Electroplating device for improving electroplating chromatic aberration of low-roughness reverse copper foil
By installing an insulating baffle on the cathode plate of the electroplating device to increase the current density, the problems of coating instability and color difference during reverse copper foil electroplating are solved, and the uniformity of the coating and production yield are improved.
Patent Information
- Application Number
- CN202420291758.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-17
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2034-02-17
AI Technical Summary
In the context of high-frequency and high-speed development, during the reverse copper foil electroplating process, the reduction in current leads to a reduction in the surface roughness of the copper foil, resulting in unstable coating quality and prone to pores and electroplating chromatic aberration problems.
Install an insulating baffle on the cathode plate of the electroplating device to reduce the conductive area and increase the current density, thereby improving the deposition rate of copper nodules on the surface of the copper foil and the uniformity of the plating layer.
By increasing the current density, the uniformity and stability of the coating are improved, the problems of pores and color difference are reduced, and the yield rate of the inverted copper foil is improved without affecting the roughness of the treated surface of the copper foil.
Smart Images

Figure CN221877203U_ABST
Abstract
Description
Technical Field
[0001] The utility model relates to the technical field of electrolytic copper foil, in particular to an electroplating device for improving the electroplating color difference of low-roughness reverse copper foil. Background Art
[0002] With the advent of the 5G era, the high-frequency development of signal transmission (signal wavelength is getting shorter and shorter), the thickness of the dielectric layer used in mobile terminal PCBs (≤1 / 8 of the wavelength) is also getting thinner. In order to maintain the stability of the stripline impedance value and reduce the side etching error, reducing the thickness of the copper foil is the main direction of improvement. In addition, the high frequency of the signal makes the signal transmission more and more concentrated in the "surface layer" of the wire. The faster the signal transmission frequency, the thinner the thickness of the "surface layer" of the wire to transmit the signal (skin effect), which puts higher requirements on the surface roughness of the copper foil (the lower the better).
[0003] Electroplating uniformity has always been a production problem in the industry, especially with the development of high frequency and high speed. In order to reduce the impact of the "skin effect", copper foil companies will do special surface treatment on high frequency and high speed copper foil, such as the common ultra-low profile copper foil and reverse copper foil. These two treatment technologies can reduce the roughness Rz of the copper foil treatment surface to about 1-2μm. Among them, in the technology of reverse copper foil, some special surface treatment processes have certain requirements for current control during electroplating. In order to reduce the surface roughness of the copper foil, it is usually chosen to reduce the current in the rough curing process to meet the roughness requirements.
[0004] However, when the current is reduced, the current density will also be reduced accordingly. If the current density is too low, the deposition rate of copper nodules on the surface of the copper foil will be slow, and a coating of sufficient thickness cannot be formed within the specified time. This will lead to unstable coating quality, prone to defects such as pores, and uneven electroplating color differences on the surface of the treated surface. Utility Model Content
[0005] In order to solve the above problems, the utility model proposes an electroplating device for improving the color difference of low-roughness reverse copper foil electroplating.
[0006] The technical solution adopted by the utility model is: a plating device for improving the color difference of low-roughness reverse copper foil electroplating, including a roughening plating tank, wherein a cathode plate, an anode plate, a cathode roller and a roughening electrolyte are arranged in the roughening plating tank, wherein the cathode roller is immersed in the roughening electrolyte, and is used to cooperate with a slot entry roller and an upper guide roller located outside the roughening plating tank to complete the material guiding of the copper foil, the anode plate and the cathode plate are arranged at intervals, and an insulating baffle is installed on the surface of the cathode plate, and the insulating baffle is used to block part of the conductive area of the cathode plate.
[0007] Several optional methods are also provided below, but they are not intended to be additional limitations on the above-mentioned overall solution, but are merely further supplements or preferences. Under the premise that there are no technical or logical contradictions, each optional method can be combined with the above-mentioned overall solution separately, and multiple optional methods can also be combined.
[0008] Preferably, the insulating baffle extends along the length direction of the cathode plate.
[0009] Preferably, the insulating baffle is wrapped around the outer circumference of the cathode plate.
[0010] Preferably, the insulating baffle and the cathode plate are in close contact.
[0011] More preferably, the cathode plate and the anode plate are located on the left and right sides of the cathode roller, respectively.
[0012] Compared with the prior art, the utility model has the following beneficial effects:
[0013] By adding an insulating baffle to the cathode plate, the conductive area of the cathode plate can be reduced. Under the premise of the same current, the current density will increase, the deposition rate of copper nodules on the copper foil surface will increase, and the morphology and color of the formed copper nodules will be relatively uniform, so that there will be no color difference on the surface of the reverse copper foil. In addition, the appropriate increase in current density will not greatly affect the roughness of the copper foil treatment surface, and it is still within the acceptable parameter range, which is equivalent to better improving the yield rate of reverse copper foil production without affecting the roughness of the copper foil treatment surface, and it is highly practical. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] In order to more clearly illustrate the embodiments of the utility model or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the utility model. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0015] Figure 1 This is an overall plan view of an embodiment of the present application;
[0016] Figure 2 This is a schematic diagram of the assembly of a cathode plate and an insulating baffle in one embodiment of the present application;
[0017] Figure 3 It is an overall plan view of the cathode plate without an insulating baffle installed in the prior art.
[0018] Markings in the attached drawing are: 1-roughening electroplating tank, 2-cathode plate, 3-insulating baffle, 4-anode plate, 5-cathode roller, 6-copper foil, 7-tank roller, 8-upper guide roller.
[0019] The realization of the purpose, functional features and advantages of the utility model will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0020] The following will be combined with the drawings in the embodiments of the utility model to clearly and completely describe the technical solutions in the embodiments of the utility model. Obviously, the described embodiments are only part of the embodiments of the utility model, not all of the embodiments. Based on the embodiments of the utility model, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the utility model.
[0021] It should be noted that all directional indications (such as up, down, left, right, front, back, etc.) in the embodiments of the present invention are only used to explain the relative position relationship, movement status, etc. between the components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication will also change accordingly.
[0022] In addition, the descriptions of "first", "second", etc. in the present utility model are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in the field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the scope of protection required by the present utility model.
[0023] Specific implementation plan: see Figure 1-Figure 3 The utility model is an electroplating device for improving the color difference of low-roughness reverse copper foil electroplating, comprising a roughening electroplating tank 1, wherein a cathode plate 2, an anode plate 4, a cathode roller 5 and a roughening electrolyte are arranged in the roughening electroplating tank 1, wherein the cathode roller 5 is immersed in the roughening electrolyte and is used to cooperate with a slot-entering roller 7 and an upper guide roller 8 located outside the roughening electroplating tank 1 to complete the material guiding of the copper foil 6, the anode plate 4 and the cathode plate 2 are arranged at intervals, and an insulating baffle 3 is installed on the surface of the cathode plate 2, and the insulating baffle 3 is used to block part of the conductive area of the cathode plate 2.
[0024] See also Figure 1 It can be seen that the slot entry roller 7 and the upper guide roller 8 are respectively located upstream and downstream of the cathode roller 5. In cooperation with the cathode roller 5, the copper foil 6 can be continuously transported into the roughening electroplating tank 1.
[0025] As a preferred implementation of this embodiment, the insulating baffle 3 extends along the length direction of the cathode plate 2 .
[0026] Then, see Figure 1 and Figure 2 It can be seen that in this embodiment, the insulating baffle 3 is wrapped around the outer circumference of the cathode plate 2.
[0027] Furthermore, in this embodiment, the insulating baffle 3 and the cathode plate 2 are in close contact.
[0028] For ease of understanding, the following example illustrates the changes in current density and the roughness of the treated surface of the copper foil 6 before and after the insulating baffle 3 is installed on the cathode plate 2:
[0029] For example, the current of the coarsening section is 1500A, the area of the cathode plate 2 is 0.75×1.35=1.0125m2, the shielding area of the insulating baffle 3 is: 0.2×1.35=0.27m2, and the conductive area of the cathode plate 2 after the insulating baffle 3 is installed is: 0.55×1.35=0.7425m2;
[0030] Before installing the insulating baffle 3 on the cathode plate 2: the original current density is J = I / S = 1500 / 1.0125 = 1481.5A / m2;
[0031] After installing the insulating baffle 3 on the cathode plate 2: J = I / S = 1500 / (0.55×1.35) = 2020.2A / m2;
[0032] It can be seen from the above that after the insulating baffle 3 is installed on the cathode plate 2, the current density of the electrodeposited copper nodule is significantly increased.
[0033] In addition, after actual testing, it was found that the roughness of the treated surface of the copper foil 6 did not change much before and after the insulating baffle 3 was installed on the cathode plate 2, and was within the acceptable parameter variation range.
[0034] In summary, under the premise of not affecting the roughness of the treated surface of the copper foil 6, by adding an insulating baffle 3 to the cathode plate 2, the current density of the electrodeposited copper nodules is increased, so that the copper nodules can be more efficiently electrodeposited on the surface of the copper foil 6, thereby forming a more uniform and stable electroplating layer, without electroplating color difference, uniform morphology and color, and no pores. The aesthetics of the treated surface of the copper foil 6 will be better, thereby improving the yield rate of the reverse copper foil 6 production.
[0035] More specifically, in this embodiment, the cathode plate 2 and the anode plate 4 are located on the left and right sides of the cathode roller 5, respectively.
[0036] The above description of the utility model is only a preferred embodiment of the utility model, and does not limit the patent scope of the utility model. All equivalent structural changes made by using the contents of the utility model specification and drawings under the inventive concept of the utility model, or direct / indirect application in other related technical fields are included in the patent protection scope of the utility model.
Claims
1. An electroplating device for improving the color difference of low-roughness reverse copper foil electroplating, comprising a roughening electroplating tank, wherein a cathode plate, an anode plate, a cathode roller and a roughening electrolyte are arranged in the roughening electroplating tank, wherein: The cathode roller is immersed in the roughening electrolyte and is used to cooperate with the inlet roller and the upper guide roller located outside the roughening plating tank to complete the material guiding of the copper foil. The anode plate and the cathode plate are arranged at intervals, and it is characterized in that an insulating baffle is installed on the surface of the cathode plate, and the insulating baffle is used to block part of the conductive area of the cathode plate.
2. The electroplating device for improving the color difference of low-roughness reverse copper foil electroplating according to claim 1, characterized in that: The insulating baffle extends along the length direction of the cathode plate.
3. The electroplating device for improving the color difference of low-roughness reverse copper foil electroplating according to any one of claims 1 to 2, characterized in that: The insulating baffle is wrapped around the outer circumference of the cathode plate.
4. The electroplating device for improving the color difference of low-roughness reverse copper foil electroplating according to claim 1, characterized in that: The insulating baffle and the cathode plate are in close contact.
5. The electroplating device for improving the color difference of low-roughness reverse copper foil electroplating according to claim 1, characterized in that: The cathode plate and the anode plate are respectively located on the left and right sides of the cathode roller.
Citation Information
Cited By
A copper foil plating device for easy peelable copper foil processing
CN224917960U