Solid electrolyte separator and electrochemical device
By injection molding polyetheretherketone or polyphenylene sulfide to cover the edges of the oxide solid electrolyte sheet and injection molding reinforcing ribs, the sealing problem of the oxide solid electrolyte in high temperature and highly corrosive environments is solved, achieving larger size and more durable Highly durable solid electrolyte separator for electrochemical devices.
Patent Information
- Application Number
- CN202323642859.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-29
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2033-12-29
AI Technical Summary
Existing oxide solid electrolytes are difficult to ensure sealing in high temperature and highly corrosive environments, and cannot produce large-sized and thin separators, which are prone to distortion, deformation or rupture.
Polyether ether ketone or polyphenylene sulfide injection molding material is used to cover the edge of the oxide solid electrolyte sheet to form a frame, sealing is achieved through the bonding interface, and reinforcing ribs are injected on the surface to improve strength and durability.
It achieves good sealing and durability under high temperature and strong corrosive environment, and can manufacture larger-sized solid electrolyte separators, which is suitable for electrochemical devices.
Smart Images

Figure CN221861711U_ABST
Abstract
Description
Technical Field
[0001] The utility model relates to a solid electrolyte diaphragm and an electrochemical device. Background Art
[0002] Solid electrolytes usually have the ability to conduct specific ions such as lithium ions and sodium ions. Unlike liquid electrolytes, solid electrolytes are safer, non-flammable or flame-retardant, and can withstand a larger capacity of current per unit area, which can facilitate fast charging and discharging of the battery. In addition, solid electrolytes can also act as a separator between the positive and negative electrodes to prevent short circuits between the positive and negative electrodes, which is of great significance to the safety of the battery. Existing solid electrolytes can be mainly divided into three categories: polymer solid electrolytes, oxide solid electrolytes, and sulfide solid electrolytes. Among them, oxide solid electrolytes have relatively superior anti-corrosion properties, are usually less affected by oxygen and water, and have a hard texture and good mechanical properties. Compared with the other two solid electrolytes, they have broader commercial prospects.
[0003] Generally speaking, the conductivity of solid electrolytes is inversely proportional to thickness and directly proportional to area: that is, the thinner the thickness, the higher the conductivity; the larger the positive and negative electrode areas, the higher the conductivity. The length of the positive and negative electrode separators of lithium-ion batteries currently popular on the market can reach 3-4 meters after unfolding, and the area can reach 20-30 square decimeters or even higher, while the existing oxide solid electrolyte manufacturing process cannot reach this size. In the prior art, oxide solid electrolytes such as perovskite, NASICON, (LLZO) garnet, LiSiCON, LiPON or BETA-alumina are all made by high-temperature firing process. Very thin and large-sized parts are easily twisted, deformed, or even broken after high-temperature firing and low-temperature shrinkage. The size of an oxide solid electrolyte sheet with a thickness of about 0.5 mm is difficult to exceed 60 mm after one-time molding. This is obviously a big gap from the 20-30 square decimeter size of the positive and negative electrode separators of the aforementioned battery. However, the method of using a frame to splice multiple pieces of solid electrolyte to form a large-sized solid electrolyte membrane cannot currently guarantee the sealing of the joints between the frame and the solid electrolyte. In the high temperature and highly corrosive environment of the battery, microchannels or gaps are very likely to form at the joints. Utility Model Content
[0004] The main purpose of the utility model is to provide a solid electrolyte diaphragm with good sealing performance for the solid electrolyte.
[0005] In order to achieve the above-mentioned object, the first aspect of the present invention provides a solid electrolyte membrane, comprising:
[0006] one or more sheets of oxide solid electrolyte, and
[0007] A frame is injection-molded and coated on the edge of the sheet, and the frame material is polyetheretherketone injection molding or polyphenylene sulfide injection molding.
[0008] In some embodiments of the first aspect of the utility model, a plurality of sheets are spliced by being laid flat or stacked through the frame.
[0009] In some embodiments of the first aspect of the utility model, one or more reinforcing ribs are injection-molded on the surface of the sheet, and the reinforcing ribs are made of polyetheretherketone injection molding or polyphenylene sulfide injection molding.
[0010] In some embodiments of the first aspect of the utility model, the edge width of the frame covering sheet is 1.0-2.5 mm.
[0011] In some embodiments of the first aspect of the utility model, the oxide solid electrolyte is a molecular sieve-based oxide solid electrolyte or a ceramic-based oxide solid electrolyte.
[0012] In some embodiments of the first aspect of the present invention, the oxide solid electrolyte is selected from a NaSiCON type solid electrolyte, a LiSiCON type solid electrolyte, a garnet type solid electrolyte, a LiPON type solid electrolyte or a BETA-alumina solid electrolyte.
[0013] In some embodiments of the first aspect of the utility model, the frame and the sheet material have a bonding interface.
[0014] The second aspect of the utility model relates to an electrochemical device, comprising one or more solid electrolyte membranes as described above.
[0015] In some embodiments of the second aspect of the present invention, the electrochemical device is a chemical battery or an electrochemical reactor.
[0016] In some embodiments of the second aspect of the present invention, a cavity is included which is made of engineering plastic, and the frame of the solid electrolyte membrane is connected to the cavity by plastic welding.
[0017] In some embodiments of the second aspect of the present invention, one or more solid electrolyte membranes separate the cavity into one or more positive electrode cavities, and one or more negative electrode cavities.
[0018] In some embodiments of the second aspect of the present invention,
[0019] The positive electrode cavity is provided with one or more separators to divide the positive electrode cavity into multiple positive electrode compartments, and / or
[0020] The negative electrode cavity is provided with one or more separators to divide the negative electrode cavity into a plurality of negative electrode compartments.
[0021] In some embodiments of the second aspect of the utility model, a first channel for adding positive electrode electrolyte and a second channel for adding negative electrode electrolyte are further included, wherein the first channel is connected to the positive electrode cavity, and the second channel is connected to the negative electrode cavity.
[0022] In the solid electrolyte membrane of the utility model, a good sealing bonding interface can be formed between the frame and the oxide solid electrolyte, and it can be resistant to high temperature and corrosion, so that the solid electrolyte membrane as a whole can adapt to the strong corrosion and high temperature environment of the electrochemical reaction without leakage. The structure of the utility model can be used to obtain a larger size solid electrolyte membrane, which also has the advantages of good sealing performance, high temperature resistance and corrosion resistance. The solid electrolyte membrane can be widely used in various electrochemical devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 Schematic diagram of the structure of the diaphragm 100a.
[0024] Figure 2 A state diagram of the mold 200a producing the diaphragm 100a.
[0025] Figure 3 Schematic diagram of the structure of the diaphragm 100b.
[0026] Figure 4 A state diagram of the mold 200b producing the diaphragm 100b.
[0027] Figure 5 Schematic diagram of the structure of the diaphragm 100c.
[0028] Figure 6 A state diagram of the mold 200c producing the diaphragm 100c.
[0029] Figure 7 Schematic diagram of the structure of the diaphragm 100d.
[0030] Figure 8 State diagram of the diaphragm 100d produced for the mold 200d.
[0031] Fig. 9 It is a diagram of the external structure of the chemical battery 300.
[0032] Fig.10 A diagram showing the internal structure of a chemical battery 300.
[0033] Fig.11 A diagram showing the internal structure of a chemical battery 300.
[0034] Fig.12 A diagram showing the internal structure of a chemical battery 300. DETAILED DESCRIPTION
[0035] In view of the fact that the existing frame-jointed solid electrolyte sheets cannot ensure the sealing of the joint positions, the utility model provides a solid electrolyte diaphragm, the structure of which mainly includes:
[0036] Provide one or more sheets of oxide solid electrolyte, one or more sheets of oxide solid electrolyte, and a frame injection-molded around the edge of the sheet, wherein the frame is made of polyetheretherketone injection molding or polyphenylene sulfide injection molding.
[0037] The inventors have found through research that when polyetheretherketone and / or polyphenylene sulfide are melted and added to the surface of an oxide solid electrolyte for injection molding, the injection molded product and the oxide solid electrolyte are bonded at their contact interface, and this bonding can still exist stably for a long time under high temperature and strong corrosion environments. Utilizing the above characteristics, a frame formed of an injection molding material whose main component is polyetheretherketone and / or polyphenylene sulfide can be used on the edge of the oxide solid electrolyte sheet. The frame and the oxide solid electrolyte are sealed at the coating position through the above-mentioned interface bonding and have the characteristics of high temperature resistance and corrosion resistance. The resulting diaphragm can be used in various electrochemical devices with high temperature and corrosive internal environments.
[0038] The above-mentioned diaphragm can be obtained by injection molding an injection molding raw material whose main components are polyetheretherketone and / or polyphenylene sulfide on the edge of the one or more sheets to form a frame covering the edge.
[0039] Polyetheretherketone injection moldings or polyphenylene sulfide injection moldings generally refer to products formed by injection molding of injection molding raw materials whose main components are polyetheretherketone and polyphenylene sulfide. The injection molding raw materials and injection molding methods all adopt the formulas and steps known to technicians in the field. The injection molding raw materials can generally also contain various components generally used in the injection molding process, such as inorganic powders and process additives. The inorganic powders are selected from one or more of calcium carbonate, sodium carbonate, and silicon dioxide. The process additives are selected from one or two of zinc stearate and talcum powder.
[0040] In some specific structures, multiple sheets are laid flat or stacked together through the frame. By splicing sheets together through the frame, a larger solid electrolyte membrane can be manufactured, and the frame and the sheets also have good sealing, corrosion resistance and high temperature resistance.
[0041] A person skilled in the art can design a mold for injection molding according to the steps and requirements provided by the utility model, and use existing injection molding equipment for injection molding. One of the achievable mold structures includes an upper mold plate and a lower mold plate that are molded together on both sides of a sheet material, the upper mold plate has an upper fitting portion and a first upper cavity, the lower mold plate has a lower fitting portion and a first lower cavity, when the upper mold plate and the lower mold plate are molded together, the upper and lower fitting portions clamp and fix the sheet material from both sides, the first upper cavity and the first lower cavity cooperate to form a first cavity for injection molding the frame, and the edge of the sheet material extends out of the upper and lower fitting portions and is located in the first cavity.
[0042] In order to improve the strength of the solid electrolyte diaphragm, one or more reinforcing ribs are injection molded on the surface of the sheet, and the reinforcing ribs are made of polyetheretherketone injection molding or polyphenylene sulfide injection molding. In order to manufacture the reinforcing ribs, the upper template has a second upper cavity for injection molding reinforcing ribs. When the mold is closed, the second upper cavity is pressed on the upper surface of the sheet, and the injection molding raw material is used to inject in the second upper cavity to form reinforcing ribs on the upper surface of the sheet, and / or the lower template has a second lower cavity for injection molding reinforcing ribs. When the mold is closed, the second lower cavity is pressed on the lower surface of the sheet, and the injection molding raw material is used to inject in the second lower cavity to form reinforcing ribs on the lower surface of the sheet. Through the above structure, reinforcing ribs can be injection molded on any one side or both sides of the sheet. The structure of the reinforcing ribs can be designed according to needs. For example, the reinforcing rib structure can be a rod or a grid body bonded to the surface of the sheet, which can also withstand corrosion and high temperature environments and will not fall off for a long time. And the design based on the shape of the reinforcing ribs.
[0043] Furthermore, the sheet can be heated before injection molding to reduce or eliminate the compressive stress generated by the frame on the sheet at room temperature. The main reason for the formation of compressive stress is the difference in the degree of thermal expansion between the sheet and the injection molding material. The expansion coefficient can be referred to Table 1. After the molten injection molding material is injected, the injection molding material is gradually fixed and formed during the cooling process. The cooling process is also accompanied by the shrinkage of the injection molding material, thereby generating compressive stress on the sheet wrapped therein. Excessive compressive stress will cause the sheet to rupture, so the sheet can be preheated to allow the sheet and the frame to cool and shrink together to reduce or eliminate this compressive stress.
[0044] Table 1 Thermal expansion coefficient reference table
[0045] Material Coefficient of thermal expansion Oxide solid electrolyte <![CDATA[3.0~9.5e -6 / K]]> PEEK <![CDATA[3.3e -5 / K]]> PPS <![CDATA[4.0~7.0e -5 / K]]>
[0046] In some specific preparation methods, the sheet is obtained by wire cutting a block of sintered oxide solid electrolyte. Compared with the sheeting method of single sintering to directly form a sheet in the background art, sintering to form a block and then forming a sheet by wire cutting can avoid the problem of cracking during sintering, and this method can manufacture thinner (less than 0.5 mm) and larger (100-150 mm) oxide solid electrolyte sheets.
[0047] Preferably, the edge width of the frame coating sheet is 1.0-2.5 mm. A larger coating width can provide more bonding area to further improve the sealing connection performance between the frame and the sheet.
[0048] The oxide solid electrolyte may be a molecular sieve-based oxide solid electrolyte or a ceramic-based oxide solid electrolyte, and may be selected from NaSiCON-type solid electrolytes, LiSiCON-type solid electrolytes, garnet-type solid electrolytes, LiPON-type solid electrolytes, or BETA-alumina solid electrolytes.
[0049] Before the injection molding, one or more reinforcing layers are bonded to the non-injection molding position of the sheet by hot melt adhesive, and after the injection molding is completed, the reinforcing layers and the hot melt adhesive are removed by heating. This step can help the oxide solid electrolyte sheet not to be damaged during the injection molding process.
[0050] The solid electrolyte membrane obtained by the above preparation method can be used in various electrochemical devices for ion conduction. The ions conducted are related to the selected oxide solid electrolyte. Those skilled in the art can select a suitable oxide solid electrolyte according to the needs of ion conduction. The electrochemical devices include but are not limited to electrochemical reactors and chemical batteries.
[0051] One specific electrochemical device structure includes a cavity made of engineering plastics, and the solid electrolyte membrane can be plastic-welded with the cavity through its own frame to achieve the connection between the electrolyte membrane and the cavity. At the same time, engineering plastics can also be selected from polyetheretherketone and / or polyphenylene sulfide, and of course other engineering plastics can also be selected, which can also maintain good sealing performance after plastic welding. Preferably, the engineering plastic used to prepare the cavity should also have high temperature resistance and corrosion resistance. In some specific electrochemical device structures, one or more solid electrolyte membranes separate the cavity into one or more positive electrode cavities, and into one or more negative electrode cavities. Furthermore, the positive electrode cavity is provided with one or more partitions to separate the positive electrode cavity into multiple positive electrode compartments, and the negative electrode cavity can also be provided with one or more partitions to separate the negative electrode cavity into multiple negative electrode compartments. The safety of electrochemical devices can be increased by separating the positive and negative electrode cavities with partitions. When problems occur in a single positive or negative electrode cavity, the partition can prevent the problem from spreading further. These problems may be rupture and leakage of the diaphragm, internal short circuits, fires, etc., or they may be external dangers.
[0052] In some specific electrochemical devices, a first channel for adding positive electrode electrolyte and a second channel for adding negative electrode electrolyte are also included, the first channel is connected to the positive electrode cavity, and the second channel is connected to the negative electrode cavity. The first channel and the second channel can facilitate the replenishment of the positive and negative electrolytes respectively.
[0053] The present invention is further described below in conjunction with specific embodiments.
[0054] Example 1 Preparation of Oxide Solid Electrolyte Sheet
[0055] Sintering is used to prepare oxide solid electrolyte blocks. The blocks are cut into cuboids with the required cross-section size. The cuboids are then cut one by one along the cross-section direction by wire cutting to form oxide solid electrolyte sheets of the required thickness and size. This single sintering method can produce oxide solid electrolyte sheets that are thinner and larger in size than direct sintering.
[0056] The oxide solid electrolyte sheets used in Examples 2 to 5 were prepared according to the above method.
[0057] Table 2 BETA-alumina sheets
[0058] Example Material Size (length / width / thickness) / mm 2 BETA-Alumina 35 / 35 / 1 3 NaSiCON 60 / 40 / 1 4 BETA-Alumina 60 / 40 / 0.9 5 BETA-Alumina 60 / 40 / 0.35
[0059] Among the above dimensions, the accuracy of thickness is within ±0.05mm, and the accuracy of length and width is within ±0.1mm.
[0060] Example 2 Preparation of Sheet Material to Prepare Diaphragm
[0061] The BETA-alumina sheet in Table 2 of Example 1 was selected to prepare Figure 1 The structure of the diaphragm 100a is shown in FIG. The frame 101a is wrapped around the periphery of the sheet 103a.
[0062] The frame is injection molded by the mold. The molded frame has a single-side width of 2.5mm, a single-side thickness of 1.4mm, and a width of 1mm at the edge of the covering sheet. The structure of the mold is as follows Figure 2 As shown. The mold 200a includes a symmetrical upper template 201a and a lower template 202a. Taking the lower template as an example, the center position of the lower template has a lower platform 206a for fitting with the middle of the lower surface of the sheet, and the surrounding side of the platform has a first lower cavity 2042a for forming the lower half of the cavity 204a. When the sheet 103 is placed on the lower platform 206a, the edge of the sheet exceeds the edge of the lower platform and is located in the first lower cavity. Similarly, the upper template 201a has an upper platform 205a symmetrical to the lower platform, and a first upper cavity 2041a symmetrical to the first lower cavity. The first upper cavity and the first lower cavity form the first cavity 204a after the mold is closed, and one or more injection ports 203a are opened on one side of the first cavity 204a.
[0063] The BETA-alumina sheet is preheated before the injection molding, and then the upper and lower templates are pressed onto the upper and lower surfaces of the solid electrolyte sheet, and a cavity 204a for covering the edge is formed at the edge 1031a of the solid electrolyte sheet. Molten polyphenylene sulfide is injected into the cavity 204a from the injection port 203a, and after cooling, a solid electrolyte membrane 100a with a frame wrapped around the edge is formed.
[0064] The prepared diaphragm was immersed in a strong alkaline solvent such as 50% sodium hydroxide at 80°C for more than 21 days, and no visible damage was found on the solid electrolyte, the polyphenylene sulfide edge, and the bonding surface between them. After cooling, a 40 mm high closed fence was bonded to the upper part of the polyphenylene sulfide frame and filled with water. After 24 hours, no water leakage was found on the outside of the fence and the bottom of the solid electrolyte, indicating the integrity of the bonding surface of the polyphenylene sulfide BETA-alumina solid electrolyte.
[0065] However, if the pre-injection molded frame and the BETA-alumina solid electrolyte sheet were bonded with a high temperature resistant epoxy glue and then placed in a strong alkaline solvent such as 50% sodium hydroxide at 80°C, within 7 days, the bonding surface showed obvious peeling. Similarly, after the pre-injection molded frame and the LATP, LiSiCON or NaSiCON type solid electrolyte sheet were bonded with a high temperature resistant epoxy glue and then immersed in a strong alkaline solvent such as 50% sodium hydroxide at 80°C for more than 21 days, the solid electrolyte and the bonding surface with the frame showed obvious cracking or even complete ablation.
[0066] Example 3 Preparation of a diaphragm with reinforcing ribs
[0067] The NASICON sheet material in Table 2 of Example 1 was selected to prepare Figure 3 The frame 101b is coated on the periphery of the sheet 103b, and the orthogonal grid-shaped reinforcing ribs 102b are injection-molded on the surfaces of both sides of the sheet 103b.
[0068] The frame is injection molded by the mold. The molded frame has a single-side width of 2.5 mm, a single-side thickness of 1 mm, and a width of the edge of the covering sheet of 1.2 mm. The structure of the mold used is as follows Figure 4 As shown. Similar to the structure of the mold 200a in Example 2, the mold 200b includes an upper template 201b and a lower template 202b, the lower template has a lower platform 206b and a first lower cavity 2042b, the upper template 201b has an upper platform 205b and a first upper cavity 2041b, the lower template 202b has a lower platform 206b and a first lower cavity 2042b, the upper and lower grooves are molded together to form a first cavity 204b, and the injection port 203b is located on one side of the first cavity 204b. In addition, the upper template 201b also has a second upper cavity 207b for injection molding the reinforcing rib, the second upper cavity 207b is connected to the first upper cavity 2041b, and the lower template has a second lower cavity 208b for injection molding the reinforcing rib, the second lower cavity 208b is connected to the first lower cavity 2042b.
[0069] Preheat the sheet, then press the upper and lower templates onto the upper and lower surfaces of the solid electrolyte sheet, form a cavity 204b covering the edge 1031b of the solid electrolyte sheet, the second upper cavity 207b covers the upper surface of the sheet 100b, the second lower cavity 208b covers the lower surface of the sheet 100b, and the molten polyetheretherketone plastic is injected into the cavity 204b, the second upper cavity 207b and the second lower cavity 208b from the injection port 203b, and after cooling, a diaphragm 100b is formed with a frame 101b wrapped around the edge and reinforcing ribs 102b on the upper and lower surfaces.
[0070] The strength of the diaphragm prepared in this embodiment is significantly improved, and there is no obvious surface crack when it falls freely from a height of 1.5 meters. At the same time, the above-mentioned diaphragm was immersed in a 145°C AlCl3-NaI-LiI molten electrolyte for 30 days, and no visible damage was found on the solid electrolyte, the polyetheretherketone edging, and the bonding surfaces between them. After cooling, the solidified molten AlCl3-NaI-LiI molten electrolyte was washed, and the weight change of the coated polyetheretherketone solid electrolyte was less than 1.5%. At the same time, when a 40 mm high closed fence was bonded to the upper part of the polyetheretherketone frame and filled with water, after 24 hours, no water leakage was found on the outside of the fence and the bottom of the solid electrolyte, indicating the integrity of the NaSiCON type solid electrolyte bonding surface of the polyetheretherketone.
[0071] Example 4: Making a diaphragm made of multiple sheets laid flat and spliced together
[0072] The BETA-alumina sheet in Table 2 of Example 1 was selected to prepare Figure 5 The structure of the diaphragm 100d. The sheet along Figure 5 The frames 101c are arranged vertically and flatly, and are wrapped around the periphery of the sheets 103c and between two sheets, so as to realize splicing of multiple sheets to form a larger diaphragm 100c. Orthogonal grid-shaped reinforcing ribs 102b are injection molded on the surfaces of both sides of each sheet 103b.
[0073] The frame is injection molded by a mold. The molded frame has a single-side width of 2 mm, a single-side thickness of 8 mm, and a width of the edge of the covering sheet of 1.3 mm. The structure of the mold used is as follows Figure 6 As shown. The structure of the mold 200b in Example 3 is similar.
[0074] The mold 200c includes an upper mold plate 201c and a lower mold plate 202c, the lower mold plate has a lower platform 206c and a first lower cavity 2042c, the upper mold plate 201c has an upper platform 205c, a first upper cavity 2041c and a second upper cavity 207b, the lower mold plate 202c has a lower platform 206c, a first lower cavity 2042c and a second lower cavity 208c, the upper and lower grooves are combined to form a first cavity 204c, the second upper cavity 207c is connected to the first upper cavity 2041c, the second lower cavity 208c is connected to the first lower cavity 2042c, and the injection port 203c is located on one side of the first cavity 204c. In addition, referring to Figure 6 In the middle position of the middle mold, the cavity also passes between two sheets and is used to simultaneously cover the edges of adjacent sheets, thereby realizing the splicing of the sheets.
[0075] The sheet is preheated, and then the upper and lower templates are pressed onto the upper and lower surfaces of the solid electrolyte sheet, a cavity 204c for covering the edge 1031c of the solid electrolyte sheet is formed, the second upper cavity 207c covers the upper surface of the sheet 100c, and the second lower cavity 208c covers the lower surface of the sheet 100c, and molten polyphenylene sulfide is injected into the cavity 204c, the second upper cavity 207c and the second lower cavity 208c from the injection port 203c, and after cooling, a diaphragm 100c is formed with a frame 101c wrapped around the edge and reinforcing ribs 102c on the upper and lower surfaces.
[0076] Since the size of the solid electrolyte membrane is much larger than that of a single solid electrolyte membrane sheet, the ionic conductivity increases linearly according to the area, and the ionic resistance of the solid electrolyte membrane decreases accordingly. The large-sized solid electrolyte membrane with interval distribution in the above solid electrolyte array was immersed in a 10% lithium sulfide ethylene glycol solution at 130°C for more than 30 days, and no visible damage was found on the solid electrolyte, the polyphenylene sulfide edge, and the bonding surface between them. When a 40 mm high closed fence was bonded to the upper part of the polyphenylene sulfide frame and filled with water, no water leakage was found on the outside of the fence and the bottom of the solid electrolyte after 24 hours, indicating the integrity of the BETA-alumina solid electrolyte bonding surface of polyphenylene sulfide.
[0077] Example 5 Preparation of a diaphragm with an interlayer
[0078] The BETA-alumina sheet in Table 2 of Example 1 was selected to prepare Figure 7 The two sheets 103d and the interlayer 110d therein are stacked as a combined structure and then injection molded into a frame, and the frame 101d is coated around the periphery of the sheet 103d and the interlayer 110d to manufacture the diaphragm 100d with a stacked combined structure.
[0079] First, the combined structure is assembled, and two sheets 103d are supported by multiple support members 106d, and the two sheets 103d are arranged in intervals and parallel to each other, and mechanical edge sealing is performed by copper sheets 107d, and an opening for injection is reserved, and a periphery for injection molding of the frame 101d is reserved on the sheet for frame injection molding. Foam copper or electrode material and molten electrolyte 105c of 50% potassium formate + 50% sodium formate are filled from the reserved opening; after the electrolyte 105c is poured in, the opening is mechanically sealed to form Figure 7 The combined structure contained in .
[0080] The frame is injection molded by the mold. The molded frame has a single-side width of 2 mm, a single-side thickness of 1 mm, and a width of the edge of the covering sheet of 2.5 mm. The structure of the mold used is as follows Figure 6As shown. Similar to the structure of the mold 200c in Example 4, the mold 200d includes an upper mold plate 201d and a lower mold plate 202d, the lower mold plate has a lower platform 206d and a first lower cavity 2042d, the upper mold plate 201d has an upper platform 205d and a first upper cavity 2041d, the lower mold plate 202d has a lower platform 206d and a first lower cavity 2042d, the upper and lower grooves are combined to form a first cavity 204d, and the injection port 203d is located on one side of the first cavity 204d. In addition, referring to Figure 6 In the middle position of the middle mold, the cavity also passes between the two combined structures, and is used to simultaneously cover the edges of adjacent combined structures, thereby realizing the splicing of the combined structures.
[0081] The combined structure is preheated, and then the upper and lower templates are pressed onto the upper and lower surfaces of the combined structure, and a cavity 204d for covering the edge is formed at the edge 1031d of the solid combined structure, and molten polyphenylene sulfide is injected into the cavity 204d from the injection port 203d. After cooling, a diaphragm 100d with a frame 101d covering the edge is formed.
[0082] The diaphragm 100d is placed in a sulfolane or ethylene glycol solution, 25% sodium sulfide powder is added to the sulfolane solution, and heated to 175°C. After all the sodium sulfide is dissolved in the sulfolane or ethylene glycol solution, liquid sulfur is added and the graphite felt that is always in contact with the liquid sulfur forms the positive electrode of the battery, and the electrolyte of 50% potassium formate + 50% sodium formate in the closed cavity unit melts at high temperature to form the negative electrode of the battery. The positive electrode and the diaphragm are combined to form a sodium-sulfur primary battery with stable charge and discharge capabilities. After 50 cycles of testing, the solid electrolyte, the polyphenylene sulfide edge and the bonding surface between them are not damaged by the naked eye.
[0083] Example 6 Chemical Battery
[0084] The diaphragm 100c prepared in Example 4 is used to make Fig. 9 Chemical battery in 300. Reference Figures 9 to 12The shell of the chemical battery is made of engineering plastics. The shell includes an upper cover 310 and a lower cover 330. The upper and lower covers are connected to form a cavity inside. A plurality of solid electrolyte membranes 100c are arranged in intervals in the lower cover 330 to divide the lower cover into alternating positive electrode cavities 332 and negative electrode cavities 331. The solid electrolyte membrane 100c is sealed and connected to the lower cover 330 through its own frame by a plastic welding process. The negative electrode cavity is further divided by a vertically arranged partition 333 to form a plurality of negative electrode compartments. A negative electrode collector electrode 350 and a positive electrode collector electrode 320 are arranged in each negative electrode compartment in each negative electrode cavity and each positive electrode cavity. A negative electrode cover plate 340 and a positive electrode cover plate 350 are covered above each negative electrode cavity and positive electrode cavity. A positive electrode leakage port 351 and a negative electrode leakage port 341 are respectively provided on the positive electrode cover plate 340 and the negative electrode cover plate 350, which are connected to each negative electrode compartment in the positive electrode cavity and the negative electrode cavity. A plurality of partition plates 313 corresponding to the positions of the solid electrolyte diaphragm 100 are provided in the upper cover body 310. The partition plates 313 divide the interior of the upper cover body 310 into a plurality of alternating positive electrode injection chambers 314 and negative electrode injection chambers 315. When the upper cover body 310 is aligned with the lower cover body 330, After connection, the lower end of the partition 313 is docked with the upper end of the solid electrolyte membrane 100, the positive electrode injection cavity 314 is docked with the positive electrode cavity 332, and is connected by the positive electrode leakage port 351 on the positive electrode cover 350, the negative electrode injection cavity 315 is docked with the negative electrode cavity 331, and is connected by the negative electrode leakage port 341 on the negative electrode cover 340, and the positive electrode injection groove 312 and the negative electrode injection groove 311 are respectively arranged on both sides of the upper cover body, the positive electrode injection groove 312 is connected with the positive electrode injection cavity 314, and the negative electrode injection groove 311 is connected with the negative electrode injection cavity 315.
[0085] When the positive and negative electrode electrolytes are injected, the positive and negative electrode electrolytes are respectively injected from the positive electrode injection tank 312 and the negative electrode injection tank 311 into the positive and negative electrode injection chambers 314 and 315. The positive electrode electrolyte passes through the positive electrode injection chamber 314 and enters the positive electrode cavity 332 from the positive electrode leakage hole 351 on the positive electrode cover plate 350. The negative electrode electrolyte passes through the negative electrode injection chamber 315 and enters the negative electrode compartments of the negative electrode cavity 331 from the negative electrode leakage hole 341 on the negative electrode cover plate 340.
[0086] The embodiments of the present invention are only used to illustrate the present invention and do not constitute a limitation on the scope of the claims. Other substantially equivalent alternatives that can be thought of by those skilled in the art are all within the protection scope of the present invention.
Claims
1. Solid electrolyte membrane, characterized in that include: one or more sheets of oxide solid electrolyte, and A frame is injection-molded and wrapped around the edge of the sheet, and the frame is made of polyetheretherketone injection molding material or polyphenylene sulfide injection molding material.
2. The solid electrolyte membrane according to claim 1, characterized in that A plurality of sheets are spliced together by being laid flat or stacked through the frame.
3. The solid electrolyte membrane according to claim 1, characterized in that One or more reinforcing ribs are injection-molded on the surface of the sheet, and the reinforcing ribs are made of polyetheretherketone injection molding material or polyphenylene sulfide injection molding material.
4. The solid electrolyte membrane according to claim 1, characterized in that The edge width of the frame covering sheet is 1.0-2.5 mm.
5. The solid electrolyte membrane according to claim 1, characterized in that The oxide solid electrolyte is a molecular sieve-based oxide solid electrolyte or a ceramic-based oxide solid electrolyte.
6. The solid electrolyte membrane according to claim 1 or 5, characterized in that The oxide solid electrolyte is selected from NaSiCON type solid electrolyte, LiSiCON type solid electrolyte, garnet type solid electrolyte, LiPON type solid electrolyte or BETA-alumina solid electrolyte.
7. The solid electrolyte membrane according to claim 1, characterized in that The frame and the sheet material have a bonding interface.
8. An electrochemical device comprising one or more solid electrolyte membranes according to any one of claims 1 to 7.
9. The electrochemical device according to claim 8, characterized in that The electrochemical device is a chemical battery or an electrochemical reactor.
10. The electrochemical device according to claim 9, characterized in that It comprises a cavity made of engineering plastics, and the frame of the solid electrolyte diaphragm is connected to the cavity through plastic welding.
11. The electrochemical device according to claim 10, wherein One or more solid electrolyte separators separate the cavity into one or more positive electrode cavities and one or more negative electrode cavities.
12. The electrochemical device according to claim 11, wherein: The positive electrode cavity is provided with one or more separators to separate the positive electrode cavity into multiple positive electrode compartments, and / or The negative electrode cavity is provided with one or more separators to separate the negative electrode cavity into multiple negative electrode compartments.
13. The electrochemical device according to claim 12, characterized in that It also includes a first channel for adding positive electrode electrolyte and a second channel for adding negative electrode electrolyte, the first channel is connected to the positive electrode cavity, and the second channel is connected to the negative electrode cavity.