Microneedle electrode array and microneedle array patch type sensing device
By setting a swelling resin layer at the tip of the microneedle electrode array to form a three-dimensional porous structure, the contamination problem of microneedle electrochemical sensors during subcutaneous detection is solved, and efficient and low-cost subcutaneous biomarker detection is achieved.
Patent Information
- Application Number
- CN202322682573.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-28
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2033-09-28
AI Technical Summary
Existing microneedle electrochemical sensors are susceptible to contamination by skin keratin, oils and skin care products during subcutaneous detection, resulting in poor anti-interference performance, complex preparation and high cost, making it difficult to produce on a large scale.
A microneedle electrode array is adopted, including working electrode, counter electrode and reference electrode, all coated with precious metal layers, and a swollen resin layer is set at the tip. After absorbing water, the swollen resin layer forms a three-dimensional porous structure, isolating the external environment, enhancing the anti-fouling and Anti-interference performance.
It realizes the clean protection and efficient detection of microneedle electrodes, reduces interference from subcutaneous detection, simplifies the preparation process, reduces costs, and improves the anti-fouling and anti-interference performance of the sensor.
Smart Images

Figure CN221931968U_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of electrochemical biosensors, and in particular, relates to a microneedle electrode array and a microneedle array patch-type sensing device. Background Art
[0002] Electrochemical biosensors have important applications in medicine, biological research, and clinical diagnosis. In recent years, wearable sensors with simple structures and convenient use have become a research hotspot, showing great potential in early disease diagnosis and daily health care. Wearable sensors can generally be divided into two categories, namely non-invasive devices and invasive devices. Recent research has mainly focused on the former, whose original biological samples are mainly sweat, saliva, or extracted interstitial fluid. Although non-invasive devices have the advantages of being non-invasive and portable, they are still in the laboratory stage. The main reason is that the correlation between the concentration of biomarkers in epidermal secretions and the concentration of biomarkers in endogenous body fluids (such as blood) has not been fully verified. It is worth noting that since the content of biological small molecule markers in subcutaneous interstitial fluid is highly correlated with the content of small molecule markers in blood, minimally invasive wearable devices for tissue fluid analysis have gradually attracted the attention of researchers.
[0003] Among them, microneedle-based electrochemical biosensors are typical representatives of minimally invasive devices. Due to the invasive action form of microneedles, they can perform functions deep into the tissue. Benefiting from their tiny size and fine structure, they are less dependent on the sample amount and can achieve efficient detection of interstitial fluid. They have been widely used in in situ monitoring of subcutaneous biomarkers. For example, J. Wang et al. developed a fully integrated wearable microneedle array for monitoring glucose, lactate and alcohol in interstitial fluid, and the test results were well correlated with the standard method test results in blood or breath. In addition, the great success of glucose monitoring systems in the international market has also verified the effectiveness of microneedle technology. However, most of the current microneedle electrochemical sensors are complex to prepare, not easy to mass produce, and are easily contaminated by skin keratin, oils, skin care products and other substances when piercing the subcutaneous tissue, resulting in reduced sensing interface performance. In addition, the components in the interstitial fluid are complex, and the electrochemical sensing of subcutaneous biomarkers is currently susceptible to the influence of complex components. Therefore, it is of great significance to develop a microneedle electrochemical sensor with simple preparation, low cost, strong anti-fouling performance and strong anti-interference performance. Utility Model Content
[0004] The purpose of the present application is to provide a microneedle electrode array and a microneedle array patch-type sensing device, aiming to solve the problem of poor anti-interference performance of electrochemical sensors for subcutaneous biomarkers.
[0005] In order to achieve the above application purpose, the technical solution adopted in this application is as follows:
[0006] In a first aspect, the present application provides a microneedle electrode array, comprising a plurality of working electrodes, counter electrodes and reference electrodes; each of the working electrodes is uniformly arranged around the counter electrode with the counter electrode as the center, the reference electrode is spaced apart from any of the working electrodes, and the reference electrode is spaced apart from the counter electrode;
[0007] Any of the working electrode and the counter electrode comprises a first metal microneedle and a noble metal layer modified on the surface of the first metal microneedle;
[0008] The reference electrode comprises a second metal microneedle spaced apart from any of the first metal microneedles and a silver / silver chloride layer modified on the surface of the second metal microneedle;
[0009] The tip surfaces of the working electrode, the counter electrode and the reference electrode are all provided with a swelling resin layer for isolating the external environment, and the swelling resin layer presents a three-dimensional porous structure after absorbing water.
[0010] In a second aspect, the present application provides a microneedle array patch-type sensing device, comprising the microneedle electrode array as described in the first aspect.
[0011] The first aspect of the present application provides a microneedle electrode array, the microneedle electrode is the core element of the electrochemical sensor device, and the present application is coated with a swelling resin layer in the needle tip sensing area of the microneedle electrode, the purpose of which is to protect the electrode interface from contamination and reduce subcutaneous interference. From the effect point of view, the unswollen resin serves as a protective layer for the microneedle electrode, and when the microneedle is inserted into the skin, the electrode surface is isolated from skin secretions, exogenous skin care products and epidermal stratum corneum, thereby keeping the microneedle clean, thereby making the sensor device with the microneedle electrode have excellent anti-fouling performance, and, because the swelling resin has excellent water absorption, when the microneedle enters the subcutaneous tissue, the resin will naturally swell and quickly form a three-dimensional porous structure, so that small molecules and ions including oxygen reach the microneedle interface, and due to the molecular sieve effect of the gel-like swelling resin, the transport of biomacromolecules is hindered, which may be conducive to ensuring the specificity of the microneedle to oxygen and reducing potential matrix interference, thereby making the sensor device with the microneedle electrode have excellent anti-interference performance.
[0012] The second aspect of the present application provides a microneedle array patch type sensor device, which is low-cost and simple to manufacture, and can be successfully used to monitor subcutaneous oxygen content during exercise and can distinguish the exercise state in a timely manner. The sensor device provides a general device strategy for the detection of other biomarkers in interstitial fluid. It is foreseeable that the microneedle array patch type sensor device provided by the present application will play an active role in respiratory disease assessment, surgical monitoring and public health care. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0014] Figure 1 It is the SEM image of the bare microneedle (Figure a) and the EDS spectrum of the bare microneedle (Figure b);
[0015] Figure 2 It is a SEM image (Figure a) of the gold-modified microneedle electrode provided in Comparative Example 1 of the present application and an EDS spectrum (Figure b) of the gold-modified microneedle electrode;
[0016] Figure 3 1 is a SEM image (a) of a microneedle electrode modified with a swollen resin and an EDS spectrum (b) of a microneedle electrode modified with a swollen resin provided in Example 1 of the present application;
[0017] Figure 4 CV curves of microneedle electrode units at different modification stages in 5mM K3[Fe(CN)6] solution (a); electrochemical impedance spectroscopy of differently modified microneedle electrodes (b)
[0018] Figure 5 is the CV response of the microneedle electrode unit at different modification stages in 150 mmHg oxygen solution;
[0019] Figure 6 Schematic diagram of the swelling phase of the microneedle array patch sensing device (MNAP) in the epidermis (i, the phase of the microneedles (SR / Au / MN) modified by the swelling resin piercing into the skin; ii, the phase of the microneedles (SR / Au / MN) modified by the swelling resin swelling under the skin; iii, the phase of the microneedles (SR / Au / MN) modified by the swelling resin being removed from the epidermis);
[0020] Figure 7 The SEM image of the microneedle (SR / Au / MN) modified with the swelling resin after freeze-drying in the swelling phase ii (a); the EDS spectrum of the microneedle (SR / Au / MN) modified with the swelling resin after freeze-drying in the swelling phase ii (b);
[0021] Figure 8 The SEM image of the microneedle (SR / Au / MN) modified with the swelling resin in the swelling stage iii (a); the EDS spectrum of the microneedle (SR / Au / MN) modified with the swelling resin in the swelling stage iii (b);
[0022] Fig. 9Swelling performance diagram of swelling resin, swelling rate curve of swelling resin material (Figure a); resistance change curve of swelling resin modified microneedle (SR / Au / MN) during swelling process (Figure b);
[0023] Fig.10 The electrochemical impedance spectroscopy (EIS) of the microneedle (SR / Au / MN) modified with the swellable resin before and after full swelling (Fig. a); the CV curve of the microneedle (SR / Au / MN) modified with the swellable resin before and after full swelling in the probe solution (Fig. b); the CV response curve of the microneedle (SR / Au / MN) modified with the swellable resin to oxygen before and after full swelling (Fig. c);
[0024] Fig.11 CV curves of the microneedle array patch sensor device (MNAP) in the probe solution when the scan rate is 10-200 mv / s (Figure a); the relationship between the redox peak current and the square root of the scan rate in each curve (Figure b);
[0025] Fig.12 is the response of swollen resin modified microneedles (SR / Au / MN) and gold modified microneedles (Au / MN) to oxygen in hydrogels covered or not covered with petroleum jelly;
[0026] Fig.13 The graphs are the responses of the swollen resin modified microneedles (SR / Au / MN) and gold modified microneedles (Au / MN) to oxygen in PBS with and without BSA interference substrates;
[0027] Fig.14 This is the current response diagram of the microneedle array patch sensor device (MNAP) to a series of oxygen concentrations in the range of 0 to 150 mmHg (Figure a). The potential was set to -0.8 V and the electrolyte solution was 0.1 M PBS; the calibration fitting curve between current and oxygen content (Figure b);
[0028] Fig.15 It is the oxygen amperometric curve obtained by using a microneedle array patch sensor device (MNAP) to test before and after adding Na2SO3 to a saturated oxygen solution to deoxygenate;
[0029] Fig.16 It is the response of the microneedle array patch sensor (MNAP) to oxygen in the presence of different interfering substrates. Note: I and I0 represent the current of MNAP in the interfering solution containing the analytical target and the current obtained from the initial solution, respectively. (Potential interfering substances include 50mmHg CO2, 680mmHg N2, 3mg / mL KCl, 0.9% NaCl, 12mg / mL IgG, 140mg / dL glucose and 15mg / dL lactic acid);
[0030] Fig.17 The oxygen concentration was detected using a microneedle array patch sensor (MNAP) and a commercial instrument (the inset shows the linear relationship between the detection results of the MNAP and the commercial instrument).
[0031] Fig.18 It was a microneedle array patch sensor device (MNAP) to detect 150 mmHg oxygen for 7 days (Note: I and I0 represent the current values obtained on a given day and the first day, respectively);
[0032] Fig.19 Figure 1 shows the in vivo performance of the microneedle array patch (MNAP). A photo of the MNAP worn on a participant's arm (a). A comparison of MNAP oxygen partial pressure measurements with reference measurements of oxygen saturation and heart rate from a sports smartwatch (b).
[0033] Fig. 20 Schematic diagram of a microneedle electrode array provided in Example 1 of the present application (Fig. a); Schematic diagram of the structure of a microneedle electrode unit (Fig. b);
[0034] Fig.21 Photos of the front and back of the microneedle array patch (MNAP) (a); exploded subassembly view of the fully integrated MNAP (b) (i, a custom-made microelectrochemical workstation; ii, microneedle electrode array fixed on a resin plate; iii, adhesive layer; iv, air barrier)
[0035] Among them, the reference numerals in the figure are:
[0036] 1—working electrode 2—counter electrode 3—reference electrode 4—first metal microneedle or second metal microneedle 5—noble metal layer or silver / silver chloride layer 6—insulating layer 7—swelling resin layer DETAILED DESCRIPTION
[0037] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0038] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.
[0039] In this application, "at least one" means one or more, and "plurality" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.
[0040] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.
[0041] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "said" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.
[0042] The weight of the relevant components mentioned in the embodiment description of the present application can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the embodiment description of the present application, it is within the scope disclosed in the embodiment description of the present application. Specifically, the mass described in the embodiment description of the present application can be a mass unit known in the chemical industry such as μg, mg, g, kg, etc.
[0043] The terms "first" and "second" are used only for descriptive purposes to distinguish objects such as substances from each other, and should not be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. For example, without departing from the scope of the embodiments of the present application, the first XX may also be referred to as the second XX, and similarly, the second XX may also be referred to as the first XX. Thus, features defined as "first" and "second" may explicitly or implicitly include one or more of the features.
[0044] In a first aspect, an embodiment of the present application provides a microneedle electrode array, such as Fig. 20As shown, it includes several working electrodes 1, counter electrodes 2 and reference electrodes 3; each working electrode 1 is uniformly arranged around the counter electrode 2 with the counter electrode 2 as the center, the reference electrode 3 is spaced apart from any working electrode 1, and the reference electrode 3 is spaced apart from the counter electrode 2; any working electrode 1 and counter electrode 2 include a first metal microneedle 4 and a noble metal layer 5 modified on the surface of the first metal microneedle 4; the reference electrode 3 includes a second metal microneedle spaced apart from any first metal microneedle 4 and a silver / silver chloride layer modified on the surface of the second metal microneedle; the tip surfaces of the working electrode 1, the counter electrode 2 and the reference electrode 3 are all provided with a swelling resin layer 7 for isolating the external environment, and the swelling resin layer 7 presents a three-dimensional porous structure after absorbing water (such as Figure 3 , Figure 6 and Figure 7 shown).
[0045] The first aspect of the present application provides a microneedle electrode array, which uses a swellable resin and a precious metal modified metal microneedle (commercial acupuncture needle) as a sensing unit. The three-dimensional porous precious metal modified microneedle significantly increases the sensing area of the microneedle, thereby greatly improving the sensing performance. In addition, the swelling resin exhibits excellent anti-fouling and anti-interference properties in the sensing platform. Coating a swelling resin layer on the sensing area of the microneedle electrode tip can play the following roles: (1) The unswollen resin acts as a protective layer for the microneedle electrode, isolating the electrode surface from skin secretions (endogenous secretion of oil and sweat), exogenous skin care and epidermal stratum corneum when the microneedle pierces the skin, thereby keeping the microneedle electrode clean. (2) The fully swollen resin acts as an electrolyte gel to provide a liquid environment for sensing, while the electrode surface is fully exposed to form a good oxygen reduction interface. When the microneedle electrode penetrates the skin and enters the subcutaneous tissue, the swelling process occurs naturally by absorbing the liquid matrix in the skin interstitial fluid. Due to the excellent water absorption performance of the resin, the resin will quickly form a three-dimensional porous structure, allowing small molecules and ions including oxygen to be freely dispersed to the microneedle electrode interface, and the molecular sieve effect of the gel-like swelling resin hinders the transport of biomacromolecules. This may be beneficial to ensure the specificity of the microneedle electrode for oxygen and reduce potential matrix interference.
[0046] In some embodiments, the swelling resin layer includes a polymer of polymethyl vinyl ether / maleic acid copolymer and polyethylene glycol, or a polymer of hyaluronic acid and methacrylic anhydride, or a polystyrene-polyacrylamide-based resin. In the present application, the swelling resin layer is preferably a polymer of polymethyl vinyl ether / maleic acid copolymer and polyethylene glycol. Further, the thickness of the swelling resin layer is 20 to 30 μm.
[0047] In some embodiments, an insulating layer is provided on the middle surface of each microneedle electrode; the middle refers to an area 2 to 4 mm away from the tip and 2 to 3 mm wide. After the noble metal is sputtered on the surface of the microneedle, an insulating layer is then provided in the middle area, with the purpose of forming a constant sensing area at the needle tip. Furthermore, the insulating layer material is selected from an insulating material with good biocompatibility and unidirectional adhesion, such as medical epoxy resin.
[0048] In some embodiments, the insulating layer is an epoxy layer.
[0049] In some embodiments, the noble metal layer includes a gold layer and / or a platinum layer. The purpose of providing a gold layer or a platinum layer on the surface of the metal microneedle is to increase the sensing area of the metal microneedle and improve the sensing performance; further, the noble metal layer is selected from a gold layer, which has good sensing performance and is easy to obtain.
[0050] In some embodiments, the diameters of the first metal microneedle and the second metal microneedle are both 0.12-0.3 mm. The metal microneedles of the present application are commercial ultrafine stainless steel needles, and their diameters mainly include: 0.12 mm, 0.14 mm, 0.16 mm, 0.18 mm, 0.20 mm, 0.25 mm, and 0.30 mm.
[0051] In some embodiments, the total number of the first metal microneedles and the second metal microneedles is 4 to 10, and the number of microneedle electrodes can be selected as 4, 5, 6, 7, 8, 9, or 10. Too few microneedles will result in a single subcutaneous sensing position, resulting in reduced detection accuracy. Too many microneedles will increase the pain of the wearer. Furthermore, it is best to select 6 to 8 microneedle electrodes, including 1 counter electrode, 1 reference electrode, and 4 to 6 working electrodes.
[0052] In some embodiments, the spacing between each two first metal microneedles is 2 to 6 mm, wherein the working electrodes are connected in series, the counter electrode is placed in the middle of the working electrode and is at an equal distance from the working electrode, and the spacing between the two microneedles can be selected to be 2 to 6 mm. Too large or too small a spacing between the microneedles will result in signal reduction or crosstalk. Therefore, further, the spacing between the microneedle electrodes is selected to be 3 to 5 mm.
[0053] In some embodiments, the first metal microneedle and the second metal microneedle are both selected from one of steel needle, silver needle, silver-plated needle, gold needle, and gold-plated needle, wherein the first metal microneedle is used as a working electrode and a counter electrode, and can be selected from steel needle, silver needle, silver-plated needle, etc. More preferably, in one embodiment, commercially available stainless steel acupuncture needles are selected, which are low in cost and simple to manufacture. The second metal microneedle is used as a reference electrode, and considering the cost reasons, silver-plated needles, silver needles, etc. can be selected, and more preferably, silver-plated stainless steel acupuncture needles are selected in one embodiment.
[0054] Specifically, the present invention provides a method for preparing a microneedle electrode array, comprising the following steps:
[0055] The metal microneedles are immersed in ethanol, metal degreasing agent and metal rust remover respectively, and ultrasonically cleaned in the above solutions for 5 to 10 minutes respectively. Optionally, each step is rinsed with deionized water, and finally the dry and clean microneedles are taken for use;
[0056] The noble metal is sputtered on the surface of the first metal microneedle by using an ion sputtering instrument with a noble metal target source, and the sputtering time is 1 to 6 minutes. The second metal microneedle is immersed in a mixed solution of chloride salt and HCl for electrochemical deposition treatment, and after being rinsed with deionized water, it is placed in the chloride salt solution away from light;
[0057] Except for the sensing area at the tip and the contact area at the end, the rest of the microneedle is coated with insulating material, with the purpose of forming a constant sensing area at the tip of the microneedle electrode. Furthermore, the insulating material is selected from medical epoxy resin;
[0058] The swelling resin precursor solution is coated on the tip of the surface-modified first metal microneedle and the second metal microneedle, and vacuum dried at 25 to 35° C. for 8 to 10 hours.
[0059] Specifically, the preparation method of the swelling resin precursor solution is: based on the total mass of the swelling resin precursor solution as 100%, a 5wt% concentration of polymethyl vinyl ether / maleic acid copolymer (PMVE / MA), a 5wt% concentration of polyethylene glycol 8000, a 3wt% concentration of sodium carbonate, and a 0.2wt% concentration of sodium polyacrylate are stirred and mixed at 60-80°C for 2-3h.
[0060] Alternatively, the swelling resin precursor solution includes a polymer of hyaluronic acid and methacrylic anhydride (MeHA) and is prepared by sequentially adding N,N-dimethylformamide (DMF) and methacrylic anhydride (MA) to a hyaluronic acid (HA) aqueous solution, stirring overnight to obtain a precursor gel (MeHA). Subsequently, NaOH is added, and the precursor gel (MeHA) is washed multiple times with ethanol while maintaining a pH of 8 to 9.
[0061] Alternatively, the swelling resin precursor solution includes a preparation method of a polystyrene-polyacrylamide-based resin: using poly tert-butyl acrylate-polystyrene block copolymer (PSb-ptBA) and dichloromethane as raw materials, using trifluoroacetic acid as a catalyst, hydrolyzing for 48 to 72 hours to prepare polystyrene-polyacrylamide (PS-b-PAA), and then precipitating PS-b-PAA with n-hexane, filtering, and washing several times. Using a solvent casting method, PS-b-PAA is dissolved in N,N-dimethylformamide (DMF) for 48 to 72 hours and then degassed.
[0062] In a second aspect, the present application provides a microneedle array patch-type sensing device, comprising the microneedle electrode array of the first aspect.
[0063] The electrochemical sensing device provided in the second aspect of the present application includes a microneedle electrode array, which uses a swellable resin and a precious metal modified metal microneedle (commercial acupuncture needle) as a sensing unit. The three-dimensional porous precious metal modified microneedle significantly increases the sensing area of the microneedle, thereby greatly improving the sensing performance. In addition, the swelling resin exhibits excellent anti-fouling and anti-interference properties in the sensing platform. Coating a swelling resin layer on the sensing area of the microneedle electrode tip can play the following roles: (1) The unswollen resin acts as a protective layer for the microneedle electrode, isolating the electrode surface from skin secretions (endogenous secretion of oil and sweat), exogenous skin care and epidermal stratum corneum when the microneedle pierces the skin, thereby keeping the microneedle electrode clean. (2) The fully swollen resin acts as an electrolyte gel to provide a liquid environment for sensing, while the electrode surface is fully exposed to form a good oxygen reduction interface. When the microneedle electrode penetrates the skin and enters the subcutaneous tissue, the swelling process occurs naturally by absorbing the liquid matrix in the skin interstitial fluid. Due to the excellent water absorption performance of the resin, the resin will quickly form a three-dimensional porous structure, allowing small molecules and ions including oxygen to be freely dispersed to the microneedle electrode interface, and the molecular sieve effect of the gel-like swelling resin hinders the transport of biomacromolecules. This may be beneficial to ensure the specificity of the microneedle electrode for oxygen and reduce potential matrix interference.
[0064] In some embodiments, a microneedle array patch-type sensing device includes: a substrate; a microneedle electrode array fixedly arranged on the substrate; an electrochemical workstation, the electrochemical workstation being provided with through holes matching the number and size of the microneedle electrode array; the substrate includes a resin plate, an adhesion layer and an air-proof layer connected in sequence; a side of the resin plate facing away from the microneedle electrode is connected to the electrochemical workstation, and the microneedle electrode is electrically connected to the electrochemical workstation through the through hole.
[0065] In some embodiments, Fig.21 As shown, the electrochemical workstation is a customized micro-potentiostat, which has through holes corresponding to the number and diameter of microneedle electrodes, and the microneedle electrodes are electrically connected to the micro-electrochemical workstation through the through holes thereon. The microneedle electrodes are fixed in a resin plate, which is integrally formed by 3D printing. The internal dimensions of the resin plate are consistent with those of the micro-potentiostat to ensure their close fit. The adhesive layer can be made of medical non-woven fabric, and the medical non-woven fabric layer can be cut into the required shape and size, such as: it can be cut into a 60×40mm capsule.
[0066] In order to prevent the oxygen in the external environment from interfering with the test, a layer of air-proof film is integrated in the microneedle array patch type sensing device. In some embodiments, the air-proof layer can be selected from materials such as polyethylene (PE), polyvinylidene chloride (PVDC), chlorinated polyvinyl chloride (CPVC), polytetrafluoroethylene (PTFE). In a preferred embodiment, polyvinylidene chloride (PVDC) film is selected because polyvinylidene chloride (PVDC) has good air-proof properties. The polyvinylidene chloride film is cut into required shapes and sizes, such as: a disc with a diameter of 20 mm, and is pasted on an adhesive layer medical nonwoven fabric.
[0067] This application combines microneedles with wearable technology, and uses commercial acupuncture needles decorated with swellable resins and precious metals as sensing units to construct a microneedle array patch that can continuously monitor subcutaneous oxygen content during exercise online. The introduction of commercial microneedles has given the array patch many advantages such as easy mass production, stable performance and cost-effectiveness. The three-dimensional porous precious metal-modified microneedles significantly increase the sensing area of the microneedles, thereby greatly improving the sensing performance. In addition, the swelling resin exhibits excellent anti-fouling and anti-interference properties in this sensing platform. After the patch is integrated with the microneedle sensing unit, it has the advantages of large sensing area, high signal strength and large detection area. The microneedle array patch can transmit data to a mobile terminal in real time by integrating with a miniaturized workstation with Bluetooth transmission function, realizing on-site continuous monitoring of subcutaneous oxygen changes during exercise. The microneedle array patch-type electrochemical sensor device has the advantages of simple preparation, low price and easy storage, and plays a good role in real-time analysis of subcutaneous oxygen content, and can be used as a general tool for analyzing other substances in interstitial fluid (ISF).
[0068] The following describes the invention in conjunction with specific embodiments.
[0069] Example 1
[0070] A microneedle electrode array is divided into 6 working electrodes, 1 reference electrode and 1 counter electrode. The working electrode and the counter electrode are both made of commercial stainless steel acupuncture needles with a diameter of 0.16 mm, and the surface is modified with a gold layer; the reference electrode is made of a silver-plated acupuncture needle with a diameter of 0.16 mm, and the surface is modified with a silver / silver chloride layer. The tip surfaces of the working electrode, the counter electrode and the reference electrode are all provided with a swelling resin layer for isolating the external environment, and the swelling resin layer presents a three-dimensional porous structure after absorbing water, and the swelling resin layer includes a polymer of polymethyl vinyl ether / maleic acid copolymer and polyethylene glycol. Each working electrode is evenly arranged around the counter electrode with the counter electrode as the center, and the reference electrode is arranged at intervals from any working electrode, and the reference electrode is arranged at intervals from the counter electrode.
[0071] A microneedle array patch-type sensing device is assembled from a customized micro-potentiostat, the above-mentioned microneedle electrode array fixed on a resin plate, a medical non-woven fabric and a polyvinylidene chloride film. The customized micro-potentiostat has 8 through holes with a diameter of 0.16 mm, and the microneedles are electrically connected to the micro-electrochemical workstation through the through holes thereon. The microneedle electrode array is fixed in the resin plate, and the distance between each two microneedles is 4 mm. The resin plate is integrally formed by 3D printing. The internal dimensions of the resin plate are consistent with those of the micro-potentiostat to ensure their close fit. The medical non-woven fabric layer is cut into a 60×40 mm capsule shape by a laser cutting machine. In addition, the polyvinylidene chloride film is cut into a disc with a diameter of 20 mm by laser and pasted on the non-woven fabric layer. Finally, the above four components are assembled in sequence, and the assembly of the microneedle array patch-type electrochemical sensing device is completed.
[0072] Example 2
[0073] A microneedle electrode array is divided into 6 working electrodes, 1 reference electrode and 1 counter electrode. The working electrode and the counter electrode are both made of commercial stainless steel acupuncture needles with a diameter of 0.14 mm, and the surface is modified with a gold layer; the reference electrode is made of a silver-plated acupuncture needle with a diameter of 0.14 mm, and the surface is modified with a silver / silver chloride layer. The tip surfaces of the working electrode, the counter electrode and the reference electrode are all provided with a swelling resin layer for isolating the external environment, and the swelling resin layer presents a three-dimensional porous structure after absorbing water, and the swelling resin layer includes a polymer of polymethyl vinyl ether / maleic acid copolymer and polyethylene glycol. Each working electrode is evenly arranged around the counter electrode with the counter electrode as the center, and the reference electrode is arranged at intervals from any working electrode, and the reference electrode is arranged at intervals from the counter electrode.
[0074] The middle surfaces of the working electrode, the counter electrode and the reference electrode are all provided with an insulating layer; the middle portion is a region located 3 mm away from the tip and having a width of 2 mm.
[0075] A microneedle array patch-type sensing device is assembled from a customized micro-potentiostat, the above-mentioned microneedle electrodes fixed on a resin plate, a medical non-woven fabric and a polyvinylidene chloride film. The customized micro-potentiostat has 8 through holes with a diameter of 0.14 mm, and the microneedles are electrically connected to the micro-electrochemical workstation through the through holes thereon. The electrode array is fixed in the resin plate, and the distance between each two microneedles is 4 mm. The resin plate is integrally formed by 3D printing. The internal dimensions of the resin plate are consistent with those of the micro-potentiostat to ensure their close fit. The medical non-woven fabric layer is cut into a 65×40 mm capsule shape by a laser cutting machine. In addition, the polyvinylidene chloride film is cut into a disc with a diameter of 20 mm by laser and pasted on the non-woven fabric layer. Finally, the above four components are assembled in sequence, and the assembly of the microneedle array patch-type electrochemical sensing device is completed.
[0076] Example 3
[0077] A microneedle electrode array is divided into 4 working electrodes, 1 reference electrode and 1 counter electrode. The working electrode and the counter electrode are both made of commercial stainless steel acupuncture needles with a diameter of 0.18 mm, and the surface is modified with a gold layer; the reference electrode is made of a silver-plated acupuncture needle with a diameter of 0.18 mm, and the surface is modified with a silver / silver chloride layer. The tip surfaces of the working electrode, the counter electrode and the reference electrode are all provided with a swelling resin layer for isolating the external environment, and the swelling resin layer presents a three-dimensional porous structure after absorbing water, and the swelling resin layer includes a polymer of polymethyl vinyl ether / maleic acid copolymer and polyethylene glycol. Each working electrode is evenly arranged around the counter electrode with the counter electrode as the center, and the reference electrode is arranged at intervals from any working electrode, and the reference electrode is arranged at intervals from the counter electrode.
[0078] The middle surfaces of the working electrode, the counter electrode and the reference electrode are all provided with an insulating layer; the middle portion is a region located 3 mm away from the tip and having a width of 3 mm.
[0079] A microneedle array patch-type sensing device is assembled from a customized micro-potentiostat, the above-mentioned microneedle electrodes fixed on a resin plate, a medical non-woven fabric and a polyvinylidene chloride film. The customized micro-potentiostat has 6 through holes with a diameter of 0.18 mm, and the microneedles are electrically connected to the micro-electrochemical workstation through the through holes thereon. The electrode array is fixed in the resin plate, and the distance between each two microneedles is 5 mm. The resin plate is integrally formed by 3D printing. The internal dimensions of the resin plate are consistent with those of the micro-potentiostat to ensure their close fit. The medical non-woven fabric layer is cut into a 55×40 mm capsule shape by a laser cutting machine. In addition, the polyvinylidene chloride film is cut into a disc with a diameter of 20 mm by laser and pasted on the non-woven fabric layer. Finally, the above four components are assembled in sequence, and the assembly of the microneedle array patch-type electrochemical sensing device is completed.
[0080] Example 4
[0081] The difference between this embodiment and embodiment 2 is that the swelling resin layer of this embodiment includes a polymer of hyaluronic acid and methacrylic anhydride. The preparation method is as follows: 50 ml of N, N-dimethylformamide (DMF) and 9.3 ml of methacrylic anhydride (MA) are added to 50 ml of 2% hyaluronic acid (HA) aqueous solution by mass volume fraction, and stirred overnight to obtain a precursor gel (MeHA). Subsequently, the precursor gel (MeHA) is washed 3 times with ethanol while adjusting the pH to 8-9 by dissolving with 1 mol / L NaOH. The air barrier layer uses a chlorinated polyvinyl chloride film.
[0082] Example 5
[0083] The difference between this embodiment and embodiment 3 is that the swelling resin layer of this embodiment includes a polystyrene-polyacrylamide-based resin, and its preparation method is as follows: 10g of poly(tert-butyl acrylate)-polystyrene block copolymer (PSb-ptBA) and 50ml of dichloromethane are used as raw materials, 10g of trifluoroacetic acid is used as a catalyst, and polystyrene-polyacrylamide (PS-b-PAA) is prepared by hydrolysis for 48 hours, and then the PS-b-PAA is precipitated with n-hexane, filtered, and washed several times. The PS-b-PAA is dissolved in N,N-dimethylformamide (DMF) by solvent casting for 48 hours and then degassed. The air barrier layer uses a polytetrafluoroethylene membrane.
[0084] Comparative Example 1
[0085] A microneedle electrode is made of a commercial stainless steel acupuncture needle with a diameter of 0.16 mm, and the surface is modified with a gold layer. The difference between the comparative example 1 and the embodiment 1 is that the tip of the microneedle electrode of the comparative example 1 does not have a swelling resin layer.
[0086] Effect Example 1
[0087] The prepared microneedle (MN) electrode was characterized by scanning electron microscopy (SEM) and energy dispersive spectroscopy (EDS).
[0088] SEM / EDS test method: Scanning electron microscopy was used for morphological and structural characterization and element determination. The tip area of bare microneedles (MN) and gold-modified microneedles (Au / MN) was cut for testing, and the microneedles modified with swollen resin (SR / Au / MN) needed to be freeze-dried in a vacuum freeze dryer for a period of time until they were completely dehydrated before characterization.
[0089] Test results: Compared with bare microneedles with smooth surface (MN) ( Figure 1 a) and the gold modified microneedle (Au / MN) with nanopore structure of Comparative Example 1 ( Figure 2 Compared with a), the swollen resin modified microneedle (SR / Au / MN) of Example 1 ( Figure 3 The surface of a) in the figure is rougher and more porous, and the thickness of the swollen resin is about 25 μm. In addition, from the element composition data of EDS, the bare MN is mainly composed of metal elements such as Fe and Cr ( Figure 1 b in the figure). After Au is sputtered, a special peak of Au element appears in the energy spectrum ( Figure 2 Similarly, the EDS data of SR / Au / MN showed that the percentage of C increased significantly, the percentage of Na increased significantly, and the O element appeared on Au / MN. The reason is that the surface of MN is modified with (MA / AA)Na copolymer swelling resin ( Figure 3 b) in the above.
[0090] Effect Example 2
[0091] The electrochemical properties of the prepared MN electrode were studied using classical cyclic voltammetry (CV) and electrochemical impedance spectroscopy (EIS) techniques.
[0092] Cyclic voltammetry (CV) test method: The test was performed using an electrochemical workstation, where the microneedle electrode sensing area was immersed in a potassium ferrocyanide probe solution of a certain concentration and scanned at a certain scan rate within a certain potential range.
[0093] Electrochemical impedance spectroscopy (EIS) test method: The test was performed using an electrochemical workstation. The sensing area of the microneedle electrode was immersed in a potassium ferrocyanide probe solution of a certain concentration and tested in a certain potential range. The electrode interface impedance value was obtained by software fitting.
[0094] Compared with the bare microneedle (MN), the redox peak current of the gold-modified microneedle (Au / MN) increased significantly, which can be explained by the fact that the gold layer with a three-dimensional porous interconnected structure formed on the surface of the MN effectively increased the specific surface area and active area of the electrode interface and promoted the transfer of electrons ( Figure 4 a and Figure 2 The peak current of the swollen resin modified microneedle (SR / Au / MN) is lower than that of Au / MN, which is due to the poor conductivity of the swollen resin. In addition, the EIS graphs also show similar trends in the charge transfer resistance of the MN, Au / MN and SR / Au / MN electrode interfaces ( Figure 4 In addition, we also studied the responsiveness of the MN electrode to oxygen ( Figure 5 ). Unfortunately, bare MN failed to electrocatalytically reduce the substance. It is noteworthy that Au / MN has excellent oxygen reduction performance at a potential of around -1.0 V. Although the response current of SR / Au / MN to oxygen is slightly lower than that of Au / MN, the friendly reduction potential of -0.8 V on SR / Au / MN has better selectivity.
[0095] Effect Example 3
[0096] SEM images and EDS spectra of the recovered swollen resin-modified microneedles (SR / Au / MN) after use.
[0097] In Example 1, a swelling resin based on polymethyl vinyl ether / maleic acid copolymer (PMVE / MA swelling resin) was used to decorate the surface of the microneedle electrode. The swelling process is as follows: Figure 6As shown (i, SR / Au / MN piercing the skin stage; ii, SR / Au / MN swelling stage under the skin; iii, SR / Au / MN removal from the epidermis stage). PMVE / MA resin can play the following roles in the microneedle array patch (MNAP) system: (i) The unswollen resin acts as a protective layer for the MN array, isolating the electrode surface from skin secretions (endogenous secreted oil and sweat), exogenous skin care and the epidermal stratum corneum when the microneedles pierce the skin, thereby keeping the MN array clean. (2) The fully swollen resin acts as an electrolyte gel to provide a liquid environment for sensing, while the electrode surface is fully exposed to form a good oxygen reduction interface. When the MN penetrates the skin and enters the subcutaneous tissue, the swelling process occurs naturally by absorbing the liquid matrix in the skin interstitial fluid. Due to the excellent water absorption properties of the resin, the resin will quickly form a three-dimensional porous structure ( Figure 7 a in Figure 7 b) in the figure allows small molecules and ions including oxygen to be freely dispersed to the MN interface, and the molecular sieving effect of the gel-like swelling resin hinders the transport of biomacromolecules. This may be beneficial to ensure the specificity of the MN array for oxygen and reduce potential matrix interference. (iii) After the monitoring is completed, the microneedles are removed and the non-biotoxic and biodegradable PMVE / MA resin is retained in the subcutaneous tissue. The SEM image and EDS spectrum of the recovered SR / Au / MN after use are shown in Figure 2. Figure 8 a and Figure 8 As shown in (b), compared with Au-MN, its microstructure morphology and composition are similar ( Figure 2 a in Figure 2 b). This means that only a small amount of resin remains on the gold surface, indicating that the interaction between the resin and the electrode surface is weak. It is worth noting that weak interactions may also be beneficial to the response of the MN array to oxygen.
[0098] Effect Example 4
[0099] Swelling performance test of the swelling resin in Example 1:
[0100] After the swelling resin-modified microneedles (SR / Au / MN) were inserted into the agar gel, the swelling capacity of SR / Au / MN s was calculated using the weight of SR / Au / MN s before and after insertion, and the formula was as follows:
[0101]
[0102] like Fig. 9 As shown in a, the equilibrium time of the resin swelling after water absorption is about 50s, and the maximum swelling ratio is about 500%. At the same time, a digital source meter was used to record the continuous resistance change of the SR / Au / MN array patch during the swelling process ( Fig. 9(b) The resistance of the SR / Au / MN array patch decreases continuously during the swelling process until it reaches a nearly constant value comparable to that of the Au / MN array at around 500 s, indicating that the resin is almost completely separated from the interface of the MN after full swelling.
[0103] Effect Example 5
[0104] From the interface charge transfer resistance ( Fig.10 a) in the electrochemically active area ( Fig.10 b) Response to oxygen ( Fig.10 The electrochemical characterization of partially swollen and fully swollen SR / Au / MN arrays was carried out in aspects such as c).
[0105] The results showed that the partially swollen microneedle electrode had a weaker response to oxygen, which may be due to the higher resistance and poorer penetration of the partially swollen resin. However, the fully swollen microneedle was able to restore the interface and significantly reduce the interfacial resistance ( Fig.10 As a result, the conductivity was significantly improved and the response to oxygen was restored to a level comparable to that of Au-MNs. In addition, the electrochemical sensing interface of fully swollen MNAP was studied and it was found that the electron transport at the electrode interface was mainly affected by diffusion control ( Fig.11 a and Fig.11 b) Fig.11 As shown in a, the redox peak current (I pa and I pc ) increases with the increase of scan rate (10mV / s to 200mV / s), and the current value is proportional to the square root of the scan rate ( Fig.11 This indicates that the electrochemical reaction of the probe ions at the MNAP sensing interface is controlled by diffusion.
[0106] Effect Example 6
[0107] Anti-fouling performance of swellable resin modified microneedles (SR / Au / MN):
[0108] In the anti-fouling study of microneedle puncture of the skin, furan-based hydrogel was used to simulate human skin tissue, and petroleum jelly was applied on the hydrogel to simulate pollutants such as skin secretions and skin care products on the skin. Fig.12 As shown in the figure, the response of SR / Au / MN to dissolved oxygen in pure hydrogel and petrolatum-covered hydrogel is not much different, while the response of Au / MN to the two hydrogels is quite different. This phenomenon can be explained by the fact that Au / MN is easily contaminated by potential pollutants such as petrolatum, resulting in a significant decrease in oxygen response. The resin adsorbed on the surface of Au / MN effectively protects Au as an electroreduction area from potential pollutants during microneedle puncture of the skin.
[0109] Detection of anti-pollution and anti-interference properties of swellable resin modified microneedles (SR / Au / MN):
[0110] Bovine serum albumin (BSA) was incorporated into the gel to simulate interfering substances in the subcutaneous interstitial fluid. Fig.13 As shown in Figure 2, the swollen resin also exhibits excellent performance in protecting the MN electrode from interference from biomacromolecules. This is due to the microporous structure formed after the resin swells, which effectively isolates biomacromolecules in the interstitial fluid (ISF) while allowing small biomolecules such as oxygen to pass through.
[0111] Effect Example 7
[0112] Current response of the microneedle array patch-type electrochemical sensing device to oxygen concentration.
[0113] At a potential of -0.8 V, the microneedle array patch electrochemical sensor device (MNAP) has an obvious electrochemical reduction reaction to oxygen ( Fig.10 c). Therefore, we used amperometric techniques to study the reduction current of MNAP in PBS (pH 7.4) containing 0.1 M KCl at the same potential and at different concentrations of oxygen ( Fig.14 Obviously, as the oxygen concentration increases, the current value gradually increases. In the range of 6 to 150 mmHg, the response current is proportional to the oxygen content, with a sensitivity of 0.3817 μA / mmHg and a detection limit (LOD) of 5.06 mmHg ( Fig.14 b). In addition, to prove that the current is generated by oxygen rather than other potential substrates, a special dissolved oxygen scavenger, Na2SO3, was added to the test sample during the measurement. It is worth noting that after the addition of the scavenger, the current dropped sharply, which is due to the rapid reaction of Na2SO3 with dissolved oxygen, further causing an immediate drop in oxygen content ( Fig.15 ).
[0114] Effect Example 8
[0115] Specificity evaluation of microneedle array patch-type electrochemical sensing device.
[0116] The present application also studies several inorganic gases and several endogenous substances distributed in the environment, including inorganic electrolytes, nutrients, and immune proteins, to evaluate the specificity of the microneedle array patch electrochemical sensing device. The amperometric response of the sensor device under 150 mmHg oxygen standard solution and oxygen solution with physiological levels of relevant interfering compounds (50 mmHg CO2, 680 mmHg N2, 3 mg / mL KCl, 0.9% NaCl, 12 mg / mL IgG, 140 mg / dL glucose, and 15 mg / dL lactate) is shown in Figure 2. Fig.16The results clearly show that the effects of these potential interferences on the oxygen response are negligible, indicating that the as-prepared device has good selectivity.
[0117] Effect Example 9
[0118] Accuracy testing of microneedle array patch-type electrochemical sensing devices.
[0119] The accuracy of the microneedle array patch electrochemical sensing device (MNAP) was explored by testing a range of dissolved oxygen concentrations using a commercial dissolved oximeter as a control. The test results showed that there was good agreement between the two methods of the proposed MNAP and the commercial instrument ( Fig.17 ). Subsequently, the good stability of the fabricated sensor array was studied by continuously detecting 150 mmHg oxygen for 7 days. The results showed that the consistency between each test was good, with a relative standard deviation (RSD) of 1.8%, and there was no significant decrease in the response after 7 days of use compared with the first test response ( Fig.18 ).
[0120] Effect Example 10
[0121] Application of microneedle array patch electrochemical sensor device in human motion monitoring.
[0122] In a real-life subcutaneous oxygen monitoring procedure, a microneedle array electrochemical sensor (NMAP) patch was worn on the upper arm of healthy subjects while performing continuous low-intensity exercise ( Fig.19 a) In the process of exercise, the oxygen content, heart rate, blood oxygen saturation and other indicators of the body are obtained intermittently online. Fig.19 As can be seen in b, when the exercise lasted for 40 minutes, the oxygen content in the interstitial fluid (ISF) increased significantly by about 33.88% compared with the resting state, the heart rate reached 126 times / min, and the oxygen saturation increased by about 2.10%, indicating that the subjects' oxygen supplementation and consumption may have reached a relatively balanced state and achieved the best oxygen supply. However, when the participants continued to exercise for 60 minutes, the ISF oxygen partial pressure dropped significantly by about 37.27% compared with the resting state, the heart rate reached or even exceeded 140 times / min, and the blood oxygen saturation dropped by about 1.03%. The subjects experienced symptoms such as sweating and shortness of breath, indicating that the oxygen supply could no longer meet the body's oxygen consumption, indicating that exercise produced excessive oxygen consumption. Within 30 minutes of rest after exercise, the volunteers' oxygen partial pressure, oxygen saturation and heart rate gradually returned to their original basal values. This shows that MNAP has a significant ability to accurately and continuously track the dynamic changes in oxygen content in the body.
[0123] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.
Claims
1. A microneedle electrode array, characterized in that: It comprises a plurality of working electrodes, counter electrodes and reference electrodes; each of the working electrodes is uniformly arranged around the counter electrode with the counter electrode as the center, the reference electrode is arranged at intervals from any of the working electrodes, and the reference electrode is arranged at intervals from the counter electrode; Any of the working electrode and the counter electrode comprises a first metal microneedle and a noble metal layer modified on the surface of the first metal microneedle; The reference electrode comprises a second metal microneedle spaced apart from any of the first metal microneedles and a silver / silver chloride layer modified on the surface of the second metal microneedle; The tip surfaces of the working electrode, the counter electrode and the reference electrode are all provided with a swelling resin layer for isolating the external environment, and the swelling resin layer presents a three-dimensional porous structure after absorbing water.
2. The microneedle electrode array according to claim 1, characterized in that: The middle surfaces of the working electrode, the counter electrode and the reference electrode are all provided with an insulating layer, and the middle portion is a region located 2 to 4 mm away from the tip portion and having a width of 2 to 3 mm.
3. The microneedle electrode array according to claim 2, characterized in that: The thickness of the swelling resin layer is 20 to 30 μm.
4. The microneedle electrode array according to claim 3, characterized in that: The noble metal layer comprises a gold layer and / or a platinum layer; and / or, The diameters of the first metal microneedle and the second metal microneedle are both 0.12 to 0.3 mm; and / or, The total number of the first metal microneedles and the second metal microneedles is 4 to 10; and / or, The distance between each two of the first metal microneedles is 2 to 6 mm; and / or, The first metal microneedle and the second metal microneedle are both selected from one of a steel needle, a silver needle, a silver-plated needle, a gold needle, and a gold-plated needle.
5. The microneedle electrode array according to claim 4, characterized in that: The insulating layer is an epoxy resin layer; and / or, The noble metal layer is a gold layer; and / or, The diameters of the first metal microneedle and the second metal microneedle are both 0.16 to 0.25 mm; and / or, The total number of the first metal microneedles and the second metal microneedles is 6 to 8; and / or, The distance between each two of the first metal microneedles is 3 to 5 mm; and / or, The first metal microneedle is a steel needle; and / or, The second metal microneedle is a silver-plated needle or a silver needle; and / or, The swelling resin layer is selected from a polymer of polymethyl vinyl ether / maleic acid copolymer and polyethylene glycol.
6. A microneedle array patch type sensing device, comprising a microneedle electrode array, characterized in that: The microneedle electrode array is the microneedle electrode array according to any one of claims 1 to 5.
7. The microneedle array patch type sensing device according to claim 6, characterized in that: include: substrate; fixing the microneedle electrode array arranged on the substrate; An electrochemical workstation, wherein the electrochemical workstation is provided with a through hole; The substrate comprises a resin plate, an adhesive layer and a gas barrier layer connected in sequence; the side of the resin plate facing away from the microneedle electrode array is connected to the electrochemical workstation, and the microneedle electrode array is electrically connected to the electrochemical workstation through the through hole.
8. The microneedle array patch type sensing device according to claim 7, characterized in that: The adhesive layer is selected as a nonwoven fabric layer.
9. The microneedle array patch type sensing device according to claim 7, characterized in that: The gas barrier layer is selected from one of polyethylene film, polyvinylidene chloride film, chlorinated polyvinyl chloride film and polytetrafluoroethylene film.
10. The microneedle array patch type sensing device according to claim 9, characterized in that: The gas barrier layer is selected as a polyvinylidene chloride film.
Citation Information
Cited By
Microneedle electrode array, preparation method and microneedle array patch type sensing device
CN117379048A