Sulfur-crosslinkable rubber compound and vehicle pneumatic tires

A triazine-based rubber mixture with an allyl group addresses the safety and environmental issues of resorcinol in traditional mixtures by enhancing adhesion and reducing contamination, maintaining vulcanizate properties.

DE102018213702B4Active Publication Date: 2024-11-14CONTINENTAL REIFEN DEUTSCHLAND GMBH
View PDF 17 Cites 0 Cited by

Patent Information

Application Number
DE102018213702
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Filing Date
2018-08-15
Publication Date
2024-11-14
Estimated Expiration
2038-08-15

AI Technical Summary

Technical Problem

Existing sulfur-crosslinkable rubber mixtures for tire reinforcements, particularly those using resorcinol and phenol-based methylene acceptors, pose occupational safety and environmental hazards due to their high vapor pressure and health risks, leading to contamination and processing inefficiencies.

Method used

A sulfur-crosslinkable rubber mixture using a triazine structure with an allyl group capable of crosslinking with rubber, replacing traditional methylene acceptors like resorcinol, to enhance adhesion and reduce health and environmental risks.

Benefits of technology

The triazine-based mixture achieves improved adhesion to reinforcements while minimizing health and environmental hazards, maintaining vulcanizate properties, and reducing contamination during processing.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

Sulfur-crosslinkable rubber compound with a free resorcinol content of less than 0.1 wt.%, containing at least one adhesive for the reinforcement-rubber bond, wherein the adhesive contains a methylene donor and at least one chemical compound having a triazine structure and at least one rubber-crosslinkable group, wherein hexamethoxymethylmelamine (HMMM) and / or hexamethylenetetramine (HMT) is used as the methylene donor, characterized in that the at least one rubber-crosslinkable group is an allyl group.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to a sulfur-crosslinkable rubber mixture with a free resorcinol content of less than 0.1 wt. %, containing at least one adhesive for reinforcement-rubber adhesion, wherein the adhesive contains a methylene donor and at least one chemical compound having a triazine structure and at least one rubber-crosslinkable group, wherein hexamethoxymethylmelamine (HMMM) and / or hexamethylenetetramine (HMT) is used as the methylene donor. Furthermore, the invention relates to a pneumatic vehicle tire comprising at least one such sulfur-crosslinked rubber mixture.

[0002] In sulfur-curable rubber compounds used as rubberizing compounds for textile reinforcements such as rayon, polyamide, and polyester, so-called methylene acceptor-methylene donor pairs are typically used to achieve a bond for the adhesive impregnation of the textile reinforcement, usually an RFL dip, in addition to the bonding via the sulfur network. The RFL dip contains resorcinol and formaldehyde or their precondensates.

[0003] As an alternative to RFL dips, maleic-functionalized polymers are now also offered for the treatment of textile fabrics or textile reinforcements to achieve improved adhesion to rubber compounds. Such so-called RF-free dips are disclosed, for example, in EP 1745079 B1 and DE 102014211365 A1.

[0004] Hexamethoxymethylmelamine (HMMM) and / or hexamethylenetetramine (HMT), for example, are used as methylene donor / formaldehyde donors. Their use is widespread in the tire industry. Resorcinol and resorcinol equivalents or their precondensates, as well as other phenols, are used as methylene acceptor reactants. During the vulcanization process, a resin is formed from the methylene donor and the methylene acceptor. In addition to the sulfur network, a second network based on the methylene donor and methylene acceptor forms, which interacts adhesively with the RFL dip.

[0005] The use of methylene acceptor-methylene donor pairs is also known for rubberizing compounds for metallic reinforcements, especially brass-plated steel cord. In the so-called direct adhesion process for brass-plated steel cord, the rubberizing compound contains, for example, cobalt salts and a resorcinol-formaldehyde-silica system, with the formaldehyde typically coming from formaldehyde donors such as hexamethoxymethylmelamine (HMMM) and / or hexamethylenetetramine (HMT). Reinforcing resins are also used to improve adhesion, and the compounds should contain high sulfur and low accelerators to ensure sufficient mechanical interlocking with the steel cord surface.

[0006] Resorcinol- or phenol-based methylene acceptors have disadvantages with regard to occupational safety and environmental protection. Resorcinol has a relatively high vapor pressure at the processing temperatures of a rubber compound, so it partially evaporates during processing and precipitates on cooler components. This leads to significant contamination and thus requires extensive cleaning effort. Furthermore, resorcinol is classified as harmful to health and the environment. It may affect the central nervous system. Therefore, efforts are being made to avoid resorcinol as a methylene acceptor reactant. Phenol, which can evaporate during the processing of rubber compounds, is also classified as harmful to health and the environment, so efforts are being made to reduce this substance.

[0007] Mixtures that do not require methylene acceptor reactants are known, for example, from EP 0 830 423 B1 and EP 2 065 219 A1. However, these documents use so-called self-condensing alkylated triazine resins with high imino and / or methylol functionality. It is assumed that the high imino and / or methylol functionality allows these resins to self-condense and thereby form a network necessary for adhesion without the need for a methylene acceptor reactant.

[0008] Other rubber compounds that do not contain resorcinol are mentioned in DE 100 16 120 A1, DE 40 20 797 A1 and US 4391318 A.

[0009] EP 2 674 452 A1 discloses the use of a reactive phenolic resin, particularly a phenolic resin modified with a vegetable and / or animal oil, an unsaturated oil, and / or an aromatic hydrocarbon, as a methylene acceptor in a sulfur-curable rubber compound for textile reinforcements in pneumatic vehicle tires. This results in good adhesion, fewer impurities during compound production, and at the same time, the use of resorcinol, which is harmful to health and the environment, could be eliminated during processing. In this case, even larger amounts of free phenol may be present in the resin.

[0010] It has been shown that the aforementioned methylene acceptor reactants do not achieve the desired adhesion and stiffness for all applications, especially for all tire body compounds. Resorcinol and / or phenol residues are often still present in the resins, which pose known health and environmental hazards during processing.

[0011] The invention is based on the object of providing a sulfur-crosslinkable rubber mixture which, with good adhesion to reinforcements, leads to an improvement in terms of occupational safety and environmental protection.

[0012] The object is achieved according to the invention in that in a mixture of the type mentioned at the outset the at least one group crosslinkable with rubber is an allyl group.

[0013] Triazines are a group of chemical compounds whose basic structure is an aromatic heterocycle containing three nitrogen atoms in a six-membered ring system.

[0014] Rubber-crosslinkable groups can be any group that can chemically bond to rubber molecules, possibly with the help of crosslinking chemicals such as sulfur or peroxide.

[0015] It has been shown that with chemical compounds that have a triazine structure and at least one group that can be crosslinked with rubber, good or even improved adhesion to reinforcements after vulcanization can be achieved.

[0016] The use of special compounds with a triazine structure has little negative impact on other vulcanizate properties; in some cases, they are even improved. At the same time, the low content of free resorcinol and free phenol makes the compounds more environmentally friendly and less hazardous to health during processing.

[0017] The rubber-crosslinkable groups of the chemical compound can be a wide variety of groups, such as double-bond, sulfur-containing, or peroxide-containing groups. Different groups can also be present within a single molecule. According to the invention, the at least one rubber-crosslinkable group is an allyl group. These can be easily bonded to the rubber via, for example, sulfur crosslinking. At the same time, the triazine structure appears to enable bonding to the reinforcements, resulting in good adhesion between the reinforcements and the rubber after vulcanization.

[0018] The chemical compound can be, for example, various cyanurates. For particularly good adhesion, triallyl cyanurate, triallyl isocyanurate, and / or trimethallyl isocyanurate are preferred. These compounds are available, for example, under the names TAC and TAICROS. ®available from Evonik.

[0019] To further improve adhesion and maintain the hardness of the vulcanized compound at a comparable level, the rubber compound contains a methylene donor. This can build a secondary network for adhesion and hardness.

[0020] Hexamethoxymethylmelamine (HMMM) and / or hexamethylenetetramine (HMT, 1,3,5,7-tetraazaadamantane, urotropine) are used as methylene donors. These are commonly available methylene donors that form a good resin network. HMMM, for example, is used as a technical product – often on an inert support – with a degree of methylation < 6.

[0021] The sulfur-curable rubber mixture contains other components commonly used in the rubber industry, in particular at least one rubber. Diene rubbers can be used as rubbers. Diene rubbers include all rubbers with an unsaturated carbon chain that are at least partially derived from conjugated dienes.

[0022] The rubber mixture can contain polyisoprene (IR, NR) as the diene rubber. This can be either cis-1,4-polyisoprene or 3,4-polyisoprene. However, the use of cis-1,4-polyisoprenes with a cis-1,4 content of > 90 wt.% is preferred. Such a polyisoprene can be obtained by stereospecific polymerization in solution with Ziegler-Natta catalysts or using finely divided lithium alkyls. Natural rubber (NR) is also such a cis-1,4-polyisoprene, and the cis-1,4 content in natural rubber is greater than 99 wt.%.

[0023] If the rubber mixture contains polybutadiene (BR) as the diene rubber, it can be cis-1,4-polybutadiene. The use of cis-1,4-polybutadiene with a cis-1,4 content of greater than 90 wt.% is preferred, which can be produced, for example, by solution polymerization in the presence of rare earth catalysts.

[0024] Other diene rubbers that can be used include vinyl-polybutadienes and styrene-butadiene copolymers. Vinyl-polybutadienes and styrene-butadiene copolymers can be solution-polymerized (styrene)-butadiene copolymers (S-(S)BR) with a styrene content, based on the polymer, of approximately 0 to 45 wt.% and a vinyl content (content of 1,2-bonded butadiene, based on the total polymer) of 10 to 90 wt.%, which can be produced, for example, using lithium alkyls in an organic solvent. S-(S)BR can also be coupled and end-group modified. However, emulsion-polymerized styrene-butadiene copolymers (E-SBR) and blends of E-SBR and S-(S)BR can also be used. The styrene content of the E-SBR is approximately 15 to 50 wt.% and the types known from the prior art, which were obtained by copolymerization of styrene and 1,3-butadiene in aqueous emulsion, can be used.

[0025] The diene rubbers used in the mixture, especially the styrene-butadiene copolymers, can also be used in partially or fully functionalized form. The functionalization can be carried out with groups that can interact with the fillers used, especially with fillers containing OH groups. This can, for example, involve functionalization with hydroxyl groups and / or epoxy groups and / or siloxane groups and / or amino groups and / or phthalocyanine groups and / or carboxyl groups and / or silane sulfide groups. The diene rubbers can also be coupled additionally or alternatively.

[0026] In addition to the diene rubbers mentioned, the mixture may also contain other types of rubber, such as styrene-isoprene-butadiene terpolymer, butyl rubber, halobutyl rubber or ethylene-propylene-diene rubber (EPDM).

[0027] Reclaim can also be added to the rubber mixture as a processing aid and to reduce the mixing cost.

[0028] The rubber mixture may contain various fillers, such as carbon black, silica, aluminosilicates, chalk, starch, magnesium oxide, titanium dioxide or rubber gels in usual quantities, whereby the fillers may be used in combination.

[0029] If carbon black is used in the rubber mixture, it is preferred to use types that have a CTAB surface area (according to ASTM D 3765) of more than 30 m 2 / g. These are easy to mix and ensure low heat buildup.

[0030] If silicas are included in the mixture, they can be those commonly used in tire rubber compounds. It is particularly preferred to use a finely divided, precipitated silica with a CTAB surface area (according to ASTM D 3765) of 30 to 350 m².2 / g, preferably from 110 to 250 m 2 / g. Both conventional silicas and type VN3 ® (trade name) from Evonik as well as highly dispersible silicas, so-called HD silicas (e.g. Ultrasil ® 7000 from Evonik).

[0031] If the rubber compound contains silica or other polar fillers, silane coupling agents can be added to the compound to improve processability and bond the polar filler to the rubber. The silane coupling agents react with the surface silanol groups of the silica or other polar groups during mixing of the rubber or rubber compound (in situ) or even before the filler is added to the rubber as a pretreatment (premodification). Silane coupling agents that are known to those skilled in the art for use in rubber compounds can be used.Such coupling agents known from the prior art are bifunctional organosilanes that possess at least one alkoxy, cycloalkoxy, or phenoxy group as a leaving group on the silicon atom and that have, as another functionality, a group that, optionally after cleavage, can enter into a chemical reaction with the double bonds of the polymer. The latter group can be, for example, the following chemical groups: -SCN, -SH, -NH2, or -S. x- (where x = 2-8). For example, 3-mercaptopropyltriethoxysilane, 3-thiocyanatopropyltrimethoxysilane, or 3,3'-bis(triethoxysilylpropyl)polysulfides with 2 to 8 sulfur atoms, such as 3,3'-bis(triethoxysilylpropyl)tetrasulfide (TESPT), the corresponding disulfide, or mixtures of sulfides with 1 to 8 sulfur atoms with varying contents of the various sulfides, can be used as silane coupling agents. The silane coupling agents can also be added as a mixture with industrial carbon black, such as TESPT on carbon black (trade name X50S). ® from Evonik). Blocked mercaptosilanes, such as those known from WO 99 / 09036, can also be used as silane coupling agents. Silanes such as those described in WO 2008 / 083241 A1, WO 2008 / 083242 A1, WO 2008 / 083243 A1, and WO 2008 / 083244 A1 can also be used. Examples of suitable silanes are those sold under the name NXT. ®in various versions from the company Momentive, USA, or those that are sold under the name VP Si 363 ® sold by Evonik Industries. So-called "silated core polysulfides" (SCPs) can also be used, as described, for example, in US 20080161477 A1 and EP 2 114 961 B1.

[0032] Furthermore, the rubber mixture according to the invention can contain customary additives in customary parts by weight. These additives include plasticizers, such as glycerides, factices, hydrocarbon resins, aromatic, naphthenic or paraffinic mineral oil plasticizers (e.g. MES (mild extraction solvate) or TDAE (treated distillate aromatic extract)), oils based on renewable raw materials (such as rapeseed oil, terpene oils (e.g. orange oils) or factices), so-called BTL oils (as disclosed in DE 10 2008 037714 A1) or liquid polymers (such as liquid polybutadiene)); ageing inhibitors, such as B. N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine (6PPD), N-isopropyl-N'-phenyl-p-phenylenediamine (IPPD), 2,2,4-trimethyl-1,2-dihydroquinoline (TMQ) and other substances, as known for example from J. Schnetger, Lexikon der Kautschuktechnik, 2nd edition, Hüthig Buch Verlag, Heidelberg, 1991, pp. 42-48, activators, such as B.Zinc oxide and fatty acids (e.g. stearic acid), waxes, tackifying resins such as hydrocarbon resins and rosin, and masticating agents such as 2,2'-dibenzamidodiphenyl disulfide (DBD).

[0033] Vulcanization is carried out in the presence of sulfur and / or sulfur donors, whereby some sulfur donors can also act as vulcanization accelerators. Sulfur or sulfur donors are added to the rubber compound in the final mixing step in amounts customary in the art (0.4 to 8 phr). Vulcanization can also be carried out in the presence of very small amounts of sulfur in combination with sulfur-donating substances.

[0034] The term phr (parts per hundred parts of rubber by weight) used in this document is the standard quantity used in the rubber industry for compound formulations. The dosage of the parts by weight of the individual substances is always based on 100 parts by weight of the total mass of all rubbers present in the compound. The mass of all rubbers present in the compound adds up to 100.

[0035] Furthermore, the rubber compound can contain vulcanization-influencing substances such as vulcanization accelerators, vulcanization retarders, and vulcanization activators in conventional amounts to control the required vulcanization time and / or temperature and improve the vulcanizate properties. The vulcanization accelerators can be selected, for example, from the following accelerator groups: thiazole accelerators such as 2-mercaptobenzothiazole; sulfenamide accelerators such as benzothiazyl-2-cyclohexylsulfenamide (CBS) and benzothiazyl-2-dicyclohexylsulfenamide (DCBS); guanidine accelerators such as N,N'-diphenylguanidine (DPG); dithiocarbamate accelerators such as zinc dibenzyldithiocarbamate; disulfides; and thiophosphates. The accelerators can also be used in combination with each other, which can result in synergistic effects.

[0036] Other network-forming systems, such as Vulcures® , Duralink ® , Percalink ® or systems as described in WO 2010 / 049261 A2 can be used in the rubber compound.

[0037] The rubber mixture according to the invention is produced in a conventional manner, whereby a base mixture containing all components except the vulcanization system (sulfur and vulcanization-influencing substances) is first prepared in one or more mixing stages. The final mixture is then produced by adding the vulcanization system. The mixture is then further processed.

[0038] The rubber compound can be used in a wide variety of rubber products that contain reinforcements. These rubber products can include drive belts, conveyor belts, hoses, rubberized fabrics, or air springs.

[0039] The rubber compound is primarily used in pneumatic vehicle tires. It can be used, for example, as a rubber lining for textile or metallic reinforcements. The textile reinforcements can be made of aramid, polyester, polyamide, rayon, or hybrid cords made of these materials.

[0040] In order to achieve good adhesion to the reinforcements, it has proven advantageous if the amount of methylene acceptor in the rubber mixture is 1 to 4 phr.

[0041] The rubber compound can be used for rubberizing a wide variety of tire components, such as the bead core, bead caps, bead reinforcements, the belt, the carcass, or the belt bandages. It can also be used for other reinforcement-related compounds such as bead fillers, squeegees, belt edge pads, shoulder pads, tread underlays, or other body compounds. It is also possible to coat multiple components within a tire with the compound according to the invention. The pneumatic vehicle tires according to the invention are manufactured using processes known to those skilled in the art.

[0042] The rubber compound is preferably used as carcass and / or bandage rubber lining, where the good adhesion values ​​between the reinforcement and the rubber compound lead to a long service life of the pneumatic vehicle tire.

[0043] Alternatively or additionally, the rubber compound can also be used as a belt rubber compound, which in turn has a positive effect on the service life of the pneumatic vehicle tire.

[0044] The invention will now be explained in more detail using the following tables.

[0045] Tables 1 and 2 provide example compounds for various components of a pneumatic vehicle tire. Table 1 shows compounds for rubberizing textile reinforcements. Table 2 shows compounds for rubberizing steel cord. The compounds according to the invention are designated E, and the comparison compounds are designated V.

[0046] In the mixtures in the tables, resorcinol precondensate or resorcinol were replaced by triallyl cyanurate.

[0047] The mixture was prepared under standard conditions by producing a base mixture and then the final mixture in a laboratory tangential mixer.

[0048] Test specimens were produced from all compounds by optimal vulcanization under pressure at 160 °C and, using these test specimens, material properties typical for the rubber industry were determined using the test methods specified below. • Shore A hardness at room temperature according to DIN 53 505 • Rebound resilience at 70 °C according to DIN 53 512 • Tensile strength at room temperature according to DIN 53 504

[0049] Adhesion tests, so-called peel tests, were conducted on textile nylon reinforcements without aging using the compounds listed in Table 1, in accordance with ISO 36:2011 (E) and DIN 53 530, with evaluation according to DIN ISO 6133. For this purpose, nylon reinforcement cords (940x2 dtex, 80 epdm) treated with RFL-Dip were coated with the unvulcanized rubber compounds and subsequently vulcanized at 170 °C. The peeling force of the compound from the cords was then determined, and the coverage of the cords with the compound after peeling was visually assessed.

[0050] Furthermore, adhesion tests were conducted with the compounds from Table 2 to brass-coated steel cord (1+5 x 0.40 HAT) according to ASTM 2229 / D1871 without aging (embedment length in the rubber compound: 10 mm, withdrawal speed: 125 mm / min). The pull-out force and coverage were determined.

[0051] The measured values ​​for the aforementioned properties were referenced to mixtures 1(V) and 3(V). Their values ​​were set equal to 100%. Values ​​less than 100% reflect a decrease in the measured value compared to the reference value. Values ​​greater than 100% reflect an increase in the measured value compared to the reference value. Table 1 Components Unit 1(V) 2(E) Polyisoprene phr 80 80 Polybutadien phr 20 20 soot phr 55 55 Silica phr 7,5 7,5 Plasticizers, anti-aging agents phr 8 8 Vulcanization activators phr 7,5 7,5 Resorcin-Vorkondensat a) phr 1,6 - Triallyl cyanurate phr - 1,6 Hexamethoxymethylmelamine phr 1,2 1,2 accelerator phr 1,6 1,6 sulfur phr 3,4 3,4 Characteristics Hardness at RT % 100 97 Rebound load at 70 °C % 100 98 Tensile strength at RT % 100 95 Liability (unaged) % 100 108 Cover (unaged) % 100 93 a) Resorcinol-formaldehyde resin with a free resorcinol content of 8-18%.

[0052] In the inventive textile cord rubber coating shown in Table 1, improved adhesion is observed by replacing resorcinol precondensate with triallyl cyanurate. The other vulcanizate properties remain at a good level. The low amounts of resorcinol in the inventive compounds also contribute to improvements in occupational safety and environmental protection. Eliminating resorcinol also reduces contamination from deposits during compound production. Table 2 Components Unit 3(V) 4(E) Polyisoprene phr 80 80 Polybutadien phr 20 20 Silica phr 60 60 Plasticizer, anti-aging agent, silane coupling agent phr 22,8 22,8 Vulcanization activators phr 8,4 8,4 Resorcin phr 2,5 - Triallyl cyanurate phr - 2,5 Hexamethoxymethylmelamine phr 2,5 2,5 accelerator phr 1,5 1,5 sulfur phr 4,3 4,3 Characteristics Hardness at RT % 100 94 Rebound load at 70 °C % 100 104 Tensile strength at RT % 100 106 Liability (unaged) % 100 101 Cover (unaged) % 100 107

[0053] Table 2 shows that the adhesion to steel cord is also slightly improved when triallyl cyanurate is used, and some of the other vulcanizate properties are even improved. Here, too, the same advantages regarding occupational safety and environmental hazards arise from the lower resorcinol content in the compound as described above in Table 1.

Claims

[1] Sulphur-crosslinkable rubber mixture with a free resorcinol content of less than 0.1% by weight, containing at least one adhesive for the reinforcement-rubber adhesion, wherein the adhesive contains a methylene donor and at least one chemical compound which has a triazine structure and at least one rubber-crosslinkable group, wherein hexamethoxymethylmelamine (HMMM) and / or hexamethylenetetramine (HMT) is used as the methylene donor, characterized by that at least one group crosslinkable with rubber is an allyl group. [2] Sulphur-crosslinkable rubber mixture according to claim 1, characterized by that the chemical compound is selected from triallyl cyanurate, triallyl isocyanurate and / or trimethallyl isocyanurate. [3] A pneumatic vehicle tire comprising a sulfur-crosslinked rubber composition according to claim 1. [4] Pneumatic vehicle tyre according to claim 3, characterized bythat it has a carcass rubber lining and / or a tire rubber lining made of the rubber compound. [5] Pneumatic vehicle tyre according to claim 3 or 4, characterized by that it has a belt rubber coating made of the rubber compound.

Citation Information

Patent Citations

  • Rubber material for production of tubing, rubber-metal composites and other products contains rubber, 6-substituted 2,4-dimercapto-1,3,5-triazine and epoxide-containing polymer which is crosslinkable with the rubber

    DE10016120A1

  • Rubber compound with environmentally friendly plasticizer

    DE102008037714A1

  • Strengthening layer and vehicle tires

    DE102014211365A1

  • Oil-resistant rubber mixt. with good adhesion to brass - contg. acrylonitrile]-diene-olefin] copolymer rubber, tri:allyl isocyanurate], organic sulphur cpd. or sulphur donor, and organic peroxide