High-reflection and high-reliability photovoltaic white film

By designing a high-resistance and reliable white film on the photovoltaic module, using a pyramid structure and a double-sided fluorine-containing weathering layer, the problems of high self-destruction rate and poor film reliability on the back of the photovoltaic module are solved, and the effect of power gain and cost reduction is achieved .

CN221940361UActive Publication Date: 2024-11-01CHANGZHOU SWICK NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202420107221.8
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2024-01-17
Publication Date
2024-11-01
Estimated Expiration
2034-01-17

AI Technical Summary

Technical Problem

The white glazed glass on the back of the existing photovoltaic module has a high self-destruction rate, which limits the thinning of the glass thickness. The ordinary white film has a relatively simple structure, poor reliability, and low power gain, making it difficult to meet the needs of the component's power gain and aesthetic appearance. Increase production costs.

Method used

A high-reverse and high-reliability white film was designed, including an adhesive layer, a white weathering layer, a carrier layer and a structural layer. The structural layer is a multi-pyramid structure, using UV glue and a double-sided fluorine-containing weathering layer, through high-precision engraving and UV curing technology, applied to the gaps and edges of photovoltaic modules.

Benefits of technology

The power gain of photovoltaic modules is improved, weather resistance is enhanced, and the glass thickness is reduced through alternative glaze plating processes, reducing production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN221940361U_ABST
    Figure CN221940361U_ABST
Patent Text Reader

Abstract

The utility model provides a high-reflection high-reliability photovoltaic white film which sequentially comprises a bonding layer, a first white weather-proof layer, a carrier layer, a structural layer and a second white weather-proof layer, the first white weather-proof layer is arranged on one side of the carrier layer, the structural layer is of a plurality of isosceles triangle structures, and the second white weather-proof layer is arranged on the other side of the carrier layer. The isosceles triangle structure is arranged on the other side of the carrier layer, and the second white weather-proof layer is arranged on one side of the second white weather-proof layer; compared with a conventional common white film of glazed glass, the white film provided by the utility model has the advantages that the surface of the white film is provided with the microstructure layer which has a certain directional reflection effect, the power gain of an assembly is more obvious, and compared with the conventional common white film, the white film provided by the utility model is protected by the double-sided fluorine-containing weather-proof layer, so that the service life of the assembly is prolonged. In addition, the white pasting film in the embodiment can replace a glaze plating process, so that glaze plating is not needed for the glass, the thickness of the glass can be further reduced, and the production cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The utility model relates to the technical field of photovoltaics, in particular to a high-reflective and high-reliability white photovoltaic film. Background Art

[0002] Solar energy is a green and environmentally friendly renewable energy. With the increase of global population and the dependence and large-scale consumption of today's mainstream non-renewable fossil fuels, the world is not only worried about energy depletion, but also about environmental pollution. At the same time, there is an urgent need to develop new green and environmentally friendly renewable energy. Today, based on the photovoltaic principle, single-crystal silicon and polycrystalline silicon photovoltaic cell modules that use sunlight to generate power have become very mature.

[0003] In recent years, the photovoltaic industry has developed rapidly, industry requirements have continued to increase, and cost reduction and efficiency improvement have become the key tasks of major component manufacturers.

[0004] At present, the mainstream glass on the back of photovoltaic modules is white glazed glass. The white glaze reflects the sunlight between the cells to increase the module power. The white grid style also further beautifies the appearance of the module. However, with the demand of module manufacturers to reduce costs, the glass thickness is getting thinner and thinner, but the self-explosion rate of glazed glass itself is higher than that of conventional glass, which limits the thinning of the glass. The other type is ordinary white film, which is mainly a glue layer and a carrier layer. It has a simpler structure, poor reliability, and low power gain.

[0005] Therefore, it is necessary to develop a film that can not only meet the power gain and aesthetic requirements of the components, but also reduce the thickness of the glass to achieve the purpose of cost reduction. Utility Model Content

[0006] The utility model provides a high-reflective and high-reliability white photovoltaic film to solve the above problems.

[0007] In order to achieve the above-mentioned purpose, an embodiment of the utility model provides a high-reflective and high-reliability white photovoltaic film, which comprises in sequence: an adhesive layer, a white weather-resistant layer 1, a carrier layer, a structural layer and a white weather-resistant layer 2, the carrier layer having a first surface and a second surface corresponding to the first surface, the white weather-resistant layer 1 is bonded to the first surface, the structural layer is bonded to the second surface, the structural layer is a plurality of isosceles triangle structures, and the white film is applied between the gaps between the cell sheets of the photovoltaic module, on the edges around the photovoltaic module and on the back glass of the photovoltaic module.

[0008] Furthermore, the adhesive layer is 70 μm-100 μm.

[0009] Furthermore, the structural layer is a plurality of pyramid structures, the height of the pyramid structures is 10 μm-20 μm, and the length of the base of the pyramid structures is 20 μm-40 μm.

[0010] Furthermore, the distance between two adjacent pyramid structures is 0 μm-5 μm.

[0011] Furthermore, the material of the structural layer is UV glue.

[0012] Furthermore, the carrier layer has a thickness of 40 μm-80 μm.

[0013] Furthermore, the material of the carrier layer is transparent PET.

[0014] Furthermore, the thickness of the white weather-resistant layer 1 is the same as the thickness of the white weather-resistant layer 2, and the thickness of the white weather-resistant layer 1 and the white weather-resistant layer 2 is 10 μm-20 μm.

[0015] Compared with the prior art, the embodiments of the present invention have the following beneficial effects:

[0016] 1. Compared with the conventional glazed glass ordinary white film, the white film in this embodiment has a microstructure layer on the surface which has a certain directional reflection effect, and the power gain of the component is more obvious compared with the conventional ordinary white film;

[0017] 2. The white film in this embodiment is protected by a double-sided fluorine-containing weather-resistant layer, which has better weather resistance;

[0018] 3. In addition, the white film in this embodiment can replace the glazing process, so that the glass does not need to be glazed, and the thickness of the glass can be further reduced, thereby reducing the production cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] The utility model is further described below in conjunction with the accompanying drawings and embodiments.

[0020] Figure 1 It is a structural diagram of an optimal embodiment of a high-reflective and high-reliability photovoltaic white film in the prior art;

[0021] Figure 2 It is a schematic diagram of the top view of the structure layer of the utility model;

[0022] Figure 3 It is a cross-sectional view of the optimal embodiment of the structural layer and the carrier layer of the utility model.

[0023] Among them, 1. Adhesive layer; 2. White weather-resistant layer 1; 3. Carrier layer; 4. Structural layer; 5. White weather-resistant layer 2. DETAILED DESCRIPTION

[0024] Now the utility model is further described in detail with reference to the accompanying drawings. These drawings are simplified schematic diagrams, which only illustrate the basic structure of the utility model in a schematic manner, and therefore only show the components related to the utility model.

[0025] See also Figures 1 to 3 , Figure 1 It is a structural diagram of an optimal embodiment of a high-reflective and high-reliability photovoltaic white film in the prior art; Figure 2 It is a schematic diagram of the top view of the structure layer of the utility model; Figure 3 This is a cross-sectional view of the optimal embodiment of the structural layer and the carrier layer of the utility model. Figures 1 to 3 As shown, the utility model provides a high-reflective and high-reliability white photovoltaic film, which comprises in sequence: an adhesive layer, a white weather-resistant layer 1, a carrier layer, a structural layer and a white weather-resistant layer 2, the carrier layer having a first surface and a second surface corresponding to the first surface, the white weather-resistant layer 1 is bonded to the first surface, the structural layer is bonded to the second surface, the structural layer is a plurality of isosceles triangle structures, and the white film is applied between the gaps between the cells of the photovoltaic module, on the edges around the photovoltaic module and on the back glass of the photovoltaic module.

[0026] The adhesive layer 1 is EVA, EEA, any one or a combination of two, and a certain amount of cross-linking agent, coupling agent, auxiliary cross-linking agent, ultraviolet absorber, and antioxidant are added. By weight, EVA or EEA is 92%-99.5%, cross-linking agent 0.1%-2%, coupling agent: 0.1%-2%, auxiliary cross-linking agent 0.1%-2%, ultraviolet absorber 0.1%-1%, and antioxidant 0.1%-1%.

[0027] The above-mentioned structural layer 4 is prepared by pre-preparing the pyramid structure on the surface of the pressure roller, and then coating the surface of the carrier layer 3 with ultraviolet curing resin and passing through the pressure roller, and at the same time performing ultraviolet curing through an ultraviolet lamp, so that the multiple pyramid structures are attached to the carrier layer 3 to form the structural layer 4.

[0028] As shown in Table 1, which is a relationship table between the thickness of the adhesive layer and the peeling strength, as the thickness of the adhesive layer 1 increases, the peeling strength between the adhesive layer 1 and the glass increases.

[0029]

[0030] Table 1

[0031] The results show that when the thickness of the adhesive layer 1 is greater than 70 μm, the design requirements are met. When the thickness is greater than 100 μm, the peel strength does not increase significantly. Therefore, the design thickness of the adhesive layer 1 is 70 μm-100 μm.

[0032] The material of the structural layer 4 is UV glue.

[0033] As shown in Table 2, Table 2 is a table showing the relationship between microstructure shape and component power gain.

[0034]

[0035] Table 2

[0036] Comparing the power gains of several structures tested, the pyramid shape has obviously higher power gain, so the structural layer 4 is a plurality of pyramid structures.

[0037] As described in Table 3, which is a graph showing the relationship between the pyramid distance and the component power gain, the height of the pyramid structure is 10 μm-20 μm, and the length of the base of the pyramid structure is 20 μm-40 μm.

[0038]

[0039] Table 3

[0040] When the distance between the pyramids is greater than 5μm, the power gain is reduced to less than 1% compared with float glass, which does not meet the design requirements (power gain>1%). Therefore, the distance between the pyramids is designed to be 0-5μm.

[0041] The thickness of the white weather-resistant layer 1 2 is the same as the thickness of the white weather-resistant layer 2 5 , as described in Table 4. Table 4 is a table showing the relationship between the appearance of the white weather-resistant layer 1 2 and the white weather-resistant layer 2 5 and PCT after 48h.

[0042]

[0043] Table 4

[0044] As shown in Table 4, the thicker the thickness of the white weather-resistant layer 2 and the white weather-resistant layer 25, the better the weather resistance (the design requires no delamination after PCT 48h). When the thickness is 10μm, the white film has no delamination or other appearance abnormalities after PCT 48h, so the thickness of the white weather-resistant layer 2 and the white weather-resistant layer 25 are designed to be 10μm-20μm.

[0045] The white weather-resistant layer 1 2 and the white weather-resistant layer 2 5 are fluorine-containing coatings, and the materials of the white weather-resistant layer 1 2 and the white weather-resistant layer 2 5 include: 78.8%-98.8% fluororesin, 0.1%-5% silica, 0.1%-5% curing agent and 0.1%-5% anti-ultraviolet agent, 0.1%-5% light stabilizer, and 0.8%-1.2% white filler.

[0046] As shown in Table 5, Table 5 shows the relationship between the titanium dioxide content and the reflectivity at a thickness of 10 μm.

[0047]

[0048] Table 5

[0049] When the thickness of the white weather-resistant layer 1 2 and the white weather-resistant layer 2 5 is 10 μm, the titanium dioxide content needs to be greater than 0.8% so that the reflectivity can meet the design requirement, that is, greater than 85%. Therefore, the titanium dioxide content in the white weather-resistant layer 1 2 and the white weather-resistant layer 2 5 is 0.8%-1.2%.

[0050] The preparation method of the white film comprises the following steps:

[0051] Step 1 Preparation of structural layer 4:

[0052] A pyramid-shaped microstructure is prepared on the surface of a pressure roller by high-precision engraving equipment, UV glue is coated on the surface of the carrier layer 3, and UV curing is performed while passing through the glue roller to obtain a structural layer 4 with excellent strength.

[0053] Step 2 Preparation of white weather-resistant layer 1 2 and white weather-resistant layer 2 5:

[0054] Component A: 90% fluororesin, 0.2% silicon dioxide, 1% curing agent, 0.5% anti-ultraviolet agent, 0.1% light stabilizer, and 0.8% titanium dioxide are mixed and stirred in a stirring kettle. The mixture is wet-coated on the back of the carrier layer 3 and the surface of the structural layer 4, and then heat-cured at 100-220°C.

[0055] Step 3 Preparation of bonding layer 1:

[0056] Adhesive layer 1 components: by weight, EVA resin 82.2%, crosslinking agent 0.7%, coupling agent 0.4%, auxiliary crosslinking agent 0.6%, UV absorber 0.5%, antioxidant 0.5% are weighed. The above components are mixed evenly in a stirring kettle, and the formula is melt-coated on the white weather-resistant layer 1 2 by a single-screw coater.

[0057] Embodiment 1

[0058] A pyramid-shaped microstructure is prepared on the surface of the pressure roller by high-precision engraving equipment, and the distance between the base edges of adjacent pyramids is 1 μm. UV glue is coated on the surface of the carrier layer 3, and UV curing is performed while passing through the glue roller to obtain the carrier layer 3 with the structural layer 4.

[0059] 97.2% of fluororesin, 0.2% of silicon dioxide, 1% of curing agent, 0.5% of anti-ultraviolet agent, 0.2% of light stabilizer and 0.9% of titanium dioxide are mixed and stirred in a stirring kettle. The mixture is wet coated on the back of the carrier layer 3 and the surface of the structural layer 4, and then heat cured at 100-220°C. The coating thickness is 12 μm.

[0060] According to weight, 97.5% EVA resin, 0.7% crosslinking agent, 0.4% coupling agent, 0.6% auxiliary crosslinking agent, 0.4% UV absorber, and 0.4% antioxidant are weighed. The above components are mixed evenly in a stirring kettle, and the formula is melt-coated on the white weather-resistant layer 2 by a single-screw coater, and the coating thickness is 75μm.

[0061] The highly reflective and weather-resistant white photovoltaic film was tested and passed the PCT reliability test with a reflectivity of 88%, meeting the design requirements.

[0062] Example 2

[0063] A pyramid-shaped microstructure is prepared on the surface of the pressure roller by high-precision engraving equipment, and the distance between the base edges of adjacent pyramids is 2 μm. UV glue is coated on the surface of the carrier layer 3, and UV curing is performed while passing through the glue roller to obtain the carrier layer 3 with the structural layer 4.

[0064] 97.4% of fluororesin, 0.2% of silicon dioxide, 0.8% of curing agent, 0.4% of anti-ultraviolet agent, 0.2% of light stabilizer and 1% of titanium dioxide are mixed and stirred in a stirring kettle. The coating is applied on the back of the carrier layer 3 and the surface of the structural layer 4 by wet method and then heat cured at 100-220°C. The coating thickness is 11 μm.

[0065] According to weight, 97.7% EVA resin, 0.5% crosslinking agent, 0.5% coupling agent, 0.4% crosslinking agent, 0.5% UV absorber, and 0.4% antioxidant are weighed. The above components are mixed evenly in a stirring kettle, and the formula is melt-coated on the white weather-resistant layer 2 by a single-screw coater, and the coating thickness is 80 μm.

[0066] The highly reflective and weather-resistant white photovoltaic film was tested and passed the PCT reliability test with a reflectivity of 89%, meeting the design requirements.

[0067] Example 3

[0068] A pyramid-shaped microstructure is prepared on the surface of the pressure roller by high-precision engraving equipment, and the distance between the base edges of adjacent pyramids is 3 μm. UV glue is coated on the surface of the carrier layer 3, and UV curing is performed while passing through the glue roller to obtain the carrier layer 3 with the structural layer 4.

[0069] 97.5% of fluororesin, 0.2% of silicon dioxide, 0.6% of curing agent, 0.4% of anti-ultraviolet agent, 0.2% of light stabilizer and 1.1% of titanium dioxide are mixed and stirred in a stirring kettle. The mixture is wet coated on the back of the carrier layer 3 and the surface of the structural layer 4, and then heat cured at 100-220°C. The coating thickness is 15 μm.

[0070] According to weight, 97.9% EVA resin, 0.4% crosslinking agent, 0.4% coupling agent, 0.4% auxiliary crosslinking agent, 0.4% UV absorber, and 0.5% antioxidant are weighed. The above components are mixed evenly in a stirring kettle, and the formula is melt-coated on the white weather-resistant layer 2 by a single-screw coater, and the coating thickness is 77 μm.

[0071] The highly reflective and weather-resistant white photovoltaic film was tested and passed the PCT reliability test with a reflectivity of 90%, meeting the design requirements.

[0072] To sum up, the beneficial effects of the utility model are as follows: compared with the ordinary white film of traditional glazed glass, the surface of the white film in this embodiment has a microstructure layer with a certain directional reflection effect, and the power gain of the component is more obvious; compared with the traditional ordinary white film, the white film in this embodiment is protected by a double-sided fluorine-containing weather-resistant layer and has better weather resistance; in addition, the white film in this embodiment can replace the glazing process, so that the glass does not need to be glazed, and the thickness of the glass can be further reduced, thereby reducing the production cost.

[0073] Based on the above ideal embodiments of the utility model, the relevant staff can make various changes and modifications without deviating from the technical concept of the utility model through the above description. The technical scope of the utility model is not limited to the content of the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. A highly reflective and reliable white photovoltaic film, characterized in that: Including in order: An adhesive layer (1), a first white weather-resistant layer (2), a carrier layer (3), a structural layer (4) and a second white weather-resistant layer (5), wherein the carrier layer (3) has a first surface and a second surface corresponding to the first surface, the first white weather-resistant layer (2) is bonded to the first surface, the structural layer (4) is bonded to the second surface, the structural layer (4) is a plurality of isosceles triangle structures, and the white film is applied between the gaps between the cells of a photovoltaic module, the edges around the photovoltaic module and the back glass of the photovoltaic module.

2. A highly reflective and highly reliable photovoltaic white film as claimed in claim 1, characterized in that: The adhesive layer (1) is 70 μm-100 μm.

3. A highly reflective and highly reliable white photovoltaic film as claimed in claim 2, characterized in that: The structural layer (4) is a plurality of pyramid structures, the height of the pyramid structures is 10 μm-20 μm, and the length of the base of the pyramid structures is 20 μm-40 μm.

4. A highly reflective and highly reliable photovoltaic white film as claimed in claim 3, characterized in that: The distance between two adjacent pyramid structures is 0 μm-5 μm.

5. A highly reflective and highly reliable white photovoltaic film as claimed in claim 4, characterized in that: The material of the structural layer (4) is UV glue.

6. A highly reflective and highly reliable white photovoltaic film as claimed in claim 5, characterized in that: The carrier layer (3) has a thickness of 40 μm-80 μm.

7. A highly reflective and highly reliable photovoltaic white film as claimed in claim 6, characterized in that: The material of the carrier layer (3) is transparent PET.

8. A highly reflective and highly reliable white photovoltaic film as claimed in claim 7, characterized in that: The thickness of the white weather-resistant layer 1 (2) is the same as the thickness of the white weather-resistant layer 2 (5), and the thickness of the white weather-resistant layer 1 (2) and the white weather-resistant layer 2 (5) is 10 μm-20 μm.