrogen content 0.1%) and 34 parts of vinyl-containing polyorganosiloxane (dynamic viscosity at 25°C is 10000 mPa·s, substituent R) 3 For butyl, substituent R 4 (Methyl), at a rotation speed of 500 rpm, the temperature was increased to 60°C. 30 ppm of platinum-alcohol complex catalyst (calculated as platinum) was slowly added dropwise to the above mixture, and then the temperature was increased to 150°C. After reacting at this temperature for 1 hour, the mixture was cooled to room temperature to obtain organosilicon composition A2.
[0091] Example 3:
[0092] Preparation of organosilicon composition A3
[0093] The 54.9 polyorganosiloxane (with a dynamic viscosity of 100 mPa·s at 25°C, substituent R being triacontane) was used. 1 1 part hydroxyl group), 1 part fumed hydrophobic silica (specific surface area of 500 m²) 2 / g, the hydrophobic treatment agent is dimethyldichlorosilane), 4 parts of vinyl silicone resin (the molar ratio of M-unit to Q-unit is 0.65, and the vinyl content is 0.33%) are added to a container, the temperature is raised to 120℃, the stirring is turned on and the speed is maintained at 5000rpm, and finally the mixture is processed by a homogenizer to make the particle size D50 of the hydrophobic silica and vinyl silicone resin 8.2μm. After cooling to room temperature, the "polyorganosiloxane dispersion" is obtained.
[0094] At room temperature, 0.1 parts of hydrogen-containing polyorganosiloxane (with a dynamic viscosity of 110 mPa·s at 25°C and substituent R) were added to the above "polyorganosiloxane dispersion". 2(containing hydrogen atoms, with a hydrogen content of 0.33%) and 40 parts of vinyl-containing polyorganosiloxane (with a dynamic viscosity of 100 mPa·s at 25°C, substituent R) 3 For vinyl, substituent R 4 (Hexyl), at a rotation speed of 2000 rpm and a temperature increase of 90°C, 20 ppm of platinum-olefin complex catalyst (calculated as platinum) was slowly added dropwise to the above mixture, and then the temperature was increased to 100°C. After holding the reaction at this temperature for 5 hours, the mixture was cooled to room temperature to obtain organosilicon composition A3.
[0095] Example 4:
[0096] Preparation of organosilicon composition A4
[0097] 55 parts of polyorganosiloxane (with a dynamic viscosity of 12500 mPa·s at 25°C, substituent R being hydroxyl, substituent R...) were mixed. 1 (C3A3) 5 parts hydrophobic silica (specific surface area 220 m²) 2 / g, the hydrophobic treatment agent is octamethylcyclotetrasiloxane), 2.5 parts of vinyl silicone resin (the molar ratio of M-units to Q-units is 0.58, and the vinyl content is 0.42%) are added to a container, the temperature is raised to 135℃, the stirring is turned on and the speed is maintained at 2800rpm, and finally the mixture is processed by a homogenizer to make the particle size D50 of the hydrophobic silica and vinyl silicone resin 3.2μm. After cooling to room temperature, the "polyorganosiloxane dispersion" is obtained.
[0098] 2.5 parts of hydrogen-containing polyorganosiloxane (with a dynamic viscosity of 23 mPa·s at 25°C, substituent R) were added to the above-mentioned "polyorganosiloxane dispersion" at room temperature. 2 (Butyl, hydrogen content 1.0%) and 35 parts of vinyl-containing polyorganosiloxane (dynamic viscosity at 25°C is 8700 mPa·s, substituent R) 3 For vinyl, substituent R 4 (Methyl), at a rotation speed of 1200 rpm, the temperature was increased to 82°C. A chloroplatinic acid / isopropanol solution catalyst of 13 ppm (calculated as platinum) was slowly added dropwise to the above mixture. Then the temperature was increased to 125°C and the reaction was maintained at this temperature for 3.5 h. After cooling to room temperature, the organosilicon composition A4 was obtained.
[0099] Example 5:
[0100] Preparation of organosilicon composition A5
[0101] 60 parts of polyorganosiloxane (with a dynamic viscosity of 560,000 mPa·s at 25°C, substituent R being methyl, substituent R being...) were used. 1 5 parts of methyl fumed silica (specific surface area 380 m²) 2 / g, the hydrophobic treatment agent is hexamethyldisilazane), 3 parts of vinyl silicone resin (the molar ratio of M-unit to Q-unit is 0.70, and the vinyl content is 0.28%) are added to a container, the temperature is raised to 127℃, the stirring is turned on and the speed is maintained at 2300rpm, and finally the mixture is processed by a homogenizer to make the particle size D50 of hydrophobic silica and vinyl silicone resin 2.9μm. After cooling to room temperature, the "polyorganosiloxane dispersion" is obtained.
[0102] At room temperature, 0.8 parts of hydrogen-containing polyorganosiloxane (with a dynamic viscosity of 13 mPa·s at 25°C, substituent R) were added to the above-mentioned "polyorganosiloxane dispersion". 2 The product is methyl (containing 0.75% hydrogen) and 31.2 parts of vinyl-containing polyorganosiloxane (with a dynamic viscosity of 9800 mPa·s at 25°C, substituent R). 3 For ethyl, substituent R 4 (For vinyl), at a rotation speed of 1800 rpm and a temperature of 88°C, 23 ppm of chloroplatinic acid / isopropanol solution catalyst (calculated as platinum) was slowly added dropwise to the above mixture, and then the temperature was further increased to 135°C. After holding the reaction at this temperature for 3 hours, the mixture was cooled to room temperature to obtain organosilicon composition A5.
[0103] The process conditions for using polyether-modified polysiloxane in the embodiments of this invention are shown in Table 1:
[0104] Table 1 Examples of raw material parameters for preparing polyether-modified polysiloxane B
[0105]
[0106] The polyethers used in the embodiments of this invention are shown in Table 2:
[0107] Table 2 Examples of Polyether D
[0108] D [R 5 ]]> M s t w D1 methyl group —nh— 1 6 1 D2 triacontyl group —O— 18 1 1 D3 hydrogen atom —nh— 30 12 1 D4 propyl group —O— 24 16 3 D5 pentaerythritol group —O— 10 30 4
[0109] Example 6:
[0110] Add 10 parts of polyether-modified polysiloxane B1, 23 parts of organosilicon composition A2 and 200 ppm of alkaline catalyst potassium hydroxide to a container, turn on the stirrer, raise the temperature to 60°C, and mix at 1000 rpm for 2 hours. After the viscosity rises to 3.5 times that before the reaction, add 15 parts of polyether D4, control the temperature at 90°C and stir at 1500 rpm for 1 hour to make the above components fully mixed. Then add 1 part of surfactant stearyl alcohol polyoxyethylene ether (2) and 1 part of stearyl alcohol polyoxyethylene ether (21), and mix at 100°C for 60 minutes to obtain an oil phase component mixture.
[0111] Under conditions of maintaining a temperature of 70℃ and a rotation speed of 1200 rpm, 0.7 parts of stabilizer polyacrylate were added to the above oil phase component mixture, followed by 27 parts of water (first part). The water addition time was controlled at 45 min. After the water was added, the pH value was adjusted to 7.0, and the rotation speed was increased to 4300 rpm and stirred for 35 min. The mixture was then ground once with a colloid mill to ensure that the particles were fully dispersed, resulting in an emulsion with a solid content of 65%. Finally, the emulsion was diluted with a mixture of 21.4 parts of water (second part) and 0.8 parts of stabilizer polyacrylate, and 0.1 parts of preservative methylisothiazolinone were added and stirred evenly to obtain emulsion E1 with a solid content of about 50% and a viscosity of 1276 mPa·s.
[0112] Example 7:
[0113] Add 20 parts of polyether-modified polysiloxane B2, 15 parts of organosilicon composition A4, and 1000 ppm of alkaline catalyst cesium hydroxide to a container. Start stirring, raise the temperature to 120°C, and mix at 2000 rpm for 3 hours. After the viscosity increases to 5 times the original value, add 10 parts of polyether D1, control the temperature at 80°C, and stir at 1000 rpm for 0.5 hours to ensure that the above components are fully mixed. Then add 2.6 parts of surfactant Span 60 and 2.4 parts of Tween 60, and mix at 80°C for 20 minutes to obtain an oil phase mixture.
[0114] Under conditions of maintaining a temperature of 50℃ and a rotation speed of 800 rpm, 0.08 parts of stabilizer polyacrylamide were added to the above oil phase component mixture, followed by 21.4 parts of water (part 1). The water addition time was controlled at 20 min. After the water was added, the pH value was adjusted to 6.5, and the rotation speed was increased to 3100 rpm and stirred for 10 min. The mixture was then ground twice using a colloid mill to ensure that the particles were fully dispersed, resulting in a 70% emulsion. Finally, the emulsion was diluted with a mixture of 28.2 parts of water (part 2) and 0.02 parts of stabilizer polyacrylamide, and 0.3 parts of preservative octylisothiazolinone were added and stirred evenly to obtain emulsion E2 with a solid content of about 50% and a viscosity of 1310 mPa·s.
[0115] Comparative Example 1: (Using a hydrogen-free polyether-modified polysiloxane instead of a hydrogen-containing one)
[0116] Add 20 parts of polyether-modified polysiloxane B21, 15 parts of organosilicon composition A4, and 1000 ppm of alkaline catalyst cesium hydroxide to a container. Start stirring, raise the temperature to 120°C, and mix at 2000 rpm for 3 hours. After the viscosity increases to 5 times the original value, add 10 parts of polyether D1, control the temperature at 80°C, and stir at 1000 rpm for 0.5 hours to ensure that the above components are fully mixed. Then add 2.6 parts of surfactant Span 60 and 2.4 parts of Tween 60, and mix at 80°C for 20 minutes to obtain an oil phase mixture.
[0117] Under conditions of maintaining a temperature of 50℃ and a rotation speed of 800 rpm, 0.08 parts of stabilizer polyacrylamide were added to the above oil phase component mixture, followed by 21.4 parts of the first part of water. The water addition time was controlled at 20 min. After the water was added, the pH value was adjusted to 6.5, and the rotation speed was increased to 3100 rpm and stirred for 10 min. The mixture was then ground twice by a colloid mill to ensure that the particles were fully dispersed, resulting in a 70% emulsion. Finally, the above emulsion was diluted with a mixture of 28.2 parts of the second part of water and 0.02 parts of stabilizer polyacrylamide, and 0.3 parts of preservative octylisothiazolinone were added and stirred evenly to obtain emulsion E21 with a solid content of about 50% and a viscosity of 1275 mPa·s.
[0118] Comparative Example 2: (without alkaline catalyst)
[0119] Add 20 parts of polyether-modified polysiloxane B2 and 15 parts of organosilicon composition A4 to a container, start stirring, raise the temperature to 120°C, and mix at 2000 rpm for 3 hours. After the viscosity increases to 5 times that before the reaction, add 10 parts of polyether D1, control the temperature at 80°C and stir at 1000 rpm for 0.5 hours to ensure that the above components are fully mixed. Then add 2.6 parts of surfactant Span 60 and 2.4 parts of Tween 60, and mix at 80°C for 20 minutes to obtain an oil phase component mixture.
[0120] Under conditions of maintaining a temperature of 50℃ and a rotation speed of 800 rpm, 0.08 parts of stabilizer polyacrylamide were added to the above oil phase component mixture, followed by 21.4 parts of water (part 1). The water addition time was controlled at 20 min. After the water was added, the pH value was adjusted to 6.5, and the rotation speed was increased to 3100 rpm and stirred for 10 min. The mixture was then ground twice using a colloid mill to ensure that the particles were fully dispersed, resulting in a 70% emulsion. Finally, the emulsion was diluted with a mixture of 28.2 parts of water (part 2) and 0.02 parts of stabilizer polyacrylamide, and 0.3 parts of preservative octylisothiazolinone were added and stirred evenly to obtain emulsion E22 with a solid content of about 50% and a viscosity of 1298 mPa·s.
[0121] Comparative Example 3: An alkaline catalyst was added, the process was changed, and the viscosity change was not considered.
[0122] Add 20 parts of polyether-modified polysiloxane B2, 15 parts of organosilicon composition A4 and 1000 ppm of alkaline catalyst cesium hydroxide to a container, start stirring, raise the temperature to 120°C, add 10 parts of polyether D1, control the temperature at 80°C and stir at 1000 rpm for 0.5 h to ensure that the above components are fully mixed and homogeneous, then add 2.6 parts of surfactant Span 60 and 2.4 parts of Tween 60, and mix at 80°C for 20 min to obtain an oil phase component mixture;
[0123] Under conditions of maintaining a temperature of 50℃ and a rotation speed of 800 rpm, 0.08 parts of stabilizer polyacrylamide were added to the above oil phase component mixture, followed by 21.4 parts of water (part 1). The water addition time was controlled at 20 min. After the water was added, the pH value was adjusted to 6.5, and the rotation speed was increased to 3100 rpm and stirred for 10 min. The mixture was then ground twice using a colloid mill to ensure that the particles were fully dispersed, resulting in a 70% emulsion. Finally, the emulsion was diluted with a mixture of 28.2 parts of water (part 2) and 0.02 parts of stabilizer polyacrylamide, and 0.3 parts of preservative octylisothiazolinone were added and stirred evenly to obtain emulsion E23 with a solid content of about 50% and a viscosity of 1157 mPa·s.
[0124] Example 8:
[0125] Add 12 parts of polyether-modified polysiloxane B5, 30 parts of organosilicon composition A3 and 650 ppm of alkaline catalyst sodium hydroxide to a container, start stirring, raise the temperature to 88°C, and mix at 500 rpm for 0.5 h. After the viscosity rises to twice the level before the reaction, add 5 parts of polyether D3, control the temperature at 100°C and stir at 2000 rpm for 0.75 h to ensure that the above components are fully mixed. Then add 2 parts of isomeric tridecyl alcohol polyoxyethylene ether (3) and 1 part of isomeric tridecyl alcohol polyoxyethylene ether (10) to the surfactant, and mix at 92°C for 45 min to obtain an oil phase component mixture.
[0126] Under conditions of maintaining a temperature of 80℃ and a rotation speed of 2000 rpm, 0.06 parts of carboxymethyl cellulose stabilizer were added to the above oil phase component mixture, followed by 21.4 parts of water (part 1). The water addition time was controlled at 60 min. After the water was added, the pH value was adjusted to 7.5, and the rotation speed was increased to 5000 rpm and stirred for 60 min. The mixture was then ground twice using a colloid mill to ensure that the microparticles were fully dispersed, resulting in a 70% emulsion. Finally, the emulsion was diluted with a mixture of 28.3 parts of water (part 2) and 0.04 parts of carboxymethyl cellulose stabilizer, and 0.2 parts of benzisothiazolinone preservative were added and stirred evenly to obtain emulsion E3 with a solid content of about 50% and a viscosity of 917 mPa·s.
[0127] Comparative Example 4: (without polyether)
[0128] Add 114 parts of polyether-modified polysiloxane B5, 33 parts of organosilicon composition A3 and 650 ppm of alkaline catalyst sodium hydroxide to a container, start stirring, raise the temperature to 88°C, and mix at 500 rpm for 0.5 h. After the viscosity rises to twice the original value, add 2 parts of isomeric tridecyl alcohol polyoxyethylene ether (3) and 1 part of isomeric tridecyl alcohol polyoxyethylene ether (10) to the surfactant, and mix at 92°C for 45 min to obtain an oil phase component mixture.
[0129] Under conditions of maintaining a temperature of 80℃ and a rotation speed of 2000 rpm, 0.06 parts of carboxymethyl cellulose stabilizer were added to the above oil phase component mixture, followed by 21.4 parts of water (part 1). The water addition time was controlled at 60 min. After the water was added, the pH value was adjusted to 7.5, and the rotation speed was increased to 5000 rpm and stirred for 60 min. The mixture was then ground twice using a colloid mill to ensure that the particles were fully dispersed, resulting in a 70% emulsion. Finally, the emulsion was diluted with a mixture of 28.3 parts of water (part 2) and 0.04 parts of carboxymethyl cellulose stabilizer, and 0.2 parts of benzisothiazolinone preservative were added and stirred evenly to obtain emulsion E33 with a solid content of about 50% and a viscosity of 4817 mPa·s.
[0130] Example 9:
[0131] Add 5 parts of polyether-modified polysiloxane B3, 30 parts of organosilicon composition A1 and 340 ppm of alkaline catalyst tetramethylammonium hydroxide to a container, start stirring, raise the temperature to 102°C, and mix at 1300 rpm for 1.5 h. After the viscosity increases to 2.8 times that before the reaction, add 10 parts of polyether D5, control the temperature at 95°C and stir at 1600 rpm for 0.8 h to make the above components fully mixed. Then add 3 parts of fatty alcohol polyoxyethylene ether (3) and 2 parts of fatty alcohol polyoxyethylene ether (9) surfactants and mix at 90°C for 35 min to obtain an oil phase component mixture.
[0132] Under conditions of maintaining a temperature of 72℃ and a rotation speed of 1800 rpm, 1.6 parts of stabilizer polyacrylate were added to the above oil phase component mixture, followed by 9 parts of water (part 1). The water addition time was controlled at 45 min. After the water was added, the pH value was adjusted to 7.0, and the rotation speed was increased to 3800 rpm and stirred for 45 min. The mixture was then ground once with a colloid mill to ensure that the particles were fully dispersed, resulting in an emulsion with a solid content of 66%. Finally, the emulsion was diluted with a mixture of 38.7 parts of water (part 2) and 0.4 parts of stabilizer polyacrylate, and 0.3 parts of preservative potassium sorbate were added and stirred evenly to obtain emulsion E4 with a solid content of about 50% and a viscosity of 853 mPa·s.
[0133] Example 10:
[0134] Add 12 parts of polyether-modified polysiloxane B4, 19 parts of organosilicon composition A5 and 500 ppm of alkaline catalyst potassium hydroxide to a container, start stirring, raise the temperature to 110°C, and mix at 1150 rpm for 2 hours. After the viscosity rises to 4.5 times that before the reaction, add 15 parts of polyether D2, control the temperature at 86°C and stir at 1200 rpm for 1 hour to ensure that the above components are fully mixed. Then add 2.6 parts of stearic acid polyoxyethylene ether (3) and 1.4 parts of stearic acid polyoxyethylene ether (12) surfactants and mix at 87°C for 55 minutes to obtain an oil phase component mixture.
[0135] Under conditions of maintaining a temperature of 63℃ and a rotation speed of 1050 rpm, 1.4 parts of stabilizer polyacrylate were added to the above oil phase component mixture, followed by 20 parts of water (part 1). The water addition time was controlled at 35 min. After the water was added, the pH value was adjusted to 7.0, and the rotation speed was increased to 4200 rpm and stirred for 52 min. The mixture was then ground twice using a colloid mill to ensure that the particles were fully dispersed, resulting in a 70% emulsion. Finally, the emulsion was diluted with a mixture of 28 parts of water (part 2) and 0.6 parts of stabilizer polyacrylate, and the preservative methylisothiazolinone was added and stirred evenly to obtain emulsion E5 with a solid content of about 50% and a viscosity of 1048 mPa·s.
[0136] Emulsion Testing and Evaluation
[0137] The performance evaluation items for the organosilicon emulsion prepared by the method of this invention include emulsion particle size, centrifugal stability, and alkali resistance stability, wherein the method for alkali resistance stability is as follows:
[0138] Add 200g of deionized water and 4g of sodium hydroxide to a 250ml beaker, stir well, then add 4g of the above-mentioned organosilicon emulsion, stir well, place in a water bath at 70℃ for 2h, and record the water precipitation status of the dispersion after 2h; then continue to stand at room temperature for 24h, and record the water precipitation status of the dispersion after 24h. The results are shown in Table 3.
[0139] The defoaming performance test method is as follows: 98.2% purified water, 0.5% AEO9 and 0.3% sodium dodecylbenzenesulfonate are added to a beaker and stirred evenly to prepare the solution.
[0140] Add 50 ml of foaming material to a 100 ml stoppered graduated cylinder, add 10 μL of 50% defoamer, shake vertically up and down 30 times, and record the time it takes for the foam to disappear to the liquid surface, expressed in seconds. The results are shown in Table 3.
[0141] Table 3 Comparison of stability and alkali resistance of emulsions prepared by the patented method
[0142]
[0143] As can be seen from the results shown in Table 3:
[0144] Emulsions from E1 to E5 have low viscosity, small particle size, and excellent defoaming performance. They also have good compatibility in alkaline solutions, and no stringy substances are precipitated in the water or on the liquid surface.
[0145] The test data from E2 and E21-E23 show that polyether-modified polysiloxane and organosilicon composition are chemically bonded together, making it easier to obtain high-content, low-viscosity, and alkali-resistant organosilicon emulsions. If no chemical reaction occurs between them, the difficulty of emulsion preparation increases, the resulting emulsion has a larger particle size, and it is unstable in alkaline solutions.
[0146] By comparing E3 and E31, it can be found that the introduction of polyether has almost no impact on alkali resistance and defoaming performance, but can significantly reduce the viscosity of the emulsion.
Claims
1. A method for preparing an alkali-resistant organosilicon emulsion, characterized in that, The raw materials for preparing the organosilicon emulsion are: organosilicon composition A, polyether-modified polysiloxane B, polyether C, alkaline catalyst D, surfactant E, water F, stabilizer G, and preservative H; The prepared silicone emulsion can be diluted with water and stabilizer in any proportion; taking the preparation of a silicone emulsion with a solid content of 50% as an example, the required mass percentages of each component are as follows: The sum of the mass percentages of the above components is 100%; The preparation method of alkali-resistant silicone emulsion is as follows: Add polyether-modified polysiloxane, organosilicon composition and alkaline catalyst to a container, start stirring, raise the temperature to 60-120℃, and mix at 500-2000 rpm for 0.5-3 hours. When the viscosity rises to 2-5 times that before the reaction, add polyether, control the temperature at 80-100℃ and stir at 1000-2000 rpm for 0.5-1 hours to ensure that the above components are fully mixed. Then add surfactant and mix at 80-100℃ for 20-60 minutes to obtain an oil phase component mixture. Under conditions of maintaining a temperature of 50–80℃ and a rotation speed of 800–2000 rpm, a stabilizer is added to the above oil phase component mixture, followed by the first portion of water. The water addition time is controlled at 20–60 minutes. After the water is added, the pH value is adjusted to 6.5–7.5, and the rotation speed is increased to 3000–5000 rpm and stirred for 10–60 minutes. The mixture is then ground 1–2 times using a colloid mill to ensure that the particles are fully dispersed, resulting in an emulsion with a solid content of 65–70%. Finally, the emulsion is diluted with a mixture of the second portion of water and the stabilizer, and a preservative is added and stirred evenly to obtain an emulsion with a solid content of approximately 50%. A. Organosilicon composition The raw materials for preparing the organosilicon composition are polyorganosiloxane A-1, hydrogen-containing polyorganosiloxane A-2, vinyl-containing polyorganosiloxane A-3, hydrophobic silica A4, vinyl silicone resin A-5, and platinum catalyst A-6. The mass percentages of the components in the organosilicon composition are as follows: The sum of the mass percentages of the above components is 100%; The method for preparing the organosilicon composition is as follows: Polyorganosiloxane, hydrophobic silica, and vinyl silicone resin are added to a container, the temperature is raised to 80-180℃, the stirring is turned on and the speed is maintained at 1000-5000 rpm, and finally the mixture is processed by a homogenizer to make the particle size D50 of the hydrophobic silica and vinyl silicone resin less than 10μm, and then cooled to room temperature to obtain "polyorganosiloxane dispersion". At room temperature, hydrogen-containing polyorganosiloxane and vinyl-containing polyorganosiloxane are added to the above "polyorganosiloxane dispersion". The rotation speed is 500-2000 rpm, the temperature is increased to 60-90℃, and platinum catalyst is slowly added dropwise to the above mixture. Then the temperature is continued to rise to 100-150℃, and the reaction is maintained for 1-5 hours. After cooling to room temperature, the organosilicon composition is obtained. B. Polyether-modified polysiloxane The structural formula of the polyether-modified polysiloxane is as follows: In formula (Ⅳ), the subscripts k, l and m are the degrees of polymerization of the three repeating units of formula (Ⅳ), where l is 2 to 5; the subscripts p and q are the degrees of polymerization of ethylene oxide EO and propylene oxide PO, and the values of p and q are 0 or 5 to 30, but cannot be 0 at the same time. C. Alkaline catalyst The alkaline catalyst is one or more of sodium hydroxide, potassium hydroxide, cesium hydroxide, and tetramethylammonium hydroxide; D. Polyether The structural formula of the polyether is as follows: R 5 {M(EO) s (PO) t H} w (Ⅴ) In equation (V), R 5 The functional group in the initiator of polyether is selected from alkyl groups with 1 to 30 carbon atoms or hydrogen atoms; M is the linking group, including: -O-, -NH-; the subscripts s and t are the degree of polymerization of EO and PO, respectively, with an average value of 1 to 40 for s and an average value of 1 to 80 for t; the subscript w is the functionality of the initiator, which is an integer from 1 to 4. D. Surfactants, specifically nonionic surfactants; E. Water, which includes tap water, process water, purified water, and ice in solid form; F. Stabilizers, wherein the stabilizers are polyacrylamide, carbomer, xanthan gum, polyacrylate, and cellulose ethers; G. Preservatives, wherein the preservatives are methylisothiazolinone, benzisothiazolinone, octylisothiazolinone, potassium sorbate, etc.
2. The alkali-resistant silicone emulsion according to claim 1, characterized in that, The general structural formula of the polyorganosiloxane used to prepare the organosilicon composition is as follows: (R 1 (CH3)2SiO 1 / 2 ) a ((CH3)2SiO 2 / 2 ) b (R(CH3)SiO 2 / 2 ) c (Ⅰ) In equation (I), a, b, and c are the degrees of polymerization of the three repeating units in equation (I), and their values determine the viscosity of the polyorganosiloxane, which ranges from 0.65 to 1,000,000 mPa·s; R and R 1 The substituents may be the same or different, and these substituents are selected from alkyl groups having 1 to 30 carbon atoms; or aryl groups; or hydroxyl groups.
3. The alkali-resistant silicone emulsion according to claim 1, characterized in that, The general structural formula of the hydrogen-containing polyorganosiloxane used in the preparation of the organosilicon composition is as follows: (R 2 (CH3)2SiO 1 / 2 ) d ((CH3)2SiO 2 / 2 ) e (H(CH3)SiO 2 / 2 ) f (Ⅱ) In formula (II), d, e, and f are the degrees of polymerization of the three repeating units in formula (II), and their values determine the viscosity of the polyorganosiloxane. The dynamic viscosity at 25°C is 5–200 mPa·s, and the hydrogen content is 0.1–1.0%. 2 The same or different substituents are selected from alkyl groups having 1 to 6 carbon atoms; or hydrogen atoms.
4. The alkali-resistant silicone emulsion according to claim 1, characterized in that, The general structural formula of the vinyl-containing polyorganosiloxane used in the preparation of the organosilicon composition is as follows: (R 3 (CH3)2SiO 1 / 2 ) g ((CH3)2SiO 2 / 2 ) h (R 4 (CH3)SiO 2 / 2 ) i (SiO 4 / 2 ) j (Ⅲ) In formula (Ⅲ), g, h, i, and j are the degrees of polymerization of the four repeating units in formula (Ⅲ), and their values determine the viscosity of the polyorganosiloxane. The dynamic viscosity at 25℃ is 100–10,000 mPa·s; R 3 and R 4 The substituents may be the same or different, and these substituents are selected from alkyl or vinyl groups having 1 to 6 carbon atoms.
5. The alkali-resistant silicone emulsion according to claim 1, characterized in that, The hydrophobic silica used in the preparation of the organosilicon composition is hydrophobic silica obtained by precipitation or fumed chromatography, with a specific surface area of 50–500 m². 2 / g.
6. The hydrophobic silica according to claim 5, characterized in that, The hydrophobic treatment of the aforementioned hydrophobic silica is obtained by heating and stirring hydrophilic silica and a hydrophobic agent in a reaction vessel; the hydrophobic agent is selected from low-viscosity trimethylsiloxy-terminated polydimethylsiloxane, low-viscosity hydroxyl-terminated polydimethylsiloxane, hexamethyldisilazane, hexamethyldisilazane, dimethyldiethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, trimethylchlorosilane, dimethyldichlorosilane, methyltrichlorosilane, tetrachlorosilane, stearic acid, tetradecyl alcohol, hexadecyl alcohol, octadecyl alcohol, stearyl alcohol, octamethylcyclotetrasiloxane, tetramethylcyclotetrasiloxane, and hexamethylcyclotrisiloxane.
7. The alkali-resistant silicone emulsion according to claim 1, characterized in that, The vinyl silicone resin used to prepare the organosilicon composition is composed of M-linkages and Q-linkages, with a molar ratio of 0.5 to 0.8; the vinyl mass percentage on the surface of the vinyl silicone resin is 0.2% to 0.5%.
8. The alkali-resistant silicone emulsion according to claim 1, characterized in that, The platinum catalyst used to prepare the organosilicon composition is one or more of the following: platinum-alcohol complex, platinum-olefin complex, platinum-alkoxide complex, platinum-ether complex, platinum-ketone complex, isopropanol chloroplatinate solution, or platinum-vinyl complex.
9. The alkali-resistant silicone emulsion according to claim 1, characterized in that, The hydrogen-containing polysiloxane used to prepare the polyether-modified polysiloxane of formula (IV) has a hydrogen content of 0.1-0.5% and a dynamic viscosity of 50-2,000 mPa·s at 25°C.
10. The alkali-resistant silicone emulsion according to claim 1, characterized in that, The nonionic surfactants mentioned are nonylphenol polyoxyethylene ether, octylphenol polyoxyethylene ether, lauric acid polyoxyethylene ether, oleic acid polyoxyethylene ether, lauryl alcohol polyoxyethylene ether, cetyl alcohol polyoxyethylene ether, octadecyl alcohol polyoxyethylene ether, sorbitan monolaurate, sorbitan monopalmitate, sorbitan monostearate, sorbitan monooleate, sorbitan tristearate, sorbitan trioleate, polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate, polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan monooleate, polyoxyethylene sorbitan monooleate, polyoxyethylene sorbitan tristearate, polyoxyethylene sorbitan trioleate, long-chain fatty alcohol polyoxyethylene ethers, and surfactants like these.
Citation Information
Patent Citations
Method for dispersing high viscosity organosilicon composition to water
CN101348571B
Method for mechanically dispersing high-viscosity organic silicon composition
CN102060999A
Method of producing a silicone defoamer composition
EP0163541A2
Cross-linked organopolysiloxanes and emulsions based thereon
US4853474A
Silicone polyether alkyl copolymer synthesis
US5451692A