A positioning fixture for segmented magnets of a multi-pole motor rotor

By combining segmented magnet design with positioning fixtures, the problems of stress concentration and insufficient insulation in multi-pole permanent magnet motors are solved, achieving high-precision coaxial positioning and insulation isolation, and improving the electromagnetic performance and operational stability of the motor.

CN224987265UActive Publication Date: 2026-11-17JINGMAG (JINHUA) MOTOR CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202522196684.3
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2025-10-17
Publication Date
2026-11-17
Estimated Expiration
2035-10-17

AI Technical Summary

Technical Problem

In existing multi-pole permanent magnet motors, integral magnets suffer from problems such as stress concentration during assembly, poor positioning accuracy, and insufficient insulation performance, which affect the motor's operational stability and lifespan.

Method used

The design employs segmented magnets, combined with positioning fixtures and insulating filling medium. High-precision coaxial positioning is achieved through a stepped platform and stepped groove structure, and insulating material is filled in the gaps between the magnets to form an electrical insulation layer.

Benefits of technology

It achieves high-precision coaxial positioning of segmented magnets, reduces eddy current losses, improves electromagnetic performance and operational reliability, and ensures the stability and insulation performance of the motor.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN224987265U_ABST
    Figure CN224987265U_ABST
Patent Text Reader

Abstract

This utility model discloses a positioning fixture for segmented magnets of a multi-pole motor rotor, belonging to the field of motor manufacturing technology. The fixture includes a positioning base, a stepped platform and stepped groove transition structure, and positioning pins. When used together, it can achieve coaxial positioning and stable support of three or more NdFeB magnets. A small gap is reserved between adjacent magnets and filled with insulating adhesive and modified epoxy insulating medium, which forms an insulating layer after curing. Through this structure, not only is the coaxiality error of the assembled magnets guaranteed to be no greater than 0.1 mm and the radial runout no greater than 0.08 mm, but the eddy current path is also effectively blocked, resulting in an insulation resistance of over 1000 MΩ. This solution significantly reduces eddy current losses and magnetic field distortion while ensuring assembly accuracy and mechanical stability, improving motor efficiency and operational reliability. It has the advantages of simple structure, strong process adaptability, and high application value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This utility model relates to the field of motor design and manufacturing technology, specifically to a positioning fixture for segmented magnets of a multi-pole motor rotor. Background Technology

[0002] With the rapid development of new energy vehicles, high-speed spindle motors, and wind turbines, multi-pole permanent magnet motors have been widely used due to their high power density and fast response speed. However, in existing technologies, the rotor permanent magnets generally adopt an integral block structure, which has the following significant defects and shortcomings in practical applications:

[0003] 1. The integral magnet is large in size and needs to be fixed by interference fit or bonding during assembly, which can easily lead to stress concentration. In addition, neodymium iron boron magnets are relatively brittle and are prone to cracks or damage during assembly.

[0004] 2. The integral magnet lacks a transition structure at the pole transition point, resulting in poor positioning accuracy after assembly. It is difficult to guarantee coaxiality and radial runout accuracy, which affects the smoothness of motor operation.

[0005] 3. The existing magnets are in direct contact with the iron core and lack effective insulation design, resulting in insufficient electrical insulation performance. This can easily lead to the formation of conductive paths, posing risks of unstable operation and shortened lifespan.

[0006] In view of this, this utility model proposes a positioning fixture for segmented magnets of a multi-pole motor rotor. Utility Model Content

[0007] The purpose of this invention is to provide a positioning fixture for segmented magnets of a multi-pole motor rotor, which solves the technical problems of difficulty in controlling coaxiality, stress concentration and lack of insulation isolation during the assembly of segmented magnets.

[0008] In a first aspect, this utility model provides a positioning fixture for segmented magnets of a multi-pole motor rotor, comprising:

[0009] The positioning base is fixed on the workbench, and the top is provided with a transition structure and positioning pin for installing the target magnet;

[0010] The transition structure, including a stepped platform and a stepped groove structure, is used to support and connect at least three target magnets, which are stacked segment by segment along the axial direction during assembly; the target magnets include a nickel-copper-nickel three-layer plasma sputtering coating with a total coating thickness of 5±0.5μm, an adhesion of not less than 50N / cm2, and a magnetic flux deviation of not more than 2%;

[0011] The positioning pin is embedded in the tooling base and, by cooperating with the positioning groove or mounting hole on the segmented magnet, ensures that the coaxiality error of the target magnet is no greater than 0.1mm; it is used to achieve the assembly and positioning of the target magnet.

[0012] As a preferred embodiment of this utility model, the target magnet consists of at least three segments.

[0013] The N45SH type neodymium iron boron magnets are composed of a transition structure at the interface of each target magnet segment; there are gaps between adjacent target magnet segments, and the gaps are filled with a cured insulating filling medium to form an insulating layer.

[0014] As a preferred embodiment of this utility model, the transition structure includes:

[0015] The height and width of the stepped platform match the segment dimensions of the target magnet for support and limitation; the stepped groove engages with the stepped platform of the adjacent magnet segment to form a stepped transition interface.

[0016] The machining accuracy of the stepped platform and stepped groove is controlled within ±0.03mm, and a tight fit is ensured to avoid misalignment during assembly; a pre-set gap between the stepped platform and the contact surface of the target magnet is reserved.

[0017] As a preferred technical solution of this utility model, the positioning pin is fixed in conjunction with the positioning groove or mounting hole on the target magnet.

[0018] The technical effects and advantages provided by this utility model in the above technical solution are as follows:

[0019] This invention involves axially and / or circumferentially segmenting neodymium iron boron magnets and machining stepped platforms and stepped grooves at the joint ends. This allows the segmented magnets to achieve high-precision coaxial positioning during assembly using specialized positioning fixtures, ensuring that the radial runout after assembly is controlled within 0.08mm. Furthermore, the synergistic effect of insulating adhesive and modified epoxy filler not only achieves a strong bond between the segments but also forms a complete insulating layer. This results in an insulation resistance of over 1000MΩ between the segmented magnets, effectively avoiding eddy current circulation and local breakdown problems under high-frequency operating conditions. This ensures that the overall magnetic flux deviation is no greater than 3%, ultimately achieving the technical effects of reducing motor eddy current losses and improving electromagnetic performance and operational reliability. Attached Figure Description

[0020] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in this utility model. For those skilled in the art, other drawings can be obtained based on these drawings.

[0021] Figure 1 This is a cross-sectional view of the segmented magnet and stepped platform of this utility model;

[0022] Figure 2 This is a schematic diagram of the segmented magnet installation structure of this utility model.

[0023] Figure 3 This is a flowchart illustrating the assembly method of segmented magnets for the rotor of a multi-pole motor according to this utility model.

[0024] In the diagram: 1. Positioning base; 2. Positioning pin; 3. Transition structure; 4. Target magnet; 5. Insulation layer; 6. Magnet gap. Detailed Implementation

[0025] To make the objectives, technical solutions, and advantages of this application clearer, the technical solutions in the embodiments of this application will be described in more detail below with reference to the accompanying drawings.

[0026] Throughout the accompanying drawings, the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions. The described embodiments are only a part of the embodiments of this application, not all of them. The embodiments described below with reference to the accompanying drawings are exemplary and intended to explain this application, and should not be construed as limiting this application. All other embodiments obtained by those skilled in the art based on the embodiments in this application without inventive effort are within the scope of protection of this application. The embodiments of this application will be described in detail below with reference to the accompanying drawings.

[0027] Example 1

[0028] Please see Figure 1-2 As shown, this embodiment provides a positioning fixture for segmented magnets of a multi-pole motor rotor, including:

[0029] The positioning base 1 is made of 6061-T6 aluminum alloy, balancing rigidity, lightweight, and thermal stability. Its bottom is designed with an installation structure compatible with the worktable. It can be rigidly connected to the worktable via T-slots and bolts, or via positioning keys and pre-set positioning slots on the worktable, ensuring the fixture's unique and stable position on the worktable. In practical applications, the worktable needs to be pre-calibrated for flatness (≤0.02mm) and parallelism (≤0.02mm). After installation, the positioning base 1 is checked for parallelism between its top surface and the worktable surface using a dial indicator, ensuring an error ≤0.03mm, providing a basic spatial reference for subsequent magnet installation.

[0030] The positioning pin 2 is made of high-strength carburized steel and is cylindrical. It is inserted into the pin hole of the positioning base 1 with an interference fit to prevent loosening after long-term clamping and maintain positioning accuracy. In practical applications, the target magnet 4 needs to be pre-machined with positioning holes (or positioning grooves) to cooperate with the positioning pin 2. The fit clearance between the positioning pin 2 and the positioning hole (groove) of the magnet is strictly controlled within 0.01 to 0.03 mm. When three (or more) target magnets 4 are stacked segment by segment along the axial direction, the positioning pin 2 ensures that the central axis of each magnet segment coincides with the reference axis of the tooling through the high-precision fit of the pin hole (groove). Ultimately, the coaxiality error of the entire set of magnets is ≤0.1 mm, which meets the coaxiality requirements of the rotor magnets of multi-pole motors.

[0031] The transition structure 3 is a combination of a stepped platform and a stepped groove integrally machined on the top of the positioning base 1. Its height, width, and step difference are precisely matched to the segmented dimensions (length, width, and thickness) of the transition structure 4, with machining accuracy controlled within ±0.03mm. In practical applications, each target magnet 4 is placed on the stepped platform of the transition structure 3. The flatness of the stepped platform is ≤0.02mm to prevent the magnet from tilting or shifting due to its own weight or assembly force, ensuring the positional stability of the segmented magnets when axially stacked. Simultaneously, in adjacent magnet segments, the stepped platform of the preceding magnet and the stepped groove of the following magnet are meshed together, such as... Figure 1 As shown, the stepped platform is embedded in the stepped groove, with gap control in place. This stepped transition interface ensures the reliability of the segmented magnet docking at the mechanical level, avoiding assembly misalignment. At the electromagnetic level, it creates a stepped transition of the magnetic field at the segment, avoiding distortion caused by sudden changes in the magnetic field and ensuring smooth transmission of magnetic flux between segments.

[0032] Between the stepped platform of transition structure 3 and the contact surface of target magnet 4, and in the docking area of ​​adjacent segmented magnets, is Figure 1 and Figure 2 The marked gap 6 between the magnets is a small gap of 0.05 to 0.1 mm. In actual processes, the gap 6 between the magnets is used to adapt to the insulation bonding and filling process: on the one hand, an insulating adhesive can be applied so that the segmented magnets form an electrical insulation layer 5 while being bonded and fixed; on the other hand, a modified epoxy resin-based composite material can be injected. The insulation layer formed after curing can not only strengthen the mechanical connection between the segmented magnets, but also block the eddy current path and effectively reduce eddy current loss. In other words, when the segmented magnets are joined, the gap 6 between the magnets provides a buffer margin for the assembly error of the positioning fixture and the stepped structure, avoiding assembly interference caused by tolerance accumulation; it allows the adhesive to maintain a tight bond after curing and shrinking, ensuring coaxiality and radial runout requirements.

[0033] Taking the axial assembly of three sections of magnets as an example, in actual assembly, the tooling is first installed and calibrated. The positioning base 1 is fixed to the worktable by T-slots or positioning keys. The positioning pin 2 is installed and its perpendicularity to the top surface of the base is checked (≤0.03mm). Then, the first section of magnet is loaded. The positioning hole (slot) of the first target magnet 4 is aligned with the positioning pin 2 and placed on the first stepped platform of the transition structure 3. The bottom surface of the magnet is manually fine-tuned to make it fit with the stepped platform, completing the initial axial and radial positioning. Then, the sections are stacked and connected one by one. The positioning hole (slot) of the second section of magnet is aligned with the positioning pin 2, and its bottom stepped slot is engaged with the top stepped platform of the first section of magnet. The third section of magnet repeats the above operation to complete the axial stacking and coaxial positioning of the three sections of magnet. Finally, the insulation process is implemented. The insulating adhesive is evenly coated in the reserved gap and the insulating filling medium is injected with a syringe to ensure that the gap is free of air bubbles and fully filled. Then, the assembly is placed in the curing oven and cured according to the process parameters.

[0034] To further explain, the positioning pin 2 is made of high-strength alloy steel, which has high hardness and good wear resistance, and can maintain precise positioning in multiple assembly cycles; the positioning pin 2 cooperates with the positioning groove or mounting hole on the target magnet 4 to achieve quick clamping and ensure that the coaxiality error of three or more magnets during assembly is no more than 0.1mm; the positioning pin 2 is embedded in the positioning base 1 with an interference fit, thereby preventing loosening after long-term use.

[0035] The tooling was designed with the influence of coating thickness and surface roughness in mind, and a gap compensation design was implemented on the contact surface to avoid assembly interference caused by local thickness differences in the coating. The high rigidity and stability of the positioning base 1 ensured the accuracy of the overall assembly process. The structural cooperation between the stepped platform and the stepped groove achieved stable support for the segmented magnets and smooth transition of the magnetic field. The limiting effect of the positioning pin 2 ensured rapid alignment and coaxiality during the assembly process. The gap reserved at the contact interface took into account the process requirements of adhesive coating and insulation material filling.

[0036] In summary, this positioning fixture not only solves the problem of difficult control of position deviation and coaxiality during the assembly of segmented magnets, but also provides process adaptability for subsequent insulation bonding and curing processes, ensuring the electromagnetic performance and mechanical stability of the rotor segmented magnet assembly.

[0037] Example 2

[0038] For parts not described in detail in this embodiment, please refer to Embodiment 1. Figure 3As shown, this embodiment provides a method for manufacturing segmented magnets for a multi-pole motor rotor. Taking an 8-pole, 10kW radial magnetic field motor as an example, it addresses the problems of high eddy current losses, severe magnetic field distortion, assembly stress concentration, and lack of insulation in existing integral magnets used in multi-pole motors. This is achieved through the comprehensive application of segmented magnet design and insulation isolation technology. The method includes the following steps:

[0039] Step S1: Pre-treat and screen target magnet 4 from raw materials. The target magnet 4 comprises a nickel-copper-nickel three-layer plasma sputtering coating with a total coating thickness of 5±0.5μm and an adhesion of not less than 50N / cm. 2 And the magnetic flux deviation is no greater than 2%;

[0040] Specifically, the selection logic for the target magnet 4 is as follows:

[0041] Select a magnet, wherein the magnet includes N45SH type neodymium iron boron magnet;

[0042] The magnets are cleaned and dried to remove surface impurities;

[0043] The surface of the magnet is subjected to plasma sputtering coating treatment. The coating consists of a nickel layer, a copper layer, and another nickel layer in sequence, with a total coating thickness of 5±0.5μm and an adhesion of not less than 50N / cm. 2 ;

[0044] The magnetic flux value of the magnet is detected under normal temperature conditions, and magnets with a magnetic flux deviation of no more than 2% are selected as target magnets 4.

[0045] Taking N45SH type neodymium iron boron magnets as an example, the specific steps are as follows:

[0046] Material procurement: N45SH type neodymium iron boron magnet blanks are selected. The magnets are placed in an ultrasonic cleaner (model KQ-500VDE) and cleaned with anhydrous ethanol (purity 99.7%) for 10 minutes to remove surface oil stains. Then they are dried in a 60℃ oven for 30 minutes.

[0047] Plasma sputtering coating: Plasma sputtering equipment (model JGP-450) was used. Sputtering parameters: argon pressure 0.5 Pa, power 200 W, sputtering time: nickel layer 15 minutes (thickness 3 μm), copper layer 5 minutes (thickness 1 μm), nickel layer 10 minutes (thickness 1 μm). After coating, the adhesion was tested using an adhesion tester (model PosiTest AT-M), and the adhesion was greater than or equal to 50 N / cm. 2 ;

[0048] Magnetic flux testing: Using a permanent magnet fluxmeter (model WT30A), place the magnet in the testing fixture at 25℃ and measure the magnetic flux value to ensure that the magnetic flux deviation of a single magnet is ≤2%.

[0049] Step S2: Segmented cutting of magnets: Using a cutting fixture, the magnets are cut into at least three segments along the axial direction, and the dimensional tolerance and surface roughness of each segment are controlled within a preset range.

[0050] The segmentation method of the magnets is designed according to the number of poles, speed, and thermal management requirements of the motor. The segmentation direction may include:

[0051] Axial segmentation: The magnet is cut into several segments along the rotor axis to shorten the eddy current path and reduce eddy current loss in the axial direction.

[0052] Circumferential segmentation: The magnets are cut along the circumferential direction of the rotor to effectively shorten the circumferential conductive loop and further suppress circumferential eddy currents;

[0053] Axial and circumferential segmentation: Under specific high-frequency or high-speed operating conditions, a combination of axial and circumferential segmentation can be used simultaneously to achieve multi-dimensional eddy current suppression and magnetic field homogenization.

[0054] Specifically, this utility model embodiment uses an axially segmented three-section magnet as an example to describe the process in detail. The steps for cutting the magnet along the axial direction are as follows:

[0055] Tooling preparation: Fabricate a magnetic shielding cutting tool (material: low carbon steel, thickness: 10mm). The tool includes a positioning groove and clamping bolts to prevent the magnetic field from interfering with the molybdenum wire during cutting.

[0056] Segmented cutting: Fix the magnet in the tooling, align the cutting line, and after each segment is cut, stop the machine to check the dimensions to ensure that the length tolerance of a single segment is ≤ ±0.05mm and the flatness of the cross section is ≤0.02mm; the target magnet 4 is cut into at least three segments along the axial direction;

[0057] Burr removal: Manually grind the cut cross-section, grinding in the direction of the cross-section normal to avoid scratching the surface coating. After grinding, use a roughness tester to check to ensure that the surface roughness Ra≤1.6μm.

[0058] It should be noted that this application is intended to clearly and completely disclose the technical solution of this utility model; however, those skilled in the art will understand that circumferential segmentation or a combination of axial and circumferential segmentation is also applicable to this utility model, and the process steps can be implemented equivalently with reference to the disclosure of this application, all of which fall within the protection scope of this utility model.

[0059] Step S3: Segmented cross-section structure processing: Transition structure 3 is processed at both ends of the segmented magnet. The transition structure 3 includes a stepped platform and a stepped groove. The butt joint tolerance of the transition structure 3 is controlled to be no greater than ±0.03mm to achieve smooth magnetic flux transition.

[0060] Specifically, the logic for segmented cross-section stepped processing is as follows:

[0061] Stepped machining: Fix a single section of magnet to the milling machine fixture, machine a stepped platform at one end of the magnet and a stepped groove at the other end. Use a dial indicator to monitor the position of the magnet during machining to avoid deviation.

[0062] Dimensional inspection: Use a coordinate measuring machine to measure the height, width and depth of the steps. Measure 3 points for each dimension and take the average value to ensure that the tolerance is ≤ ±0.03mm and the surface roughness Ra is ≤ 1.6μm.

[0063] Step S4: Preparation of insulating filler medium: Prepare modified epoxy resin-based composite material according to the formula, and use the modified epoxy resin-based composite material as insulating filler medium to make it have high temperature resistance, insulation and mechanical strength properties;

[0064] Specifically, the modified epoxy resin-based composite material includes epoxy resin, curing agent, coupling agent, fumed silica and flame retardant, which are uniformly mixed to form an insulating filling medium.

[0065] The preparation logic of the modified epoxy resin-based composite material is as follows:

[0066] Add 100g of E-51 epoxy resin, 60g of MHHPA, 2g of KH-550, 3g of fumed silica, and 5g of decabromodiphenyl ether; stir for 10 minutes, then add KH-550 and fumed silica, and continue stirring for 20 minutes to ensure uniform mixing.

[0067] Step S5: Segmented magnet assembly: The segmented magnets are coaxially assembled using positioning fixtures. Insulating adhesive is applied to the mating interface, and insulating filling medium is injected into the gaps. After initial curing, an insulating layer is formed.

[0068] Wherein: the insulating adhesive is an epoxy-based high-insulation adhesive (e.g., EP-528), with a shear strength of not less than 18 MPa and a volume resistivity ≥ 1.0 × 10⁻⁶. 14 The coating thickness ranges from 0.05 to 0.15 mm, with an Ω·cm coating thickness of 0.05 to 0.15 mm, to ensure bonding strength and insulation performance.

[0069] Specifically, the installation method of the positioning fixture:

[0070] The positioning fixture for the segmented magnets of the multi-pole motor rotor is fixed on the worktable. Positioning pin 2 is installed inside the fixture to ensure that the coaxiality of the three magnets is ≤0.1mm.

[0071] Apply insulating adhesive (EP-528) evenly to the mounting surface of the magnetic steel ladder, using a scraper to control the adhesive thickness (0.1mm) and ensure uniform application. Figure 1 As shown;

[0072] Magnet docking: Install the three magnet sections from left to right on the stepped platform according to positioning pin 2, and dock them through the stepped structure, such as... Figure 2 As shown. The gap between the joints should be controlled at 0.05-0.1mm. Then, apply a pressure of 0.3MPa using a tooling clamping block and hold for 10 minutes to ensure initial adhesion of the adhesive.

[0073] Insulation filling: Pour the prepared insulating filling medium into the syringe and slowly inject it into the gaps at the junction behind the stepped platform and below the three magnets. Simultaneously, fill the gaps between the three magnets with insulating filling medium as well. During injection, illuminate the gaps with a flashlight to observe the filling process and ensure there are no air bubbles. After filling, use a scraper to smooth out any excess material on the surface.

[0074] Initial curing: Place the assembled magnet assembly along with the tooling into the curing oven, set the temperature to 80℃, keep it at that temperature for 1 hour, remove it after curing, let it cool naturally to room temperature, and check whether the insulation layer is cracked or peeled off.

[0075] Step S6: Rotor core assembly: The assembled segmented magnet assembly is embedded into the rotor core slot and an insulating adhesive is injected. It is then cured under pressure to ensure a reliable bond.

[0076] Specifically, the rotor core assembly logic is as follows:

[0077] Magnet installation: Place the assembled segmented magnet assembly (three sections in one) into the magnet groove, use a dial indicator to check the radial runout of the outer circle of the magnet, and adjust the tooling position to make the radial runout ≤0.08mm. Then inject insulating adhesive (EP-528) into the gap between the magnet and the groove wall. The amount of adhesive injected should be such that the adhesive slightly overflows from the groove opening.

[0078] Pressure curing: Install spring clamping fixtures at both ends of the magnet, place it in the curing oven, and execute the curing curve: room temperature × 2 hours → 80℃ × 2 hours (heating rate 5℃ / min) → 120℃ × 1 hour (heating rate 5℃ / min). Check the pressure every 30 minutes during the curing process to ensure that the pressure is stable.

[0079] Tooling removal: After curing, allow the furnace to cool to room temperature (cooling rate 10℃ / min), remove the spring tooling, and use a knife to clean up any excess adhesive overflowing from the groove (to avoid affecting subsequent assembly).

[0080] Step S7: Overall curing and performance testing: The rotor assembly is subjected to high-temperature curing treatment, and the insulation resistance between segments and the overall magnetic flux are tested to verify that the insulation performance and electromagnetic performance meet the design requirements.

[0081] Specifically, the curing and performance testing steps for the rotor assembly are as follows:

[0082] Final curing: Place the assembled rotor in an oven, set the temperature to 150℃, and keep it at that temperature for 4 hours (heating rate 5℃ / min) to ensure that the insulating filling medium and the adhesive are completely cured.

[0083] Insulation resistance test: Use a 2500V megohmmeter to connect the probes to two adjacent sections of magnet (with conductive plating) and measure the insulation resistance between the sections. The requirement is ≥1000MΩ (at 25℃). If it fails, the insulation layer needs to be re-inspected for damage.

[0084] Overall magnetic flux detection: Wrap 10 turns of detection coil around the outer circumference of the rotor, connect a fluxmeter (WT30A), slowly rotate the rotor, measure the overall magnetic flux value, and compare it with the design value (e.g., 1.2Wb). The deviation should be ≤3%.

[0085] The above description is merely a specific embodiment of this application, but the scope of protection of this application is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in this application should be included within the scope of protection of this application. Therefore, the scope of protection of this application should be determined by the scope of the claims.

Claims

1. A positioning fixture for segmented magnets on a multi-pole motor rotor, characterized in that, include: The positioning base (1) is fixed on the workbench and has a transition structure (3) and a positioning pin (2) on the top for installing the target magnet (4); The transition structure (3) includes a stepped platform and a stepped groove structure for supporting and docking at least three target magnets (4). The target magnets (4) are stacked segment by segment along the axial direction during assembly. The target magnets (4) include a nickel-copper-nickel three-layer plasma sputtering coating with a total coating thickness of 5±0.5μm and an adhesion of not less than 50N / cm. 2 And the magnetic flux deviation is no greater than 2%; The positioning pin (2) is embedded in the tooling base and, by cooperating with the positioning groove or mounting hole on the segmented magnet, ensures that the coaxiality error of the target magnet (4) is no greater than 0.1 mm; it is used to realize the assembly positioning of the target magnet (4).

2. The positioning fixture for segmented magnets of a multi-pole motor rotor according to claim 1, characterized in that, The target magnet (4) is composed of at least three N45SH type neodymium iron boron magnets, and each target magnet (4) has a transition structure (3) at the docking interface; there is a magnet gap (6) between adjacent target magnet segments (4), and the magnet gap (6) is filled with an insulating layer (5) formed by curing.

3. The positioning fixture for segmented magnets of a multi-pole motor rotor according to claim 2, characterized in that, The transition structure (3) includes: The height and width of the stepped platform match the segment size of the target magnet (4) for support and limitation; the stepped groove engages with the stepped platform of the adjacent segment magnet to form a stepped transition interface. The machining accuracy of the stepped platform and stepped groove is controlled within ±0.03mm; a pre-set magnet gap (6) is reserved between the contact surface of the stepped platform and the target magnet (4).

4. The positioning fixture for segmented magnets of a multi-pole motor rotor according to claim 2, characterized in that, The positioning pin (2) is fixed in place by engaging with the positioning groove or mounting hole on the target magnet (4).