Planar alloy diode structure

By first performing metal photolithography and annealing of the P-type alloy area in the planar alloy diode to form a P-type alloy junction, the problems of poor oxide layer quality and large leakage current in the Al alloy process are solved, and low leakage and high reliability are achieved. Planar alloy diodes.

CN221861669UActive Publication Date: 2024-10-18CHINA ZHENHUA GRP YONGGUANG ELECTRONICS CO LTD STATE OWNED NO 873 FACTORY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202323453177.0
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2023-12-18
Publication Date
2024-10-18
Estimated Expiration
2033-12-18

AI Technical Summary

Technical Problem

In the existing planar alloy diode, due to the entire surface coverage of Al metal in the Al alloy process, the quality of the oxide layer deteriorates, thereby increasing the leakage current, and Al diffuses to the edge of the P diffusion junction, causing the reverse leakage to increase.

Method used

The P-type alloy junction is formed by first performing metal photolithography and annealing in the P-type alloy area, controlling the distance between the alloy area boundary and the P-diffusion junction ring boundary, preventing Al from diffusing to the ring boundary, and preventing Al from entering the oxide layer through the passivation layer, and is prepared Develop planar alloy diodes with low leakage and high reliability.

Benefits of technology

It effectively reduces the reverse leakage current of the device, prevents Al from diffusing into the oxide layer, improves the quality of the oxide layer, and realizes an ultra-low voltage and high-reliability planar alloy diode.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN221861669U_ABST
    Figure CN221861669U_ABST
Patent Text Reader

Abstract

A planar alloy diode structure comprises an N-type substrate region; the P-type diffusion junction is positioned around the edge of the N-type substrate region; a P-type alloy junction is arranged in the active region of the N-type substrate region; a passivation layer is arranged on the edge of the surface of the N-type substrate region; an anode metal layer is arranged on the surface of the P-type alloy junction; and a cathode metal layer is arranged on the back surface of the N-type substrate layer. The Zener diode works in a reverse bias state, the doping concentration of the P-type alloy region and the doping concentration of the N-type substrate region are high, when the reverse bias voltage of the device is gradually increased, the device has a tunnel breakdown effect, the doping concentration of the P-type diffusion region on the edge of the device is low, the junction depth is large, the electric field concentration effect on the edge of the device can be reduced, and the device reliability is improved. The breakdown point of the device is generally located at the junction of the P-type alloy junction and the N-type substrate, so that the reverse leakage current of the device can be effectively reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The utility model relates to a planar alloy diode structure. Background Art

[0002] In the prior art, the edge of the planar alloy diode is formed into a diffused P-type region by boron diffusion, and then a metal contact window is formed by photolithography. Then, metal Al is evaporated on the front of the chip, and the alloy and corrosion are performed to form a P-type alloy junction. Then, the front metallization is performed to form an anode, and the back metallization is performed to form a diode cathode. This device is a typical alloy diode structure. The active area is obtained by Al alloy. The doping concentration is relatively high, and the concentration of the substrate is also very high. The high-concentration P and N regions can just undergo Zener breakdown to form an ultra-low voltage device. The edge P diffusion junction is a junction terminal protection to prevent edge electric field concentration. In principle, this device can form a low-leakage Zener diode. However, when performing the Al alloy process, since the Al metal is covered on the entire surface, Al will enter the oxide layer when the alloy is heated, resulting in a deterioration in the quality of the oxide layer, which in turn causes the device leakage current to increase. In addition to longitudinal diffusion, Al will also undergo lateral diffusion. Al may diffuse to the edge of the P diffusion junction, resulting in the concentration of the chip edge electric field and thus increasing the reverse leakage. Utility Model Content

[0003] In order to solve the above technical problems, the utility model provides a planar alloy diode structure.

[0004] The utility model is realized through the following technical solutions.

[0005] The utility model provides a planar alloy diode structure, comprising an N+ substrate; a P-type diffusion junction located around the edge of the N+ substrate; a P-type alloy junction is provided in the active area of ​​the N+ substrate; a passivation layer is provided at the surface edge of the N+ substrate; an anode metal layer is provided on the surface of the P-type alloy junction; and a cathode metal layer is provided on the back of the N-type substrate layer.

[0006] The edge of the anode metal layer covers the inner end surface of the passivation layer.

[0007] The edge of the P-type alloy junction extends into the P-type diffusion junction by a certain distance.

[0008] The resistivity of the N+ substrate is 0.002-0.004Ω·cm.

[0009] The P-type diffusion junction has a junction depth of 3-4 μm and a surface square resistance of 15-20 Ω / □.

[0010] The thickness of the P alloy layer is 1-2 um.

[0011] A method for preparing a planar alloy diode comprises the following steps:

[0012] S1 makes a low-resistance N+ substrate;

[0013] S2 thermal oxidation growth oxide layer;

[0014] S3 performs photolithography and etching of the oxide layer of the P diffusion region;

[0015] S4 performs front ion implantation and boron main diffusion;

[0016] S5 performs photolithography and etching of the active area oxide layer;

[0017] S6 performs P-type alloy metal evaporation;

[0018] S7 performs metal photolithography and etching of the P-type alloy region;

[0019] S8 performs annealing to form a P-type alloy junction and corrode unreacted metal;

[0020] S9 performs front electrode metal evaporation;

[0021] S10 performs metal photolithography and etching of the front electrode;

[0022] S11 performs backside thinning;

[0023] S12 performs back side metallization.

[0024] In step S1, the N+ substrate is <111> Crystal orientation N-type material, resistivity 0.002-0.004Ω·cm, thickness 450±10μm.

[0025] In step S2, the growth temperature of the oxide layer is 1150° C., the growth time is 100 min, and the oxide layer adopts a dry oxygen+wet oxygen+dry oxygen process.

[0026] In step 3, the implantation dose of P ions is 5e15 cm-2 and the energy is 100 keV.

[0027] The beneficial effect of the utility model is that by operating the Zener diode in reverse bias, the doping concentration of the P-type alloy region and the N+ substrate is relatively high. When the reverse bias of the device gradually increases, a tunnel breakdown effect occurs in the device. The doping concentration of the P-type diffusion region at the edge of the device is relatively low and the junction depth is deeper, which can reduce the electric field concentration effect at the edge of the device. The breakdown point of the device is generally located at the junction of the P-type alloy junction and the N-type substrate, which can effectively reduce the reverse leakage current of the device. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a structural schematic diagram of the utility model;

[0029] In the figure: 1-N+ substrate, 2-P type diffusion junction, 3-front passivation layer, 4-P type alloy junction, 5-front electrode, 6-back electrode. DETAILED DESCRIPTION

[0030] The technical solution of the utility model is further described below, but the scope of protection required is not limited to the description.

[0031] A planar alloy diode structure comprises an N+ substrate; a P-type diffusion junction located around the edge of the N+ substrate; a P-type alloy junction is provided in the active area of ​​the N+ substrate; a passivation layer is provided at the edge of the surface of the N+ substrate; an anode metal layer is provided on the surface of the P-type alloy junction; and the edge of the cathode metal layer is covered on the inner end surface of the passivation layer on the back of the N-type substrate layer.

[0032] like Figure 1 As shown, this structure is a Zener diode structure. Zener diodes generally work in reverse bias. The doping concentrations of the P-type alloy region and the N+ substrate are relatively high. When the reverse bias of the device gradually increases, the device undergoes a tunnel breakdown effect. The doping concentration of the P-type diffusion region at the edge of the device is relatively low and the junction depth is deeper, which can reduce the electric field concentration effect at the edge of the device. The device breakdown point is generally located at the junction of the P-type alloy junction and the N-type substrate, which can effectively reduce the reverse leakage current of the device.

[0033] Compared with conventional Zener diodes, the device of the present application evaporates metal Al on the front side after photolithography to form a metal contact window, then performs photolithography to form a metal alloy area, then performs annealing to form a P-type alloy junction, and then performs front metal evaporation photolithography to form a device anode. Therefore, the device mainly adds metal photolithography of the alloy area, and first photolithography of the alloy area metal and then annealing to form a P-type alloy junction, rather than using a whole surface metal alloy. This scheme can effectively control the distance between the alloy area boundary and the P diffusion junction ring boundary, preventing Al from diffusing to the ring boundary and causing the junction terminal electric field concentration; and the invention uses first photolithography of the alloy area metal and then annealing, which can prevent Al from entering the oxide layer and causing the oxide layer quality to deteriorate. Therefore, the invention can prepare an ultra-low voltage, low leakage and high reliability planar alloy diode. The resistivity of the N+ substrate is 0.002-0.004Ω·cm. The P-type diffusion junction has a junction depth of 3-4um and a surface square of 15-20Ω / □. The thickness of the front P alloy layer is 1-2um. The front electrode uses metal Al with a thickness of 3-4um. The back electrode uses a Ti / Ni / Ag composite layer structure with thicknesses of 0.1±0.02 / 0.6±0.03 / 0.8±0.1mm respectively.

[0034] 1. A method for preparing a planar alloy diode, comprising the following steps:

[0035] 2. Make the substrate and select <111> The crystal orientation is N-type material, the substrate parameters are 0.002-0.004Ω·cm, and the thickness is 450±10μm.

[0036] 3. Perform high-temperature thermal oxidation. The growth temperature of the oxide layer is 1150°C, the growth time is 100 minutes, and the oxide layer adopts dry oxygen + wet oxygen + dry oxygen process.

[0037] 4. Use existing technology to perform photolithography and etching of the P diffusion region oxide layer.

[0038] 5. Perform boron ion implantation in the P-type diffusion region, with the ion implantation dose and energy being 5e15cm-2 and 100keV respectively.

[0039] 6. Carry out the main boron diffusion (oxidation + trap pushing) in the diffusion zone. The diffusion temperature and time are 1150°C and 80 minutes respectively.

[0040] 7. Use existing technology to perform photolithography and etching of the active area oxide layer.

[0041] 8. Evaporation of P-type alloy metal aluminum is performed, and the thickness of the aluminum layer is 3-4um.

[0042] 9. Use existing technology to perform metal photolithography and etching of the P-type alloy area.

[0043] 10. Anneal the P-type alloy area metal to form an alloy junction, and then corrode the unreacted metal on the surface. The annealing temperature and time are 550-600°C and 20 minutes respectively.

[0044] 11. Perform Al metal evaporation on the front electrode, and the thickness of the aluminum layer is 3-4um.

[0045] 12. Use existing technology to perform metal photolithography and etching of the front electrode.

[0046] 13. Perform backside thinning and evaporate Ti / Ni / Ag metal on the backside.

Claims

1. A planar alloy diode structure, characterized in that: The invention comprises an N+ substrate (1); a P-type diffusion junction (2) located around the edge of the N+ substrate (1); a P-type alloy junction (4) is provided in the active area of ​​the N+ substrate (1); a passivation layer (3) is provided at the edge of the surface of the N+ substrate (1); an anode metal layer (5) is provided on the surface of the P-type alloy junction (4); and a cathode metal layer (6) is provided on the back of the N+ substrate (1).

2. The planar alloy diode structure according to claim 1, characterized in that: The edge of the anode metal layer (5) covers the inner end surface of the passivation layer (3).

3. The planar alloy diode structure according to claim 1, characterized in that: The edge of the P-type alloy junction (4) extends into the P-type diffusion junction (2) by a certain distance.

4. The planar alloy diode structure according to claim 1, characterized in that: The resistivity of the N+ substrate (1) is 0.002-0.004Ω·cm.

5. The planar alloy diode structure according to claim 1, characterized in that: The P-type diffusion junction (2) has a junction depth of 3-4 μm and a surface square resistance of 15-20 Ω / □.

6. The planar alloy diode structure according to claim 1, characterized in that: The thickness of the P-type alloy junction (4) is 1-2 um.