Torsion bar stabilizer and method for manufacturing a torsion bar stabilizer

The torsion bar stabilizer addresses weight and reliability issues by using hardened end sections with press hardening and tempering, ensuring high strength and sealed ends for improved durability and reduced weight.

DE102015114897B4Active Publication Date: 2024-10-02MUHR UND BENNDER KG
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
DE102015114897
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Filing Date
2015-09-04
Publication Date
2024-10-02
Estimated Expiration
2035-09-04

AI Technical Summary

Technical Problem

Existing stabilizers for motor vehicle chassis require additional reinforcements for high loads, leading to increased weight and potential leaks at the ends, compromising component reliability and longevity.

Method used

A torsion bar stabilizer with a tubular body, torsion spring section, and bent legs, featuring hardened end sections with a strength of at least 800 MPa, produced through press hardening and tempering, ensuring high strength and reduced weight, with sealed end sections for improved durability.

Benefits of technology

The stabilizer withstands high loads, reduces weight, and maintains long service life with enhanced sealing properties, achieved through a combination of high strength and efficient manufacturing processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
  • Figure 00000000_0001_ABST
    Figure 00000000_0001_ABST
Patent Text Reader

Abstract

Torsion bar stabilizer for a motor vehicle chassis, made from a tubular body, comprising: a torsion spring section (3) and two legs (4, 4') bent from the torsion spring section (3), wherein the legs (4, 4') each have a formed end section (7, 7') with a through-opening (10, 10') and a tubular section (6, 6'), wherein the torsion spring section (3) has a hardened structure with a strength of at least 1000 MPa, and wherein the formed end sections (7, 7') are produced by press hardening and have a hardened structure with a strength of at least 800 MPa.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to a torsion bar stabilizer for a chassis of a motor vehicle and a method for Manufacturing of such a stabilizer. A torsion bar stabilizer is a spring element that prevents the motor vehicle and thus improves the driving dynamics and the roadholding of the The ends of the stabilizer are each connected to a wheel suspension of a vehicle axle The stabilizer is attached to the vehicle body between the two ends.

[0002] From DE 11 2011 100 846 T5 a solid stabilizer and a manufacturing process of the solid Stabilizer is known. The manufacturing process includes a forming step for forming the steel material, a Hot forging step for producing the eye-shaped end sections of the formed steel material, a Hardening step and a tempering step. During the hardening step, the eye-shaped end sections are clamped and Current is applied between the eye-shaped end sections to heat the steel material to a hardening temperature of 970° C. The steel material is then quickly cooled and tempered. After tempering, the tensile strength 1,200 MPa or more.

[0003] From US 2011 / 0290382 A1 a high-strength steel for a stabilizer is known, which contains 0.07% to 0.2% C and 1% to 3% Mn and other alloying elements. The stabilizer has a torsion section and a pair of arms with cone-shaped end pieces. US 2014 / 0060709 A1 describes a similar stabilizer with cone-shaped End pieces known.

[0004] From US 2007 / 0216126 A1 a method for producing a tubular stabilizer is known. A tube body is provided, which is heated and then quenched. In the quenched state, the tube body has a strength of about 1400 MPa. The tube body is then formed into the desired shape, whereby the formed stabilizer comprises a substantially elongated body with two stabilizer arms having first and second ends In one embodiment, the ends of the stabilizer are formed after the forming operations and hardening further formed and holes drilled into the ends.

[0005] From DE 197 58 292 A1 a tubular stabilizer is known in which the individual stabilizer sections are are dimensioned so that a virtually equal fatigue strength is achieved in the main stabilizer sections. The basic strength values ​​of the material are given as 1,500 MPa to 1,800 MPa. the tensile strength of the surface layer is increased compared to the tensile strength of a decarburized material. The ends of the stabilizer are cone-shaped.

[0006] From DE 10 2009 011 818 A1 a method for producing a stabilizer with two stabilizer bearings is known. For this purpose, the stabilizer is heated in sections, then connected to the stabilizer bearing in surface contact and pressed.

[0007] From DE 10 2013 101 276 A1 a method for producing a motor vehicle stabilizer is known. It is intended that strip material made of a high-manganese steel alloy is formed into a tubular profile and which is then welded into a continuous tube using high-frequency welding. The tube thus produced is then a mandrel, whereby depending on the degree of deformation of the redrawing, an intermediate annealing may take place One advantage is that the stabilizer produced in this way does not require any further treatment.

[0008] The end sections of stabilizers can be geometrically and due to cross-sectional changes forming and cooling processes also have a reduced load-bearing capacity in terms of material structure. The wall thicknesses of the End sections of stabilizers are usually designed according to the forces introduced by the wheel-guiding components. forces or loads.

[0009] In case of high loads and low material thickness of the stabilizer ends, it may be necessary to incorporate additional reinforcements, which counteracts the demand for lightweight construction. Leakage may occur at the stabilizer ends, which in the worst case could lead to component failure can.

[0010] Based on this, the present invention is based on the object of proposing a stabilizer which, at which is highly resilient with the lowest possible use of materials and which is easy to manufacture with good sealing properties The task is also to propose a corresponding manufacturing process that allows the production of a highly resilient and as light as possible stabilizer, whose ends have good sealing properties, process-safe enabled.

[0011] One solution consists in a hardened torsion bar stabilizer for a chassis of a motor vehicle, made of a tubular body comprising: a torsion spring section and two legs bent therefrom; wherein the legs respectively a formed end portion with a through-opening and a tubular portion; wherein the Torsion spring section has a hardened structure with a strength of at least 1000 MPa; and wherein the formed end sections are produced by press hardening and have a hardened structure with a strength of at least 800 MPa.

[0012] One advantage is that the torsion bar stabilizer can also be used in can withstand high loads and has a long service life. Due to the high strength, the wall thickness of the end sections may be reduced if necessary, so that the weight of the The formed and hardened stabilizer ends can, for example, be easily and can be manufactured reliably by press hardening.

[0013] The stabilizer is hardened or tempered, which in the context of the present disclosure means that the stabilizer has a higher hardness than the starting material. For this purpose, the starting material is heated and subsequently quenched to produce a harder structure than the initial structure. Preferably, the Stabilizer made of a hardenable steel material which is heated to austenitizing temperature for hardening and The rapid cooling results in at least partial, preferably complete transformation of the microstructure to martensite. Steels suitable for this purpose are those in which the time-temperature Transformation diagram the transformations in the pearlite and bainite stages are shifted to longer times, so that the upper critical cooling rate is relatively low and is also reached in the core of the workpiece Preferably, the steel material has a carbon content of less than 0.5 percent by weight and / or a manganese content of 0.5 to 3.0 percent by weight.

[0014] After hardening, the stabilizer can be tempered. Through tempering, the strength of the initially The brittle martensite decreases, but the toughness increases. Overall, the desired combinations of properties of the component can be achieved. The combination of hardening and subsequent tempering of the Component is also called hardening and tempering.

[0015] The hardness and strength of the stabilizer are interdependent. Depending on the desired strength, the Torsion spring section according to a possible embodiment has a hardness of at least 310 HV, preferably at least 410 HV, in particular at least 500 HV. The formed end areas can have a hardness of at least 250 HV, preferably at least 310HV, in particular at least 400 HV.

[0016] The stabilizer can be made from a tubular body as starting material, from which the legs The formed end sections of the legs are produced by hot forming. the end sections to be formed are first heated so that the hardness in these sections is lower than the hardness of the starting material is reduced again, and then formed. In particular, it is intended that the formed end sections each have a flat end area which is perforated and an adjoining Transition area. The holes created by the perforation serve to connect the stabilizer with a connecting component, for example a chassis component of the motor vehicle. Preferably, the End sections or end areas are sealed liquid-tight and / or gas-tight. This can be done by Forming operation to produce the formed end sections. In particular, it is intended that the Manufactured in such a way that the stabilizer ends are gas-tight up to at least 2 bar internal pressure and / or the Internal pressure after 5 minutes is still at least 0.75 times the maximum applied pressure. hardened structures of the end areas in addition to the forming process contribute to achieving these tightness values.

[0017] The transition area between the flattened end area and the tube section of the leg has a variable cross-section over the length of the transition area. In other words, the transition area forms a cross-section-changing transition between the flat end area and the tubular leg section. The The transition area has a strength of preferably at least 800 MPa, in particular at least 1000 MPa, each According to technical requirements, even more than 1200 MPa. According to a favorable design, the transition area at least approximately the same strength and hardness as the perforated end area of ​​the leg.

[0018] The transition area is followed by the tubular leg section, which forms a section with low strength or hardness. The strength in this sub-area can, for example, be less than 0.7 times the strength of the torsion spring section and / or greater than 0.5 times the strength of the To ensure that the section with reduced strength does not have a negative impact on the Overall strength and service life of the stabilizer tor, it is particularly intended that this has a distance from the transition area that is preferably at least half the diameter of the tubular leg section.

[0019] According to a possible embodiment, the torsion bar stabilizer can have a variable wall thickness over the length The wall thickness can be adjusted according to the technical requirements, i.e. higher A greater wall thickness can be provided in areas subject to stress or in areas where a greater If elasticity is desired, the wall thickness can be reduced accordingly. In particular, it is intended that a wall thickness of at least the end regions is smaller than a maximum wall thickness of the torsion bar stabilizer. For example, the wall thickness of the end areas can be at least 20% smaller than the maximum wall thickness of the Stabilizer. The maximum wall thickness is formed especially in the bending sections. A medium wall thickness of the transition area may be reduced compared to a maximum wall thickness of the stabilizer.

[0020] The solution to the above-mentioned problem further consists in a method for producing a torsion bar Stabilizer for a chassis of a motor vehicle, comprising the steps of: producing a tube; bending legs of the pipe; quenching and tempering of the pipe before or after bending the legs, so that the hardened pipe has a hardness structure with a strength of at least 1000 MPa; heating an end section of the legs after Hardening or tempering of the pipe, whereby the strength in the end section is reduced to below 800 MPa is; hot forming the end section after heating to produce a formed end section; Punching the formed end section to create a through hole; hardening the formed end section such that the formed end section has a hardened structure with a strength of at least 800 MPa.

[0021] The process according to the invention offers the same advantages as the product according to the invention, so that In this regard, reference is made to the above description. It is understood that all product-related characteristics refer to the processes, and vice versa. Overall, the stabilizer according to the invention can be used due to the high Strength of the end sections can withstand high loads and has a long service life, or rather Material and weight can be saved while maintaining the same load on the stabilizer. In the process according to the invention The end sections undergo two hardening processes, namely a first one as part of the tempering of the tube used as the starting material, and a second one, namely the partial Hardening the end sections.

[0022] According to a possible procedure, the heating of the end sections by means of inductive Heating occurs during induction heating. Inductive heating occurs in the electrically conductive component by means of the Eddy current losses, whereby the heat is generated directly in the component itself. As a device for inductive heating An induction coil, induction heater or induction furnace can be used. The induction device generates via a coil through which alternating current flows, an alternating magnetic field is created which induces eddy currents in the component.

[0023] It is particularly provided that the steps of hot forming the end section and punching a Through hole in the formed end section can be made in a common tool.

[0024] The hardening of the formed end sections can, according to a first possibility, be carried out in the same tool such as hot forming and punching. In this case, the tool would be used as a combined Hot forming, punching and hardening tool. By hot forming, punching and hardening in a single Tool enables rapid production with short cycle times. In particular, it can be provided that First, one leg of the stabilizer is heated at its end section, then into the combined Hot forming, punching and hardening tool is inserted, whereby the end section becomes the formed end section is formed, the hole is punched into the end section and the end section is hardened by rapid cooling Then the stabilizer with its formed and hardened first leg is removed from the tool removed so that the second leg can then be manufactured accordingly. The combined tool is preferably designed in such a way that the machining sequence of the leg in the chronology of forming, punching and Hardening takes place. In principle, however, it is also conceivable that the punching takes place with a temporal overlap or after hardening An advantage of manufacturing in the combined tool is that the energy required for manufacturing is low overall, since the component only needs to be heated once for hot forming and hardening. The process of Combined hot forming and hardening can also be called press hardening.

[0025] According to an alternative possibility, the hardening of the formed end sections can also be carried out as A separate process step can be carried out using a separate device. The hardening can be timed to the Hot forming process, in particular in such a way that the stabilizer is removed from the tool and by means of the The rapid cooling can be achieved, for example, by means of an air flow or in a liquid bath, such as an oil or water bath. However, curing can also be carried out in a time and be spatially separated from the combined hot forming and stamping process. In this case, the formed End sections of the stabilizer are first heated to austenitizing temperature and then quickly heated in a In the separate hardening process, it is possible, according to a first variant, to first cool both End sections to austenitizing temperature and then quickly in the hardening or cooling device According to a second variant, the two end sections can also be heated and cooled one after the other become.

[0026] According to a possible process, the production of the pipe can be carried out by the following sub-steps: rolling of a steel strip; forming the steel strip into the slotted pipe body; and longitudinal welding of the slotted pipe body to the closed tube. To create a variable sheet thickness over the length of the stabilizer, In a first possibility, the pipe is produced by drawing over a stepped mandrel. The pipes produced in this way are also called Tailor Drawn Tube. Alternatively, the variable wall thickness of the stabilizer can also be achieved by be manufactured by processing the steel strip used as the starting material for the pipe by means of flexible rolling before being formed into a tube. In flexible rolling, strip material with a substantially uniform Sheet thickness by changing the roll gap during the process to produce strip material with variable sheet thickness over the Length rolled out. The sections of different thickness produced by flexible rolling extend transversely to the Longitudinal direction or to the rolling direction of the strip material. After flexible rolling, the strip material can be wound up into a coil again and sent to another location for further processing, or it can be directly be further processed, for example by forming into a tube body and longitudinal welding. Alternatively, the Pipe can also be manufactured seamlessly as a drawn pipe.

[0027] The tempering of the tube is carried out by the following steps: heating the tube to austenitizing temperature; Quenching the heated tube; and tempering the quenched tube. By heating the material to Austenitizing temperature means that the material is heated to a temperature at which at least partially Austenite is formed. The austenitizing temperature is preferably above the Ac3 point, which means Steel materials preferably above 800°C. The subsequent quenching to a lower temperature takes place especially between the upper and lower critical cooling rate, that is so fast that at least Martensite is partially formed. Quenching prevents the diffusion of iron and carbon, so that the cubic face-centered austenite into the tetragonally distorted body-centered lattice of martensite by a Depending on the cooling rate, intermediate structures can also be or bainite. After quenching, tempering takes place, whereby the hardened tube is heated to moderately high Temperatures below the A1 temperature are heated and then cooled down again. internal stresses are reduced, meaning that hardness and strength decrease, while toughness increases. The process combination of hardening and tempering is also called quenching and tempering.

[0028] Preferred embodiments are described below with reference to the drawing figures. Herein: Fig. 1 a torsion bar stabilizer according to the invention in plan view A) with hardness progression over the length; B) with wall thickness progression over the length; Fig. 2 the detail X of the torsion bar stabilizer from Fig. 1 A) top view; B) in side view; C) with hardness gradient; Fig. 3 a device for producing a stabilizer according to Fig. 1A in different steps A) with the first leg inserted into the device for processing; B) after forming an end section of the first leg; C) after cutting and punching the formed section of the first leg; Fig. 4 the device from Fig. 3 A) with the second leg inserted into the device for processing; B) after forming an end section of the second leg; C) after cutting and punching the formed section of the second leg.

[0029] Figures 1 and 2, which are described together below, show a device according to the invention Stabilizer 2 for use in the chassis of a motor vehicle. The stabilizer 2 has a torsion spring section 3, which can also be referred to as torsion bar spring section or stabilizer back, and two of the torsion spring section 3 angled legs 4, 4', which can also be called lever arms. Between the A bending section 5, 5' is formed between the torsion spring section 3 and the legs 4, 4'. It can be seen that the The present stabilizer 2 is constructed mirror-symmetrically relative to a center plane E and has a Legs 4, 4'. However, it is understood that the stabilizer can also be designed asymmetrically and, depending on Depending on the installation space conditions, it may also have unequal legs. If, within the scope of the present disclosure only one of the legs 4, 4' is referred to, it is understood that this always also applies to the other leg 4', 4 of the stabilizer applies.

[0030] The torsion spring section 3 is essentially straight and is supported, for example, by means of two bearings (not shown) attached to the vehicle body, for example in the engine compartment or on the underbody of the vehicle. Legs 4, 4' are used to connect the stabilizer 2 with the two wheel suspensions (not shown) of an axle of the motor vehicle. In this case, the legs 4, 4' are essentially straight and end with the Torsion spring section 3 forms a right angle in plan view of the stabilizer 2. However, it is understood that the Legs can also have other designs depending on the installation space and application. For example, The legs can also be cranked or bent and / or at an angle other than 90° to the Torsion spring section 3.

[0031] By connecting the legs 4, 4' of the stabilizer 2 with an associated wheel suspension of the motor vehicle, the two wheel suspensions are spring-coupled to each other. When cornering, a One-sided compression of the outside vehicle wheel and simultaneous rebound of the inside wheel, a roll of the vehicle. This compression movement is transmitted via the deflecting leg 4, 4' and the Torsion spring section 3 is transferred to the opposite leg 4', 4. In this way, a rolling of the motor vehicle, i.e. a rotational movement around the vehicle's longitudinal axis.

[0032] The stabilizer 2 is made of a one-piece tubular body with a closed cross-section, from which End sections are bent, which form the legs 4, 4'. The starting material is a hardenable steel material which preferably has a carbon content of less than 0.5% by weight and a manganese content of 0.5 to 3.0 weight percent. In addition to iron, other common alloying elements such as chromium and / or boron The stabilizer 2 or the tubular body used to manufacture the stabilizer is tempered, i.e. hardened and tempered. The tube body can be tempered before or after bending the legs 4, 4'.

[0033] Each of the legs 4, 4' has, starting from the bending section 5, 5', a tubular section 6, 6' with a at least approximately constant cross-section over the length and a formed end section 7, 7'. The formed End sections 7, 7' each have a flattened area 8, 8' and a transition area 9, 9'. Transition area 9, 9' connects the flattened end area 8, 8' with the tubular leg 6, 6' and have accordingly a variable cross-section over the length of the respective transition area 9, 9'.

[0034] It can be seen in particular in Fig. 2B that the flat end regions 8, 8' of the formed end sections 7, 7' The through holes 10, 10' are used to connect the stabilizer 2 with a Chassis component of the motor vehicle. The flat end areas 8, 8' are liquid-tight and gas-tight, respectively sealed, preferably up to at least 2 bar internal pressure, so that the penetration of dirt and water The gas-tight sealing takes place during the forming process. It is advantageous if the Stabilizer ends are so gas-tight that the internal pressure after 5 minutes is still at least 0.75 times the maximum applied pressure.

[0035] It can also be seen in Fig. 2A that the transition areas 9, 9' between the respective adjoining flat End area 8, 8' and the pipe section 6, 6' of the leg 4, 4' have a variable cross-section over the length, so that a cross-section-changing transition between the flat end region 8, 8' and the tubular Leg section 6, 6' is formed.

[0036] As already mentioned above, the stabilizer 2 is made of a tempered steel material. Basic strength of the tempered steel material, depending on the starting material, at least 1000 MPa, in particular at least 1200 MPa, if necessary also at least 1400 MPa. For example, a stabilizer tube body made of quenched and tempered steel material 26MnB5 have a basic strength of approximately 1400 MPa to 1585 MPa. A pipe body made of Tempered steel material 34MnB5 can have an even higher basic strength of about 1585 MPa to 1680 MPa.

[0037] In the finished state of the stabilizer, the formed end sections 7, 7' have a strength of at least 800 MPa, in particular at least 1000 MPa. The strength of the formed end sections 7, 7' can be lower than the basic strength of the quenched and tempered steel material and in particular at least 0.8 to 0.9 times times the strength of the tempered steel material. With a strength of the tempered steel material of 1200 MPa, the strength of the formed end sections 7, 7' could therefore be between 960 MPa and 1080 MPa.

[0038] The strength of the stabilizer correlates with the hardness, for which an exemplary curve is shown in Fig. 1A and, as enlarged detail for one of the legs 4, 4' of the stabilizer 2, shown in Fig. 2C. The basic hardness of the The hardness of the stabilizer is designated H2 and the hardness of the end sections 7, 7' is H7. A medium base hardness is designated 0.5H2. It can be seen that the hardness H7 of the end sections 7, 7' is slightly lower than the basic hardness H2, in particular, approximately 0.9 times the basic hardness H2. Example values ​​for the hardness of stabilizer 2 can be specified as follows. The basic hardness H2 can be at least 410 HV, in particular at least 500 HV. formed end sections 7, 7' can have a hardness H7 of at least 310 HV, in particular of at least 400 HV have.

[0039] It can also be seen that the end sections 7, 7', starting from a front end 12, 12', extend over the respective End area 8, 8' and the adjoining transition area 9, 9' a substantially constant hardness H7 or strength which is in particular greater than 0.8 times the basic hardness H2 or Basic strength of the stabilizer 2. Only in the tubular section 6, 6' of the leg 4, 4', which due to its geometry is a has a larger area moment of inertia than the formed end section 7, 7', a partial area 13, 13' with reduced hardness Hmin. The reduced hardness Hmin is greater than the average basic hardness 0.5H2 of the stabilizer 2 and less than 0.7 times the basic hardness, i.e. 0.7H2 > Hmin > 0.5H2. The soft part 13, 13' is Transition area 9, 9' clearly spaced, in particular by a length greater than half the diameter D6 of the tubular leg section 6, 6'.

[0040] In Fig. 1B, the wall thickness d of the stabilizer 2 is plotted over the length L. It can be seen that the Torsion bar stabilizer has a variable wall thickness d over the length L, whereby it is understood that the wall thickness can also can be constant over the length. In this case, the wall thickness is in relation to a center plane of the Stabilizer symmetrical. In particular, it is intended that the wall thickness d4 of the legs 4, 4' is Wall thickness d5 of the bending sections 5, 5' is reduced. In the bending sections 5, 5' the stabilizer has the largest Wall thickness d5. Starting from the two bending sections 5, 5' towards the center plane, the stabilizer has Torsion spring section 3 again has a reduced wall thickness d3, which in this case comprises two sections with of different thickness. It is understood that depending on the loads on the stabilizer, a two different number of sub-areas such as one, three or more than three can be incorporated into the stabilizer 2. The Transition areas between two wall thickness ranges d3, d4, d5 are continuous, so that the best possible uniform stress and avoid stress peaks. Specifically, it is intended that the formed end sections 7, 7' have a wall thickness that is at least 20% smaller than the maximum wall thickness d5 of the stabilizer.

[0041] To produce a tubular body with variable thickness over the length, for example, a tube initially A pipe made with a constant wall thickness is drawn over a stepped mandrel so that sections with different wall thicknesses (Tailor Drawn Tube). Alternatively, the tube can be made of flexible rolled strip material can be produced as the starting material, which will be discussed in more detail below. Such flexibly rolled strip material is also called tailor rolled blank.

[0042] A method according to the invention for producing the stabilizer 2 comprises the following process steps: Manufacturing a pipe; bending the legs 8, 8' from the pipe; tempering the pipe before or after bending the Legs, so that the quenched and tempered tube has a hardened structure with a strength of at least 1000 MPa; heating of an end section of one of the legs 8, 8' after hardening of the pipe, wherein the strength in the end section is reduced to below 800 MPa; hot forming of the end section after heating to Production of the formed end section 7, 7'; punching of the formed end section 7, 7' to produce the Through opening 10, 10'; hardening the formed end section such that in the formed end section a hardened structure with a strength of at least 800 MPa. Then the second leg 8', 8 in processed accordingly.

[0043] The production of the pipe can be carried out by the following steps: rolling a steel strip; forming the steel strip into a slotted pipe body; and longitudinal welding of the slotted pipe body to the closed pipe. To produce a variable sheet thickness over the length of the stabilizer 2, the steel strip can be formed into a tube be rolled flexibly beforehand, or a pipe with an initially constant wall thickness can be made flexible after welding During flexible rolling, the strip material is given a certain degree of flexibility by changing the roll gap a variable sheet thickness along the length. The bending of the legs 8, 8' takes place in a corresponding bending device. The tempering of the tube is carried out by the following steps: heating the tube to austenitizing temperature; quenching of the heated tube; and tempering of the quenched tube. Tempering is preferably carried out after bending the leg 8, 8', but in principle can also be carried out beforehand. After tempering, the tempered Pipe body 2' with a substantially constant cross-section over the length L of the pipe body and the above-mentioned Basic strength of at least 1000 MPa.

[0044] Starting from this, the end sections of the legs 8, 8' are produced, which is described below with reference to the Figs. 3A to 3C explain this.

[0045] In Figs. 3A to 3C, a combined hot forming, punching and hardening tool 14 is shown, which is described below for the sake of simplicity also referred to as tool. Before inserting the tempered tube body 2' into the Tool 14 heats the end section 15 of the first leg 8, which can be done by inductive heating The length of the heated section 15 corresponds at least approximately to the length of the formed End section 7 of the leg 8. After heating the section 15, the pipe body 2' is quickly inserted into the tool inserted, which is shown in Fig. 3A.

[0046] The combined hot forming, punching and hardening tool 14 comprises a frame 16, an upper tool part 17 and a lower tool part 18. On the upper tool part 17, an upper mold insert 19 is provided, which is provided with a corresponding lower mold insert 20 of the lower tool part 18. For forming the leg 8 the upper tool part 17 is moved towards the lower tool part 18, whereby the inserted Tubular body 2' is formed at the end leg section 15 by the mold inserts 19, 20, or flattened and pressed. The two mold inserts 19, 20 thus form parts of the hot forming device and can also referred to as pressing or flattening inserts. To move the upper tool part 17, a drive unit 21 is provided, which may in particular comprise two hydraulic cylinders 22, 22'. Fig. 3B shows the tool 14 with extended hydraulic cylinders 22, 22' and correspondingly lowered upper tool part 17 as well as the formed Condition of the tubular body 2'. It can be seen that the previously tubular section 15 of the leg 4 to formed section 7 with flattened end region 8 and transition region 9.

[0047] Subsequently, the protruding end of the formed section 7 is cut off and the flattened End area 8 is perforated. For this purpose, the tool 14 has a cutting device 23 on the upper tool part 17 for Trimming the protruding end and a punching device 24 for punching the flattened end area 8. The Cutting device 23 and the punching device 24, which can also be referred to as a hole device, have a common drive unit 25, which in particular comprises a hydraulic cylinder. While the press force of the Forming device for forming the leg 8 is maintained, a knife and a punch move through the Form inserts 19, 20 and punch the flattened area 7 and trim the end. Fig. 3C shows the tool 14 with extended hydraulic cylinder 25 and correspondingly lowered cutting and punching device 23, 24. It is It can be seen that a projecting end of the formed section 7 is cut off and the through opening 10 in the flattened end area 8 has been incorporated.

[0048] The hardening of the formed end section 8 is carried out by rapid cooling of the end section by flat Contact of the workpiece with the mold or press inserts 18, 20. The rapid cooling takes place in such a way quickly that an at least partially martensitic structure is formed in the formed end section 8. In this case, a Diffusion of iron and carbon is avoided, so that the cubic face-centered austenite into the tetragonally distorted body-centered lattice of martensite by a thrust or The advantage with regard to the tightness of the flattened end area 8 is that Martensite has a slightly larger volume than austenite due to its lattice structure, so that the superimposed Walls of the flattened end area 8 lie particularly firmly and tightly against one another.

[0049] After producing the formed and hardened section 7 of the first leg 8, the stabilizer 2 removed from the tool 14. Subsequently, the second end 15' or the second leg 8' is processed in analog form. This process is shown in Figures 4A to 4C which is identical to the process for producing the first leg 8. In this respect, abbreviated reference is made to the above description for machining the first leg 8.

[0050] It is understood that the process described is only exemplary and can also be modified. In particular The stabilizer can also be removed directly from the forming tool after hot forming and special means to harden or quickly cool down. For example, the formed End sections 8, 8' after removal of the stabilizer 2 from the forming tool in a separate cooling device cooled by means of a liquid medium.

[0051] Optionally, the tube body can be internally blasted before forming and hardening the leg ends 7, 7'. After After producing the formed and hardened sections 7, 7', the stabilizer 2 can be externally blasted, coated and can optionally be fitted with add-on parts.

[0052] An advantage of the stabilizer 2 or the method for its production is that due to the high strength of the end sections 7, 7' can withstand high loads and has a long service life The stabilizer ends 7, 7' can be advantageously formed in a single tool 14, namely the The combined hot forming, punching and hardening tool 14 described above can be produced easily, quickly and reliably. The hardening of the end sections 7, 7' not only results in higher strength, but also has a positive effect on the Tightness of the stabilizer 2, which contributes to a long service life overall. List of reference symbols 2, 2' stabilizer, tubular body 3 Torsion spring section 4, 4' leg 5.5' bending section 6, 6' tubular section 7, 7' reshaped section 8, 8' flattened area 9, 9' transition area 10, 10' passage opening 11 12, 12' front side 13, 13' sub-area 14 tools 15, 15' end section 16 frame 17 upper tool part 18 lower tool part 19 upper mold insert 20 lower mold insert 21 Drive unit 22, 22' hydraulic cylinder 23 Cutting device 24 punching device 25 drive unit d wall thickness D Diameter E Level H Hardness L length

Claims

1. Torsion bar stabilizer for a chassis of a motor vehicle, made from a tubular body, comprising: a torsion spring section (3) and two legs (4, 4') bent from the torsion spring section (3), wherein the legs (4, 4') each have a formed end section (7, 7') with a through opening (10, 10') and a tubular section (6, 6'), wherein the torsion spring section (3) has a hardened structure with a strength of at least 1000 MPa, and wherein the formed end sections (7, 7') are produced by press hardening and form a hardened structure with a Have a strength of at least 800 MPa.

2. Torsion bar stabilizer according to claim 1, characterized in that the formed end sections (7, 7') have a Have a strength that is at least 0.8 times the strength of the torsion spring section (3).

3. Torsion bar stabilizer according to claim 1 or 2, characterized in that the torsion spring section (3) has a hardness (H2) of at least 310 HV, and that the formed end sections (7, 7') have a hardness (H7) of at least 250 HV.

4. Torsion bar stabilizer according to one of claims 1 to 3, characterized in that the formed end section (7, 7') a flat end region (8, 8') with an approximately constant cross-section over the length (L) and a transition region (9, 9') with a variable cross-section over the length (L).

5. Torsion bar stabilizer according to one of claims 1 to 4, characterized in that the legs (4, 4') in tubular section (6, 6') each have a partial area (13, 13') with a low strength which is smaller than 0.7 times the strength of the torsion spring section (3) and / or which is greater than 0.5 times the strength of the Torsion spring section (3).

6. Torsion bar stabilizer according to claim 5, characterized in that the partial area (13, 13') with low strength from the formed end section (7, 7') a distance which is at least half the diameter (D6) of the tubular section (6, 6').

7. Torsion bar stabilizer according to one of claims 1 to 6, characterized in that the end sections (7, 7') of the Legs (4, 4') are sealed liquid-tight and / or gas-tight.

8. Torsion bar stabilizer according to one of claims 1 to 7, characterized by a variable wall thickness (d) over the Length (L), wherein a wall thickness of the end sections (7, 7') is smaller than a maximum wall thickness (d5) of the torsion bar Stabilizer (2).

9. Torsion bar stabilizer according to claim 8, characterized in that the wall thickness of the end sections (7, 7') is at least 20% smaller than the maximum wall thickness, wherein the maximum wall thickness (d5) in a bending section (5, 5') is formed between the torsion spring section (3) and a leg (4, 4').

10. Torsion bar stabilizer according to one of claims 1 to 9, characterized in that the torsion bar stabilizer consists of a steel material with a carbon content of less than 0.5% and a manganese content of 0.5% to 3.0% is manufactured.

11. A method for producing a torsion bar stabilizer for a chassis of a motor vehicle, comprising the steps: - Manufacturing a pipe, - Bending of legs (4, 4') from the pipe, - Tempering the tube before or after bending the legs (4, 4') so that the tempered tube has a hardened structure with a strength of at least 1000 MPa, - heating an end section (15, 15') of a first of the legs (4, 4') after tempering the tube, wherein the strength in the end section (15, 15') is reduced to below 800 MPa, - hot forming the end section (15, 15') after heating to form a formed end section (7, 7'), - punching the formed end section (7, 7') to produce a through opening (10, 10'), - hardening the formed end section (7, 7') in such a way that a hardened structure is formed in the formed end section (7, 7') with a strength of at least 800 MPa.

12. Method according to claim 11, characterized in that the heating of the end sections (15, 15') by means of inductive heating.

13. Method according to claim 11 or 12, characterized in that the steps of hot forming the end-side Partial section (15, 15') to the formed end section (7, 7') and punching the formed end section (7, 7') to Creation of a through opening (10, 10') in a combined tool (14).

14. Method according to one of claims 11 to 13, characterized in that the hardening of the formed end section (7, 7') is cooled in the combined tool (14).

15. Method according to one of claims 11 to 14, characterized in that the production of the pipe by the Substeps: - rolling a steel strip, - Forming the steel strip into the slotted pipe body, and - longitudinal welding of the slotted pipe body to the closed pipe takes place, and that the heat treatment of the pipe is carried out by the sub-steps: - Heating the pipe to austenitizing temperature, - Quenching the heated pipe and - Tempering of the pipe takes place.

Citation Information

Patent Citations

  • Method for producing stabilizer between e.g. stabilizer pipe and half shell shaped stabilizer support, in motor vehicle chassis, involves sectionally heating metal part, and pressing metal part and polymer molded part with each other

    DE102009011818A1

  • Method for manufacturing a motor vehicle stabilizer

    DE102013101276A1

  • Massive stabilizer, steel material for the massive stabilizer and manufacturing process of the massive stabilizer

    DE112011100846T5

  • stabilizer

    DE19758292A1

  • stabilizer

    DE2846445A1