Cooling structure, lithium ion battery and electric equipment
By designing a microwave structure cooling structure in lithium-ion batteries, combining heat dissipation materials and polymer materials, the problem of uneven temperature distribution of the battery cell is solved, and the rapid cooling and performance improvement of the battery is achieved.
Patent Information
- Application Number
- CN202323488453.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-20
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2033-12-20
AI Technical Summary
In the high-temperature environment and large-scale charging and discharging conditions, the temperature distribution of the existing lithium-ion batteries is uneven, resulting in lithium-ion evolution in local high temperature areas, affecting battery performance.
Design a cooling structure including heat dissipation material, adopts a microwave structure, by adjusting the length and width of the microwave structure, combining polymer materials, forming a film or coating, and performing partition cooling for different temperature areas.
It realizes rapid local cooling of the battery, avoids electrochemical performance degradation and failure caused by uneven temperature distribution, and improves the cycling performance and safety of the battery.
Smart Images

Figure CN222029156U_ABST
Abstract
Description
Technical Field
[0001] The utility model belongs to the technical field of lithium ion batteries, and specifically relates to a cooling structure, a lithium ion battery and electrical equipment. Background Art
[0002] In a high temperature environment and under high rate charge and discharge conditions, the battery temperature is generally highest in the middle, so lowering the local temperature to make the overall temperature distribution of the battery cell uniform is the key to improving performance. Existing technologies for cooling batteries mostly use additional accessories, structures or other control systems, which puts higher requirements on battery design and is difficult to use universally. Different cooling structures are not set for different temperature zones. Traditional cooling methods all use a unified structure and do not reduce the temperature difference between local areas of the battery cell. This still leads to uneven distribution of the overall problem of the battery cell, affecting battery performance. In severe cases, lithium precipitation will occur in areas with higher battery cell temperatures. Therefore, it is necessary to develop a cooling structure that can achieve zoned cooling for different temperature zones of the battery. Utility Model Content
[0003] In order to solve the technical problem of uneven temperature distribution of existing battery cells during use, the present application provides a cooling structure, a lithium-ion battery and an electrical device.
[0004] In order to solve the above technical problems, this application provides the following technical solutions:
[0005] In a first aspect, the present application provides a cooling structure, wherein the cooling structure comprises a heat dissipation material, and a middle area of the cooling structure is a micro-wave structure.
[0006] In some embodiments, the cooling structure includes a first direction and a second direction, the first direction is the length direction of the cooling structure, the second direction is the width direction of the cooling structure, and the micro-wave structure extends along the first direction or the second direction.
[0007] In some embodiments, a line passing through the center of the cooling structure and perpendicular to the first direction is a first center line, a line passing through the cooling structure and perpendicular to the second direction is a second center line, and the microwave structure is symmetrical about the first center line or the second center line of the cooling structure.
[0008] In some embodiments, in the first direction, the length of the microwave structure accounts for 1 / 5 to 1 / 2 of the length of the cooling structure, and / or, in the second direction, the width of the microwave structure accounts for 1 / 5 to 1 / 2 of the width of the cooling structure.
[0009] In some embodiments, in the first direction or the second direction of the cooling structure, the wavelength of the middle region of the micro-wave structure is smaller than the wavelength of the regions on both sides of the micro-wave structure.
[0010] In some embodiments, the wavelength of the middle area of the micro-wave structure is A, and the wavelength of the areas on both sides of the micro-wave structure is B, satisfying: 0<A≤5mm; 5mm<B≤10mm.
[0011] In some embodiments, the heat dissipation material includes one of paraffin, polylactic acid, polyethylene glycol, and hydrated inorganic salt.
[0012] In some embodiments, the cooling structure further comprises a polymer material, and the polymer material comprises one of polyvinylidene fluoride-hexafluoropropylene copolymer, polyacrylic acid, polyacrylonitrile, polyester, and polyolefin polymers.
[0013] In some embodiments, the mass ratio of the heat dissipation material to the polymer material is (5% to 50%): (50% to 95%).
[0014] In some embodiments, the coating is in the form of a thin film, and the thickness d of the thin film satisfies: 0<d≤2mm.
[0015] In a second aspect, the present application provides a lithium-ion battery, comprising the cooling structure described in the above claims.
[0016] In a third aspect, the present application provides an electrical device comprising the lithium-ion battery described in the above claims.
[0017] The cooling structure provided in the present application has the following technical effects: it can achieve rapid local cooling of the battery, avoiding the degradation of the electrochemical performance and failure of the battery caused by local high temperature and uneven temperature distribution of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] In order to more clearly illustrate the embodiments of the utility model or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the utility model. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0019] The structures, proportions, sizes, etc. illustrated in the drawings of this specification are only used to match the contents disclosed in the specification so as to facilitate understanding and reading by persons familiar with this technology. They are not used to limit the conditions under which the present invention can be implemented, and therefore have no substantive technical significance. Any structural modification, change in proportion or adjustment of size, without affecting the effects and purposes that can be achieved by the present invention, should still fall within the scope of the technical contents disclosed by the present invention.
[0020] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0021] Figure 1 It is a schematic diagram of the cooling structure in some embodiments of the utility model;
[0022] Figure 2 It is a schematic diagram of the cooling structure in some embodiments of the utility model;
[0023] Figure 3 It is a top view of the cooling structure in some embodiments of the utility model;
[0024] Explanation of the accompanying drawings: G: micro-wave structure; A: wavelength of the middle area of the micro-wave structure; B: wavelength of the areas on both sides of the micro-wave structure; C: cooling structure; D: substrate; E: areas on both sides of the micro-wave structure; F: middle area of the micro-wave structure; X: first direction; Y: second direction; H: thickness direction. DETAILED DESCRIPTION
[0025] In order to make the technical problems, technical solutions and beneficial effects solved by the utility model more clear, the utility model is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described here are only used to explain the utility model and are not used to limit the utility model.
[0026] The utility model provides a cooling structure. The cooling structure C comprises a heat dissipation material. The middle area of the cooling structure C is a micro-wave structure G.
[0027] It can be understood that under high-rate charging conditions, the temperature in the middle of the battery cell is higher than the temperature around the battery cell. Excessive temperature of the battery cell will affect the cycle performance of the battery cell, and in severe cases will cause lithium deposition in the battery cell. The cooling structure C provided in the present application sets a micro-wave structure G for the high-temperature area in the middle of the battery cell, increases the reaction area and reaction amount, and achieves rapid cooling of the high-temperature area in the middle of the battery cell, so that the overall temperature distribution of the battery cell is uniform, and different degrees of cooling are achieved in different temperature areas.
[0028] The cooling structure provided in the present application has the following technical effects: it can achieve rapid local cooling of the battery, avoiding the degradation of the electrochemical performance and failure of the battery caused by local high temperature and uneven temperature distribution of the battery.
[0029] Specifically, the cooling structure may be a cooling coating or a cooling film.
[0030] It can be understood that the cooling coating can be applied on the inner wall of the aluminum shell of the aluminum shell battery, the inner film of the aluminum-plastic film packaging of the soft-pack battery, the protective film of the battery cell packaging, and the surface of a variety of packaging materials. It can also be processed together with other packaging film materials in the battery, such as large-surface protective film and aluminum-plastic film. The application scenarios are flexible, and the materials in the substrate will not react with the electrolyte. It can achieve rapid cooling at high temperatures and improve the cycle performance of the battery.
[0031] When the cooling structure is a cooling coating, it can be realized in battery production without the need for additional accessories and equipment support. The coating can be applied on the inner wall of the aluminum shell of the aluminum shell battery, the inner film of the aluminum-plastic film packaging of the soft-pack battery, the protective film of the battery cell packaging, and any packaging film in the battery cell.
[0032] In some embodiments, the cooling structure C includes a first direction X and a second direction Y, wherein the first direction X is the length direction of the cooling structure C, and the second direction Y is the width direction of the cooling structure C. The micro-wave structure extends along the first direction X or the second direction Y.
[0033] Specifically, refer to Figure 1 and Figure 2 , the cooling structure C also includes the thickness direction H.
[0034] Specifically, refer to Figure 3 The cooling structure C includes a first direction X and a second direction Y, the first direction X is the length direction of the cooling structure, and the second direction Y is the width direction of the cooling structure. The micro-wave structure G extends along the first direction X or the second direction Y. It means that when the cooling structure C is a rectangle, the first direction X is the length direction of the cooling structure C, and the micro-wave structure G exists in the middle area of the length direction of the cooling structure C, and the wave form of the micro-wave structure G extends in the first direction X; or, the second direction Y is the width direction of the cooling structure C, and the micro-wave structure G exists in the middle area of the width direction of the cooling structure C, and the wave form of the micro-wave structure G extends in the second direction Y.
[0035] In some embodiments, a line passing through the center of the cooling structure C and perpendicular to the first direction X is a first center line, a line passing through the cooling structure C and perpendicular to the second direction Y is a second center line, and the micro-wave structure G is symmetrical about the first center line or the second center line of the cooling structure C.
[0036] It can be understood that the center of the cooling structure C refers to the intersection of two diagonal lines of the cooling structure C on the XY plane, the first center line passes through the center and is perpendicular to the first direction X; the second center line passes through the center and is perpendicular to the second direction Y.
[0037] It can be understood that the micro-wave structure G is symmetrical about the first center line or the second center line. Corresponding to the battery cell, it can better correspond to the high temperature area in the battery cell, quickly reduce the temperature of the high temperature area, reduce the overall temperature difference of the battery cell, and improve the electrochemical performance and cycle performance of the battery.
[0038] In some preferred embodiments, in the first direction X, the length of the microwave structure G accounts for 1 / 5 to 1 / 2 of the length of the cooling structure C, and / or, in the second direction Y, the width of the microwave structure G accounts for 1 / 5 to 1 / 2 of the width of the cooling structure C.
[0039] Specifically, in the first direction X, the length of the micro-wave structure G accounts for 1 / 5 to 1 / 2 of the length of the cooling structure C, which can be but not limited to 1 / 5, 3 / 10, 2 / 5, 1 / 2, etc. The extension direction of the micro-wave structure G can be the first direction X or the second direction Y; the longer the length of the micro-wave structure G accounts for the length of the cooling structure C, the larger the area occupied by the micro-wave structure G on the cooling structure C, the more the reaction area and reaction amount are increased, and the faster the cooling speed, so the length of the micro-wave structure G accounts for the length of the cooling structure C cannot be less than 1 / 5; the smaller the length of the micro-wave structure G accounts for the length of the cooling structure C, the more effectively it can correspond to the higher temperature area in the battery cell, reduce the temperature of the high temperature area, reduce the overall temperature difference of the battery, ensure that the overall temperature of the battery cell is more uniform, and the cooling is more efficient, so the length of the micro-wave structure G accounts for the length of the cooling structure C cannot be greater than 1 / 2. The length of the micro-wave structure G accounts for 1 / 5 to 1 / 2 of the length of the coating C, which can not only ensure the cooling reaction area, but also more effectively reduce the overall temperature difference of the battery cell and improve the performance of the battery cell.
[0040] It can be understood that in the second direction Y, the width of the micro-wave structure G accounts for 1 / 5 to 1 / 2 of the width of the cooling structure C, which is the same as the above statement.
[0041] It can be understood that in the first direction X and the second direction Y, the length and width of the micro-wave structure G are 1 / 5 to 1 / 2 of the length and width of the cooling structure C, respectively, as described above.
[0042] In some embodiments, in the first direction X or the second direction Y of the cooling structure C, the wavelength A of the middle region F of the micro-wave structure is smaller than the wavelength B of the regions E on both sides of the micro-wave structure.
[0043] It can be understood that different wavelengths of the micro-wave structure G can increase different reaction areas and achieve different degrees of cooling. Because the temperature of the middle area of the battery cell is high, and the temperature of the two sides E of the middle area is lower than the temperature of the center F of the middle area, setting the wavelength A of the middle area F of the micro-wave structure G smaller than the wavelength B of the two side areas E can increase different reaction areas in a targeted manner according to different temperatures. The area with high temperature on the battery cell corresponds to the small wavelength of the middle area F of the micro-wave area G, the large reaction area, and the fast cooling speed; the area with slightly higher temperature on the battery cell corresponds to the large wavelength of the two side areas E of the micro-wave area G, the slightly increased reaction area, and the slightly faster cooling speed, thereby ensuring that the overall temperature difference of the battery cell is reduced and the stability of the overall performance of the battery cell is maintained.
[0044] It can be understood that the sizes of the middle area F and the two side areas E of the micro-wave structure correspond to different temperature areas of the battery cell, and therefore need to be changed according to different battery models, which is not specifically limited here.
[0045] In some preferred embodiments, the wavelength A of the middle region F of the micro-wave structure and the wavelength B of the regions E on both sides of the micro-wave structure satisfy: 0<A≤5mm; ; 5mm<B≤10mm.
[0046] Specifically, the wavelength A of the middle region F of the micro-wave structure can be, but not limited to, 0.5 mm, 1 mm, 1.5 mm, 2 mm, 2.5 mm, 3 mm, 3.5 mm, 4 mm, 5 mm, etc.; the wavelength B of the middle region E of the micro-wave structure can be, but not limited to, 5.5 mm, 6 mm, 6.5 mm, 7 mm, 7.5 mm, 8 mm, 8.5 mm, 9 mm, 10 mm, etc. The shorter the wavelength of the micro-wave structure G, the larger the reaction area, the faster the cooling speed, the longer the wavelength, the lower the difficulty of production in the process, and the wavelength of the micro-wave structure G is between 0 and 10 mm, which not only ensures the feasibility of the process, but also improves the cooling rate.
[0047] In some embodiments, the heat dissipation material includes one of paraffin, polylactic acid, polyethylene glycol, and hydrated inorganic salt.
[0048] Specifically, paraffin has a large heat capacity and a melting point of 50°C to 70°C. It will melt and cool down when heated; the glass transition temperature of polylactic acid is between 55°C and 65°C, and the glass transition process absorbs heat and cools down; polyethylene glycol is an organic solid-solid phase change material (the solid-state ordered molecular connection structure becomes a solid-state disordered molecular connection structure), and its phase change temperature will increase with the increase of polymerization degree. When its phase change temperature (37°C to 41°C) is reached, a solid-solid phase change will occur, absorbing heat, thereby reducing the temperature of the battery cell surface; hydrated inorganic salts have a suitable phase change temperature (generally 20°C to 50°C) and a large phase change latent heat, which can effectively dissipate heat.
[0049] Specifically, the hydrated inorganic salts include CaCl2·6H2O, Na2SO4·10H2O, Na2HPO4·12H2O and the like.
[0050] In some embodiments, the cooling structure further comprises a polymer material, and the polymer material comprises one of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP), polyacrylic acid (PAA), polyacrylonitrile (PAN), polyester, and polyolefin polymers.
[0051] Specifically, polyesters include polymethyl methacrylate, polyethylene glycol diacrylate, etc.; polyolefin polymers include polyethylene, polypropylene, etc.
[0052] Specifically, the heat dissipation material can be combined with the polymer material to prepare a cooling coating or a cooling insulating film, which can be stably present in the battery to further improve the safety performance of the battery.
[0053] In some embodiments, the mass ratio of the heat dissipation material to the polymer material is (5% to 50%): (50% to 95%).
[0054] Specifically, by changing the mass ratio of heat dissipation material and polymer material, the battery cells with different cooling requirements can be matched. The mass ratio of heat dissipation material and polymer material for battery cells with weak cooling requirements is small; the mass ratio of heat dissipation material and polymer material for battery cells with strong cooling requirements is large. At the same time, the addition of polymer material can change the morphological structure of the coating, and the heat dissipation material and polymer material can be combined to form a thin film, which can be used for packaging film, aluminum-plastic film, protective film or other internal and external packaging materials of battery cells, etc. It is widely applicable, safe and stable.
[0055] In some embodiments, the thickness d of the cooling structure C satisfies: 0<d≤2mm.
[0056] Specifically, the thickness d of the cooling structure C is 0-2 mm, and specifically can be but not limited to 0.1 mm, 0.3 mm, 0.5 mm, 1 mm, 1.5 mm, 2 mm, etc. When the thickness of the cooling structure C is within this range, it can effectively achieve rapid cooling without affecting the overall performance of the battery.
[0057] In a second aspect, the present application provides a lithium-ion battery, comprising the cooling structure C described above.
[0058] The cooling structure C provided in the present application can be a cooling coating, which can be coated on the inner wall of the aluminum shell of an aluminum shell battery, the inner film of the aluminum-plastic film packaging of a soft-pack battery, the protective film of the battery cell packaging, and any packaging film in the battery cell; the cooling structure can also be prepared into a film, and the cooling film can be processed together with the aluminum-plastic film or other protective films in the battery cell. The thickness and amount of the coating and the film can be adjusted according to the battery cell design and actual use, and will not have other negative effects on battery production and performance, and can be widely used.
[0059] The substrate D can be the inner and outer walls of an aluminum shell, an aluminum-plastic film packaging film, a battery cell, a battery cell packaging protective film, and other materials that need to be cooled.
[0060] It should be noted that the lithium-ion battery provided in the present application includes the above-mentioned cooling coating and / or cooling film.
[0061] In a fourth aspect, the present application provides an electrical device comprising the lithium-ion battery described above.
[0062] Specifically, the electrical equipment may be an electric car, an electric motorcycle, an electric bicycle, a mobile power supply, a drone, a mobile phone, a computer, a camera, an electric tool, a smart home or a wearable device.
[0063] The electrical equipment provided in the embodiment of the present application includes the lithium-ion battery described above. The lithium-ion battery can achieve different degrees of cooling according to the different temperatures of the battery cells. The battery has high charging and discharging efficiency, good safety and long cycle life, which helps to improve the safety and cycle stability of the electrical equipment and is beneficial to the long-term use of the electrical equipment.
[0064] The present invention is further described in detail below through embodiments.
[0065] Example 1
[0066] This embodiment is used to illustrate the cooling structure, lithium-ion battery and electrical equipment disclosed in the utility model, and includes the following steps:
[0067] 1. Preparation of cooling structure: 20% polylactic acid and 80% polypropylene are mixed and the cooling structure is prepared by solution casting method; the cooling structure prepared has a length of 120 mm and a width of 60 mm, and has a micro-wave structure on the cooling structure, which is prepared by molds of different sizes, with a length of 40 mm and a width of 30 mm; the wavelength A of the middle area of the micro-wave structure is 3 mm, and the wavelength B of the areas on both sides of the micro-wave structure is 8 mm.
[0068] 2. Preparation of lithium-ion batteries: Wrap the prepared coating film on the large surface of the battery core, and then complete the battery preparation according to the processes of casing, packaging, liquid injection, formation, sealing, and capacity division.
[0069] Example 2
[0070] The difference between Example 2 and Example 1 is that the size of the micro-wave structure is different, and the rest is the same as Example 1. The specific steps are as follows:
[0071] 1. Preparation of cooling structure: 20% polylactic acid and 80% polypropylene are mixed and coated by solution casting method to prepare cooling structure; the cooling structure prepared has a length of 120 mm and a width of 60 mm, and has a micro-wave structure on the cooling structure, the length of the micro-wave structure is 24 mm, and the width of the micro-wave structure is 30 mm; the wavelength A of the middle area of the micro-wave structure is 3 mm, and the wavelength B of the areas on both sides of the micro-wave structure is 8 mm.
[0072] Example 3
[0073] The difference between Example 3 and Example 1 is that the size of the micro-wave structure is different, and the rest is the same as Example 1. The specific steps are as follows:
[0074] 1. Preparation of cooling structure: 20% polylactic acid and 80% polypropylene are mixed and coated by solution casting method to prepare cooling structure; the cooling structure prepared has a length of 120 mm and a width of 60 mm, and has a micro-wave structure on the cooling structure, the length of the micro-wave structure is 60 mm, and the width of the micro-wave structure is 30 mm; the wavelength A of the middle area of the micro-wave structure is 3 mm, and the wavelength B of the areas on both sides of the micro-wave structure is 8 mm.
[0075] Example 4
[0076] The difference between Example 4 and Example 1 is that the size of the micro-wave structure is different, and the rest is the same as Example 1. The specific steps are as follows:
[0077] 1. Preparation of cooling structure: 20% polylactic acid and 80% polypropylene are mixed and coated by solution casting method to prepare cooling structure; the cooling structure prepared has a length of 120 mm and a width of 60 mm, and has a micro-wave structure on the cooling structure, the length of the micro-wave structure is 40 mm, and the width of the micro-wave structure is 12 mm; the wavelength A of the middle area of the micro-wave structure is 3 mm, and the wavelength B of the areas on both sides of the micro-wave structure is 8 mm.
[0078] Example 5
[0079] The difference between Example 5 and Example 1 is that the size of the micro-wave structure is different, and the rest is the same as Example 1. The specific steps are as follows:
[0080] 1. Preparation of cooling structure: 20% polylactic acid and 80% polypropylene are mixed and coated by solution casting method to prepare cooling structure; the prepared cooling structure has a length of 120 mm and a width of 60 mm, and has a micro-wave structure on the cooling structure, the length of the micro-wave structure is 40 mm, and the width of the micro-wave structure is 20 mm; the wavelength A of the middle area of the micro-wave structure is 3 mm, and the wavelength B of the areas on both sides of the micro-wave structure is 8 mm.
[0081] Example 6
[0082] The difference between Example 6 and Example 1 is that the wavelengths of the middle area and the two side areas of the micro-wave structure are different, and the rest is the same as Example 1. The specific steps are as follows:
[0083] 1. Preparation of cooling structure: 20% polylactic acid and 80% polypropylene are mixed and coated by solution casting method to prepare cooling structure; the prepared cooling structure has a length of 120 mm and a width of 60 mm, and has a micro-wave structure on the cooling structure, the length of the micro-wave structure is 40 mm, and the width of the micro-wave structure is 30 mm; the wavelength A of the middle area of the micro-wave structure is 1 mm, and the wavelength B of the areas on both sides of the micro-wave structure is 8 mm.
[0084] Example 7
[0085] The difference between Example 7 and Example 1 is that the wavelengths of the middle area and the two side areas of the micro-wave structure are different, and the rest is the same as Example 1. The specific steps are as follows:
[0086] 1. Preparation of cooling structure: 20% polylactic acid and 80% polypropylene are mixed and coated by solution casting method to prepare cooling structure; the prepared cooling structure has a length of 120 mm and a width of 60 mm, and has a micro-wave structure on the cooling structure, the length of the micro-wave structure is 40 mm, and the width of the micro-wave structure is 30 mm; the wavelength A of the middle area of the micro-wave structure is 5 mm, and the wavelength B of the areas on both sides of the micro-wave structure is 8 mm.
[0087] Example 8
[0088] The difference between Example 8 and Example 1 is that the wavelengths of the middle area and the two side areas of the micro-wave structure are different, and the rest is the same as Example 1. The specific steps are as follows:
[0089] 1. Preparation of cooling structure: 20% polylactic acid and 80% polypropylene are mixed and coated by solution casting method to prepare cooling structure; the prepared cooling structure has a length of 120 mm and a width of 60 mm, and has a micro-wave structure on the cooling structure, the length of the micro-wave structure is 40 mm, and the width of the micro-wave structure is 30 mm; the wavelength A of the middle area of the micro-wave structure is 3 mm, and the wavelength B of the areas on both sides of the micro-wave structure is 6 mm.
[0090] Example 9
[0091] The difference between Example 9 and Example 1 is that the wavelengths of the middle area and the two side areas of the micro-wave structure are different, and the rest is the same as Example 1. The specific steps are as follows:
[0092] 1. Preparation of cooling structure: 20% polylactic acid and 80% polypropylene are mixed and coated by solution casting method to prepare cooling structure; the cooling structure prepared has a length of 120 mm and a width of 60 mm, and has a micro-wave structure on the cooling structure, the length of the micro-wave structure is 40 mm, and the width of the micro-wave structure is 30 mm; the wavelength A of the middle area of the micro-wave structure is 3 mm, and the wavelength B of the areas on both sides of the micro-wave structure is 10 mm.
[0093] Example 10
[0094] The difference between Example 10 and Example 1 is that the materials used to prepare the cooling structure are different. The rest is the same as Example 1. The specific steps are as follows:
[0095] 1. Preparation of cooling structure: 20% polyethylene glycol and 80% polyacrylic acid are mixed and coated by solution casting method to prepare cooling structure; the prepared cooling structure has a length of 120 mm and a width of 60 mm, and has a micro-wave structure on the cooling structure, the length of the micro-wave structure is 40 mm, and the width of the micro-wave structure is 30 mm; the wavelength A of the middle area of the micro-wave structure is 3 mm, and the wavelength B of the areas on both sides of the micro-wave structure is 8 mm.
[0096] Embodiment 11
[0097] The difference between Example 11 and Example 1 is that the material used to prepare the cooling structure is different. The rest is the same as Example 1. The specific steps are as follows:
[0098] 1. Preparation of cooling structure: 20% polyethylene glycol and 80% polyacrylonitrile are mixed and coated by solution casting method to prepare cooling structure; the prepared cooling structure has a length of 120 mm and a width of 60 mm, and has a micro-wave structure on the cooling structure, the length of the micro-wave structure is 40 mm, and the width of the micro-wave structure is 30 mm; the wavelength A of the middle area of the micro-wave structure is 3 mm, and the wavelength B of the areas on both sides of the micro-wave structure is 8 mm.
[0099] Example 12
[0100] The difference between Example 12 and Example 1 is that the material used to prepare the cooling structure is different. The rest is the same as Example 1. The specific steps are as follows:
[0101] 1. Preparation of cooling structure: 10% polyethylene glycol and 90% polyacrylic acid are mixed and coated by solution casting method to prepare cooling structure; the prepared cooling structure has a length of 120 mm and a width of 60 mm, and has a micro-wave structure on the cooling structure, the length of the micro-wave structure is 40 mm, and the width of the micro-wave structure is 30 mm; the wavelength A of the middle area of the micro-wave structure is 3 mm, and the wavelength B of the areas on both sides of the micro-wave structure is 8 mm.
[0102] Embodiment 13
[0103] The difference between Example 13 and Example 1 is that the material used to prepare the cooling structure is different. The rest is the same as Example 1. The specific steps are as follows:
[0104] 1. Preparation of cooling structure: 30% polyethylene glycol and 70% polyacrylic acid are mixed and coated by solution casting method to prepare cooling structure; the prepared cooling structure has a length of 120 mm and a width of 60 mm, and has a micro-wave structure on the cooling structure, the length of the micro-wave structure is 40 mm, and the width of the micro-wave structure is 30 mm; the wavelength A of the middle area of the micro-wave structure is 3 mm, and the wavelength B of the areas on both sides of the micro-wave structure is 8 mm.
[0105] Comparative Example 1
[0106] The difference between Comparative Example 1 and Example 1 is that there is no micro-wave structure in the cooling structure, and the rest is the same as Example 1:
[0107] 1. Preparation of cooling structure: 20% polylactic acid and 80% polypropylene were mixed and coated by solution casting to prepare cooling structure; the cooling structure prepared was 120 mm in length and 60 mm in width. Performance test method:
[0108] 60℃ high temperature cycle test: The battery was placed in a 60℃ environmental cabinet for 6 hours, and the temperature of the large surface of the battery cell was collected using Omron.
[0109] 60℃ cycle capacity retention rate: Place the battery in a 60℃ environmental cabinet for 6 hours, charge and discharge the battery at 1C / 1C constant current, place the battery for 30 minutes between each charge and discharge, and record the capacity retention rate of the battery after 100 cycles.
[0110] Table 1 is a summary table of parameter settings for the above embodiments and comparative examples.
[0111]
[0112]
[0113] Table 2 is a summary of the performance test results.
[0114] Group Battery surface temperature at 60℃ 100-cycle capacity retention rate Example 1 45.6℃ 97.2% Example 2 47.3℃ 96.6% Example 3 44.7℃ 97.5% Example 4 46.2℃ 96.8% Example 5 46.0℃ 96.8% Example 6 45.4℃ 97.3% Example 7 46.4℃ 96.7% Example 8 45.4℃ 97.2% Example 9 45.9℃ 96.8% Example 10 45.8℃ 97.1% Embodiment 11 45.8℃ 97.0% Example 12 46.0℃ 96.9% Embodiment 13 45.4℃ 97.3% Comparative Example 1 53.0℃ 95.2%
[0115] It can be seen from the experimental results of Examples 1 to 13 and Comparative Example 1 in Table 1 and Table 2 that by arranging a micro-wave structure in the middle of the cooling structure to increase the reaction area, and arranging micro-wave structures of different wavelengths according to different temperature zones of the battery cell to increase different reaction areas, the local temperature of the battery cell can be reduced, the overall temperature of the battery cell can be reduced, the capacity retention rate of the battery can be improved, the power performance and cycle performance of the battery can be improved, and the safety of the battery can be improved.
[0116] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A cooling structure, characterized in that: The cooling structure comprises a heat dissipation material, and the middle area of the cooling structure is a micro-wave structure.
2. The cooling structure according to claim 1, characterized in that: The cooling structure includes a first direction and a second direction, the first direction is the length direction of the cooling structure, the second direction is the width direction of the cooling structure, and the micro-wave structure extends along the first direction or the second direction.
3. The cooling structure according to claim 2, characterized in that: A line passing through the center of the cooling structure and perpendicular to the first direction is a first center line, a line passing through the cooling structure and perpendicular to the second direction is a second center line, and the micro-wave structure is symmetrical about the first center line or the second center line of the cooling structure.
4. The cooling structure according to claim 3, characterized in that: In the first direction, the length of the micro-wave structure accounts for 1 / 5 to 1 / 2 of the length of the cooling structure, and / or, in the second direction, the width of the micro-wave structure accounts for 1 / 5 to 1 / 2 of the width of the cooling structure.
5. The cooling structure according to claim 2, characterized in that: In the first direction or the second direction of the cooling structure, the wavelength of the middle area of the micro-wave structure is smaller than the wavelength of the areas on both sides of the micro-wave structure.
6. The cooling structure according to claim 5, characterized in that: The wavelength of the middle area of the micro-wave structure is A, and the wavelength of the areas on both sides of the micro-wave structure is B, which satisfies: 0<A≤5mm; 5mm<B≤10mm.
7. The cooling structure according to claim 1, characterized in that: The heat dissipation material includes one of paraffin, polylactic acid, polyethylene glycol, and hydrated inorganic salt.
8. The cooling structure according to claim 1, characterized in that: The cooling structure further comprises a polymer material, and the polymer material comprises one of polyvinylidene fluoride-hexafluoropropylene copolymer, polyacrylic acid, polyacrylonitrile, polyester, and polyolefin polymers.
9. The cooling structure according to claim 8, characterized in that: The mass ratio of the heat dissipation material to the polymer material is (5% to 50%): (50% to 95%).
10. The cooling structure according to claim 1, characterized in that: The thickness d of the cooling structure satisfies: 0<d≤2mm.
11. A lithium ion battery, characterized in that: It comprises the cooling structure described in any one of claims 1 to 10.