Contact rail

By using a composite plate structure and pressure welding to connect the contact rails, the problems of poor welding quality and high production costs were solved, achieving high flatness and stable power supply, and improving the shoe-rail coupling performance and service life.

CN224979548UActive Publication Date: 2026-11-17CRRC ZHUZHOU ROLLING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202522451290.8
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2025-11-19
Publication Date
2026-11-17
Estimated Expiration
2035-11-19

AI Technical Summary

Technical Problem

The poor welding quality of the existing contact rail results in poor flatness of the flow receiving surface, poor shoe-rail coupling, and high production costs.

Method used

The composite plate structure is adopted, and the metal layer is connected to the substrate by pressure welding. Combined with the interlocking structure and honeycomb reinforcing groove design, the contact area and connection stability are ensured, and the production cost is reduced.

Benefits of technology

This improved the compatibility of the contact rail, ensuring a continuous and stable power supply for the train, extending its service life, and reducing manufacturing difficulty and cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN224979548U_ABST
    Figure CN224979548U_ABST
Patent Text Reader

Abstract

This application discloses a contact rail, comprising: a substrate; and a composite plate, including a wear-resistant layer and a metal layer stacked and integrally formed along the thickness direction. A first interlocking structure is provided on the side of the metal layer away from the wear-resistant layer, and a second interlocking structure is provided on the top surface of the substrate facing the composite plate. The first interlocking structure and the second interlocking structure are interlocked. The metal layer and the substrate are pressure welded together. By using the composite plate, the width of the receiving surface (i.e., the width of the wear-resistant layer) and the shape of the substrate can be freely selected according to actual needs, significantly improving the adaptability of the contact rail and reducing the manufacturing difficulty for different scenarios. The interlocking connection between the metal layer and the substrate significantly improves the contact area and connection stability, providing a good foundation for welding connections. The pressure welding connection method not only reduces production costs but also effectively ensures the flatness of the composite plate, thereby improving the shoe-rail coupling performance and ensuring a continuous and stable power supply for the train.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of contact rail technology, and particularly relates to a contact rail. Background Technology

[0002] As a core component of the rail transit power supply system, the contact rail's main function is to provide continuous and stable electrical energy to the train through sliding contact with the vehicle's current collector. Therefore, it must simultaneously meet three core requirements: high conductivity, high wear resistance, and high connection stability. In related technologies, contact rails are generally made of composite materials, with the top layer using a material with good wear resistance and the base material using a material with high conductivity. They are connected using argon arc welding or other fusion electrode shielded welding methods. This connection method generally makes it difficult to guarantee welding quality, resulting in poor flatness of the current-receiving surface and poor shoe-rail coupling after final molding. Utility Model Content

[0003] This application aims to address at least one of the technical problems existing in the prior art. To this end, this application proposes a contact rail with good welding quality, low production cost, high flatness of the flow-receiving surface, and good shoe-rail coupling performance.

[0004] In a first aspect, this application provides a contact rail, comprising: Matrix; The composite panel includes a wear-resistant layer and a metal layer that are stacked and integrally formed along the thickness direction. A first interlocking structure is provided on the side of the metal layer away from the wear-resistant layer, and a second interlocking structure is provided on the top surface of the substrate facing the composite panel. The first interlocking structure and the second interlocking structure are interlocked. The metal layer is pressure welded to the substrate.

[0005] According to the contact rail of this application, by setting a composite plate, the width of the flow-receiving surface (i.e., the width of the wear-resistant layer) and the shape of the substrate can be freely selected according to actual needs, which greatly improves the adaptability of the contact rail and reduces the manufacturing difficulty for different scenarios; by interlocking the metal layer with the substrate, the contact area and connection stability of the two are significantly improved, providing a good foundation for welding connection; the pressure welding connection method not only reduces the production cost, but also effectively ensures the flatness of the composite plate, thereby improving the shoe-rail coupling performance and ensuring that the train receives a continuous and stable power supply.

[0006] According to one embodiment of this application, one of the first fitting structure and the second fitting structure includes a plurality of protrusions spaced apart along the width direction of the composite plate, and the other of the first fitting structure and the second fitting structure includes a plurality of recesses spaced apart along the width direction of the composite plate, wherein the plurality of protrusions and the plurality of recesses are fitted together in a one-to-one correspondence.

[0007] According to one embodiment of this application, the outer wall of the protrusion fits against the inner wall of the concave portion.

[0008] According to one embodiment of this application, among the plurality of protrusions, the height of the two protrusions located at both ends in the width direction of the composite plate is less than the height of the other protrusions.

[0009] According to one embodiment of this application, the protrusion extends along the length direction of the composite plate, the cross-section of the protrusion is rectangular, or the width of the protrusion tends to decrease along the direction close to the concave portion.

[0010] According to one embodiment of this application, a flow guide hole is provided at the bottom of the recess, and the flow guide hole penetrates the substrate.

[0011] According to one embodiment of this application, at least one of the plurality of protrusions is provided with a first anti-mistake part, and at least one of the plurality of recesses is provided with a second anti-mistake part, wherein the first anti-mistake part and the second anti-mistake part are correspondingly engaged.

[0012] According to one embodiment of this application, the surface of the metal layer facing the wear-resistant layer is provided with uniformly distributed honeycomb reinforcing grooves, and the side of the wear-resistant layer facing the metal layer is provided with a reinforcing portion that fits into the honeycomb reinforcing grooves.

[0013] According to one embodiment of this application, the wear-resistant layer has slots extending along the length direction at both ends in the width direction, and the metal layer has slots extending along the length direction at both ends in the width direction, with the slots fitting into the slots.

[0014] According to one embodiment of this application, the thickness of the composite plate is 10mm-12mm, the thickness of the wear-resistant layer is 3mm-5mm, and the thickness of the metal layer is 5mm-9mm.

[0015] Additional aspects and advantages of this application will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of this application. Attached Figure Description

[0016] The above and / or additional aspects and advantages of this application will become apparent and readily understood from the description of the embodiments taken in conjunction with the following drawings, in which: Figure 1 This is a schematic diagram of the contact rail structure provided in an embodiment of this application; Figure 2 This is another structural schematic diagram of the contact rail provided in an embodiment of this application; Figure 3 This is a schematic diagram of the structure of the composite plate provided in the embodiment of this application.

[0017] Figure label: 100. Contact rail; 110. Substrate; 111. Protrusion; 120. Composite plate; 121. Wear-resistant layer; 122. Metal layer; 1221. Recess. Detailed Implementation

[0018] The embodiments of this application are described in detail below. Examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions throughout. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain this application, and should not be construed as limiting this application.

[0019] The following is for reference. Figure 1-Figure 1 , Figure 2 and Figure 3 A contact rail is described according to an embodiment of this application.

[0020] Please see Figure 1 , Figure 2 and Figure 3 This application provides a contact rail 100, which includes a substrate 110 and a composite plate 120.

[0021] The composite plate 120 includes a wear-resistant layer 121 and a metal layer 122 that are stacked and integrally formed along the thickness direction. A first fitting structure is provided on the side of the metal layer 122 away from the wear-resistant layer 121, and a second fitting structure is provided on the top surface of the substrate 110 facing the composite plate 120. The first fitting structure and the second fitting structure are fitted together. The metal layer 122 is pressure welded to the substrate 110.

[0022] The base 110 is the fundamental load-bearing and conductive core component of the contact rail 100. Its material can be a metal with high conductivity, such as 6-series aluminum alloy (AlMgSi alloy), CuCrZr alloy, CuNi2SiCr alloy, Cu-Ag alloy, etc. These materials ensure that the contact rail 100 has good conductivity, transmitting continuous and stable electrical energy to the train. The overall shape of the base 110 can be designed according to the actual installation requirements of rail transit, commonly including I-shaped and C-shaped designs, to adapt to different track installation spaces and load-bearing requirements.

[0023] The composite plate 120 is formed by stacking and molding a wear-resistant layer 121 and a metal layer 122 along the thickness direction. This integral molding structure ensures a tight connection between the two layers and prevents delamination during subsequent use. The wear-resistant layer 121, as the part that directly contacts the contact rail 100 with the vehicle's current receiver, needs to have excellent wear resistance. Its material can be stainless steel, wear-resistant alloys, such as 304 stainless steel or high manganese steel. These materials can effectively reduce the wear caused by sliding friction of the current receiver and extend the service life of the contact rail 100. The metal layer 122 serves as a transitional connection and provides conductivity. Its material should be a metal with good weldability to the base material 110 and high conductivity, such as pure copper or a copper-aluminum composite layer, to achieve a stable connection with the base material 110 and smooth power transmission.

[0024] A first fitting structure is provided on the side of the metal layer 122 away from the wear-resistant layer 121, and a second fitting structure is provided on the top surface of the substrate 110 facing the composite plate 120. The first fitting structure and the second fitting structure are fitted together. The fitting structure can take various forms, such as the first fitting structure being a protrusion and the second fitting structure being a groove matching the protrusion; or the first fitting structure being a dovetail groove and the second fitting structure being a dovetail block adapted to the dovetail groove; or the first fitting structure being a boss and the second fitting structure being a stepped groove, etc. Taking the fitting form of a protrusion and a groove as an example, the protrusion can be set as a long strip extending along the length of the metal layer 122, and the groove is correspondingly set on the top surface of the substrate 110, matching the length and cross-sectional shape of the protrusion. This fitting method can significantly increase the contact area between the metal layer 122 and the substrate 110, improve the stability of their connection, and provide precise positioning for subsequent pressure welding, avoiding misalignment during welding.

[0025] The metal layer 122 and the substrate 110 are connected by pressure welding. Pressure welding is a welding method that uses pressure to connect the workpieces in a solid state. Common types of pressure welding include resistance welding, friction welding, and diffusion welding. Compared with traditional argon arc welding and other metal arc welding, pressure welding does not require filler material, which reduces welding costs and avoids defects such as porosity and cracks that may occur during fusion welding, thus ensuring welding quality. During pressure welding, by applying certain pressure and temperature, the connection surface between the metal layer 122 and the substrate 110 undergoes plastic deformation, achieving diffusion bonding between atoms. This connection method not only further enhances the connection strength between the two but also effectively ensures the flatness of the composite plate 120 surface. Because the clamping and pressure on the workpiece during pressure welding suppresses welding deformation, it ensures the flatness of the receiving surface of the contact rail 100, improves the shoe-rail coupling performance, and makes the contact between the current collector and the contact rail 100 more stable, resulting in more reliable power transmission.

[0026] In actual operation, the substrate 110 acts as the conductive body, transmitting electrical energy through the metal layer 122 and the wear-resistant layer 121 of the composite plate 120. When the vehicle current collector slides into contact with the wear-resistant layer 121, the wear-resistant layer 121 resists frictional loss, while the metal layer 122 smoothly conducts the current to the substrate 110, which then supplies it to the train. The fitting of the first and second interlocking structures ensures a stable connection between the composite plate 120 and the substrate 110 during stress and current transmission, while the pressure welding further strengthens this connection and ensures the flatness of the current-receiving surface.

[0027] According to the contact rail 100 provided in the embodiments of this application, by setting the composite plate 120, the width of the flow-receiving surface (i.e., the width of the wear-resistant layer 121) and the shape of the substrate 110 can be freely selected according to actual needs, which greatly improves the adaptability of the contact rail 100 and reduces the manufacturing difficulty for different scenarios; through the interlocking connection of the metal layer 122 and the substrate 110, the contact area and connection stability of the two are significantly improved, providing a good foundation for welding connection; the pressure welding connection method not only reduces the production cost, but also effectively ensures the flatness of the composite plate 120, thereby improving the shoe-rail coupling performance and ensuring that the train receives a continuous and stable power supply.

[0028] Please see Figure 1 , Figure 2 and Figure 3 According to some embodiments of this application, one of the first fitting structure and the second fitting structure includes a plurality of protrusions 111 spaced apart along the width direction of the composite plate 120, and the other of the first fitting structure and the second fitting structure includes a plurality of recesses 1221 spaced apart along the width direction of the composite plate 120, wherein the plurality of protrusions 111 and the plurality of recesses 1221 are fitted together in a one-to-one correspondence.

[0029] The protrusions 111 are outwardly extending protrusions in the mating structure, and are disposed on the first or second mating structure, spaced apart along the width direction of the composite plate 120. The number of protrusions 111 is not specifically limited and can be flexibly set according to factors such as the width of the composite plate 120 and the load-bearing requirements of the contact rail 100; for example, two, three, four, or more protrusions can be provided. If two protrusions 111 are provided, they will be symmetrically distributed on both sides of the width direction of the composite plate 120, making the force more balanced; if three protrusions 111 are provided, they can be evenly distributed at equal intervals along the width direction of the composite plate 120, further improving the stability of the mating. The cross-sectional shape of the protrusions 111 can be designed as rectangular, trapezoidal, semi-circular, etc., among which the trapezoidal cross-section of the protrusion 111 can form a lateral restraint after mating, reducing the risk of relative sliding and providing better stability. The height and length of the protrusions 111 need to be adapted to the dimensions of the recesses 1221 to ensure a tight fit after mating and avoid gaps.

[0030] The recess 1221 is a recessed structure adapted to the protrusion 111, and is provided on the corresponding second or first interlocking structure. It is also spaced along the width direction of the composite plate 120, and the number and spacing of the recesses 1221 are completely consistent with those of the protrusions 111 to achieve a one-to-one interlocking. The cross-sectional shape, depth, and length of the recess 1221 match those of the protrusion 111. For example, when the protrusion 111 has a trapezoidal cross-section, the recess 1221 is a corresponding trapezoidal groove. After the protrusion 111 is inserted into the recess 1221, the sidewalls of the two fit tightly together, forming a reliable mechanical engagement. The processing of the recess 1221 can be carried out simultaneously with the forming of the substrate 110 or the metal layer 122, reducing additional processing steps and lowering manufacturing costs.

[0031] When the first fitting structure consists of multiple protrusions 111, the second fitting structure consists of corresponding multiple recesses 1221; conversely, if the first fitting structure consists of multiple recesses 1221, the second fitting structure consists of corresponding multiple protrusions 111. The fitting effect of both configurations is consistent, and both can be selected according to actual processing technology and structural requirements. After the multiple protrusions 111 and multiple recesses 1221 are fitted one-to-one, a multi-point mechanical connection is formed. Compared with a single fitting structure, this can significantly increase the contact area and engagement points between the metal layer 122 and the substrate 110, which not only improves the mechanical strength of the connection but also forms multiple paths of conduction during current transmission, reducing contact resistance and improving conductivity. At the same time, the spaced protrusions 111 and recesses 1221 can disperse the stress of the contact rail 100 under the pressure of the current collector, avoiding structural damage caused by local stress concentration and extending the service life of the contact rail 100.

[0032] This interlocking design of multiple protrusions 111 and multiple recesses 1221 can further enhance the connection reliability between the metal layer 122 and the substrate 110, reduce the stress load on the welding parts, make the pressure welding connection effect more durable, and further optimize the conductivity by increasing the contact area and conductive path, thus ensuring the stability of the shoe-rail coupling.

[0033] According to some embodiments of this application, the outer wall of the protrusion 111 is fitted with the inner wall of the recess 1221.

[0034] The outer wall of the protrusion 111 refers to the entire outer surface of the outwardly extending portion of the protrusion 111, including the two side surfaces, the top end face, and the two end faces along the length of the composite plate 120; the inner wall of the recess 1221 refers to the entire inner surface formed by the recess of the recess 1221, corresponding to the two side inner walls, the bottom inner wall, and the two end inner walls along the length of the composite plate 120. Here, "fitting" means that after the protrusion 111 is embedded in the recess 1221, there are no obvious gaps between the various surfaces of the outer wall of the protrusion 111 and the corresponding surfaces of the inner wall of the recess 1221, achieving comprehensive and tight contact, with the contact area approaching the total area of ​​the outer wall of the protrusion 111.

[0035] To maximize the mechanical engagement strength between the protrusion 111 and the recess 1221, loosening or relative wobbling after engagement is avoided. When the contact rail 100 is subjected to sliding friction from the current collector, vibration from train operation, and thermal stress from current transmission, the tightly fitted outer and inner walls can disperse these forces through surface-to-surface contact, reducing local stress concentration and lowering the risk of deformation or breakage of the protrusion 111 or recess 1221. Secondly, the fully fitted structure further increases the conductive contact area between the metal layer 122 and the substrate 110, making the current transmission path between them smoother, reducing contact resistance, and avoiding localized heating due to poor contact. This improves conductivity and prevents high temperatures from damaging the welded parts and the engagement structure, extending the service life of the contact rail 100.

[0036] Please see Figure 1 , Figure 2 and Figure 3 According to some embodiments of this application, among the plurality of protrusions 111, the height of the two protrusions 111 located at both ends in the width direction of the composite plate 120 is less than the height of the other protrusions 111.

[0037] The height of the protrusion 111 refers to the vertical distance from the reference surface of the metal layer 122 or the substrate 110 (the surface on one side where the protrusion 111 is located) to the top of the protrusion 111. This dimension directly affects the fitting depth and contact effect between the protrusion 111 and the recess 1221. The protrusions 111 located at both ends of the composite plate 120 in the width direction are called "end protrusions", and the remaining protrusions 111 located in the middle area are called "middle protrusions". The height of the end protrusions 111 is less than the height of the middle protrusions 111. The height difference between the two can be set according to actual needs. For example, the height difference can be 0.5mm-3mm, which ensures the differentiation effect without affecting the overall fitting strength.

[0038] From a structural perspective, the smaller height of the end protrusion 111 serves a guiding function during assembly. When the protrusion 111 engages with the recess 1221, the lower height of the end protrusion 111 allows it to quickly enter the corresponding position of the recess 1221, achieving initial positioning and preventing misalignment or collision between the middle protrusion 111 and the recess 1221, thus reducing assembly difficulty and improving assembly efficiency. Secondly, this height distribution ensures more uniform engagement stress. During use, the pressure of the current collector in the contact rail 100 primarily acts on the middle region of the composite plate 120. The higher height of the middle protrusion 111 allows for a deeper engagement depth and a larger contact area with the recess 1221, thus better bearing the stress in the middle region. The end region experiences relatively less stress, and the lower height of the end protrusion 111 is sufficient to meet the connection requirements, preventing stress concentration due to excessive height and reducing the risk of deformation or breakage of the protrusion 111.

[0039] Please see Figure 1 , Figure 2 and Figure 3 According to some embodiments of this application, the protrusion 111 extends along the length direction of the composite plate 120, the cross-section of the protrusion 111 is rectangular, or the width of the protrusion 111 tends to decrease along the direction close to the recess 1221.

[0040] The protrusion 111 extends along the length of the composite plate 120, meaning that the protrusion 111 is a long strip structure with a length that is the same as or close to the length of the composite plate 120. This extension method allows the engagement of the protrusion 111 and the recess 1221 to be continuously distributed along the entire length of the contact rail 100, forming a full-length mechanical engagement. Compared to the short-segment protrusion 111, the long strip protrusion 111 can significantly increase the contact length and contact area with the recess 1221, which not only improves the consistency of the connection between the metal layer 122 and the substrate 110 along the length direction, but also avoids the occurrence of weak areas in the local engagement, ensuring the structural stability and electrical uniformity of the contact rail 100 throughout its entire length. At the same time, this continuously extending structure is also easy to process and can be prepared by integral forming processes such as rolling and extrusion, reducing subsequent processing steps.

[0041] The cross-sectional shape of the protrusion 111 includes two specific embodiments: the first is a rectangular cross-section, and the second is a cross-section whose width tends to decrease along the direction close to the recess 1221.

[0042] For the convex portion 111 with a rectangular cross-section, all four sides of its cross-section are straight lines, and the two opposite sides are parallel. The width and height are consistent throughout the entire extension direction of the convex portion 111. The advantage of this structure is that it is easy to process and can be quickly formed through conventional mechanical cutting, rolling and other processes. Moreover, the rectangular cross-section allows the outer wall of the convex portion 111 and the inner wall of the concave portion 1221 to form a surface-to-surface fit, with a regular contact area and strong mechanical interlocking stability. At the same time, the rectangular structure of the convex portion 111 results in a uniform current path distribution during current transmission, which can effectively reduce contact resistance and ensure conductivity efficiency.

[0043] For the convex portion 111 whose width decreases towards the concave portion 1221, its cross-section can be specifically designed as trapezoidal, triangular, or frustum-shaped. Taking the trapezoidal cross-section as an example, the width of the end of the convex portion 111 near the concave portion 1221 (i.e., the embedded end) is smaller, and the width of the end away from the concave portion 1221 (i.e., the connecting end) is larger, and the two side walls are inclined; for the triangular cross-section of the convex portion 111, the embedded end is a sharp corner, and the connecting end is the base; for the frustum-shaped cross-section of the convex portion 111, the side walls have an arc transition. The core advantage of this shrinking design lies in its enhanced fitting guidance and anti-disengagement properties. During assembly, the narrower insertion end can quickly align with the opening of the recess 1221, guiding the protrusion 111 to smoothly insert, reducing the difficulty of alignment and the risk of structural damage during assembly. After fitting, the inclined sidewall of the protrusion 111 fits tightly with the corresponding inclined inner wall of the recess 1221, forming a lateral restraint, which effectively prevents the protrusion 111 from dislodging from the recess 1221. Especially when the contact rail 100 is subjected to vibration, impact, or thermal expansion and contraction, this anti-disengagement structure can significantly improve the reliability of the connection. At the same time, even with the shrinking cross-section, the outer wall of the protrusion 111 can still fully fit with the inner wall of the recess 1221, ensuring sufficient contact area without affecting mechanical strength and electrical conductivity.

[0044] According to some embodiments of this application, the bottom of the recess 1221 may be provided with a flow guide hole, which may penetrate the substrate 110.

[0045] The bottom of the recess 1221 is the inner wall of the end of the recess 1221 away from the opening. A flow guide hole is opened at this bottom and completely penetrates the substrate 110. That is, one end of the flow guide hole connects to the internal space of the recess 1221, and the other end extends to the surface of the substrate 110 away from the composite plate 120, forming a through channel. The number of flow guide holes is not specifically limited and can be set according to the number and size of the recesses 1221 and actual usage requirements. For example, one, two, or more flow guide holes can be provided at the bottom of each recess 1221. If each recess 1221 has two flow guide holes, they can be symmetrically distributed on both sides of the bottom of the recess 1221 to ensure uniform flow or exhaust.

[0046] By incorporating air guide holes, air can be released during assembly. When the protrusion 111 is inserted into the recess 1221 for fitting and assembly, or during subsequent pressure welding, the air inside the recess 1221 will be compressed. If this air cannot be released, it will lead to a loose fit between the protrusion 111 and the recess 1221, and may even cause defects such as porosity due to residual air during welding, affecting connection stability and conductivity. The air guide holes can promptly release the compressed air, ensuring a complete fit between the outer and inner walls of the protrusion 111 and the recess 1221, while also ensuring the welding quality of the pressure weld. Furthermore, the air guide holes also serve a heat dissipation and impurity removal function during use. The contact rail 100 generates heat during current transmission, especially in the contact area between the protrusion 111 and the recess 1221. The air guide holes form a heat dissipation channel, accelerating heat dissipation and preventing localized high temperatures that could lead to material performance degradation or weld failure. Simultaneously, if a small amount of impurities or condensate enters the gap of the recess 1221, the air guide holes can discharge them, preventing impurity accumulation that could lead to poor contact or structural corrosion, thus extending the service life of the contact rail 100.

[0047] According to some embodiments of this application, at least one of the plurality of protrusions 111 is provided with a first anti-mistake part, and at least one of the plurality of recesses 1221 is provided with a second anti-mistake part, with the first anti-mistake part and the second anti-mistake part correspondingly cooperating.

[0048] The first error-proof part is a differentiated structure set on the protrusion 111. Its function is to form a unique fit with the second error-proof part through unique shape or positional features, thus limiting the incorrect assembly direction. The number of first error-proof parts is not specifically limited and can be selected according to the total number of protrusions 111 and the assembly accuracy requirements. For example, only one first error-proof part can be set in multiple protrusions 111, or the first error-proof part can be set on two or three protrusions 111 that are spaced apart. The structural form of the first error-proof part can adopt various designs, such as opening a square notch in the side wall of the protrusion 111, designing the cross-section of the protrusion 111 to be an asymmetrical shape (such as one side being a straight line and the other side being an arc), setting a cylindrical protrusion at the top of the protrusion 111, or making the width of the protrusion 111 different from other protrusions 111 (such as being 2-5mm wider than other protrusions 111). Taking the square notch on the side wall of the protrusion 111 as an example, the notch extends along the length of the protrusion 111 and the depth is 1 / 4 to 1 / 2 of the width of the protrusion 111. This notch will not affect the overall strength of the protrusion 111 and can form a clear anti-mistake mark.

[0049] The second anti-misfit part is an adapter structure set on the recess 1221. Its position and shape completely correspond to the first anti-misfit part, ensuring that the first anti-misfit part can smoothly cooperate with the second anti-misfit part only when the composite plate 120 and the substrate 110 are in the correct assembly direction. If the first anti-misfit part is a square notch on the side wall of the protrusion 111, the second anti-misfit part is a square protrusion at the corresponding position on the inner wall of the recess 1221. The size of the protrusion matches the notch perfectly, and there is no gap after insertion. If the first anti-misfit part is an asymmetrical cross section of the protrusion 111, the second anti-misfit part is an asymmetrical inner wall of the recess 1221, and full fit can only be achieved in the correct direction. If the first anti-misfit part is a cylindrical protrusion at the top of the protrusion 111, the second anti-misfit part is a cylindrical groove at the bottom of the recess 1221, and the diameter and depth of the protrusion and the groove are adapted. The location of the second anti-mistake part must be consistent with the recess 1221 that is fitted into the protrusion 111 corresponding to the first anti-mistake part. That is, the protrusion 111 with the first anti-mistake part must have the second anti-mistake part in its corresponding recess 1221 to ensure a one-to-one correspondence.

[0050] During the assembly stage, when the operator aligns the protrusions 111 of the composite plate 120 with the recesses 1221 of the base 110, if the orientation is incorrect, the first and second anti-misalignment parts will mechanically interfere, preventing proper engagement and thus providing a clear indication of an incorrect assembly orientation. Only when the assembly orientation is correct can the first anti-misalignment part smoothly engage with the second anti-misalignment part, simultaneously aligning all protrusions 111 and recesses 1221 precisely, achieving rapid and accurate assembly. Correct assembly position ensures uniform stress on the welding surface during subsequent pressure welding, preventing welding defects due to misalignment and guaranteeing welding quality. Simultaneously, precise engagement maintains the flatness of the composite plate 120, preventing tilting of the flow-receiving surface due to assembly deviations and ensuring shoe-rail coupling performance. During use, the anti-misalignment structure further restricts the relative rotation or displacement between the composite plate 120 and the base 110, forming a triple fixation with the engagement structure and pressure welding connection, thus enhancing connection stability.

[0051] Please see Figure 1 , Figure 2 and Figure 3 According to some embodiments of this application, the surface of the metal layer 122 facing the wear-resistant layer 121 may be provided with uniformly distributed honeycomb reinforcing grooves, and the side of the wear-resistant layer 121 facing the metal layer 122 is provided with a reinforcing part that fits into the honeycomb reinforcing grooves.

[0052] The surface of the metal layer 122 facing the wear-resistant layer 121 is the bonding surface between the two. Honeycomb-shaped reinforcing grooves are formed on this surface and evenly distributed, exhibiting a honeycomb-like arrangement. This means multiple grooves are tightly arranged in regular hexagonal, square, or rhomboid shapes, forming a honeycomb-like structure. The number of honeycomb-shaped reinforcing grooves is not specifically limited and can be adjusted according to the area of ​​the metal layer 122 and the stress requirements of the contact rail 100. For example, 2-8 grooves can be set per square centimeter to ensure coverage of the entire bonding surface between the metal layer 122 and the wear-resistant layer 121. The depth of a single reinforcing groove is 1 / 3-2 / 3 of the thickness of the metal layer 122, ensuring connection strength without weakening the conductivity and overall structural strength of the metal layer 122. The cross-sectional shape of the groove can be hexagonal, circular, or square. The hexagonal structure provides a more uniform stress distribution and better disperses the pressure transmitted by the wear-resistant layer 121, making it a preferred embodiment.

[0053] The wear-resistant layer 121 has a reinforcing section on the side facing the metal layer 122. The reinforcing section is a protruding structure extending from the wear-resistant layer 121 towards the metal layer 122. Its overall arrangement, quantity, and position perfectly match the honeycomb-shaped reinforcing grooves, ensuring that each reinforcing section can be embedded into its corresponding groove. The height of the reinforcing section is consistent with the depth of the reinforcing groove, and its cross-sectional shape matches the shape of the groove. For example, when the reinforcing groove is a regular hexagon, the reinforcing section is a regular hexagonal protrusion. After embedding, the outer wall of the reinforcing section fully fits the inner wall of the reinforcing groove without any obvious gaps. The reinforcing section and the wear-resistant layer 121 are integrally formed, allowing for simultaneous molding during the preparation of the wear-resistant layer 121 without additional processing steps, thus ensuring structural integrity.

[0054] The interlocking fit between the honeycomb reinforcing grooves and the reinforcing parts significantly increases the contact area and mechanical engagement points between the metal layer 122 and the wear-resistant layer 121. Compared to planar bonding, the increased contact area of ​​the honeycomb structure makes the connection between the two tighter, effectively resisting the shear force generated by the sliding contact of the current receiver and preventing delamination and detachment. Secondly, the honeycomb structure has excellent stress dispersion performance. When the current receiver comes into contact with the wear-resistant layer 121 and generates pressure, the pressure is transmitted through the reinforcing parts to the inner wall of the reinforcing grooves, and then evenly distributed to the entire metal layer 122 by the honeycomb-shaped grooves, avoiding cracking or deformation of the wear-resistant layer 121 caused by local stress concentration. In addition, this interlocking structure can also improve the conductivity continuity between the two. Although the conductivity of the wear-resistant layer 121 is low, the tight fit between the reinforcing parts and the reinforcing grooves can reduce contact resistance, making the current transmission between the wear-resistant layer 121 and the metal layer 122 smoother and ensuring the overall conductivity of the contact rail 100.

[0055] It should be noted that the metal layer 122 and the wear-resistant layer 121 are still stacked along the thickness direction and formed as a whole. The interlocking of the honeycomb reinforcing groove and the reinforcing part is to strengthen this integrally formed structure, rather than replace it. After the reinforcing part is embedded in the reinforcing groove, it can be further fixed by processes such as rolling and hot pressing to ensure that the two form a stable whole, while not affecting the interlocking connection and pressure welding connection between the metal layer 122 and the substrate 110.

[0056] According to some embodiments of this application, the wear-resistant layer 121 may have slots extending along the length direction at both ends in the width direction, and the metal layer 122 may have slots extending along the length direction at both ends in the width direction, with the slots fitting into the slots.

[0057] The two ends of the wear-resistant layer 121 in the width direction refer to the two end sides of the wear-resistant layer 121 extending along its own width. The slot is opened at these two ends and extends continuously along the length direction of the wear-resistant layer 121, with its length consistent with the length of the wear-resistant layer 121, ensuring lateral constraint along the entire length of the composite plate 120. The cross-sectional shape of the slot can be designed as L-shaped, U-shaped, or dovetail-shaped, etc.

[0058] The two ends of the metal layer 122 in the width direction correspond to the end positions of the wear-resistant layer 121. The locking part is a protruding structure formed by the extension of the metal layer 122 towards the wear-resistant layer 121. It extends continuously along the length direction of the metal layer 122, and its length is consistent with that of the metal layer 122. The cross-sectional shape and size of the locking part are completely matched with the locking groove to ensure a tight fit after fitting. For example, when the locking groove is dovetail-shaped, the locking part is the corresponding dovetail-shaped protrusion, and its outer width is slightly larger than the opening width of the locking groove. A firm fit is achieved through a slight interference fit. If the locking groove is U-shaped, the locking part is a rectangular protrusion. After fitting, the two side walls of the locking part are fully fitted with the inner wall of the locking groove. The locking part and the metal layer 122 are integrally formed structures and can be formed simultaneously with the metal layer 122 through processes such as rolling and extrusion to ensure structural integrity and connection strength.

[0059] The engagement of the slot and the card part mainly achieves two functions: First, lateral limiting. During use, the sliding contact between the current receiver and the wear-resistant layer 121 of the contact rail 100 will generate lateral friction. Especially when the train turns or vibrates, the lateral force may cause the wear-resistant layer 121 and the metal layer 122 to slip relative to each other in the width direction. The engagement of the slot and the card part can effectively limit this slippage and ensure the stability of their relative positions. Second, edge fixing. The edge of the wear-resistant layer 121 and the metal layer 122 is a weak connection area, which is prone to delamination or warping due to stress concentration. After the card part is embedded in the slot, it can form a wrapping fixation on the edge of the wear-resistant layer 121, disperse the edge stress, avoid warping or delamination, and at the same time increase the contact area of ​​the edge area and improve the connection reliability.

[0060] According to some embodiments of this application, the composite plate 120 has a thickness of 10mm-12mm, the wear-resistant layer 121 has a thickness of 3mm-5mm, and the metal layer 122 has a thickness of 5mm-9mm.

[0061] The thickness of the composite plate 120 refers to the total thickness of the wear-resistant layer 121 and the metal layer 122 after being laminated along the thickness direction, and is limited to 10mm-12mm. This size range is determined based on the conventional installation space of the rail contact rail 100, the contact pressure of the current collector, and the structural load-bearing requirements. When the thickness is less than 10mm, the overall structural strength of the composite plate 120 is insufficient, making it difficult to withstand the pressure and friction generated by the long-term sliding contact of the current collector, and it is prone to deformation or damage. When the thickness is greater than 12mm, it will not only increase the overall weight of the contact rail 100, increasing the installation difficulty and transportation costs, but also lead to material waste. Furthermore, an excessively thick structure will affect heat dissipation efficiency, and may affect conductivity and material stability due to heat accumulation.

[0062] The wear-resistant layer 121 has a thickness of 3mm-5mm. As a wear-resistant component that directly contacts the current collector, this thickness range ensures sufficient wear allowance and extends its service life. If the thickness is less than 3mm, the wear-resistant layer 121 wears too quickly, requiring frequent replacement of the composite plate 120 and increasing maintenance costs. If the thickness is greater than 5mm, since the wear-resistant layer 121 is usually made of materials with relatively low conductivity (such as stainless steel or wear-resistant alloys), excessive thickness will increase the overall resistance of the contact rail 100, affecting conductivity efficiency, and also increasing the manufacturing difficulty and cost of the composite plate 120. The thickness can be adjusted according to the wear intensity of the application scenario. For example, on lines with high train traffic density and high current collector pressure, a 4mm-5mm wear-resistant layer 121 can be used; on lines with low traffic density, a 3mm-4mm wear-resistant layer 121 can be used, meeting both usage requirements and cost optimization.

[0063] The thickness of the metal layer 122 is 5mm-9mm, and its thickness, together with that of the wear-resistant layer 121, equals the total thickness of the composite plate 120, forming a scientific ratio. As the conductive transition and connection core, the metal layer 122 needs sufficient thickness to ensure conductivity and structural strength: if the thickness is less than 5mm, the conductive cross-sectional area is insufficient, contact resistance increases, localized heating is easily generated, and it is difficult to stably support the wear-resistant layer 121, which also affects the reliability of its integration with the substrate 110 and pressure welding connection; if the thickness is greater than 9mm, it will squeeze the effective thickness space of the wear-resistant layer 121, resulting in insufficient thickness of the wear-resistant layer 121. Furthermore, an excessively thick metal layer 122 will increase the weight of the composite plate 120, and the synergistic stress-bearing effect with the wear-resistant layer 121 will also decrease. The specific thickness of the metal layer 122 needs to be compatible with the thickness of the wear-resistant layer 121. For example, when the thickness of the wear-resistant layer 121 is 3mm, the thickness of the metal layer 122 can be 7mm-9mm; when the thickness of the wear-resistant layer 121 is 5mm, the thickness of the metal layer 122 can be 5mm-7mm, to ensure that the two work together to meet the comprehensive requirements of conductivity, wear resistance and connection.

[0064] In this embodiment, the wear-resistant layer 121 can be made of a wear-resistant material with good electrical conductivity, and the Brinell hardness of the wear-resistant layer 121 is greater than or equal to 170 HBW.

[0065] The conductivity of the material of metal layer 122 should be greater than or equal to 28 Ms / m, and the tensile strength should be greater than or equal to 200 MPa.

[0066] As the core component that directly contacts the contact rail 100 with the vehicle current receiver, the wear-resistant layer 121 must meet stringent performance requirements. Through specific material selection and structural design, it ensures that the contact rail 100 has excellent wear and corrosion resistance, extends its overall service life, and is suitable for complex rail transit conditions.

[0067] The wear-resistant layer 121 must meet multiple performance indicators. Regarding wear performance, it is tested according to the CJ / T414 standard. The wear-resistant layer rotates at 160 km / h, applying a normal pressure of 120–180 N to the wear-resistant slider while a test current of 500 A is applied. After reaching the specified 700,000 wear cycles (two opposing wear-resistant sliders, one rotation of the sample counts as two cycles), the measured wear amount of the wear-resistant layer 121 must be ≤0.05 mm. This indicator ensures that the wear-resistant layer 121 maintains an extremely low wear rate even under long-term high-speed sliding contact with the current receiver and current transmission conditions, preventing a decrease in conductivity or structural failure due to excessive wear, effectively extending the maintenance cycle of the contact rail 100, and reducing operating costs.

[0068] In terms of corrosion resistance, the wear-resistant layer 121 can withstand 4000 hours of 50g / L sodium chloride salt spray testing, and its service life can reach 60 years even in a marine C-4 environment. The marine C-4 environment is a harsh corrosive environment characterized by high salt spray and high humidity. This property of the wear-resistant layer 121 makes it suitable for coastal rail transit lines, effectively resisting the corrosive effects of sea winds and salt spray on the receiving surface, preventing rust or peeling of the wear-resistant layer 121, ensuring the long-term stable conductivity and wear resistance of the contact rail 100, and reducing safety hazards caused by corrosion.

[0069] In terms of hardness performance, the Brinell hardness of wear-resistant layer 121 is ≥201HBW. The higher hardness enhances its resistance to external friction and impact, reduces scratches, dents and other damage caused by sliding contact of the current receiver, and maintains the flatness of the current receiving surface. The flatness of the current receiving surface directly affects the shoe-rail coupling performance, avoiding current transmission fluctuations caused by uneven surfaces, and ensuring that the train receives a continuous and stable power supply.

[0070] The wear-resistant layer 121 can be made of various materials, including 10Cr17 high-quality ferritic stainless steel strip, 06Cr19Ni10 high-quality austenitic stainless steel strip, graphene composite nano-ceramic material, and DLC diamond-like carbon material. Among these, 10Cr17 ferritic stainless steel strip and 06Cr19Ni10 austenitic stainless steel strip possess excellent wear and corrosion resistance, and exhibit good bonding with the metal layer 122. They can be integrally formed with the metal layer 122 through rolling, hot pressing, or other methods. Graphene composite nano-ceramic material utilizes the high thermal conductivity and high strength of graphene with the wear resistance of nano-ceramics to achieve synergistic performance. The material has high density and can effectively block corrosive media. DLC diamond-like carbon material has an extremely low coefficient of friction and extremely high hardness, exhibiting outstanding wear resistance, while also possessing good electrical conductivity, thus not adversely affecting the current transmission of the contact rail 100. These materials can be selected based on the performance priorities of specific application scenarios. For example, for lines in coastal areas, 06Cr19Ni10 austenitic stainless steel strip or graphene composite nano-ceramic materials with better corrosion resistance can be preferred, while for lines with extremely high wear resistance, DLC diamond-like carbon materials are the preferred choice.

[0071] The wear-resistant layer 121 and the metal layer 122 are stacked and formed as a single unit along the thickness direction. The connection method can be determined according to the material type. For example, stainless steel strips can be fixed to the metal layer 122 through hot pressing, welding, etc., while ceramic or DLC materials can be prepared on the surface of the metal layer 122 through physical vapor deposition, chemical vapor deposition, etc., to ensure a tight bond between the two and avoid delamination or peeling during use. By using the wear-resistant layer 121 that meets the above performance requirements, the flow-receiving surface performance of the contact rail 100 is guaranteed. It works synergistically with the connection structure of the metal layer 122, the embedding of the substrate 110, and the pressure welding connection to comprehensively improve the reliability and durability of the contact rail 100 under complex working conditions.

[0072] Regarding conductivity, the overall volume resistivity of the contact rail 100 at 20℃ must be ≤14μΩ / m (CJ / T414 standard). This indicator directly determines the energy loss during current transmission. Low volume resistivity can effectively reduce heat generation during power transmission, improve power supply efficiency, and avoid material performance degradation or structural damage caused by local overheating. As the core conductive component of the contact rail 100, the substrate 110 must have a conductivity ≥28MS / m. High conductivity ensures that the substrate 110 has excellent current carrying capacity, enabling it to quickly transfer electrical energy from the power supply end to the composite plate 120, and then through the composite plate 120 to the train current collector, ensuring transmission stability under high current conditions.

[0073] In terms of hardness performance, the Brinell hardness of the substrate 110 is ≥75HBW. This hardness value enables the substrate 110 to have sufficient structural strength to resist external impacts, vibrations and pressure transmitted by the composite plate 120 during installation and use, and avoid problems such as deformation and dents in the substrate 110. At the same time, it provides a stable support foundation for the interlocking and pressure welding connection between the metal layer 122 and the substrate 110, and ensures the reliability of the connection parts.

[0074] The terms "first," "second," etc., used in the specification and claims of this application are used to distinguish similar objects and not to describe a specific order or sequence. It should be understood that such use of data can be interchanged where appropriate so that embodiments of this application can be implemented in orders other than those illustrated or described herein, and the objects distinguished by "first," "second," etc., are generally of the same class and the number of objects is not limited; for example, a first object can be one or more. Furthermore, in the specification and claims, "and / or" indicates at least one of the connected objects, and the character " / " generally indicates that the preceding and following objects are in an "or" relationship.

[0075] In the description of this application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "upper", "lower", "front", "rear", "left", "right", "vertical", "horizontal", "top", "bottom", "inner", "outer", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc., indicating the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings, are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of this application.

[0076] In the description of this application, "first feature" and "second feature" may include one or more of the features.

[0077] In the description of this application, "multiple" means two or more.

[0078] In the description of this application, the first feature being "above" or "below" the second feature may include the first and second features being in direct contact, or the first and second features being in contact through another feature between them.

[0079] In the description of this application, the terms "above," "over," and "on top" for the first feature and the second feature include the first feature being directly above or diagonally above the second feature, or simply indicate that the first feature is at a higher horizontal level than the second feature.

[0080] In the description of this specification, the references to terms such as "one embodiment," "some embodiments," "illustrative embodiment," "example," "specific example," or "some examples," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of this application. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.

[0081] Although embodiments of this application have been shown and described, those skilled in the art will understand that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of this application, the scope of which is defined by the claims and their equivalents.

Claims

1. A contact rail, characterized in that include: Matrix; A composite board includes a wear-resistant layer and a metal layer that are stacked and integrally formed along the thickness direction. The metal layer has a first interlocking structure on the side away from the wear-resistant layer, and the substrate has a second interlocking structure on the top surface facing the composite board. The first interlocking structure and the second interlocking structure are interlocked. The metal layer is pressure welded to the substrate.

2. A contact rail according to claim 1, characterized in that One of the first fitting structure and the second fitting structure includes a plurality of protrusions spaced apart along the width direction of the composite plate, and the other of the first fitting structure and the second fitting structure includes a plurality of recesses spaced apart along the width direction of the composite plate, wherein the plurality of protrusions and the plurality of recesses are fitted together in a one-to-one correspondence.

3. The contact rail according to claim 2, characterized in that, The outer wall of the protrusion fits against the inner wall of the concave part.

4. The contact rail according to claim 3, characterized in that, Of the plurality of protrusions, the height of the two protrusions located at both ends in the width direction of the composite plate is less than the height of the other protrusions.

5. The contact rail according to claim 2, characterized in that, The protrusion extends along the length of the composite plate, and the cross-section of the protrusion is rectangular, or the width of the protrusion tends to decrease along the direction close to the concave portion.

6. The contact rail according to claim 2, characterized in that, The bottom of the recess is provided with a flow guide hole, which penetrates the substrate.

7. The contact rail according to any one of claims 2-5, characterized in that, At least one of the plurality of protrusions is provided with a first anti-mistake part, and at least one of the plurality of recesses is provided with a second anti-mistake part, wherein the first anti-mistake part and the second anti-mistake part are correspondingly engaged.

8. The contact rail according to any one of claims 1-5, characterized in that, The surface of the metal layer facing the wear-resistant layer is provided with uniformly distributed honeycomb-shaped reinforcing grooves, and the side of the wear-resistant layer facing the metal layer is provided with a reinforcing part that fits into the honeycomb-shaped reinforcing grooves.

9. The contact rail according to any one of claims 1-5, characterized in that, The wear-resistant layer has slots extending along the length direction at both ends in the width direction, and the metal layer has a locking part extending along the length direction at both ends in the width direction, and the locking part is fitted into the slot.

10. The contact rail according to any one of claims 1-5, characterized in that, The composite plate has a thickness of 10mm-12mm, the wear-resistant layer has a thickness of 3mm-5mm, and the metal layer has a thickness of 5mm-9mm.