A thermal insulation casting sand mold

By using insulated casting sand molds in the casting process, combined with insulation components and intermediate riser cavities, the shrinkage problem at the isolated hot spot on the outer circle of the guide wheel was solved, enabling mass production of high-quality castings.

CN224977436UActive Publication Date: 2026-11-17HEBEI NORTH CASTING IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202522622398.9
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2025-12-10
Publication Date
2026-11-17
Estimated Expiration
2035-12-10

AI Technical Summary

Technical Problem

Without setting risers or adding physical subsidies, shrinkage defects are prone to occur at the isolated hot spot on the outer circle of the guide wheel, affecting the internal quality of the casting and failing to meet the usage requirements, thus becoming a technical bottleneck for mass production.

Method used

The heat-insulating casting sand mold is adopted, which includes the sand mold body, heat insulation components and isolation layer. The heat insulation components are set on the side wall of the wheel spoke area of ​​the casting. The middle riser cavity is connected to the isolated hot spot area. The heat insulation components slow down the heat diffusion, and the middle riser cavity provides feeding to avoid coarse grains and quenching cracks, thereby improving the quality of the casting.

Benefits of technology

Eliminating the need for risers and physical subsidies reduces production costs, avoids quenching cracks and shrinkage defects, improves the internal quality of castings, and breaks through the technical bottleneck of mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN224977436U_ABST
    Figure CN224977436U_ABST
Patent Text Reader

Abstract

This utility model relates to the field of casting technology, and provides a heat-insulating sand mold for casting guide wheel castings. It includes a sand mold body, with multiple isolated hot spot areas corresponding to the inner side of the outer circle of the guide wheel casting connected to the central area of ​​the sand mold body. The central area of ​​the sand mold body is provided with an intermediate riser cavity for feeding. A heat-insulating component is disposed on the inner wall of the sand mold body corresponding to the spoke area of ​​the guide wheel casting. The heat-insulating component is used to slow down the diffusion of heat from the spoke area of ​​the guide wheel casting into the interior of the sand mold body. This effectively solves the shrinkage cavity defect at the isolated hot spots, eliminates the risk of shrinkage cavities up to 100,000 cubic millimeters in volume, improves the internal quality of the casting, and solves the technical problem in the prior art where shrinkage cavities easily occur at the isolated hot spots on the outer circle without adding risers or physical subsidies.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This utility model relates to the field of casting technology, specifically to a heat-insulating casting sand mold. Background Technology

[0002] As a key load-bearing and guiding component of the chassis travel system, the idler wheel of large mechanical excavators is experiencing continuously increasing demand and technical requirements. During the research and development and production of idler wheels, it was discovered that currently produced idler wheels weigh nearly 5 tons each. Due to the need to withstand long-term heavy loads, impacts, and complex working conditions, their outer surface requires surface hardening to enhance hardness and wear resistance. At the same time, extremely high requirements are placed on the surface finish and internal density of the castings, and the castings must not contain defects that affect structural strength.

[0003] However, due to the design characteristics of the outer circumference of the guide wheel, there are obvious isolated hot spots in its outer circumference area. In traditional casting processes, to eliminate shrinkage defects caused by the solidification shrinkage of molten steel at the hot spots, risers are usually set at the corresponding positions of the hot spots to achieve feeding. However, since the outer circumference of this guide wheel needs to be surface hardened, setting risers would result in coarse grains inside the casting in the area corresponding to the riser, which would easily cause quenching cracks during subsequent surface hardening, leading to direct scrapping. Considering the overall assembly and structural performance stability, it is not allowed to adjust the existing casting structure of the guide wheel, making the traditional riser feeding solution completely infeasible.

[0004] After ruling out the two conventional solutions of riser feeding and structural adjustment, some companies in the industry use physical subsidies to increase the thermal modulus and optimize the feeding channel to address the shrinkage cavity problem in isolated hot sections. However, physical subsidies not only increase steel consumption and subsequent machining allowance, raising production costs, but may also affect the overall stress distribution of the casting due to the subsidy structure, posing potential structural risks. Therefore, it is not the optimal solution, making it difficult to solve the shrinkage cavity defect at the isolated hot section on the outer circle of the guide wheel. Without adding risers or physical subsidies, the isolated hot section on the outer circle of the guide wheel is prone to shrinkage cavities with a volume of up to 100,000 cubic millimeters, which seriously affects the internal quality of the casting and fails to meet the usage requirements. This has become the core technical bottleneck restricting the mass production and quality stability of guide wheels. Utility Model Content

[0005] To overcome the above-mentioned defects, the present invention provides an insulated casting sand mold, which solves the technical problem that shrinkage defects are easily generated at the isolated hot spot on the outer circle in the prior art without the use of risers or additional physical subsidies.

[0006] According to one aspect, at least one embodiment of the present invention provides a heat-insulating casting sand mold for casting guide wheel castings, comprising: The sand mold body has multiple isolated hot spot areas on the inner side of the outer circle of the guide wheel casting connected to the central area of ​​the sand mold body, and the central area of ​​the sand mold body is provided with an intermediate riser cavity for feeding. A heat insulation component is disposed on the inner sidewall of the guide wheel casting spoke area corresponding to the sand mold body. The heat insulation component is used to slow down the diffusion of heat from the guide wheel casting spoke area into the sand mold body.

[0007] Optional, also includes: An isolation layer is provided between the heat insulation component and the cavity of the guide wheel casting corresponding to the surface of the sand mold body, in order to prevent the heat insulation component from directly contacting the guide wheel casting body.

[0008] Optionally, the isolation layer is a chromite sand isolation layer, and the thickness of the isolation layer is 10-15mm.

[0009] Optionally, there are several heat insulation components, each corresponding to a spoke area of ​​a guide wheel casting, and the several heat insulation components are arranged around the circumference of the sand mold body.

[0010] Optionally, the central axis of each insulation component coincides with the central axis of the corresponding isolated hot spot region.

[0011] Optionally, the insulation component is a high-silica insulation board.

[0012] Optionally, the intermediate riser cavity is a cylindrical structure with a height-to-inner diameter ratio of 1.2-1.5.

[0013] Optionally, a sealing layer is provided in the gap between the root of the intermediate riser cavity and the inner wall of the sand mold body.

[0014] Optionally, the thickness of the sealing layer is 2-3 mm.

[0015] Optionally, the sand mold body is provided with a core cover assembly.

[0016] The beneficial effects of this utility model are as follows: In this invention, there is no need to set a riser at the hot spot on the outer circle of the guide wheel, thus avoiding the problem of quenching cracks caused by coarse grains in the riser area and meeting the requirements of surface quenching process; no physical subsidies are added, reducing steel consumption and subsequent machining allowance, lowering production costs, and avoiding the stress distribution risk brought by the subsidy structure; it effectively solves the shrinkage cavity defect at the isolated hot spot, eliminates the hidden danger of shrinkage cavities with a volume of up to 100,000 cubic millimeters, improves the internal quality of castings, and breaks through the technical bottleneck of mass production. Attached Figure Description

[0017] To more clearly illustrate the technical solutions in the embodiments of this utility model, the accompanying drawings used in the description of the embodiments of this utility model will be briefly introduced below. Obviously, the drawings described below are merely some exemplary embodiments of this utility model. For those skilled in the art, other drawings can be obtained based on the content of the exemplary embodiments of this utility model and these drawings without any creative effort.

[0018] Figure 1 This is a schematic diagram of the structure of the heat-insulating casting sand mold in one embodiment of the present invention; Figure 2 for Figure 1 The front view of the insulating casting sand mold in the embodiment; Figure 3 for Figure 2 The cross-sectional view at point AA in the embodiment.

[0019] In the diagram: 1. Sand mold body, 2. Isolated hot spot area, 3. Intermediate riser cavity, 4. Insulation component, 5. Spoke area, 6. Isolation layer. Detailed Implementation

[0020] The present invention will now be described in further detail with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative of the present invention and not intended to limit its scope.

[0021] To keep the drawings concise, only the parts relevant to the utility model are shown schematically in each drawing; these do not represent the actual structure of the product. Furthermore, for ease of understanding, in some drawings, only one of the components with the same structure or function is schematically shown, or only one is labeled. In this document, "a" not only means "only one," but can also mean "more than one," and "several" includes "two" and "more than two."

[0022] In this document, it should be noted that, unless otherwise explicitly specified and limited, the terms "installation," "connection," and "linking" should be interpreted broadly. For example, they can refer to fixed connections, detachable connections, or integral connections; they can refer to mechanical connections or electrical connections; they can refer to direct connections or indirect connections through an intermediate medium; and they can refer to the internal connection between two components. Those skilled in the art can understand the specific meaning of the above terms in this utility model based on the specific circumstances.

[0023] In this invention, unless otherwise explicitly specified and limited, "above" or "below" the second feature can include direct contact between the first and second features, or contact between the first and second features through another feature between them. Furthermore, "above," "over," and "on top" of the second feature includes the first feature directly above or diagonally above the second feature, or simply indicates that the first feature is at a higher horizontal level than the second feature. "Below," "below," and "under" the second feature includes the first feature directly below or diagonally below the second feature, or simply indicates that the first feature is at a lower horizontal level than the second feature.

[0024] In the description of this embodiment, terms such as "upper," "lower," "left," and "right" are based on the orientation or positional relationship shown in the accompanying drawings. They are used only for the convenience of description and simplification of operation, and are not intended to indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this utility model.

[0025] Furthermore, in the description of this application, the terms "first," "second," etc., are used only to distinguish descriptions and should not be construed as indicating or implying relative importance.

[0026] like Figures 1-3 As shown, this invention illustrates a heat-insulating casting sand mold in one embodiment of the present invention, used for casting guide wheel castings. It includes a sand mold body 1, with multiple isolated hot spot regions 2 corresponding to the inner side of the outer circle of the guide wheel casting connected to the central region of the sand mold body 1. The central region of the sand mold body 1 is provided with an intermediate riser cavity 3 for feeding. A heat-insulating component 4 is disposed on the inner wall of the sand mold body 1 corresponding to the spoke region 5 of the guide wheel casting. The heat-insulating component 4 is a cut heat-insulating plate with an original thickness of 50mm. The cut shape and size of the heat-insulating plate are adapted to the heat dissipation of the spoke region 5 of the guide wheel casting. The heat-insulating component 4 is used to slow the diffusion of heat from the spoke region 5 of the guide wheel casting into the sand mold body 1. The heat insulation component 4 reduces the heat dissipation surface area of ​​the guide wheel casting spoke area 5 and increases the thermal modulus of the spoke area 5 (thermal modulus = casting area volume / heat dissipation surface area), thereby opening up the feeding channel between the intermediate riser cavity 3 and the four isolated hot section areas 2 corresponding to the sand mold body 1.

[0027] In the above-described scheme, this embodiment provides a heat-insulating casting sand mold for casting large mechanical excavator idler wheel castings with a single weight of nearly 5 tons. The sand mold body 1 is adapted to the overall outline of the idler wheel casting. Multiple isolated hot spot regions 2 are evenly distributed along the circumference of the inner side of the outer circle of the sand mold body 1 corresponding to the idler wheel casting. For example, there are 4 isolated hot spot regions 2, each of which has a radial flow channel. The inner diameter of the flow channel is adapted to the maximum cross-sectional width of the isolated hot spot region 2, and all flow channels are connected to the central area of ​​the sand mold body 1. The central area of ​​the sand mold body 1 has an integrally formed intermediate riser cavity 3 for feeding, and the axis of the cavity coincides with the central axis of the sand mold body 1. The heat insulation component 4 is a prefabricated heat insulation structural component, which is positioned and installed through the groove reserved in the inner wall of the sand mold body 1, and is fitted to the inner wall of the four spoke regions 5 of the idler wheel casting corresponding to the sand mold body 1. The coverage area of ​​the heat insulation component 4 is completely matched with the inner wall area of ​​the spoke region 5.

[0028] During casting, molten steel enters the mold cavity from the sand mold gate, sequentially filling the outer circumference of the guide wheel, the spokes, and the central area, ultimately filling the intermediate riser cavity 3. During solidification, the heat insulation component 4 slows the heat diffusion from the spoke area 5 into the sand mold body 1, maintaining the temperature of the spoke area 5 at a higher level and preventing the formation of a closed solidified layer in the isolated hot spot area 2 due to rapid cooling of the spokes. Simultaneously, the central riser cavity 3, due to its concentrated volume and long heat dissipation path, retains molten steel in a liquid state for a longer time than the isolated hot spot area 2, continuously replenishing the isolated hot spot area 2 with the molten steel required for solidification shrinkage through radial flow channels. After overall solidification is complete, the remaining solidified molten steel in the intermediate riser and flow channels is cleaned. There is no need to set a riser at the hot spot on the outer circle of the guide wheel, which avoids the problem of quenching cracks caused by coarse grains in the riser area and meets the requirements of surface quenching process; no physical subsidies are added, which reduces the consumption of molten steel and subsequent machining allowance, lowers production costs, and avoids the stress distribution risk brought by the subsidy structure; it effectively solves the shrinkage cavity defect at the isolated hot spot, eliminates the hidden danger of shrinkage cavity with a volume of up to 100,000 cubic millimeters, improves the internal quality of castings, and breaks through the technical bottleneck of mass production.

[0029] Furthermore, the heat-insulating casting sand mold also includes an isolation layer 6, which is disposed between the heat-insulating component 4 and the cavity corresponding to the guide wheel casting spoke surface of the sand mold body 1, to prevent the heat-insulating component 4 from directly contacting the guide wheel casting body. The chromite sand isolation layer 6 fills the cavity between the heat-insulating component 4 and the cavity corresponding to the guide wheel casting spoke surface of the sand mold body 1.

[0030] In the above scheme, the isolation layer 6 is made of high-temperature resistant granular refractory material. After the insulation component 4 is installed, the isolation layer 6 is placed between the insulation component 4 and the cavity of the corresponding guide wheel casting spoke surface of the sand mold body 1 using a special tool. The isolation layer 6 ensures that the insulation component 4 does not directly contact the spoke casting body. During casting, when molten steel fills the spoke cavity, it first comes into contact with the isolation layer 6, which prevents the insulation component 4 from directly contacting the high-temperature molten steel and the casting body. During solidification, the insulation component 4 indirectly insulates the spoke area 5 through the isolation layer 6, slowing down heat diffusion. At the same time, the isolation layer 6 prevents the insulation component 4 from sticking to the casting at high temperatures. During cleaning, the isolation layer 6 disintegrates along with the sand mold, separating from the insulation component 4 and sand mold residue. To prevent the insulation component 4 from directly contacting the high-temperature casting body, and to prevent the insulation component 4 from softening or melting and sticking to the casting surface due to high temperature, thus ensuring the surface smoothness of the casting spokes; the isolation layer 6 can buffer the assembly error between the insulation component 4 and the sand mold body 1, ensuring the stability of the insulation effect; and to simplify the casting cleaning process, reducing the risk of surface damage to the casting caused by the adhesion of the insulation component 4.

[0031] Furthermore, the isolation layer 6 is a chromite sand isolation layer 6, and the thickness of the isolation layer 6 is 10-15mm.

[0032] In the above scheme, the isolation layer 6 of this embodiment is made of chromite sand. Uniformly sized chromite sand particles are selected through sieving and laid between the insulation component 4 and the spoke cavity. During casting, the high-temperature molten steel comes into contact with the chromite sand isolation layer 6. The chromite sand maintains structural stability due to its high-temperature resistance, preventing melting or decomposition. The heat from the insulation component 4 is slowly transferred to the spoke area 5 through the chromite sand isolation layer 6, maintaining the temperature of the spoke area 5. After solidification, the chromite sand disintegrates together with the sand mold body 1, easily separating from the casting.

[0033] Furthermore, there are several heat insulation components 4, and each heat insulation component 4 corresponds one-to-one with the spoke area 5 of the guide wheel casting. The several heat insulation components 4 are arranged along the circumference of the sand mold body 1.

[0034] In the above scheme, this embodiment has four heat-insulating components 4, each corresponding to one of the four spoke regions 5 of the guide wheel casting. The outer contour of each heat-insulating component 4 is perfectly fitted with the curved surface of the inner wall of the corresponding spoke region 5, and is fixed by a positioning pin preset on the sand mold body 1. The four heat-insulating components 4 are evenly arranged around the central axis of the sand mold body 1. After casting, the four heat-insulating components 4 simultaneously insulate their respective spoke regions 5. Due to the uniform arrangement, the heat diffusion rate of each spoke region 5 is the same, resulting in a uniform temperature field distribution throughout the guide wheel casting. The central riser cavity 3 feeds the corresponding four isolated hot spot regions 2 synchronously through four radial flow channels, ensuring that the feeding amount of each hot spot region is consistent. The one-to-one correspondence makes the heat-insulating effect more precise, avoiding the problem of excessively rapid local cooling due to deviations in the heat-insulating range; the uniform circumferential arrangement ensures the symmetry of the overall temperature field of the casting, reduces the internal stress caused by uneven temperature, and improves the structural stability of the casting.

[0035] Furthermore, the central axis of each insulation component 4 coincides with the central axis of the corresponding isolated hot spot region 2.

[0036] In the above scheme, the central axis of each insulation component 4 in this embodiment is completely coincident with the central axis of the corresponding isolated hot spot region 2. During solidification, the heat released by the insulation component 4 diffuses outward from its own central axis. Because it is coaxial with the isolated hot spot region 2, the heat can accurately cover the core area of ​​the hot spot, significantly slowing down the cooling rate of this area. At the same time, the coaxial design allows the flow channels to be arranged along the axial direction, so that the molten steel from the intermediate riser can reach the hot spot region along the shortest path, improving the feeding efficiency. The feeding channels are arranged along the axial direction, shortening the feeding path, reducing feeding resistance, ensuring that molten steel is replenished to the hot spot region in a timely manner, further reducing the risk of shrinkage and ensuring the consistency of the feeding effect in each hot spot region.

[0037] Furthermore, the insulation component 4 is a high-silica insulation board. The high-silica insulation board has a bulk density ≤0.6g / cm3 and a thermal conductivity ≤0.12W / (m·K) at room temperature (25℃). An adhesive fixing layer is provided between the insulation component 4 and the inner wall of the sand mold body 1. The adhesive fixing layer is a water glass adhesive layer with a thickness of 1-3mm, which is used to firmly attach the insulation component 4 to the inner wall of the corresponding spoke area 5 of the sand mold body 1.

[0038] In the above scheme, after casting, as heat from the spoke region 5 diffuses to the sand mold body 1, the high-silica insulation board, due to its low thermal conductivity, significantly reduces the heat transfer rate, thus prolonging the time the temperature of the spoke region 5 remains above the liquidus. Simultaneously, the high-silica insulation board maintains structural stability at high temperatures, without deformation or decomposition, and continues to provide insulation until the casting solidifies.

[0039] Furthermore, the intermediate riser cavity 3 has a cylindrical structure with a height-to-inner-diameter ratio of 1.2-1.5. The cylindrical structure facilitates the integral molding of the sand mold body 1, reducing processing difficulty and manufacturing costs. The 1.2-1.5 height-to-diameter ratio ensures sufficient feeding capacity of the riser while preventing shrinkage cavities within the riser itself. A ratio of 1.35 achieves a balance between feeding efficiency and riser quality. Polished inner walls reduce resistance to molten steel flow, ensuring unobstructed feeding channels and improving the feeding effect.

[0040] Furthermore, a sealing layer is provided at the gap between the root of the intermediate riser cavity 3 and the inner wall of the sand mold body 1.

[0041] In the above scheme, during casting, high-temperature molten steel impacts the root area of ​​the intermediate riser cavity 3. The sealing layer, with its high-temperature resistance and tight-fitting structure, prevents molten steel from seeping into the gaps. During solidification, the sealing layer maintains structural stability, avoiding insufficient feeding due to gap leakage. During cleaning, the sealing layer disintegrates along with the sand mold body 1, making it easy to clean. This effectively seals the gaps at the root of the intermediate riser cavity 3, preventing molten steel leakage, ensuring effective feeding of the intermediate riser, and avoiding shrinkage defects caused by leakage. The refractory clay material is suitable for high-temperature conditions, does not melt or detach, and provides stable sealing performance. The sealing layer disintegrates synchronously with the sand mold, without increasing the difficulty of casting cleaning, thus improving production efficiency.

[0042] Furthermore, the sealing layer thickness is 2-3 mm.

[0043] In the above scheme, during casting, the sealing layer effectively blocks the penetration of high-temperature molten steel. Simultaneously, due to its moderate thickness, it does not excessively increase the thermal resistance at the riser root and does not affect the solidification sequence of the riser. During solidification, the thickness stability of the sealing layer ensures the continuity of the sealing effect until the casting is completely solidified.

[0044] Furthermore, a cover core assembly is provided on the sand mold body 1.

[0045] In the above scheme, after the sand mold body 1 is assembled, the cover core assembly is placed on top of the sand mold body 1 and fixed by positioning bosses and grooves. During casting, the cover core assembly prevents cold air from entering the sand mold, reducing heat loss and maintaining a high-temperature environment inside the sand mold. At the same time, the circular hole in the center of the cover core assembly provides a top opening for the intermediate riser cavity 3, without affecting the venting and feeding functions of the riser. After solidification, the cover core assembly is removed first, followed by subsequent sand mold cleaning. The cover core assembly can reduce heat loss inside the sand mold, maintain a stable solidification temperature field, and provide a more favorable environment for intermediate riser feeding and insulation component 4; it prevents external impurities from entering the sand mold, ensuring the surface finish and internal quality of the casting; and the use of the same material avoids deformation of the cover core assembly or cracking of the sand mold due to differences in thermal expansion coefficients, improving the overall structural stability of the sand mold.

[0046] It should be noted that the above embodiments are only used to illustrate the technical solution of this utility model and are not intended to limit it. Although this utility model has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solution of this utility model without departing from the spirit and scope of the technical solution of this utility model, and all such modifications or substitutions should be covered within the scope of the claims of this utility model.

Claims

1. An insulating casting sand mold for casting a guide wheel casting, characterized in that, include: Sand mold body (1), the multiple isolated hot spot areas (2) on the inner side of the outer circle of the guide wheel casting are connected to the central area of ​​the sand mold body (1), and the central area of ​​the sand mold body (1) is provided with an intermediate riser cavity (3) for feeding. The heat insulation component (4) is disposed on the inner side wall of the guide wheel casting spoke area (5) of the sand mold body (1). The heat insulation component (4) is used to slow down the heat diffusion from the guide wheel casting spoke area (5) into the sand mold body (1).

2. The heat-insulating casting sand mold according to claim 1, characterized in that, Also includes: An isolation layer (6) is provided between the heat insulation component (4) and the cavity of the guide wheel casting surface of the sand mold body (1) to prevent the heat insulation component (4) from directly contacting the guide wheel casting body.

3. The heat-insulating casting sand mold according to claim 2, characterized in that, The isolation layer (6) is a chromite sand isolation layer (6), and the thickness of the isolation layer (6) is 10-15mm.

4. The heat-insulating casting sand mold according to claim 1, characterized in that, The heat insulation component (4) has several units, and each heat insulation component (4) corresponds to a wheel spoke area (5) of a guide wheel casting. The several heat insulation components (4) are arranged around the circumference of the sand mold body (1).

5. The heat-insulating casting sand mold according to claim 1, characterized in that, The central axis of each insulation component (4) coincides with the central axis of the corresponding isolated hot spot region (2).

6. The heat-insulating casting sand mold according to claim 1, characterized in that, The insulation component (4) is a high-silica insulation board.

7. The heat-insulating casting sand mold according to claim 1, characterized in that, The intermediate riser cavity (3) is a cylindrical structure with a height-to-inner diameter ratio of 1.2-1.

5.

8. The heat-insulating casting sand mold according to claim 1, characterized in that, A sealing layer is provided at the gap between the root of the intermediate riser cavity (3) and the inner wall of the sand mold body (1).

9. The heat-insulating casting sand mold according to claim 8, characterized in that, The thickness of the sealing layer is 2-3 mm.

10. The heat-insulating casting sand mold according to claim 1, characterized in that, The sand mold body (1) is provided with a cover core assembly.