Soft magnetic core with location-dependent permeability
Soft magnetic cores with location-dependent permeability variations address inhomogeneous field distributions, enhancing inductance and reducing saturation, thus improving core efficiency and cost-effectiveness.
Patent Information
- Application Number
- DE102012206225
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2012-04-16
- Publication Date
- 2024-11-28
- Estimated Expiration
- 2032-04-16
AI Technical Summary
Existing soft magnetic cores exhibit inhomogeneous field distributions leading to suboptimal performance, increased measurement errors, and higher costs due to oversizing to avoid saturation, as they do not effectively utilize the core material across different locations.
The solution involves designing soft magnetic cores with location-dependent permeability variations, allowing for optimized inductance and reduced saturation effects by adjusting permeabilities at different core locations.
This approach enables a few 10% increase in inductance with the same core volume, reduces saturation effects, and achieves more cost-effective solutions by optimizing core material utilization.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[0001] The invention relates to ring-shaped cores made of soft magnetic material, for example for the production of inductors.
[0002] In electronic control devices such as DC-DC converters, storage chokes, storage transformers, or filter chokes with low-permeability core material are frequently used as inductive energy storage devices. Depending on the design, highly inhomogeneous field distributions can occur in the cores of such inductive components. Therefore, the core material is generally not optimally controlled or utilized across its entire surface. This is still noticeably the case even with relatively highly symmetrical toroidal chokes and leads to less-than-optimal solutions with a larger inner-to-outer diameter ratio, because the maximum possible inductance is not achieved for a given volume, or the smallest or most cost-effective solution is not obtained for a given inductance.
[0003] The core distortion effects mentioned above also lead to distortion-dependent effective core permeabilities in today's commonly used cores with homogeneous permeability distribution via partial saturation effects. This results in noticeable deteriorations in component properties, such as an increase in measurement error in current transformers. Currently, these deteriorations can only be mitigated by appropriately oversizing the core, which avoids operation in the broadened transition range to saturation, but this in turn increases costs. DE 18 04 835 B2, EP 0 121 839 A1, EP 2 130 936 A1, DE 975 437 B, DE K 228 88M AZ and JP 2007 - 180 135 A also deal with magnetic cores.
[0004] The object of the invention is to provide soft magnetic cores which, compared to known cores, have better properties at the same volume or a smaller volume at the same properties.
[0005] The problem is solved by a soft magnetic core according to claim 1, in which the permeabilities occurring at at least two different locations of the core are different.
[0006] The term "different permeabilities" means that the difference between two permeabilities is greater than the differences caused by production tolerances and measurement inaccuracies. For example, the ratio between the minimum and maximum permeability can be greater than 1:1.1, 1:1.2, 1:1.5, 1:2, 1:3, or 1:5.
[0007] The invention is explained in more detail below with reference to the exemplary embodiments shown in the figures of the drawing. It shows: Fig. 1 schematically a soft magnetic ring core with a conductor passed through the ring core opening; Fig. 2. In a diagram, show the course of the field strength and the radially linear increase in permeability over the core radius; Fig. 3 in a diagram the relative increase in inductance with radial-linear permeability increase compared to a constant permeability curve; Fig. 4 in a diagram the radial dependence of the inductance contribution in the core; Fig. 5 in a diagram the permeability versus the current generating an effective field strength for a first case study; Fig. 6. In a diagram, show the permeability versus the current generating an effective field strength for a second case study; Fig. 7 in a diagram the effective permeability versus the effective field strength for the in Fig. 5 shown case; Fig. 8 in a diagram the magnetic flux versus the effective field strength for the in Fig. 6 shown case; Fig. 9 in a diagram exemplary measurements of the geometry-dependent rounding of the flux-field strength loop for cores with constant permeability at different outer and inner diameters; Fig. 10. In a diagram, show the course of the inductance as a function of the direct current through the conductor at the point where... Fig. 1 arrangement shown in a first dimensioning; Fig. 11 in a diagram the course of the inductance as a function of the direct current through the conductor in the Fig. 1 arrangement shown for a second dimensioning; Fig. 12 parameters in a table of the in Fig. 1 arrangement shown for four different cases; Fig. 13 in a diagram the course of the inductance as a function of the direct current through the conductor of the in Fig. 1 arrangement shown for the connection with Fig. 12 cases shown; Fig. 14 schematically shows the structure of a two-part core with a stepped permeability profile; Fig. 15 in a diagram the inductance as a function of the direct current through the conductor of the in Fig. 1 arrangement shown when using a two-part core compared to a one-part core; Fig. 16 in a diagram the inductance contribution over the mean diameter for one-piece and two-piece cores at different current strengths; Fig. 17 in a diagram the induced anisotropy versus tensile stress under different heat treatments; Fig. 18 in a diagram the permeability as a function of tensile stress for different heat treatments; Fig. 19 in a block diagram an arrangement for the production of a nucleus with variable nuclear permeability; Fig. 20 the course of permeability versus field strength for a system arranged according to Fig. 19 manufactured cores; Fig. 21 in a diagram the course of the core permeability as a function of the strip position in a process for producing a strip with a permeability that changes over the strip length; Fig. 22 in a diagram the magnetization versus the field strength of different ring cores made of nanocrystalline material with tensile stress-induced anisotropy; Fig. 23 schematically the structure of a one-piece wound core with permeability varying over the radius; Fig. 24 schematically shows the structure of a two-part core with pressed and wound core parts; Fig. 25 in a diagram the course of nuclear permeability as a function of band position at a level corresponding to the one in Fig. The 21 methods shown are alternative methods for producing a tape with a permeability that changes along the tape length; Fig. 26 in a schematic sketch a winding arrangement for use in the Fig. 25 methods shown; Fig. 27 in a diagram the magnetic flux as a function of the magnetic field strength for an exemplary gradient kernel; and Fig. 28 in a diagram the course of permeability and nuclear field strength versus band position.
[0008] The present invention allows for optimized solutions for specific applications by adjusting the permeability of an arbitrarily shaped magnetic core based on its location, thus enabling, for example, the use of cores with reduced volume or lower costs. Depending on the core geometry, an increase in inductance of several tens of percent can be achieved with the same core volume, as is ideally the case with toroidal cores. This also results in such cores exhibiting a significantly sharper transition from the linear hysteresis range to saturation, or an increased operating range with constant or less variable permeability. Furthermore, it opens up the possibility of selectively setting rounded, effective hysteresis shapes by appropriately controlling deviations from the ideal case.This is achieved by adapting the spatial dependence of the core permeability to the inhomogeneous field distributions resulting from the geometric shape of the component. This minimizes or even avoids saturation effects that occur unevenly across the core volume. Depending on the core material and shape used, this is achieved in various ways. Common core shapes include, for example, ring shapes, U-shapes, I-shapes, and similar forms.
[0009] In the case of toroidal cores, the magnetic field strength H decreases inversely with the radius r, so that H = N⋅I / (2πr) is where N is the number of turns of a conductor passing through the core opening and I is the current flowing through this conductor. Such an arrangement is in Fig. Figure 1 shows a conductor 1 with a number of turns N = 1 passing through the opening of a toroidal core 2. The core 2 has an inner diameter D defining the opening. i, an outer diameter D a as well as a height h. The aforementioned decrease in field strength means that a homogeneous magnetic core material is increasingly less strongly driven towards the outside along its material-specific field-strength-dependent flux curve, also known as the B(H) curve (magnetic flux density B, field strength H). In simplified terms, the inner regions of the core can therefore already operate near or at saturation, i.e., with correspondingly reduced efficiency, while the outer regions are only weakly driven. This effect is more pronounced the larger the ratio of outer diameter to inner diameter. As a good approximation, for example, for height h→∞ or Φ=∫(1 / 2πr)·µ0·µ(r)·I)·h·dr In the case of constant permeability: L = Φ / l = ((μ0μh) / 2π)⋅ln(Da / Di) In the case of radial-linear permeability increase: L = Φ / l = (μ0μh / 2π)⋅(Da / Di−1) where μ(r)=(μi / Di)⋅r.
[0010] Here, Φ is the magnetic flux, µ0 is the magnetic constant, µ is the permeability, µ i the permeability at the inner diameter D i and µ(r) for the radial-linear permeability increase.
[0011] The problem described can be addressed by increasing the permeability of the core material towards the outside. This significantly increases the energy density in the radially outer core layers and thus their inductance contribution.
[0012] Fig. Figure 2 shows the relationship between the radius r and a core with an inner diameter D. i = 30mm and an outer diameter D a= 60 mm. Firstly, the magnetic field is represented as the magnetic field strength H over the radius r (curve 3), and secondly, a possible adjustment of the permeability µ (curve 4) is shown. As curve 3 illustrates, significantly different field strengths H are effective in the radial direction. The magnetic material is therefore driven to varying degrees. With a correspondingly opposite permeability µ, the radially differing field strengths H can be compensated for. With respect to the locally applicable B(H) curve, all core areas are now driven similarly, resulting in an optimized current-dependent inductance control curve, such as the L(Idc) control curve (inductance L as a function of the direct current I flowing through it). DC ) a choke, i.e. with increased inductance values at small output levels and minimized, often unused, inductance values at output levels above the required operating range.
[0013] Fig. Figure 3 shows the relative increase in inductance with radial-linear permeability increase compared to constant permeability as a function of the ratio of outer diameter D. a to inner diameter D i This shows that with small D a / D i -ratios only result in a moderate advantage of up to approximately 30% for typical cores. However, considerable potential emerges for cores where the ratios are larger (starting at a D a / D i >2.
[0014] Fig. Figure 4 shows the gain in total inductance depending on the radius r, i.e., the difference between a core with radially linearly increasing permeability µ(r) and a core with constant permeability µ = µ max (D i ). This in connection with Fig. The example 4 explained was based on a core where the outer diameter D a= 24mm, the inner diameter D i The diameter was 6 mm, the height h was 20 mm, and the saturation flow rate Bs was 1.2 T. The qualitative aspect of the... Fig. As can be seen from figure 4, the gain increases significantly with increasing radius.
[0015] The effects of 1 / r field strength control for a band core with outer diameter D a = 25mm, inner diameter D i = 15mm and a height h = 10mm is in the Fig. 5 and Fig. Figure 6 shows the permeability µ effective in the core as a function of the core control I. DC prop. H DC,eff resolved into different core regions or core shells of diameter D. Fig. Figure 5 shows the case where the permeability µ = 1000 for a field strength H less than or equal to a saturation field strength H. SATand which is otherwise 1. For different diameters D of the nuclear shells, for example with values between D = 15 and D = 25, a clear dispersal of the onset of saturation across the nucleus is evident. Fig. Figure 6 shows the case where the permeability µ depends on the radius r for different core shell diameters D = 15...25 mm. It can be seen from this that an optimal radial permeability dependence leads to a uniform transition to saturation.
[0016] The Fig. 7 and Fig. 8 show the µ eff (H DC )-courses and the L(I DC )-curves, i.e. the effective permeability µ eff and the L(Idc) control curve (inductance L as a function of the direct current I flowing through it) DC ) for the example in connection with the embodiments according to Fig. 5 and Fig. 6 wound tape cores were used. Fig. Figure 7 again shows the case µ=1000 for H≤HSAT and otherwise 1, where H SAT The saturation field strength is... Fig. 8 concerns the case µ(r) = a·r, where a is a constant proportionality factor. In Fig. 7 is the effective permeability µ. eff above the effective field strength H eff and at the one in Fig. In diagram 8, the flux density B is plotted against the effective field strength H. eff is applied. From the Fig. 7 and Fig. Figure 8 immediately shows that a significantly broader transition to saturation occurs for a core with constant permeability. In contrast, with radially linearly increasing permeability, a constant inductance can be provided for considerably higher fields (choke currents), and the region with constant permeability can be significantly enlarged, which is advantageous, for example, in current sensor applications.
[0017] In Fig. Figure 9 shows an example of the geometry-dependent rounding of the B(H) loop for cores with constant permeability µ at different outer and inner diameters. As can be seen, the experimental observations, whose corresponding measurement points are represented by the symbols ◯, □, and × for three different outer and inner diameter ratios (curves 7), confirm with good agreement the model predictions represented by dashed lines for the three different outer and inner diameter ratios. The inserted image in Fig. Figure 9 shows, as curves 8, an enlarged representation of the conditions in the area of the bending to magnetic saturation in curves 7.
[0018] In the Fig. 10 and Fig. 11 is another example of the current-dependent inductance curve (L(I) DC )-course) shown, where a core has an outer diameter D aThe following parameters were assumed: diameter = 24 mm, height h = 20 mm, and a saturation flux Bs = 1.2 T with a number of turns N = 1. The aim is to determine the inductance value L for currents I. DC to keep it constant up to approximately 200A.
[0019] Fig. Figure 10 shows the case where the inner diameter D i = 6mm and therefore D a / D i = 4. The permeability µ i = µ(D i ) at the inner diameter D i is 90 and the permeability µ a = µ(D a ) on the outer diameter D a The value is 360. A distinction is made here between a core with a constant permeability profile (curve 10) and a core with an adapted permeability profile (curve 11). The inner diameter D i In this case, it is 6mm.
[0020] Even in the Fig. In diagram 11, a distinction is made between a core with a constant permeability profile (curve 12) and a core with a variable permeability profile (curve 13), each with a core inner diameter of D. i = 16mm is used. This results in a D a / D i -ratio of 1.5 with a permeability µ i = µ(D i ) on the inner diameter D i of 240 and a permeability µ a = µ(D a ) on the outer diameter D a from 360.
[0021] In the Fig. In the table shown, four cores are placed opposite each other, with all cores having an inner diameter of D. i = 6 mm and a height h = 25 mm. It is a CSC-MF core 13 with a constant permeability µ = µ over the radius. i = 90, a CSC-HF core 14 with a permeability µ = µ constant over the radius r i= 160, a kernel VP with a permeability µ constant over the radius r = µ i = 66 and a core VP with variable permeability µ = µ(r) between 66 and 191. The table contains the respective outer diameter D for each core. a , the respective core volume, the respective permeability range used at maximum current I max as well as the saturation flux density B s The cores are intended, for example, for the production of single-turn filter chokes with target inductance values of 500 mH at DC and > 350 mH at 250 A. The inductance L is then plotted against the (DC) current I flowing through the choke. DC is in Fig. Figure 13 shows that, despite the lower saturation magnetization of Bs, the specification can be well met with a low-permeable VP with a smaller volume (compare curves for cores 13 to 16).
[0022] In Fig. Figure 14 shows a core exhibiting different permeabilities in certain regions. The core 17 shown there is constructed in two parts, such that two ring-shaped sections 17a and 17b are fitted concentrically into one another. Each of the two core sections 17a and 17b has a homogeneous permeability distribution, but the permeabilities differ from each other; that is, the inner core section 17a has a lower permeability than the outer core section 17b. In this case, both core sections 17a and 17b are powder cores, but the two cores can be manufactured differently in any way (see also [reference to be added]). Fig. 24 and related description).
[0023] In Fig. 15 are the inductance curves of a device like the one in Fig. Figure 14 compares the optimized, two-part core (curve 18) and a conventional one-part core (curve 19). Curves 18 and 19 are based on a FeSi powder core with an outer diameter D. a = 47mm, with an inner diameter D i = 24 mm and a height h = 18 mm. The permeability µ ia The inner diameter of the core part 17a is 60 and the permeability p ib The inner diameter of the core part 17b is 90. Fig. Figure 16 shows the inductance contributions across the core diameter for one-piece and two-piece cores at currents of 0 A, 10 A, and 20 A, represented as curves 20 to 25. The superiority of cores with radially varying permeability is immediately apparent from this as well.
[0024] Instead of a multi-part magnetic core with stepwise changing permeability as in Fig. As shown in Figure 14, a powder core with continuously changing permeability can also be produced by layering materials of different permeabilities into a mold, or by mixing two materials with constant but mutually different permeabilities (especially one of the materials with µ=0) in radially different mixing ratios. Furthermore, it is also possible to achieve a core with continuously changing permeability by winding a strip with a permeability that varies along its length. A strip with a permeability that varies along its length can be produced, for example, by utilizing tensile stress-induced anisotropy. In wound strip cores, a continuous heat treatment of the strip under tensile stress allows for very precise adjustment of the permeability profile µ(I) along the strip direction I, which can be varied over a wide range.In particular, the permeability profile can be selected so that the desired radially increasing µ(r) function is achieved in the finished core during the winding of the strip. In a coupled "in-line" core production process, the core winding can directly follow the heat treatment of the strip (strip tempering) under tension and thus be actively controlled to meet the current, radially dependent permeability requirement via tension control. Alternatively, core winding can be completely decoupled from strip production using strips with different constant permeabilities. Correspondingly automated winding machines can draw strips with different permeabilities from various magazines and process them successively. However, these methods can only produce stepped, not radially continuous, variations in the core.
[0025] The course of the induced anisotropy K µ above the tensile stress σ is in Fig. Figure 17 shows different heat treatments. The corresponding permeability curve µ versus tensile stress σ is shown. Fig. 18. The permeability depends on the vacuum permeability µ0 of the band, whose induced anisotropy K, as follows. u as well as the saturation flux density Bs as follows: μ=0.5⋅Bs2 / (μ0Ku).
[0026] Fig. Figure 19 schematically shows a device 26 for producing soft magnetic strip material. This device comprises an inlet material feed 27 for supplying strip-shaped material 39, a heat treatment device 28 for heat-treating the supplied strip-shaped material 39 to produce a heat-treated strip material 40, and a clamping device 30, 31, 32, which is configured to introduce a tensile force into the strip-shaped material 39 and to generate a tensile stress in the longitudinal direction of the strip, at least in the area of the heat treatment device 28. The clamping device 30, 31, 32 is designed to be controllable for varying the tensile force.
[0027] The device 26 also comprises a measuring arrangement 33 for determining the permeability of the produced soft magnetic strip material 40 and a control unit 34 for controlling the clamping device 30, 31, 32, wherein the control unit 34 is configured and coupled to the measuring arrangement 33 such that the clamping device 30, 31, 32 regulates the tensile force in response to the determined permeability µ relative to a predetermined (desired) reference value. In the embodiment shown, the clamping device 30, 31, 32 comprises two coupled S-shaped roller drives 30, 32 and a dancer control 31. The speeds of the roller drives 30 and 32 are controlled by the control unit 34, i.e., adjusted, such that the desired tensile tension builds up depending on the permeability in the strip material 39 (and 40) determined by the measuring arrangement 33.Dancer rule 31 is used to compensate for short-term speed fluctuations.
[0028] Additionally, the device 26 can include a magnetic field generator 29 that generates at least one magnetic field for the magnetic field treatment of the heat-treated strip material, such as a magnetic field perpendicular to the strip direction, also known as a transverse field. Optionally, a winding unit 35 with several winding mandrels 36 on a rotatable turret plate 37 can be included for winding a defined section of the produced strip material 40. The winding unit 35 can include an additional S-shaped roller drive 38 that feeds the treated strip material, i.e., the strip material 40, to the respective winding mandrel 36.
[0029] Fig. Figure 20 shows the relationship between a tensile stress introduced into the ribbon-shaped material 39 by means of a tensile force F and the resulting anisotropy Ku and permeability µ. A tensile stress σ occurring locally in the ribbon-shaped material 39 results from the applied tensile force F and a local magnetic cross-sectional area A. Fe (Material cross-section) σ=F / AFe, such that an induced anisotropy Ku in the transverse direction to the longitudinally extended ribbon-shaped material 39 increases as a function of the tensile stress σ. The permeability µ is set via the generated tensile stress σ and results from the mean slope of the hysteresis loop, or from the saturation flux density Bs, or from the magnetic field strength H, namely the anisotropic field strength H. A , as well as the magnetic field constant µ0 in conjunction with the anisotropy Ku as above in connection with Fig. 17 explained.
[0030] If, for example, the thickness of the strip-shaped material varies due to manufacturing processes, then, assuming a constant width, the local cross-sectional area A will also vary accordingly. Fe and with it, at constant tensile force F, the applied tensile stress σ. This in turn causes a corresponding change in the induced anisotropy Ku, which, via the relationships mentioned above, influences the permeability µ accordingly, so that this also changes over the length of the soft magnetic strip material 40 produced from the ribbon-shaped material 39.
[0031] In a strip manufacturing process, for example, the strip material can be unwound from a magazine and drawn through a tubular heat treatment furnace, where it is subjected to tensile stress along its longitudinal axis. At annealing temperatures above the crystallization temperature, the initially amorphous material in the heat treatment zone can transition into a nanocrystalline state, which in this case is responsible for the excellent soft magnetic properties of the resulting strip. The applied tensile stress induces transverse anisotropy in the magnetic material, resulting in a pronouncedly flat hysteresis loop in the resulting soft magnetic strip with a tightly controlled permeability µ (in the range of 10,000 to below 100 when measured along the strip axis). The achievable level of permeability µ is determined by the specific parameters of the strip.The induced anisotropy Ku is proportional to the applied tensile stress in the band. These relationships are described in the... Fig. 17 and Fig. 18 for the nanocrystalline alloy VP800 of the vacuum melt is clearly illustrated.
[0032] Subsequently, the strip of tape, now no longer under tension, is guided through the measuring arrangement 33, which measures the permeability µ (and possibly other parameters such as tape cross-section, coercive field, remanence ratio, losses, etc.) in real time. Knowing these values, the continuously running tape is then processed into a toroidal core, in which a specific length of the magnetic tape is always unwound onto a winding mandrel.
[0033] The described technology enables the production of soft magnetic tape material with a wide range of permeability levels and extremely small deviations from the target permeability value along the entire tape length. The permeability can be selectively increased or decreased over certain sections of the tape length to achieve a desired radially variable permeability profile along the tape for each core type, as mentioned above. The measuring setup required for the control process also provides continuous information about the magnetic tape cross-section (local A). Fe of the band). By combining controlled permeability and information about the band cross-section and applying a core winding process at the end, toroidal band cores with a predefined permeability profile and very low sample variations with respect to A are obtained. Fe -value of the core.
[0034] The Fig. Diagram 21 illustrates how core permeability can be controlled by varying the permeability along the barrel length. The diagram assumes a core with a height of 30 mm and a mean diameter of 60 mm. The permeability is 100 at the inner circumference and 200 at the outer circumference, resulting in a mean permeability µ. m This results in a value of 150. The respective (adjusted) permeability µ is specified over the belt length. The tension is controlled such that the permeability µ increases over the length of approximately 90 m required for one core. Upon reaching the 90-meter mark, the permeability is reduced as quickly as possible from µ = 200 back to µ = 100 so that the control process can begin again for the next core.
[0035] Fig. Figure 22 shows the magnetization J versus the magnetic field strength A for various ring cores made of nanocrystalline material with tensile stress-induced anisotropy for a permeability range from µ = 2000 to 60.
[0036] In Fig. Figure 23 shows a wound ring core 38 made of strip material with permeability increasing along its length in three views.
[0037] In a Fig. In the further development shown in 24, a powder core part 39a with, for example, a homogeneous permeability distribution is used, onto which a strip material with a permeability value increasing over the length is wound to form a wound core part 39b.
[0038] In Fig. 25 is one of the ones in Fig. The procedure shown in Figure 21 schematically illustrates an alternative method for controlling permeability. In this method, after reaching the upper permeability value of 200, the permeability is not reduced as quickly as possible back to the initial value of 100. Instead, it is reduced from 200 to 100 with the same slope as during the increase. Once the value of 100 is reached, it is then increased again from 100 to 200. This avoids the losses that occur when reducing the permeability from the upper to the lower value, as in the procedure described above. Fig. 21 arise, avoided.
[0039] However, a modified winding technique will then be necessary. The required modified winding technique is described in Fig. 26 schematically explains this, distinguishing between the rising and falling flanks, i.e., between increasing and decreasing permeability values along the belt length. At each reversal point of the permeability, a switch 43 directs the belt onto path 1 if the permeability subsequently increases, and onto path 2 if the permeability subsequently decreases. Winding in path 1 is carried out as in the case described in Fig. In the case shown in 19, the core winding is carried directly, whereas in path 2, for example, a roll magazine is wound via an intermediate storage area and from there it is led to the actual core winding station, for example, another core winding station 2.
[0040] Fig. Figure 27 shows, in an exemplary embodiment, comparative measurements between a gradient core and a core with constant permeability (µ=1000), each with dimensions of 13 mm × 25 mm (inner diameter × outer diameter) and a core height of 6.1 mm. With such a core, which has an outer-to-inner diameter ratio of approximately 2, the geometrically induced confluence effect into magnetic saturation can be clearly observed (curve 47). Specifically, the idealized hysteresis curve 45 is shown on the strip. Curve 47 shows the measurement on the core with constant permeability, and curve 46 shows the measurement for the gradient core. Thus, curve 45 approximates the hysteresis curve on the strip (curve 54) through the spatial adaptation of the permeability. In the curve 47 corresponding to the Fig. Figure 27a shows that the permeability was kept constant across the 17 meters of strip material required for the core. In contrast, the Fig. 27b, that the permeability was increased from 700 to approximately 1400 over 14 m of ribbon material in a special form to achieve a spatial adaptation of the permeability at the core, which as a result yields the hysteresis curve 46.
[0041] Regarding the above in connection with Fig. 27 illustrated embodiment shows Fig. Figure 28 shows the actual (i.e., measured) permeability profile (46b, x-measurement points) and the predicted profile (target profile 46a) of permeability along the strip required for a core in a diagram. During the continuous annealing process, the tensile stress in the strip material was adjusted based on the predicted "target" permeability profile so that the Fig. The increase in permeability shown in Figure 28 (measuring points 46b) occurs.
[0042] Optimized amorphous and nanocrystalline gradient band cores offer a comparatively wide permeability range with high saturation flux and simultaneously very precisely adjustable permeability. This makes them suitable for a wide variety of applications. For storage inductors, in particular, permeability values well above approximately 100 are now accessible, opening up new possibilities for realizing inductors with comparatively lower numbers of turns to reduce copper losses. For highly linear, DC-tolerant current transformers, the permeability range from several hundred to a few thousand is of interest, since the strips, heat-treated under tensile stress, exhibit a nearly constant permeability up to saturation (µ(H) = constant), independent of the signal level, and this property can also be maintained for the entire core (see [reference]). Fig. 9). First application example: Ring band core choke:
[0043] The band permeability of a tensile stress-tempered, amorphous or nanocrystalline band behaves to a good approximation in a step-like manner over the modulation range, that is, there is a practically linear B(H) curve up to saturation, corresponding to a permeability that is constant up to saturation and then drops extremely sharply (cf. Fig. 6) A core wound from such a material with constant permeability and typical dimensions exhibits an L(I DC )-characteristic with a broadly smeared, sloping shoulder at the control limit (cf. Fig. 7) Accordingly, the effective B(H) curve of the kernel shows a noticeable rounding at the transition to saturation (cf. Fig. 8) If, on the other hand, a radially increasing permeability profile is chosen, i.e., µ(r) = a*r (with a* = constant), the original band characteristic can be maintained for the entire core in the limiting case of optimal matching. Furthermore, only the permeability value, and thus the inductance value, remains at a uniform maximum value up to saturation. Should this sharp transition not be desired, intermediate states deviating from the optimum can also be deliberately set. Second application example: Powder core throttle
[0044] The permeability of powder nuclei behaves as follows for various, typical initial permeabilities µ. i (Permeabilities at the inner diameter) such as those in Fig. 15 and Fig. 16 shown progressions. In Fig. 16 becomes an L(I DCThe curve for a core with typical dimensions and made of typical material is shown in comparison to a core made of two concentric rings of the same dimensions and material. Here too, optimization with respect to L(I) is possible. DC )-characteristic can be achieved.
[0045] The main application for the core optimization described here will primarily concern wound, rotationally symmetric toroidal cores, as these require a comparatively simple spatial adjustment of the core permeability with relatively moderate permeability changes along the tape length. However, the method could also be used for U-shaped cores, I-shaped cores, and cores of other shapes, although the permeability variation along the tape length would then have to be performed over much shorter distances to compensate for the field strength inhomogeneities at the inner corners.
[0046] The prospects for producing tensile-stress tempered strip material with extremely low permeabilities (permeability values around and below 50) are limited. Conversely, above µ i =90 or 160 more suitable powder core material. It could therefore be advantageous to use combined strip and powder ring cores, i.e., with an inner, low-permeability powder core and an outer, higher-permeability, non-radially permeability-matched strip core, as in, for example, Fig. Figure 24 shows that in single-wind chokes, the cores can be wound directly onto a stacked copper conductor and then fixed, for example, by overmolding or by a trough that is slipped over and potted.
[0047] The following materials can be considered suitable core materials for such a process: amorphous cobalt-, nickel-, and iron-based alloys, such as all Vitrovac and Vitroperm alloys, or all iron-based alloys with the following composition range: Fe100-abcdxyz CuaNbbMcTdSixByZz where: 10 ≤ × < 18 atom%; 5 ≤ y < 11 atom%; 0 ≤ a < 1.5 atom%; 0 ≤ b < 4 atom%. M represents the elements: Mo, TA or Zr with 0 ≤ (b+c) < 4 atom%. T represents the elements: V, Mn, Cr, Co or Ni with 0 ≤ d < 5 atom%. Z represents the elements: C, P or Ge with 0 ≤ z < 2 atom%.
Claims
[1] Soft magnetic core, in which permeabilities occurring at at least two different locations in the core are different; the core is ring-shaped; and the core has at least two soft magnetic elements joined to one another, one of the magnetic elements having an inherently inhomogeneous permeability distribution and the other having a radially changing permeability profile. [2] A soft magnetic core according to claim 1, wherein at least one of the soft magnetic elements comprises ribbons. [3] A soft magnetic core according to any one of claims 1 or 2, wherein an element of the core is a one-piece powder core or a one-piece powder core element. [4] Method for producing a soft magnetic toroidal core having different permeabilities at at least two different locations, wherein the core in one piece and with a permeability that varies over the location, wherein to produce a toroidal core by means of a strip of soft magnetic material the strip is subjected to heat treatment, the heat-treated strip is subjected to a tensile force in the longitudinal direction of the strip in order to generate a tensile stress in the strip-shaped material, the permeability per length of the tensioned heat-treated strip is determined, the tensile force is adjusted so that the determined permeability for each length section corresponds to the value of a given permeability profile and the tape is wound onto the toroidal core. [5] A method according to claim 4, wherein the ratio between minimum and maximum permeability is greater than 1: 1.1 or 1: 1.2 or 1: 1.5 or 1:2 or 1:3 or 1:5.
Citation Information
Patent Citations
Toroidal core choke for radio interference suppression of semiconductor circuits that work according to the phase control principle
DE1804835B2
DE22888A
suppression choke
DE975437C
Transformer with ferromagnetic circuits of unequal saturation inductions
EP0121839A1
Soft magnetic ribbon, magnetic core, magnetic part and process for producing soft magnetic ribbon
EP2130936A1