Cavitation-erosion-resistant cylinder sleeve
By using atmospheric plasma spraying technology coating on the waterway part and the surface of the ring belt, the cavitation problem caused by the piston impact of the internal combustion engine cylinder liner is solved, the cavitation resistance and thermal conductivity are improved, the service life is extended and the service life is reduced. Production cost.
Patent Information
- Application Number
- CN202420048944.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-09
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2034-01-09
AI Technical Summary
The prior art cannot effectively solve the cavitation problem caused by the piston impact of the internal combustion engine cylinder liner, resulting in a decrease in the airtightness of the combustion chamber, an increase in oil temperature and a shortened service life.
Atmospheric plasma spraying technology is used to coat the waterway parts and the surface of the ring belt in the cylinder liner, and carbon steel or stainless steel materials are used to form a high-hardness and high-density coating to improve corrosion resistance, and optimize the coating thickness and porosity. and roughness, enhancing the bond strength with the cylinder liner.
It significantly improves the corrosion resistance of the cylinder liner, extends the service life, reduces production costs, and meets the requirements of high thermal conductivity.
Smart Images

Figure CN222066897U_ABST
Abstract
Description
Technical Field
[0001] The utility model relates to the technical field of internal combustion engine cylinder sleeves, in particular to a cavitation-resistant cylinder sleeve. Background Art
[0002] When the engine is working, due to the pressure on the connecting rod side, the piston will impact the cylinder liner, causing the cylinder liner to be subjected to lateral force. Under the action of the impact force, the cooling water in the water jacket vibrates at a high frequency. This vibration causes the cooling water in the water jacket to be stretched and squeezed alternately, especially the water near the surface of the cylinder liner in contact with the cooling water, which fluctuates at a high speed. Stretching causes a local vacuum in the water near the cylinder wall to produce bubbles. Local high temperature will intensify this reaction, and squeezing will cause the bubbles to burst. Under the upward impact of the piston, the cavitation bubbles attached to the outer periphery of the cylinder wall burst instantly, generating a strong pressure wave, violently impacting and eroding the cylinder liner. This process is repeated, and honeycomb-shaped holes are formed on the surface of the cylinder liner, which is called cavitation. In severe cases, it even penetrates the cylinder wall.
[0003] As the explosion pressure of the cylinder liner increases, the lateral impact force also increases accordingly, which increases cavitation. Cavitation causes the air tightness of the combustion chamber to decrease, the oil temperature and fuel consumption to increase, which seriously affects the service life of the internal combustion engine and even causes serious accidents. It has become a problem that needs to be solved in cylinder liner design.
[0004] At present, the industry widely uses nitriding surface processing technology. One is QPQ treatment, which adopts low-temperature salt bath nitriding and oxidation process, that is, a metal parts surface modification technology, and the process flow is cleaning-preheating-salt bath nitriding-oxidation; the other is gas nitriding, which uses a pit gas furnace and introduces ammonia gas to decompose nitrogen atoms at high temperature. The nitrogen atoms are adsorbed by the workpiece and diffuse inward to form a nitriding layer. After nitriding, the structure from outside to inside is: loose nitriding layer-dense nitriding layer-diffusion layer-matrix; this high-hardness, high-density treatment layer has high adhesion and density, and can effectively improve the corrosion resistance of the metal.
[0005] However, existing process technology, structural design, material design and surface treatment methods can only alleviate or delay the occurrence of cavitation, which is generally unavoidable.
[0006] Therefore, how to improve the cavitation resistance of the cylinder liner is a technical problem that those skilled in the art currently need to solve. Utility Model Content
[0007] In view of this, the purpose of the utility model is to provide a cavitation-resistant cylinder liner to improve the cavitation-resistant performance of the cylinder liner;
[0008] In order to achieve the above purpose, the utility model provides the following technical solutions:
[0009] A cavitation-resistant cylinder liner comprises a cylinder liner body and an atmospheric plasma spray coating. The cylinder liner body comprises a water channel portion, and the atmospheric plasma spray coating is arranged on the outer surface of the water channel portion.
[0010] Optionally, in the above-mentioned cavitation-resistant cylinder liner, the cylinder liner body also includes an upper ring belt and a lower ring belt, the upper ring belt is connected to the top of the water channel part, and the lower ring belt is connected to the bottom of the water channel part, and the atmospheric plasma spray coating is arranged on the outer surface of the water channel part, the outer surface of the upper ring belt and the outer surface of the lower ring belt.
[0011] Optionally, in the above-mentioned cavitation-resistant cylinder liner, the material of the atmospheric plasma spraying coating is carbon steel or stainless steel.
[0012] Optionally, in the above-mentioned cavitation-resistant cylinder liner, the thickness of the atmospheric plasma spraying coating is 0.1 mm to 0.5 mm.
[0013] Optionally, in the above-mentioned cavitation-resistant cylinder liner, the porosity of the atmospheric plasma sprayed coating is less than or equal to 4%.
[0014] Optionally, in the above-mentioned cavitation-resistant cylinder liner, the roughness RZ of the atmospheric plasma spraying coating is ≤80 um.
[0015] Optionally, in the above-mentioned cavitation-resistant cylinder liner, the bonding strength between the atmospheric plasma sprayed coating and the outer surface of the water channel portion is greater than 30 MPa.
[0016] Optionally, in the above-mentioned cavitation-resistant cylinder liner, the edge of the atmospheric plasma sprayed coating is flush with or smoothly transitions to the cylinder liner body.
[0017] Optionally, in the above-mentioned cavitation-resistant cylinder liner, the cylinder liner body further includes an annular groove and a sealing ring, the annular groove is provided on the outer surface of the cylinder liner body, and the sealing ring is clamped with the annular groove.
[0018] The cavitation-resistant cylinder liner provided by the utility model has a water channel portion that is in direct contact with cooling water between the cylinder block and the cylinder liner when the cylinder block and the cylinder liner are matched, so an atmospheric plasma spray coating is arranged on the outer surface of the water channel portion, which can prevent cavitation from occurring on the surface of the water channel portion, thereby improving the cavitation-resistant performance of the cylinder liner.
[0019] It should be noted that the commonly used nitriding treatment method is to use nitriding technology to infiltrate a nitride on the metal surface and cover the surface of the metal material. However, because a certain proportion of graphite is exposed on the processed surface of cast iron materials, the exposed graphite is easily peeled off under the erosion of cooling water to form a cavitation source. Although the nitriding treatment forms a nitride layer with stable performance on the surface, the nitride layer is formed by the combination of nitrogen atoms and metal atoms in the workpiece substrate. The exposed graphite on the workpiece surface cannot be covered or filled and will still become a cavitation source. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the embodiments of the utility model or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the utility model. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0021] Figure 1 The overall structure diagram of the cavitation-resistant cylinder liner disclosed in the embodiment of the utility model;
[0022] Figure 2 It is a schematic diagram of the structure of the cavitation-resistant cylinder liner and the cylinder disclosed in the embodiment of the utility model;
[0023] in:
[0024] Cylinder liner body 100 , water channel portion 101 , atmospheric plasma spray coating 102 , upper annular band 103 , lower annular band 104 , annular groove 105 , and cylinder block 200 . DETAILED DESCRIPTION
[0025] The following will be combined with the drawings in the embodiments of the utility model to clearly and completely describe the technical solutions in the embodiments of the utility model. Obviously, the described embodiments are only part of the embodiments of the utility model, not all of the embodiments. Based on the embodiments of the utility model, all other embodiments obtained by ordinary technicians in this field without making novel work are within the scope of protection of the utility model.
[0026] In the description of the present invention, it should be understood that the terms "upper", "lower", "top surface", "bottom surface" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the positions or elements referred to must have a specific orientation, be constructed and operate in a specific orientation, and therefore cannot be understood as limitations of the present invention. In addition, the terms "first" and "second" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance.
[0027] like Figure 1 and Figure 2As shown, the cavitation-resistant cylinder liner disclosed in the utility model comprises a cylinder liner body 100 and an atmospheric plasma spray coating 102. The cylinder liner body 100 comprises a water channel portion 101, and the atmospheric plasma spray coating 102 is arranged on the outer surface of the water channel portion 101. Specifically, the cavitation-resistant cylinder liner is a wet cylinder liner, which is characterized in that the water channel portion 101 is in direct contact with cooling water, and the water channel portion 101 is the cavitation occurrence area, so it is only necessary to perform the main spraying at this portion, and spraying is performed at other portions of the cylinder liner body 100, especially the assembly portion, and higher requirements are placed on the dimensional tolerance and surface roughness of the outer surface of the cylinder liner body 100.
[0028] It should be noted that the atmospheric plasma spray coating 102 is formed by using a plasma sprayer to form a plasma beam by ionizing and exciting gas in a low-pressure atmosphere, and spraying particles onto the surface of the workpiece through a high-speed airflow. The use of atmospheric plasma spraying on the local outer surface (water channel portion 101) of the cavitation-resistant cylinder liner can achieve a good anti-cavitation effect, which is superior to the existing nitriding treatment process. The cavitation-resistant cylinder liner provided by the utility model has a direct contact with the cooling water between the cylinder body 200 and the cavitation-resistant cylinder liner because the water channel portion 101 is in direct contact with the cooling water between the cylinder body 200 and the cavitation-resistant cylinder liner when the cylinder body 200 is matched with the cavitation-resistant cylinder liner. Therefore, the atmospheric plasma spray coating 102 is arranged on the outer surface of the water channel portion 101, which can prevent cavitation from occurring on the surface of the water channel portion 101, thereby improving the cavitation resistance of the cavitation-resistant cylinder liner.
[0029] In order to optimize the above technical solution, the cylinder liner body 100 also includes an upper annular band 103 and a lower annular band 104. The upper annular band 103 is connected to the top of the water channel portion 101, and the lower annular band 104 is connected to the bottom of the water channel portion 101. The atmospheric plasma spray coating 102 is arranged on the outer surface of the water channel portion 101, the outer surface of the upper annular band 103, and the outer surface of the lower annular band 104. Specifically, the upper annular band 103 and the lower annular band 104 are used to radially position the cylinder body 200. The upper annular band 103 and the lower annular band 104 are clearance-matched with the cylinder body 200, so some cooling water will enter between the upper annular band 103 and the cylinder body 200, and between the lower annular band 104 and the cylinder body 200. Therefore, the atmospheric plasma spray coating 102 is simultaneously provided on the outer surface of the waterway portion 101, the outer surface of the upper annular band 103, and the outer surface of the lower annular band 104, which can further protect the cylinder liner body 100 and play a good anti-corrosion and cavitation resistance effect, thereby improving the cavitation resistance of the cavitation-resistant cylinder liner.
[0030] In order to optimize the above technical solution, the material of the atmospheric plasma spray coating 102 is carbon steel or stainless steel. Specifically, from the material point of view, the material of the atmospheric plasma spray coating 102 is set to carbon steel or stainless steel. On the one hand, the stiffness of the material can be improved by alloying, that is, the elastic modulus of the material can be improved; on the other hand, a surface treatment process can be adopted, that is, the atmospheric plasma spraying process is adopted to spray the outer surface of the cavitation-resistant cylinder liner to form the coating 102, and the carbon steel or stainless steel is in a wire state, and the plasma flame is used as a heat source for heating, so that the coating 102 material is evenly dispersed and refined on the outer surface of the cavitation-resistant cylinder liner, and the graphite holes and cracks on the outer surface of the cavitation-resistant cylinder liner are completely covered, thereby eliminating the early cavitation source. At the same time, the wet cylinder liner has a high requirement for thermal conductivity, and the thermal conductivity of carbon steel or stainless steel is higher, and its thermal conductivity is better than that of ceramic materials, and carbon steel or stainless steel wires are all made of national standard grades. Compared with the ceramic powder formed and sintered at high temperature, the preparation process of carbon steel or stainless steel is simpler, the process cost is lower, and it is easier to obtain materials. Therefore, setting the material of the atmospheric plasma spray coating 102 to carbon steel or stainless steel can eliminate the early cavitation source, improve the cavitation resistance of the cavitation-resistant cylinder liner, meet the thermal conductivity requirements of the cavitation-resistant cylinder liner, and reduce production costs.
[0031] In order to optimize the above technical solution, the thickness of the atmospheric plasma spray coating 102 is 0.1mm to 0.5mm. Further, the utility model preferably, when the material of the atmospheric plasma spray coating 102 is carbon steel, the thickness of the atmospheric plasma spray coating 102 is 0.45mm, and when the material of the atmospheric plasma spray coating 102 is stainless steel, the thickness of the atmospheric plasma spray coating 102 is 0.41mm. During use, the operator can change the thickness of the atmospheric plasma spray coating 102 according to the different materials of the atmospheric plasma spray coating 102 to further improve the cavitation resistance of the cylinder liner.
[0032] In order to optimize the above technical solution, the porosity of the atmospheric plasma sprayed coating 102 is less than or equal to 4%. Specifically, the smaller the porosity of the atmospheric plasma sprayed coating 102, the fewer cavitation sources, and the higher the cavitation resistance of the cylinder liner. At the same time, a certain amount of porosity can also improve the thermal shock resistance of the atmospheric plasma sprayed coating 102. After actual use and data calculation, the utility model preferably has a porosity of less than or equal to 4% for the atmospheric plasma sprayed coating 102.
[0033] In order to optimize the above technical solution, the roughness RZ of the atmospheric plasma sprayed coating 102 is ≤80um. Specifically, the smaller the roughness of the atmospheric plasma sprayed coating 102, the smoother its surface, and the slower the cavitation occurs. After actual use and data calculation, the utility model preferably sets the roughness RZ of the atmospheric plasma sprayed coating 102 to ≤80um.
[0034] In order to optimize the above technical solution, the bonding strength between the atmospheric plasma spray coating 102 and the outer surface of the waterway portion 101 is greater than 30MPa. Specifically, when the atmospheric plasma spray coating 102 is simultaneously provided on the outer surface of the waterway portion 101, the outer surface of the upper annular belt 103, and the outer surface of the lower annular belt 104, the bonding strength between the atmospheric plasma spray coating 102 and the outer surface of the waterway portion 101, the outer surface of the upper annular belt 103, and the outer surface of the lower annular belt 104 is greater than 30MPa. Specifically, the greater the bonding strength between the atmospheric plasma spray coating 102 and the outer surface of the cylinder liner body 100, the less likely the atmospheric plasma spray coating 102 will fall off. After actual use and data calculation, the utility model preferably has a bonding strength between the atmospheric plasma spray coating 102 and the outer surface of the cylinder liner body 100 greater than 30MPa.
[0035] In order to optimize the above technical solution, the edge of the atmospheric plasma spray coating 102 is flush with or smoothly transitions to the cylinder liner body 100. Specifically, the edge of the atmospheric plasma spray coating 102 can be turned to make it flush with or smoothly transition to the adjacent area, and the part of the cylinder liner body 100 where the atmospheric plasma spray coating 102 is not arranged, the operator can make tooling as needed to protect it. After the atmospheric plasma spray coating 102 is sprayed, the atmospheric plasma spray coating 102 and the part of the cylinder liner body 100 where the atmospheric plasma spray coating 102 is not arranged need to be processed, such as removing burrs, etc., to ensure that all surfaces of the cylinder liner meet the use requirements.
[0036] In order to optimize the above technical solution, the cylinder liner body 100 further includes an annular groove 105 and a sealing ring. The annular groove 105 is provided on the outer surface of the cylinder liner body 100, and the sealing ring is engaged with the annular groove 105. Specifically, the number of the annular groove 105 is one or more. When the sealing ring is engaged with the annular groove 105, the cooling water is sealed between the cavitation-resistant cylinder liner and the cylinder body 200. When the cooling water impacts the cylinder liner body 100, the atmospheric plasma spray coating 102 protects the cylinder liner body 100 to avoid cavitation, thereby improving the cavitation resistance of the cylinder liner.
[0037] The advantages of the utility model are:
[0038] (1) Improved the cavitation resistance of the cylinder liner;
[0039] (2) Easy to produce and highly practical;
[0040] (3) High thermal conductivity and low production cost.
[0041] It should be noted that the cavitation-resistant cylinder liner provided by the utility model can be used in the technical field of internal combustion engine cylinder liners or other fields. Other fields are any fields other than the technical field of internal combustion engine cylinder liners. The above is only an example and does not limit the application field of the cavitation-resistant cylinder liner provided by the utility model.
[0042] The various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.
[0043] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but will conform to the widest scope consistent with the principles and novel features disclosed herein.
[0044] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the utility model. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0045] The preferred embodiments of the utility model disclosed above are only used to help explain the utility model. The preferred embodiments do not describe all the details in detail, nor do they limit the utility model to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the utility model, so that technicians in the relevant technical field can well understand and use the utility model. The utility model is limited only by the claims and their full scope and equivalents.
Claims
1. A cavitation-resistant cylinder liner, characterized in that: The invention comprises a cylinder liner body and an atmospheric plasma spray coating, wherein the cylinder liner body comprises a water channel portion, and the atmospheric plasma spray coating is arranged on the outer surface of the water channel portion.
2. The cavitation-resistant cylinder liner according to claim 1, characterized in that: The cylinder liner body also includes an upper ring belt and a lower ring belt, the upper ring belt is connected to the top of the water channel part, and the lower ring belt is connected to the bottom of the water channel part, and the atmospheric plasma spray coating is arranged on the outer surface of the water channel part, the outer surface of the upper ring belt and the outer surface of the lower ring belt.
3. The cavitation-resistant cylinder liner according to claim 1, characterized in that: The material of the atmospheric plasma spraying coating is carbon steel or stainless steel.
4. The cavitation-resistant cylinder liner according to claim 1, characterized in that: The thickness of the atmospheric plasma spraying coating is 0.1 mm to 0.5 mm.
5. The cavitation-resistant cylinder liner according to claim 1, characterized in that: The porosity of the atmospheric plasma sprayed coating is less than or equal to 4%.
6. The cavitation-resistant cylinder liner according to claim 1, characterized in that: The roughness of the atmospheric plasma sprayed coating is RZ≤80um.
7. The cavitation-resistant cylinder liner according to claim 1, characterized in that: The bonding strength between the atmospheric plasma sprayed coating and the outer surface of the waterway portion is greater than 30 MPa.
8. The cavitation-resistant cylinder liner according to claim 1, characterized in that: The edge of the atmospheric plasma sprayed coating is flush with or smoothly transitions to the cylinder liner body.
9. The cavitation-resistant cylinder liner according to claim 2, characterized in that: The cylinder liner body further comprises an annular groove and a sealing ring. The annular groove is arranged on the outer surface of the cylinder liner body, and the sealing ring is clamped with the annular groove.