Passivation contact crystalline silicon solar cell with back contact structure
By adopting a back contact structure and periodic dot matrix distribution in crystalline silicon solar cells, combined with local passivation contact zones, the problem of difficulty in applying passivation contact technology in the prior art is solved, and high-efficiency photoelectric conversion is achieved and cost-reduced, suitable for different types of silicon substrates.
Patent Information
- Application Number
- CN202420860361.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-24
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2034-04-24
AI Technical Summary
When the existing TOPCon and PERC crystalline silicon solar cells use passivation contact technology, it is difficult to leverage the advantages of hole and electron passivation contact structures at the same time, resulting in limited photoelectric conversion efficiency and high manufacturing cost.
The passivation contact crystalline silicon solar cell design with a back contact structure is adopted. Through the periodic dot matrix distribution through through holes and local passivation contact areas, silicon nitride covers and fills, to achieve efficient connection of electrodes and improve optical performance. Reduce the electrode shading rate.
It improves the photoelectric conversion efficiency, reduces the battery manufacturing cost, is suitable for n-type and p-type silicon substrates, simplifies the battery structure and preparation process, and enhances market competitiveness.
Smart Images

Figure CN222126546U_ABST
Abstract
Description
Technical Field
[0001] The utility model belongs to the field of solar cells, and in particular relates to a passivated contact crystalline silicon solar cell with a back contact structure. Background Art
[0002] Photovoltaic power generation is green and environmentally friendly, can be sustainable, can solve the energy and environmental crisis of mankind, and has an important strategic position in the future energy development. The development of high-efficiency, low-cost solar cells is the key to promoting the stable and rapid development of the photovoltaic power generation industry. Among all types of solar cells, crystalline silicon solar cells (referred to as crystalline silicon cells) have the fastest development in applications, the most mature industrial technology, and the highest market share due to their high photoelectric conversion efficiency, stable performance, and low manufacturing cost. At present, industrial crystalline silicon solar cells mainly include PERC (passivated emitter and rear cell), passivated contact TOPCon (Tunnel oxide and passivated contact) cells, and heterojunction (Silicon Heterojunction) cells. Among them, the production capacity of PERC cells with p-type silicon as the substrate occupies about 60% of the market, and the industrial photoelectric conversion efficiency is 24%-24.5%. The production capacity of TOPCon cells with n-type silicon as the substrate occupies about 34% of the market, and the industrial photoelectric conversion efficiency is 25.5%-26%.
[0003] TOPCon cells achieve excellent surface passivation, selective passage of photogenerated carriers, and one-dimensional efficient collection by tunneling silicon oxide and doped polysilicon. The n-region of the TOPCon cell is an electron passivation contact layer, and the p-region still uses a boron-doped pn junction. For passivated contact cells with n-type silicon as the substrate, the effect of the hole passivation contact layer on improving the cell efficiency is significantly higher than that of the electron passivation contact layer. Therefore, the current industrial TOPCon cells cannot take advantage of the maximum advantage of the passivation contact structure. The main reason restricting the simultaneous use of hole and electron passivation contact technology in TOPCon cells is the high optical parasitic absorption coefficient of doped (boron or phosphorus) polysilicon, which will make the excellent passivation performance improvement that can be obtained on the light-receiving surface of the cell after the passivation contact technology is adopted at the expense of significantly sacrificing optical performance. Therefore, how to apply both hole and electron passivation contact technology to TOPCon cells is the key to improving cell efficiency and reducing manufacturing costs.
[0004] Relatively speaking, PERC cells still use traditional pn junctions or high-low junctions as field passivation, and do not use more advanced passivation contact technology, which has caused a bottleneck in the improvement of PERC cell conversion efficiency. Since the cost of pulling single crystals of p-type silicon is lower than that of n-type silicon, crystalline silicon cells with p-type silicon as substrate are more cost-effective when the photoelectric conversion efficiency is the same. Moreover, the current PERC cell production capacity still occupies a dominant position. Therefore, it is also of great significance to further develop efficient and low-cost crystalline silicon cells with p-type silicon as substrate. If the passivation contact technology can be applied to PERC cells, this can solve the bottleneck of improving its cell efficiency, and the manufacturing cost can be further reduced, thereby effectively enhancing the market competitiveness of PERC cells.
[0005] In addition, both PERC cells and TOPCon cells adopt a double-sided structure, and the metal grid lines on the front of the cell bring non-negligible shading losses, which also limits the further improvement of their industrial cell efficiency. Utility Model Content
[0006] The utility model provides a passivated contact crystalline silicon solar cell with a back contact structure (referred to as a back contact passivated contact cell). The back contact passivated contact cell has through holes with periodic lattice distribution, and the side walls of the through holes are covered and filled with silicon nitride and electrodes from the inside to the outside in sequence; the electrode on the front of the cell is located at the intersection of the through hole and the front of the cell, and is connected to the electrode filling the through hole, extending to the back of the cell; in the surrounding adjacent area of the through hole projected on the front of the cell, there is a local passivated contact area with the same doping conductivity type as the silicon substrate; other areas on the front of the cell have high and low junction areas with the same doping conductivity type as the silicon substrate. The back of the cell has a passivated contact area with a doping conductivity type opposite to that of the silicon substrate.
[0007] The utility model discloses a passivated contact crystalline silicon solar cell with a back contact structure, which comprises: a silicon substrate; a through hole penetrating the silicon substrate and distributed in a periodic lattice; the side wall of the through hole is sequentially covered by an electrical insulating isolation layer and a first electrode unit from the inside to the outside, and is formed by the through hole of the first electrode unit; a local passivation contact area formed on the first surface of the silicon substrate, the local passivation contact area has a plurality of passivation contact units distributed in a periodic lattice, the passivation contact unit is an annular area, the overall area included in the outer contour thereof and the projection of the through hole on the first surface of the silicon substrate have the same shape and geometric center, and the area of the overall area is larger than the projection of the through hole on the silicon substrate. The projected area of the first surface of the substrate; the local passivation contact area includes tunneling silicon oxide and first doped polysilicon, the doping type of the first doped polysilicon is the same as that of the silicon substrate; a high-low junction area is formed outside the local passivation contact area on the first surface of the silicon substrate, the doping type of the high-low junction area is the same as that of the silicon substrate; an anti-reflection film is formed on the first surface of the silicon substrate; a second electrode is formed on the first surface of the silicon substrate, the second electrode has a plurality of second electrode units distributed in a periodic lattice, the second electrode unit and the projection of the through hole on the first surface of the silicon substrate have the same shape and geometric center, and the area is larger than the projection area of the through hole on the first surface of the silicon substrate. The area of the passivation contact unit is less than or equal to the area of the passivation contact unit; an electrically insulating isolation region formed on the second surface of the silicon substrate, the electrically insulating isolation region having a plurality of electrically insulating isolation units distributed in a periodic lattice, the electrically insulating isolation unit being an annular region, the overall region included in the outer contour of which has the same shape and geometric center as the projection of the through hole on the second surface of the silicon substrate, and the area of the overall region is greater than the projection area of the through hole on the second surface of the silicon substrate; a passivation contact region formed outside the electrically insulating isolation region on the second surface of the silicon substrate, the passivation contact region comprising tunneling silicon oxide and second doped polysilicon, the doping type of the second doped polysilicon being the same as that of the through hole. The silicon substrate is opposite; a passivation layer is used to passivate the second surface of the silicon substrate; a third electrode is formed at the intersection of the through hole and the second surface of the silicon substrate, the third electrode has a plurality of first electrode units distributed in a periodic lattice, the projection of the third electrode unit and the through hole on the first surface of the silicon substrate have the same shape and geometric center, and the area is smaller than the projection area of the through hole on the second surface of the silicon substrate; the first electrode unit is connected to the second electrode unit and the third electrode unit at the intersection with the first surface and the second surface of the silicon substrate respectively; a fourth electrode is formed in the passivation contact area of the second surface of the silicon substrate, and the projection of the fourth electrode and the through hole on the same horizontal plane are completely staggered.
[0008] Optionally, the pattern of the periodic lattice distribution of the through holes is rectangular or rhombus; the shape of the through holes is any one of circular, rectangular, rhombus, and elliptical; the arrangement period of the through holes is 250-5000 microns, and the area percentage is 0.05%-0.7%.
[0009] Optionally, when the through hole is circular in shape, the diameter of the through hole is 10-500 microns, and the diameter of the overall area included in the outer contour of the electrically insulating isolation unit is 100-2500 microns; when the through hole is square, the side length of the through hole is 10-500 microns; the side length of the overall area included in the outer contour of the electrically insulating isolation unit is 100-2500 microns.
[0010] Optionally, the shading rate of the second electrode is 0.05%-0.8%.
[0011] Optionally, the electrically insulating isolation layer and the passivation layer are both made of silicon nitride and have the same thickness.
[0012] Optionally, the passivation layer is silicon nitride with a thickness of 50-300 nm and a refractive index of 1.9-2.2.
[0013] Optionally, in the local passivation contact area on the first surface of the silicon substrate, the thickness of the tunneling silicon oxide is 1.2-1.6nm, and the refractive index is 1.45-1.5; the thickness of the first doped polysilicon is 5-500nm; in the passivation contact area on the second surface of the silicon substrate, the thickness of the tunneling silicon oxide is 1.2-1.6nm, and the refractive index is 1.45-1.5; the thickness of the second doped polysilicon is 5-500nm.
[0014] Optionally, the anti-reflection film is silicon nitride with a thickness of 70-80 nm and a refractive index of 1.9-2.1.
[0015] Optionally, the second electrode and the third electrode are silver electrodes; and the first electrode unit is an aluminum electrode.
[0016] Optionally, the fourth electrode is a gate line electrode.
[0017] The utility model has the following beneficial effects:
[0018] 1. The back contact passivated contact cell provided by the utility model has through holes with periodic lattice distribution, and the front electrode of the cell is connected to the electrode filling the through hole and extends to the back of the cell. The surrounding adjacent area of the front electrode of the cell is a local passivated contact area with the same doping type as the silicon substrate, and the other areas of the front of the cell are high-low junction areas with the same doping type as the silicon substrate. The back of the cell is a passivated contact area with the opposite doping type to the silicon substrate.
[0019] Through the above-mentioned structural design, it is possible to avoid the entire light-receiving surface of the battery using a passivation contact structure (typically, the area percentage of the local passivation contact area on the front of the battery is less than 1.5%), thereby solving the disadvantages of high optical parasitic absorption coefficient and high optical loss of doped (boron or phosphorus) polysilicon, so that both sides of the battery can adopt a passivation contact structure. Furthermore, by efficiently conducting the photogenerated carriers on the front of the battery to the back of the battery through the through hole, and then conducting them to the external circuit, efficient extraction, transmission and collection of photogenerated carriers can be achieved. On this basis, the shading rate of the front electrode can also be greatly reduced (typically, less than 0.25%), significantly increasing the area ratio of the battery receiving photons. In summary, the back-contact passivated contact battery provided by the utility model can achieve excellent performance in both optical and electrical aspects, and therefore can achieve excellent photoelectric conversion efficiency.
[0020] 2. The back contact passivated contact cell provided by the utility model uses aluminum to fill the through hole and silver as the electrode at the intersection of the through hole and the front and back of the cell in the metallization of the through hole and the intersection of the through hole and the front and back of the cell. Because the area ratio of the front and back dot matrix electrodes of the cell is significantly lower than the area ratio of the front grid line electrodes of the current double-sided TOPCon or PERC cells, the use of silver can be effectively saved, thereby effectively reducing the cost of cell manufacturing.
[0021] 3. The back-contact passivated contact cell provided by the utility model can be applied to both n-type and p-type silicon substrates. The cell structure and preparation method are simple and can be realized by using the existing cell preparation method. It can effectively improve the photoelectric conversion efficiency of TOPCon cells and PERC cells, reduce the cell manufacturing cost, and is suitable for industrialization. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 .Schematic diagram of the structure of the back contact passivated contact cell (n-type single crystal silicon substrate).
[0023] Among them, 1 is n-type single crystal silicon substrate, 2 is phosphorus-doped n + -n high-low junction, 3 is tunneling silicon oxide, 4 is phosphorus-doped polysilicon, 5 is boron-doped polysilicon, 6 is the electrical insulation isolation area around the intersection of the through hole and the back of the battery, 7 is silicon nitride on the front of the battery, 8 is silicon nitride on the sidewall of the through hole, 9.1 is silicon nitride on the back of the battery as an auxiliary passivation layer, 9.2 is silicon nitride on the back of the battery to enhance the electrical insulation isolation performance, 10 is the second electrode on the front of the battery (located at the intersection of the through hole and the front of the battery), 11 is the first electrode filling the through hole, 12 is the third electrode at the intersection of the through hole and the back of the battery, and 13 is the fourth electrode on the back of the battery. Among them, 14 indicates that a through hole is formed in the battery area corresponding to the two vertical dotted lines. The front of the battery and the sidewall of the through hole have the same silicon nitride.
[0024] Figure 2 .Schematic diagram of the structure of the back contact passivated contact cell (p-type single crystal silicon substrate).
[0025] Among them, 1 is a p-type single crystal silicon substrate, 2 is a boron-doped p + -p high-low junction, 3 is tunneling silicon oxide, 4 is boron-doped polysilicon, 5 is phosphorus-doped polysilicon, 6 is the electrical insulation isolation area around the intersection of the through hole and the back of the battery, 7 is silicon nitride on the front of the battery, 8 is silicon nitride on the sidewall of the through hole, 9.1 is silicon nitride on the back of the battery as an auxiliary passivation layer, 9.2 is silicon nitride on the back of the battery to enhance the electrical insulation isolation performance, 10 is the second electrode on the front of the battery (located at the intersection of the through hole and the front of the battery), 11 is the first electrode filling the through hole, 12 is the third electrode at the intersection of the through hole and the back of the battery, and 13 is the fourth electrode on the back of the battery. Among them, 14 indicates that a through hole is formed in the battery area corresponding to the two vertical dotted lines. The front of the battery and the sidewall of the through hole have the same silicon nitride.
[0026] Figure 3 .Schematic diagram of the through hole lattice distribution pattern of the back contact passivated contact battery from the top of the battery front. The through hole lattice adopts a periodic diamond distribution, and the through hole shape is circular. Among them, 1 is the front of the battery, 2 is the projection of the circular through hole on the front of the battery, 3 is the front second electrode unit, 4 is the front passivation contact unit, and 5 is the front high and low junction area.
[0027] Figure 4 .Schematic diagram of the through hole lattice distribution pattern of the back contact passivated contact battery and the fourth electrode on the back of the battery viewed from the back of the battery. The through hole lattice adopts a periodic rhombus distribution, and the through hole shape is circular. Among them, 1 is the back of the battery, 2 is the projection of the circular through hole on the back of the battery, 3 is the third electrode unit at the intersection of the through hole and the back of the battery, 4 is the electrical insulation isolation unit (annular area) adjacent to the intersection of the through hole and the back of the battery, 5 is the passivation contact area on the back of the battery, and 6 is the fourth electrode in the passivation contact area on the back of the battery. DETAILED DESCRIPTION
[0028] In order to better understand the utility model, the utility model will be further described below in conjunction with specific embodiments and drawings. Obviously, the embodiments described are only part of the embodiments of the utility model, not all of the embodiments. Based on the embodiments in the utility model, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the utility model.
[0029] Before describing the technical solution of the present utility model, the relevant terms are first defined as follows:
[0030] 1) Definition: n-type (i.e., donor) doping in silicon and p-type (i.e., acceptor) doping in silicon are "opposite doping conductivity types" to each other, or "opposite doping types" for short.
[0031] 2) The passivation contact structure consists of tunneling silicon oxide and doped (boron or phosphorus) polysilicon, referred to as the passivation contact area. The localized passivation contact area on the surface of the silicon wafer is referred to as the local passivation contact area. Tunneling silicon oxide and boron-doped polysilicon form the hole passivation contact area. Tunneling silicon oxide and phosphorus-doped polysilicon form the electron passivation contact area.
[0032] 3) The doped junction formed by n-type or p-type doping and silicon substrate (n-type silicon or p-type silicon), referred to as pn junction or high-low junction. + -n knot or n + -p junction, high and low junction including n + -n junction or p + -p knot.
[0033] Combination Figure 1-4 As shown, the substrate of the back contact passivation contact solar cell provided by the utility model is a silicon material (referred to as silicon substrate), which can be single crystal silicon or polycrystalline silicon, and the substrate doping type can be n-type (phosphorus-doped) or p-type (boron-doped).
[0034] The battery has through holes distributed in a periodic lattice, and these through holes penetrate the entire battery: starting from the front side of the battery and penetrating to the back side of the battery in a direction perpendicular to the battery surface.
[0035] The front structure of the battery mainly includes the following features:
[0036] like Figure 1 As shown, the surrounding area of the intersection of the front of the battery and the through hole has a localized passivation contact area, referred to as the local passivation contact area on the front of the battery. The doping type of the doped polysilicon is the same as the doping type of the silicon substrate. The local passivation contact area on the front of the battery has a number of periodic lattice distributed passivation contact units, which are annular areas, and the overall area contained in its outer contour has the same shape and geometric center as the projection of the through hole on the front of the battery, and the area of the overall area is larger than the projection area of the through hole on the front of the battery.
[0037] In the local passivation contact area on the front of the battery, the thickness of the tunneling silicon oxide is 1.2-1.6nm and the refractive index is 1.45-1.5; the thickness of the doped (boron or phosphorus) polysilicon is 5-500nm.
[0038] The other areas outside the local passivation contact area on the front side of the battery have high-low junctions with the same doping type as the substrate, referred to as high-low junction areas.
[0039] Above the local passivation contact area and high and low junction areas on the front of the battery, there is a layer of silicon nitride as an anti-reflection film with a thickness of 70-80nm and a refractive index of 1.9-2.1.
[0040] The front of the battery has a second electrode, the second electrode has a plurality of second electrode units distributed in a periodic lattice, the second electrode unit is located at the intersection of the through hole and the front of the battery, and has the same shape and geometric center as the projection of the through hole on the front of the battery. The specific selection of the electrode material is not limited, and metals such as silver are generally used.
[0041] The pattern design of the through hole includes the following aspects: the distribution form of the periodic lattice of the through hole on the surface of the battery, the shape and size of the through hole, and the horizontal spacing between the center points of each adjacent through hole. It can be understood that the through hole design scheme has many forms. Specifically, the periodic lattice distribution form of the through hole can be in the form of rectangle or rhombus, etc., but it is not limited to this. The specific shape of the through hole is not limited, and it can be circular, rectangular, rhombus, elliptical, etc. The size of the through hole, that is, its diameter, side length, and the length of the major and minor axes of the ellipse, etc., is not specifically limited; typically, the diameter of the circular through hole is 10-500μm; the side length of the square through hole is 10-500μm. Generally, the horizontal spacing between the center points of each adjacent through hole is 250-5000μm. The percentage of the total projected area of all through holes on the front of the battery to the battery area is referred to as the through hole area percentage. Generally, the through hole area percentage is between 0.05%-0.7%, typically less than 0.2%.
[0042] It should be noted that, for the periodic lattice-distributed through holes, when viewed from the normal direction of the battery surface, the projections of the through holes and the fourth electrode unit on the back of the battery on the same horizontal plane should be completely staggered, preferably with a sufficient horizontal distance to prevent shunting or short-circuiting of photogenerated carriers.
[0043] The sidewalls of the through hole are uniformly covered by silicon nitride and the first electrode unit in sequence from the inside to the outside, and are filled by the first electrode unit.
[0044] The role of silicon nitride is to electrically insulate and isolate the photogenerated carriers collected and derived from the front and back of the battery to avoid shunting or short-circuiting of the photogenerated carriers. The sidewalls of the through-holes have the same silicon nitride as the front of the battery, so the same process steps can be used in the specific preparation. The refractive index of the silicon nitride on the sidewalls of the through-holes is 1.9-2.1, and the thickness is 50-300nm, which can typically be the same as the thickness of the silicon nitride on the front of the battery.
[0045] Next to the silicon nitride on the side wall of the through hole, the first electrode unit uniformly covers and fills the through hole. The material of the first electrode unit is generally metal, and is not limited to metal. The first electrode unit on the side wall of the through hole is interconnected with the second electrode unit on the front side of the battery, so that the photogenerated carriers generated on the front side of the battery are efficiently transmitted to the back side of the battery through the through hole.
[0046] It is understandable that the silicon nitride covering the through-hole sidewall is nanometer-sized, while the size of the first electrode unit filled in the through-hole is micrometer-sized, therefore, the thickness of the silicon nitride on the through-hole sidewall may not be considered when comparing the areas.
[0047] It can be understood that the battery front passivation contact unit, the battery front second electrode unit, and the projection of the through hole on the battery front have the same shape and geometric center. On the battery front, the area of the second electrode unit is less than or equal to the area of the passivation contact unit, and both are larger than the projection area of the through hole on the battery front.
[0048] Generally, the area percentage of the local passivation contact area on the front side of the battery is between 0.1% and 3.5% (inclusive), and typically less than 1.5%. Generally, the light shielding rate of the electrode on the front side of the battery (i.e., the second electrode) is between 0.05% and 0.8% (inclusive), and typically less than 0.25%.
[0049] A third electrode is provided at the intersection of the through hole and the back of the battery, and its function is to conduct the photogenerated carriers collected from the front of the battery to the external circuit. The third electrode has a plurality of third electrode units distributed in a periodic lattice, and the projection of the third electrode unit and the through hole on the back of the battery has the same shape and geometric center, and its area is smaller than the projection area of the through hole on the back of the battery.
[0050] It can be understood that in the metallization interconnection and packaging of the back-contact passivated contact cell, it is necessary to connect the third electrode units at the periodic lattice distribution and discrete through-hole projections on the back of the cell to achieve current convergence, so as to conduct the photogenerated carriers collected by the front of the cell to the external circuit.
[0051] The first electrode filling the through hole and the second and third electrodes at the intersection of the through hole and the front and back sides of the battery can be made of the same or different materials. To reduce the cost of battery preparation, preferably, the first electrode is made of aluminum and the second and third electrodes are made of silver.
[0052] There is an electrically insulating isolation area in the vicinity of the intersection area between the through hole and the back of the battery. The electrically insulating isolation area has a number of electrically insulating isolation units distributed in a periodic lattice. The electrically insulating isolation unit is an annular area, and the overall area included in its outer contour has the same shape and geometric center as the projection of the through hole on the back of the battery. The area of the overall area is larger than the projection area of the through hole on the back of the battery, such as Figure 4As shown. The function of the electrical insulation isolation area is to electrically insulate and isolate the photogenerated carriers collected and exported from the back and front of the battery to avoid shunting or short circuit. On the basis of meeting the electrical insulation isolation performance, the area of the electrical insulation isolation unit can be designed to be as small as possible; taking the ring shape as an example, the diameter of the circular area surrounded by the outer contour ranges from 100-2500μm, and the typical diameter is 200-1000μm.
[0053] The other areas outside the electrically insulating isolation area on the back of the cell are passivation contact areas with a doping type opposite to that of the silicon substrate. The thickness of the tunneling silicon oxide is 1.2-1.6nm, and the refractive index is 1.45-1.5; the thickness of the doped polysilicon is 5-500nm.
[0054] There is a layer of silicon nitride as an auxiliary passivation layer below the back passivation contact area and the electrical insulation isolation area (the side away from the silicon substrate), with a thickness of 50-300nm and a refractive index of 1.9-2.2. It should be pointed out that the silicon nitride below the back electrical insulation isolation area can further enhance the electrical insulation isolation performance.
[0055] The back of the battery has a fourth electrode, whose pattern is a grid line type. The material of the fourth electrode is not limited, and generally metal, such as silver, is used.
[0056] The utility model can avoid using a passivated contact structure on the entire light-receiving surface of the battery through the above-mentioned battery structure design, thereby solving the drawback of high optical parasitic absorption coefficient of doped polycrystalline silicon, so that both sides of the battery can adopt a passivated contact structure. Furthermore, by efficiently conducting the photogenerated carriers collected on the front of the battery to the back of the battery through the through-holes, and then conducting them to the external circuit, efficient extraction, transmission and collection of photogenerated carriers can be achieved. On this basis, the shading rate of the front electrode can also be greatly reduced. The back-contact passivated contact battery can be applied to both n-type and p-type silicon substrates. Therefore, the back-contact passivated contact battery provided by the utility model can effectively improve the photoelectric conversion efficiency of TOPCon batteries and PERC batteries, and the battery structure and preparation process are concise and practical, suitable for industrialization.
[0057] The above solution is further illustrated below with reference to a specific embodiment.
[0058] Example 1 provides a back contact passivation contact cell with n-type single crystal silicon as substrate. Figure 1 As shown, the back contact passivation contact cell mainly includes: an n-type single crystal silicon substrate 1, a phosphorus-doped n +-n high-low junction 2, tunneling silicon oxide 3, phosphorus-doped polysilicon 4, boron-doped polysilicon 5, electrical insulation isolation area adjacent to the intersection of the through hole and the back of the battery 6, silicon nitride on the front of the battery 7, silicon nitride on the side wall of the through hole 8, silicon nitride on the back of the battery as an auxiliary passivation layer 9.1, silicon nitride on the back of the battery to enhance the electrical insulation isolation performance 9.2, the second electrode unit 10 on the front of the battery (located at the intersection of the through hole and the front of the battery), the first electrode unit 11 filling the through hole, the third electrode unit 12 at the intersection of the through hole and the back of the battery, and the fourth electrode 13 on the back of the battery.
[0059] First, the pattern design of through holes distributed on the battery surface is given. Figure 3 As shown, the through-hole dot matrix pattern adopts a periodic rhombus distribution, which is exactly a square (i.e., a square dot matrix rotated 45 degrees clockwise along the y direction), and the side length of the square is 1500μm. The through-hole, the second electrode unit on the front of the battery, and the passivation contact unit are all circular, with diameters of 60μm, 80μm, and 150μm, respectively. The third electrode unit at the intersection of the through-hole and the back of the battery and the overall area included in the outer contour of the electrical insulation isolation unit on the back of the battery are also circular, with diameters of 30μm and 500μm, respectively. Therefore, the area percentage of the local passivation contact area on the front of the battery is 0.77%, the shading rate of the electrode on the front of the battery is 0.22%, and the area percentage of the through-hole is 0.12%.
[0060] From the normal direction of the battery surface, Figure 4 As shown, the positional relationship between the through hole and the fourth electrode of the passivation contact area on the back side of the battery is as follows: starting from the first column of through holes in the y direction on the left side of the battery, the horizontal spacing between the line of the axis line of this column of through holes on the normal projection of the back side of the battery and the first back electrode on the left side of the battery is 530μm; based on this, the back electrodes are arranged along the x direction, and the horizontal spacing between every two adjacent back electrodes is 2120μm.
[0061] Then, a method for preparing the back contact passivated contact solar cell is given, which is specifically as follows.
[0062] Step 1. Select a 182mm*182mm n-type single crystal silicon wafer with a bulk resistivity of 1Ω·cm.
[0063] Step 2. First, use sodium hydroxide solution to polish and etch the n-type silicon wafer to remove the damaged layer on the surface of the silicon wafer. Then, use hydrofluoric acid solution to etch away the naturally grown thin silicon oxide that may exist on the surface of the silicon wafer. The concentration of hydrofluoric acid is 1%, and the cleaning time is 15-30 seconds. Define any side as the front side of the battery, and then perform phosphorus doping; in the subsequent battery preparation process, the front side of the battery will be textured at an appropriate step. Correspondingly, the other side is defined as the back side of the battery, and then perform boron doping.
[0064] Step 3. Prepare the hole passivation contact area (tunneling silicon oxide and boron-doped polysilicon) on the back of the battery by PECVD method. The temperature for preparing the tunneling silicon oxide is 250-350°C, and the process gas is silane, nitrous oxide (N 2 The temperature for preparing boron-doped amorphous silicon is 400-500°C, and the process gas is diborane (B 2 H 6 ), silane and hydrogen. Then, furnace annealing is used to complete the crystallization of amorphous silicon to polycrystalline silicon, as well as the activation of boron doping and redistribution in polycrystalline silicon. The annealing temperature is 975°C, the time is 30-40 minutes, and the atmosphere is nitrogen. The thickness of the tunneling silicon oxide is 1.3nm, and the refractive index is 1.46. The thickness of the boron-doped polysilicon layer is 150nm, and the square resistance is 80-100Ω / □. In this step, the amount of boron-doped polysilicon doped to the front of the battery is very small, and it is mainly produced in a very narrow range at the edge of the front. This effect can be eliminated later by wet chemical etching.
[0065] Step 4. Use the APCVD method to prepare a layer of silicon oxide on the back of the battery, with a thickness of 40nm and a refractive index of 1.46. In-line APCVD technology is used, so this layer of silicon oxide is only prepared on the back of the battery and used as a protective layer on the back of the battery, which can effectively protect and prevent the impact on the back of the battery during subsequent battery preparation.
[0066] Step 5. Use the single-sided water-floating wet etching method to chemically etch a small amount of boron-doped polysilicon and silicon oxide on the front side of the battery (mainly concentrated at the edge) and completely etch them away; and use this step to texturize the front side of the battery. The details are as follows:
[0067] First, a mixed solution of nitric acid and hydrofluoric acid is combined with a single-sided water-floating wet etching method to etch away the boron-doped polysilicon that is plated and doped around the front edge of the battery. In the mixed solution of nitric acid and hydrofluoric acid, the mass concentration of nitric acid is 40%, the mass concentration of hydrofluoric acid is 4%, the solution temperature is 7°C, and the etching time is 1-2 minutes.
[0068] Then, a hydrofluoric acid solution is used in combination with a single-sided water-floating wet etching method to etch away the silicon oxide plated on the front side of the battery. The hydrofluoric acid concentration is 1% and the etching time is 15-45 seconds.
[0069] Next, the front of the battery is textured by a wet etching method using a KOH solution with a single-sided water float. The mass concentration of the KOH solution is 2%, the temperature is 70°C, and the etching time is 5-6 minutes. Thus, a random pyramid-shaped texture is formed on the front of the battery.
[0070] Finally, a hydrofluoric acid solution was used in combination with a single-sided water-floating wet etching method to etch away the naturally grown thin silicon oxide on the front side of the battery. The hydrofluoric acid concentration was 0.5% and the etching time was 15 seconds.
[0071] Among all the wet chemical etching in this step, the APCVD silicon oxide in step 4 provides good protection for the back of the battery.
[0072] Step 6. Prepare tunneling silicon oxide on the front side of the silicon wafer using a thermal oxidation method. The thickness is 1.3 nm and the refractive index is 1.46.
[0073] Step 7. Use LPCVD to prepare intrinsic amorphous silicon on the front of the cell with a thickness of 200nm. There is very little intrinsic amorphous silicon plated around the back (edge) of the cell, which can be eliminated by wet chemical etching later.
[0074] Step 8. Use screen printing chemical etching slurry to etch away the intrinsic amorphous silicon and tunneling silicon oxide on the front of the battery except for the local electronic passivation contact design area. BES etching slurry contains a certain concentration of phosphate, which can etch amorphous silicon and silicon oxide. In use, after screen printing the slurry, it is heated to 350-400°C on a heating plate and left to stand for 1-2 minutes. The screen printing screen pattern is consistent with the design pattern of the local electronic passivation contact area on the front of the battery given above. The intrinsic amorphous silicon and tunneling silicon oxide in the printed slurry area are etched away, and the velvet surface prepared on the front of the battery will not be damaged.
[0075] After this step, only the intrinsic amorphous silicon and tunneling silicon oxide in the local electronic passivation contact design area are retained on the front of the battery, and the other areas are n-type silicon substrates with velvet morphology. Then, the surface of the silicon wafer is cleaned with a 40-50°C hydrochloric acid solution combined with ultrasonic cleaning to clean the residual Merck slurry on the surface of the silicon wafer and obtain a clean surface.
[0076] Step 9. Using the masked ion implantation method, localized phosphorus ion implantation is performed in the non-local electronic passivation contact design area and the local electronic passivation contact design area on the front of the battery. The process mask pattern of the ion implantation is consistent with the battery front design pattern given above. In the non-local electronic passivation contact design area, the phosphorus implantation energy is 7keV and the dose is 2·10 15 cm -2 In the local electron passivation contact design area, the phosphorus implantation energy is 20keV and the dose is 5·10 15 cm -2 The temperature of the silicon wafer substrate during ion implantation is room temperature 25°C.
[0077] Then, furnace thermal annealing is performed. During the annealing, the ion-implanted phosphorus in the non-local electronic passivation contact design area is activated and redistributed in silicon to form phosphorus-doped n + -n high-low junction. The amorphous silicon in the local electronic passivation contact design area is fully crystallized into polysilicon, and the ion-implanted phosphorus also completes the impurity activation and redistribution in the polysilicon layer. The annealing temperature is 850℃, the time is 30-40min, and the nitrogen atmosphere.
[0078] After this step, the square resistance of the phosphorus-doped junction in the non-local electronic passivation contact area on the front side of the cell is 100-120Ω / □. The square resistance of the phosphorus-doped polysilicon layer in the local electronic passivation contact area is 70-90Ω / □.
[0079] Step 10. Use laser etching technology to prepare through holes. From the front to the back of the battery, phosphorus-doped polysilicon, tunneling silicon oxide, n-Si substrate, tunneling silicon oxide, boron-doped polysilicon, and APCVD SiO 2 The through hole pattern is as given above. A diode-pumped Yb:YAG disk laser is used, with a wavelength of 1030nm, a pulse width of 250-500ns, a repetition frequency of 10-20kHz, and a nitrogen atmosphere.
[0080] Step 11. Use low-damage laser etching technology to etch the area around the intersection of the back of the battery and the through hole into an electrically insulating area. Laser etching needs to be able to achieve alignment, and the specific pattern design has been given above.
[0081] Step 12. Use a mixed solution of hydrofluoric acid and hydrochloric acid at room temperature to etch away the small amount of phosphosilicate glass generated in step 9 on the front of the battery and the silicon oxide prepared by APCVD in step 4 on the back of the battery. Simultaneously, the laser-etched damaged layer on the through hole in step 10 and the back of the battery in step 12 is cleaned and etched. The volume concentration of hydrofluoric acid is 3%, the volume concentration of hydrochloric acid is 2%, and the cleaning time is 3-4 minutes.
[0082] Step 13. Use PECVD method to deposit silicon nitride on the front of the battery and in the through hole, with a thickness of 75nm and a refractive index of 2.0. The silicon nitride on the front of the battery serves as a passivation anti-reflection film, and also as a buffer barrier layer for the metallization of screen-printed silver paste in the subsequent step 16, to ensure that the silver paste can be confined as much as possible in the phosphorus-doped polysilicon layer of the local passivation contact area on the front of the battery after rapid heat treatment and sintering, and as little as possible enter the silicon substrate through diffusion through phosphorus-doped polysilicon and tunneling silicon oxide. The role of silicon nitride on the side wall of the through hole is to electrically insulate and isolate the photogenerated carriers derived from the front and back of the battery respectively to avoid shunting or short circuiting.
[0083] Step 14. Prepare silicon nitride on the back of the battery by PECVD method, with a thickness of 75nm and a refractive index of 2.0. This layer of silicon nitride is an auxiliary passivation layer for the hole passivation contact area on the back of the battery to enhance the working stability of the battery in extreme application environments (especially high humidity and high temperature environments). In addition, this layer of silicon nitride can also serve as a buffer barrier layer for screen-printed silver paste metallization in the subsequent step 16 to ensure that the silver paste can be confined within the boron-doped polysilicon layer after rapid thermal treatment and sintering, and diffuse through the boron-doped polysilicon and tunnel silicon oxide as little as possible to enter the silicon substrate.
[0084] Furthermore, the silicon nitride deposited in the electrically insulating isolation region on the back of the battery can enhance the electrical insulation performance. In this step, a layer of silicon nitride is deposited on the sidewall of the through hole again. As a result, the thickness of the silicon nitride on the sidewall of the through hole reaches 150nm, so that the electrical insulation performance of the sidewall of the through hole is further enhanced.
[0085] Step 15. Metallize the through-hole sidewalls by screen printing aluminum paste combined with rapid heat treatment alloying, and fill the through-holes with aluminum paste to form the first electrode. The aluminum paste composition does not contain glass powder that assists in penetrating the silicon nitride film, so that the aluminum can be evenly attached to the silicon nitride film on the through-hole sidewalls after alloying heat treatment. Screen printing needs to be aligned with the through-hole formation, and the screen pattern is the same as the through-hole design pattern. The temperature of rapid heat treatment alloying is 580-600℃, the time is 3-5 minutes, and the compressed air atmosphere.
[0086] Step 16. Use screen printing and rapid thermal processing sintering to metallize: 1) the intersection between the front side of the battery and the through hole, 2) the intersection between the through hole and the back side of the battery, and 3) the hole passivation contact area on the back side of the battery, that is, prepare the second, third and fourth electrodes.
[0087] 1) Silver paste is used for metallization at the intersection of the front of the battery and the through hole, and at the intersection of the through hole and the back of the battery. Screen printing needs to be aligned with the through hole formation, and the screen pattern is consistent with the through hole design pattern. The front electrode of the battery (i.e., the second electrode) and the electrode at the intersection of the through hole and the back of the battery (the third electrode) are both circular, with diameters of 80μm and 30μm respectively.
[0088] 2) The fourth electrode of the hole passivation contact area on the back of the battery uses silver paste, and alignment technology is required. The fourth electrode pattern is a grid line type, as given above ( Figure 4 ), line width is 45μm and spacing is 2120μm.
[0089] 3) The actual peak temperature of rapid thermal treatment sintering is 720-750°C, the time at peak temperature is 2-4 seconds, and the atmosphere is compressed air.
[0090] At this point, the preparation of the back contact passivated contact solar cell is completed. In the metallization interconnection and packaging of the components, a conductive backplane (including a printed circuit board) can be used to connect the third electrode units at the projection of the periodic lattice and discrete through holes on the back of the cell to achieve current convergence, thereby conducting the photogenerated carriers collected by the front of the cell to the external circuit.
[0091] Example 2 provides a back contact passivation contact solar cell with a p-type single crystal silicon substrate. The cell structure is as follows: Figure 2 The dot pattern design of the through holes on the battery surface is similar to the design method of Example 1. In the battery preparation, the p + The boron doping required for the -p high-low junction and local hole passivation contact area can be prepared by masked ion implantation combined with thermal annealing. The tunneling silicon oxide and phosphorus-doped polysilicon in the electronic passivation contact area on the back of the battery are prepared by PECVD online doping combined with thermal annealing. The through-hole is prepared by a low-damage laser etching method, and the through-hole metallization is achieved by screen printing aluminum paste combined with rapid thermal treatment alloying. The lattice area metallization at the intersection of the through-hole and the front and back of the battery is achieved by screen printing silver paste combined with rapid thermal treatment sintering. The specific battery preparation process is similar to Example 1 and will not be described here.
[0092] Finally, it should be noted that, although the implementation scheme of the utility model is described above in conjunction with the accompanying drawings, the utility model is not limited to the above-mentioned specific implementation scheme and application field. The above-mentioned specific implementation scheme is only illustrative and instructive, and is used to help understand the method and its core idea of the utility model, but is not restrictive. Under the enlightenment of this specification, ordinary technicians in this field can make many forms of changes, improvements and equivalent implementations in the specific implementation scheme and application scope without departing from the scope of protection of the principles of the utility model and the claims, which should also be regarded as the protection scope of the utility model.
Claims
1. A passivated contact crystalline silicon solar cell with a back contact structure, characterized in that: include: Silicon substrate; A through hole that penetrates the silicon substrate and is distributed in a periodic lattice; the sidewalls of the through hole are sequentially covered by an electrical insulating isolation layer and a first electrode unit from the inside to the outside, and are formed by the through hole of the first electrode unit; A local passivation contact area is formed on the first surface of the silicon substrate, the local passivation contact area has a plurality of periodic lattice distributed passivation contact units, the passivation contact unit is an annular area, the overall area included in the outer contour and the projection of the through hole on the first surface of the silicon substrate have the same shape and geometric center, and the area of the overall area is larger than the projection area of the through hole on the first surface of the silicon substrate; the local passivation contact area includes tunneling silicon oxide and first doped polysilicon, and the doping type of the first doped polysilicon is the same as that of the silicon substrate; A high-low junction region is formed outside the local passivation contact region on the first surface of the silicon substrate, and the doping type of the high-low junction region is the same as that of the silicon substrate; an anti-reflection film formed on the first surface of the silicon substrate; A second electrode formed on the first surface of the silicon substrate, the second electrode having a plurality of second electrode units distributed in a periodic lattice, the second electrode unit and the projection of the through hole on the first surface of the silicon substrate having the same shape and geometric center, and an area greater than the projection area of the through hole on the first surface of the silicon substrate and less than or equal to the area of the passivation contact unit; An electrically insulating isolation region is formed on the second surface of the silicon substrate, wherein the electrically insulating isolation region has a plurality of electrically insulating isolation units distributed in a periodic lattice, wherein the electrically insulating isolation unit is an annular region, wherein the overall region included in the outer contour thereof and the projection of the through hole on the second surface of the silicon substrate have the same shape and geometric center, and the area of the overall region is greater than the projection area of the through hole on the second surface of the silicon substrate; A passivation contact region is formed outside the electrically insulating isolation region on the second surface of the silicon substrate, the passivation contact region comprising tunneling silicon oxide and second doped polysilicon, wherein the doping type of the second doped polysilicon is opposite to that of the silicon substrate; A passivation layer for passivating the second surface of the silicon substrate; A third electrode is formed at the intersection of the through hole and the second surface of the silicon substrate, wherein the third electrode has a plurality of first electrode units distributed in a periodic lattice, and the projection of the third electrode unit and the through hole on the first surface of the silicon substrate have the same shape and geometric center, and the area is smaller than the projection area of the through hole on the second surface of the silicon substrate; The first electrode unit is connected to the second electrode unit and the third electrode unit respectively at the intersection with the first surface and the second surface of the silicon substrate; A fourth electrode is formed in the passivation contact region on the second surface of the silicon substrate, and projections of the fourth electrode and the through hole on the same horizontal plane are completely offset.
2. The passivated contact crystalline silicon solar cell according to claim 1, characterized in that: The pattern of the periodic lattice distribution of the through holes is rectangular or rhombus; the shape of the through holes is any one of circular, rectangular, rhombus, and elliptical; the arrangement period of the through holes is 250-5000 microns, and the area percentage is 0.05%-0.7%.
3. The passivated contact crystalline silicon solar cell according to claim 2, characterized in that: When the through hole is circular in shape, the diameter of the through hole is 10-500 microns, and the diameter of the overall area included in the outer contour of the electrically insulating isolation unit is 100-2500 microns; when the through hole is square, the side length of the through hole is 10-500 microns; the side length of the overall area included in the outer contour of the electrically insulating isolation unit is 100-2500 microns.
4. The passivated contact crystalline silicon solar cell according to any one of claims 1 to 3, characterized in that: The light shielding rate of the second electrode is 0.05%-0.8%.
5. The passivated contact crystalline silicon solar cell according to any one of claims 1 to 3, characterized in that: The electrical insulating isolation layer and the passivation layer are both made of silicon nitride and have the same thickness.
6. The passivated contact crystalline silicon solar cell according to claim 5, characterized in that: The passivation layer is silicon nitride with a thickness of 50-300 nm and a refractive index of 1.9-2.
2.
7. The passivated contact crystalline silicon solar cell according to any one of claims 1 to 3, characterized in that: In the local passivation contact area on the first surface of the silicon substrate, the thickness of the tunneling silicon oxide is 1.2-1.6 nm, and the refractive index is 1.45-1.5; the thickness of the first doped polysilicon is 5-500 nm; In the passivation contact area on the second surface of the silicon substrate, the thickness of the tunneling silicon oxide is 1.2-1.6 nm, and the refractive index is 1.45-1.5; the thickness of the second doped polysilicon is 5-500 nm.
8. The passivated contact crystalline silicon solar cell according to any one of claims 1 to 3, characterized in that: The anti-reflection film is silicon nitride with a thickness of 70-80 nm and a refractive index of 1.9-2.
1.
9. The passivated contact crystalline silicon solar cell according to any one of claims 1 to 3, characterized in that: The second electrode and the third electrode are silver electrodes; and the first electrode unit is an aluminum electrode.
10. The passivated contact crystalline silicon solar cell according to any one of claims 1 to 3, characterized in that: The fourth electrode is a gate line electrode.