PIEZOELECTRIC COMPOSITION AND PIEZOELECTRIC DEVICE
A bismuth-barium-titanium oxide composition with a perovskite structure addresses the challenge of achieving high piezoelectric constant and stability, providing a lead-free solution with enhanced d33 and depolarization temperature for piezoelectric devices.
Patent Information
- Application Number
- DE102020100340
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-01-22
- Filing Date
- 2020-01-09
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2040-01-09
AI Technical Summary
Existing piezoelectric compositions face challenges in achieving a large piezoelectric constant (d33) while maintaining stability and high depolarization temperatures, leading to issues in practical applications due to lead contamination and performance degradation during manufacturing processes.
A piezoelectric composition comprising bismuth, barium, and titanium oxides with a perovskite structure, characterized by specific X-ray diffraction peaks and intensity ratios, which enhances the piezoelectric constant and depolarization temperature, and includes additives to improve electrical resistance and reduce leakage current.
The composition achieves a significantly large piezoelectric constant (d33) and high depolarization temperature, ensuring stable performance in piezoelectric devices, free from lead contamination and resistant to heating processes.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
TECHNICAL AREA
[0001] The present invention relates to a piezoelectric composition and a piezoelectric device. BACKGROUND
[0002] Most piezoelectric compositions currently in practical use are solid solutions (so-called PZT piezoelectric compositions) of lead zirconate (PbZrO3) and lead titanate (PbTiO3). PZT piezoelectric compositions contain a large amount of lead oxide (PbO) as their main component. Since lead oxide evaporates remarkably easily at low temperatures, a large portion of the lead oxide diffuses into the atmosphere during the manufacturing processes of piezoelectric compositions or piezoelectric devices that use them. Since lead is an environmental pollutant that harms the human body, lead-free piezoelectric compositions are required.
[0003] A typical piezoelectric composition without lead is bismuth ferrite (BiFeO3), which is described in the following non-patent literature 1. Bismuth ferrite (BFO) has a large spontaneous polarization. However, because the anisotropy of BFO is high and a large leakage current can be generated in BFO, BFO does not have sufficient piezoelectricity (e.g., piezoelectric constant d 33 ). Therefore, piezoelectric compositions with a larger d 33 as BFO is required. For example, in the following patent literature 1, a ternary compound (xBaTiO3-yBiFeO3-yBi(Mg 0,5 Ti 0,5 )O3) consisting of barium titanate, bismuth ferrite, and bismuth magnesia titanate. Furthermore, in the following patent literature 2, a binary compound (Ba 1-y Bi y ) a (Ti 1-x-z Zr x Fe z)O3) from barium zirconate titanate and bismuth ferrite. Another known compound of the type BaTiO3-BiFeO3 is disclosed in the aforementioned non-patent literature 2. Quotation list JP 2013- 191 751 A JP 2013- 191 751 A Non-patent literature 1 Zhenyong Cen et al., “Influence of sintering temperature on the microstructure and piezoelectric properties of Pb-free BiFeO3-BaTiO3 ceramics in the composition range of high BiFeO3 concentrations,” J Electroceram, 31, pp. 15-20, 2013 Non-Patent Literature 2 Yang, S.-C. et al., “Room-temperature magnetoelectric coupling in single-phase BaTiO3-BiFeO3 system,” Journal of Applied Physics 113, 144101 (2013). SUMMARY
[0004] A piezoelectric composition described in Patent Literature 1 is strongly deformed when a sufficiently large electric field is applied. However, the piezoelectric composition described in Patent Literature 1 has difficulty in maintaining a sufficiently large piezoelectric constant (d) after polarization treatment. 33). A piezoelectric composition described in Patent Literature 2 has a large piezoelectric constant. However, the Curie temperature and depolarization temperature of the piezoelectric composition described in Patent Literature 2 are very low. Consequently, in a manufacturing process of a piezoelectric device using the piezoelectric composition, the piezoelectricity of the piezoelectric composition is easily deteriorated by heating of the piezoelectric composition. For example, the piezoelectricity of the piezoelectric composition is deteriorated by heating during soldering. Therefore, the piezoelectric composition described in Patent Literature 2 cannot withstand practical application.A piezoelectric composition described in Non-Patent Literature 1 also has difficulty maintaining a sufficiently large piezoelectric constant after polarization treatment.
[0005] The present invention aims to provide a piezoelectric composition having a large piezoelectric constant and a piezoelectric device comprising the piezoelectric composition.
[0006] A piezoelectric composition according to one aspect of the present invention is a piezoelectric composition comprising an oxide having a perovskite structure, wherein the oxide contains bismuth, barium, iron, and titanium. An X-ray diffraction pattern of the piezoelectric composition after polarization treatment has a first peak and a second peak in the range of the diffraction angle θ of 38.6° or more and 39.6° or less; the diffraction angle θ of the first peak is smaller than the diffraction angle θ of the second peak; the intensity of the first peak is expressed as I L shown; the intensity of the second peak is shown as I H shown; and I H / I L is 0.00 or more and 2.00 or less. The scope of the invention is further limited according to claim 1.
[0007] At least part of the above oxide can be replaced by x[Bi m FeO3-y[Ba nTiO3]; x may be 0.6 or more and 0.8 or less; y may be 0.2 or more and 0.4 or less; x + y may be 1; m may be 0.96 or more and 1.06 or less; and n may be 0.96 or more and 1.06 or less.
[0008] m may be 1.02 or more and 1.05 or less; and n may be 1.02 or more and 1.05 or less.
[0009] At least part of the oxide may be a rhombohedral crystal.
[0010] A piezoelectric composition according to one aspect of the present invention may comprise a rhombohedral crystal of an oxide containing bismuth and iron.
[0011] A piezoelectric device according to one aspect of the present invention comprises the above piezoelectric composition. Composition includes, is provided.
[0012] According to the present invention, a piezoelectric composition having a large piezoelectric constant and a piezoelectric device comprising the piezoelectric composition are provided. The scope of the invention is defined by the claims. BRIEF DESCRIPTION OF THE DRAWINGS Fig. 1 is a perspective view of a unit cell of a perovskite structure of an oxide included in a piezoelectric composition according to an embodiment of the present invention; Fig. 2 is a perspective view of a rhombohedral crystal of an oxide included in the piezoelectric composition according to an embodiment of the present invention; Fig. Figure 3 is a perspective view of a unit cell forming the rhombohedral crystal as shown in Fig. 2 shown; Fig.4 is a schematic perspective view of a piezoelectric device according to an embodiment of the present invention; Fig. 5 is a temperature profile in a production process (sintering step) of the piezoelectric composition according to an embodiment of the present invention; and Fig. 6 is an X-ray diffraction pattern of a piezoelectric composition of Example C1 of the present invention and an X-ray diffraction pattern of a piezoelectric composition of Comparative Example 1. DETAILED DESCRIPTION
[0013] The preferred embodiments of the present invention will be described below with reference to the drawings. The present invention is not limited to the following embodiments.
[0014] A piezoelectric composition according to the present embodiment comprises an oxide containing bismuth (Bi), barium (Ba), iron (Fe), and titanium (Ti). For convenience of description, the oxide containing Bi, Ba, Fe, and Ti is represented as "BFO-BTO." The BFO-BTO has a perovskite structure. The BFO-BTO may contain at least one crystal selected from the group consisting of a rhombohedral crystal of the perovskite structure, a tetragonal crystal of the perovskite structure, and a cubic crystal of the perovskite structure. An example of a unit cell of the perovskite structure is shown in Fig. 1. The unit cell uc of the perovskite structure can consist of elements A positioned on A sites, an element B positioned on the B site, and oxygen (O). The elements A can be Bi or Ba. The element B can be Fe or Ti. An example of the rhombohedral crystal of BFO-BTO is shown in Fig.2. Unit cells uc, which form the rhombohedral crystal in Fig. 2, each correspond to a unit cell uc in Fig. 3. To simplify the drawing of the figure, the elements B and O are Fig. 3 omitted. a1, b1 and c1 in Fig. 1 and Fig. 2 are primitive vectors that form a cubic crystal or a tetragonal crystal. a2, b2 and c2 in Fig. 3 are primitive vectors that form a diamond-shaped crystal. The
[111] (crystal orientation) based on a1, b1, and c1 corresponds to the
[001] h based on a2, b2 and c2. As in Fig. 2, the rhombohedral crystal of the perovskite structure can exhibit an antiferromagnetic strain displacement like BiFeO3. As shown in Fig.As shown in Figure 2, the rhombohedral crystal can consist of two unit cells arranged periodically along the
[111] plane. The piezoelectric composition can exhibit spontaneous polarization. That is, the piezoelectric composition can be a pyroelectric material or a ferroelectric material.
[0015] The X-ray diffraction pattern of the piezoelectric composition after polarization treatment has a first peak and a second peak in the range of the diffraction angle 2θ of 38.6° or more and 39.6° or less. The polarization treatment means that the piezoelectric composition is polarized along an electric field by applying the electric field to the piezoelectric composition. The diffraction angle 2θ of the first peak is smaller than the diffraction angle 2θ of the second peak. For example, the diffraction angle 2θ of the first peak may be about 38.851°. For example, the diffraction angle 2θ of the second peak may be about 39.177°. The incident X-ray radiation to be used to measure the X-ray diffraction pattern may include a CuKα1 line. The intensity of the first peak is referred to as I L and the intensity of the second peak is shown as I H shown. I H / IL is 0.00 or more and 2.00 or less. The unit of I L and I H can be an arbitrary unit (au). The piezoelectric composition containing BFO-BTO and having an I H / I L of 0.00 or more and 2.00 or less, a large piezoelectric constant (d 33 ). The respective diffraction angles 2θ of the first peak and the second peak are not limited to the above values and may vary depending on the composition of the BFO-BTO.
[0016] The diffraction angle 2θ of the intensity of the first peak is approximately equal to the diffraction angle 2θ of the diffracted X-rays from the (006) planes of a rhombohedral crystal of bismuth ferrite (BFO). The diffraction angle 2θ of the intensity of the second peak is approximately equal to the diffraction angle 2θ of the diffracted X-rays from the (202) planes of the rhombohedral crystal of bismuth ferrite. Therefore, there is a possibility that some or all of the oxide (BFO-BTO) contained in the piezoelectric composition is the same rhombohedral crystal as bismuth ferrite. That is, there is a possibility that some or all of the oxide (BFO-BTO) contained in the piezoelectric composition has a bismuth ferrite-type perovskite structure. The corresponding relationship between the diffraction angle 2θ of the diffracted X-rays of bismuth ferrite and the crystal plane can be obtained, for example, using code No.194991 of the Inorganic Crystal Structure Database (ICSD). The orientation of spontaneous polarization in the rhombohedral crystal of bismuth ferrite is
[001] . h , and the normal direction of the (006) planes. That is, the more the (006) planes are aligned in one direction, the lighter the bismuth ferrite becomes along the
[001] h polarized. Likewise, the orientation of the spontaneous polarization in the rhombohedral crystal of BFO-BTO is also
[001] h , and the normal direction of the (006) planes. The higher the intensity I Lof the first peak, which corresponds to the diffracted X-rays of the (006) planes, the more the (006) planes point in the spontaneous polarization orientation and the more easily the piezoelectric composition is polarized. For example, if the thickness of the piezoelectric composition is uniform and the first peak is measured by an out-of-plane measurement (2θ / θ method) on the surface of the piezoelectric composition perpendicular to the thickness direction, the higher I L , the higher the parallelism of the (006) planes to the surface of the piezoelectric composition and the more easily the piezoelectric composition is polarized in its thickness direction (
[001] h ). On the other hand, the rhombohedral crystal of bismuth ferrite in
[101] hbarely polarized. This means that the rhombohedral crystal of bismuth ferrite is barely polarized in the normal direction of the (202) planes. Similarly, the rhombohedral crystal of BFO-BTO is also barely polarized in the normal direction of the (202) planes. Therefore, the higher the intensity I H of the second peak, which corresponds to the diffracted X-rays of the (202) planes, the greater the number of (202) planes that do not contribute to the spontaneous polarization, and the lower the polarization of the piezoelectric composition. For this reason, when the I L is relatively higher than the I H , the piezoelectric composition is easier to polarize and the piezoelectric constant (d 33 ) of the piezoelectric composition increases. Then the piezoelectric composition can have a sufficiently large piezoelectric constant if I H / I L0.00 or more and 2.00 or less. For the same reason, I H / I L preferably 0.00 or more and 1.50 or less, and preferably 0.00 or more and 1.00 or less. Since the piezoelectric composition easily has a sufficiently large piezoelectric constant, part or all of the oxide (BFO-BTO) may be the rhombohedral crystal.
[0017] The reason why the piezoelectric composition has a large piezoelectric constant (d 33 ) is not limited to the above mechanism.
[0018] At least part of the oxide (BFO-BTO) can be represented by chemical formula 1. Chemical formula 1 can be equal to chemical formula 2. x[Bi m FeO3]-y[Ba n TiO3] (1) (Bi xm Ba yn )(Fe x Ti y )O3 (2)
[0019] x + y is 1. x can be 0.6 or more and 0.9 or less, and preferably 0.6 or more and 0.8 or less. y can be 0.1 or more and 0.4 or less, and preferably 0.2 or more and 0.4 or less. m can be 0.93 or more and 1.07 or less, preferably 0.96 or more and 1.06 or less, and preferably 1.02 or more and 1.05 or less. n can be 0.93 or more and 1.07 or less, preferably 0.96 or more and 1.06 or less, and more preferably 1.02 or more and 1.05 or less. Chemical formula 1 indicates that the composition of the oxide contained in the piezoelectric composition is represented by the sum of two phases: a rhombohedral crystal of bismuth ferrite (BFO) and a tetragonal crystal of barium titanate (BTO). The composition in which these two phases easily coexist exhibits morphotropic phase boundaries (MPB).Consequently, polarization rotation is easily caused in the piezoelectric composition, and the piezoelectric composition easily exhibits a large piezoelectric constant (i.e., 33 ). Furthermore, when the oxide contained in the piezoelectric composition is represented by the chemical formula 1, the piezoelectric composition easily has a high depolarization temperature.
[0020] Since a heterophase without piezoelectricity is hardly formed in the piezoelectric composition when m and n are within the above ranges, the piezoelectric constant easily increases. Especially in cases where m is 1.02 or more and 1.05 or less and n is 1.02 or more and 1.05 or less, deficiencies of Bi and Ba at A sites of the perovskite structure hardly appear, and the crystallinity of the perovskite structure is improved. Deficiencies of Bi and Ba inhibit the movement of domains. By avoiding deficiencies of Bi and Ba, the crystallinity of the perovskite structure is improved and domain pinning is suppressed. The domains in the piezoelectric composition can then be easily rotated. As a result, the piezoelectric constant easily increases.
[0021] The piezoelectric composition may only consist of an oxide consisting of Bi, Fe, Ba, Ti and O. Part of the piezoelectric composition may contain a phase consisting of Bi m FeO3. Since the piezoelectric composition easily has a sufficiently large piezoelectric constant (d 33 ), the piezoelectric composition may contain a rhombohedral crystal of the oxide containing bismuth and iron. For example, part of the piezoelectric composition may also be a rhombohedral crystal of Bi m FeO3. Part of the piezoelectric composition may also include a phase of Ba nTiO3. The piezoelectric composition may contain elements other than Bi, Fe, Ba, Ti, and O as additives or impurities. For example, the piezoelectric composition may further contain at least one element selected from the group consisting of silver (Ag), vanadium (V), niobium (Nb), tantalum (Ta), molybdenum (Mo), tungsten (W), and manganese (Mn). By incorporating these elements into the piezoelectric composition, the electrical resistance (ρ) of the piezoelectric composition is easily increased and the leakage current in the piezoelectric composition is suppressed. Therefore, a high voltage can be easily applied to the piezoelectric composition; the piezoelectric composition can be easily polarized sufficiently; and the piezoelectric composition easily has a large piezoelectric constant.The piezoelectric composition may contain, as additives or impurities, at least one selected from the group consisting of sodium (Na), potassium (K), magnesium (Mg), aluminum (Al), sulfur (S), zirconium (Zr), silicon (Si), phosphorus (P), copper (Cu), zinc (Zn), and hafnium (Hf). The piezoelectric composition according to the present embodiment may not contain Pb. However, the piezoelectric composition containing Pb is not necessarily excluded from the technical scope of the present embodiment.
[0022] The average composition of the entire piezoelectric composition can be analyzed using, for example, an X-ray fluorescence (XRF) analysis method or inductively coupled plasma (ICP) atomic emission spectroscopy. The structure of the piezoelectric composition can be specified using an X-ray diffraction (XRD) method.
[0023] The d 33The thermal conductivity of the piezoelectric composition after polarization treatment can be, for example, 102 pC / N or more and 250 pC / N or less. The depolarization temperature of the piezoelectric composition can be, for example, 200°C or more and 643°C or less.
[0024] As in Fig.4, a piezoelectric device 10 includes a substrate 2, a first electrode 4 stacked on the surface of the substrate 2, a piezoelectric body 6 stacked on the surface of the first electrode 4, and a second electrode 8 stacked on the surface of the piezoelectric body 6. The piezoelectric body 6 contains the above piezoelectric composition according to the present embodiment. The piezoelectric body 6 may be a sintered body of the piezoelectric composition. The piezoelectric body 6 may contain other components besides the piezoelectric composition. Although the Fig.4 is a thin rectangular cuboid, the shape and dimensions of the piezoelectric body 6 are not limited. The substrate 2 may be made of, for example, a metal, a semiconductor, a resin, or a ceramic. The compositions of the first electrode 4 and the second electrode 8 are not limited as long as they have electrical conductivity. The first electrode 4 and the second electrode 8 may each be a simple substance made of a metal or an alloy. The first electrode 4 and the second electrode 8 may each also be a metal oxide with electrical conductivity. The structure of the piezoelectric device 10 according to the present embodiment is not limited to the structure shown in Fig. 4 shown structure.
[0025] The applications of the piezoelectric device according to the present embodiment are diverse. The piezoelectric device can be, for example, a piezoelectric microphone, a sonar, an ultrasonic detector, a ceramic filter, a piezoelectric transformer, a harvester, a piezoelectric buzzer, an ultrasonic motor, an oscillator, a resonator, or an acoustic multilayer film. The piezoelectric device can be, for example, a piezoelectric actuator. The piezoelectric actuator can be used for haptics. That is, the piezoelectric actuator can be used for various devices that require feedback based on the sense of touch. The devices that require feedback based on the sense of touch can be, for example, wearable devices, touchpads, displays, or game controllers.The piezoelectric actuator can be used for head assemblies, head stack assemblies, or hard disks. The piezoelectric actuator can be used for printheads or inkjet printers. The piezoelectric actuator can be used for piezoelectric switches. The piezoelectric device can be, for example, a piezoelectric sensor. The piezoelectric sensor can be used for gyro sensors, pressure sensors, AE (acoustic emission) sensors, pulse wave sensors, ultrasonic sensors, acceleration sensors, or shock sensors. The respective piezoelectric device can be part or the whole of a microelectromechanical system (MEMS).
[0026] The piezoelectric composition according to the present embodiment can be manufactured by the following manufacturing method.
[0027] In the production of the piezoelectric composition, a raw material powder (raw material particles) is prepared from starting materials. Pressing the raw material particles produces a green compact. A sintered body is obtained by sintering the green compact. A piezoelectric body is obtained by subjecting the sintered body to a polarization treatment. The piezoelectric composition according to the present embodiment includes both the sintered body before the polarization treatment and the sintered body after the polarization treatment. The details of each step are described below.
[0028] In a granulation step, the starting materials for the piezoelectric composition are weighed. A variety of different starting materials can be used. The starting materials include Bi, Fe, Ba, and Ti. Each starting material can be a simple substance (metal) or a compound of the respective element. The compound can be, for example, an oxide, a carbonate salt, a hydroxide, an oxalate salt, a nitrate salt, or the like. Each starting material can be a solid (e.g., a powder). By weighing each starting material, the molar ratios of Bi, Fe, Ba, and Ti in the entire starting material can be adjusted to the molar ratios of Bi, Fe, Ba, and Ti in the chemical formula 1.
[0029] A bismuth compound can be bismuth oxide (Bi2O3), bismuth nitrate (Bi(NO3)3), or the like. An iron compound can be iron oxide (Fe2O3), ferric chloride (FeCl3), ferric nitrate (Fe(NO3)3), or the like. A barium compound can be barium oxide (BaO), barium carbonate (BaCO3), barium oxalate (BaC2O4), barium acetate (CH3COO)2Ba), barium nitrate (Ba(NO3)2), barium sulfate (BaSO4), barium titanate (BaTiO3), or the like. A titanium compound can be titanium oxide (TiO2) or the like.
[0030] In the granulation step, raw material particles are produced from the above-mentioned starting materials. A wide variety of raw material particles with different compositions can be produced. A manufacturing process for the raw material particles might be as follows, for example.
[0031] A slurry can be prepared by mixing the starting materials and a solvent. The starting materials in the slurry can be pulverized by wet mixing the slurry with a ball mill or the like. The solvent to be used for preparing the slurry can be, for example, water. The solvent can also be an alcohol such as ethanol. The solvent can be a mixture of water and ethanol. The starting materials after wet mixing can be dried by a spray dryer or the like.
[0032] By molding the mixture of pulverized raw materials, a temporary green compact is formed. A temporarily sintered body is obtained by heating (calcining) the temporary green compact in an oxidative atmosphere. The oxidative atmosphere can be, for example, air. The calcination temperature can be 700°C or more and 1050°C or less. The calcination time can be about 1 to 3 hours. Raw material particles are obtained by pulverizing the temporarily sintered body. A slurry can be prepared by mixing the raw material particles and a solvent. The raw material particles in the slurry can be pulverized by wet mixing the slurry with a ball mill or the like. The average primary particle diameter of the raw material particles can be adjusted in the wet mixing.The average primary particle diameter of the raw material particles can be, for example, 0.01 μm or more and 20 μm or less. The raw material particles after wet mixing can be dried by a spray dryer or the like.
[0033] A green compact is obtained by pressing a mixture of the raw material particles and a binder. The binder can be an organic binder such as polyvinyl alcohol or ethylcellulose. A dispersant can be added to the binder.
[0034] In a sintering step, a sintered body is obtained by sintering the green compact in an oxidative atmosphere. Before sintering, a debinding treatment can be performed on the green compact. This means that the binder in the green compact can be decomposed by heating the green compact. The debinding treatment and sintering can be carried out continuously. The debinding treatment and sintering can be carried out separately.
[0035] As in Fig.5, in the sintering step, it is preferable that the green compact is heated in two stages. That is, it is preferable that the sintering step includes a first sintering process and a second sintering process after the first sintering process. It is preferable that the green compact is heated to a first sintering temperature in the first sintering process; it is preferable that the green compact is heated to a second sintering temperature in the second sintering process; and that the first sintering temperature is higher than the second sintering temperature. By heating the green compact in the two stages of the sintering step, the piezoelectric composition with a large piezoelectric constant (d 33) and a high depolarization temperature are easily achieved. It is preferable that the temperature rise rate of the first sintering process is 15°C / min or more and 1000°C / min or less. The temperature rise rate of the first sintering process is a temperature rise rate at which the temperature of the green compact is raised from room temperature to the first sintering temperature in the first sintering process. It is preferable that the first sintering temperature is 1100°C or more and 1300°C or less. It is preferable that the second sintering temperature is 900°C or more and 1000°C or less. In the case where the temperature rise rate of the first sintering process and the first sintering temperature and the second sintering temperature are within the above ranges, the piezoelectric composition having a large piezoelectric constant and a high depolarization temperature is easy to obtain.For example, the time of the first sintering process can be 0.5 hours or more and 2 hours or less. The time of the second sintering process can be 2 hours or more and 32 hours or less. After the sintering step, the sintered body can be annealed at a temperature lower than that of the second sintering process.
[0036] Prior to a polarization treatment described later, a thin plate can be formed from the sintered body by cutting the sintered body. The surface of the thin plate of the sintered body can be subjected to lap polishing. A cutting machine such as a milling cutter, dicing saw, or other cutting machine can be used to cut the sintered body. After lap polishing, a temporary electrode for the polarization treatment is formed on each of the two opposite surfaces of the sintered body. The temporary electrodes can be formed by a vacuum deposition method or sputtering. The temporary electrodes can be easily removed by etching with a ferric chloride solution or the like.
[0037] During the polarization treatment, a polarizing electric field is applied between a pair of temporary electrodes that sandwich the sintered body. During the polarization treatment, the sintered body may be heated. The temperature of the sintered body during the polarization treatment can be between 80°C and 300°C. The application time of the polarizing electric field can be between 1 minute and 30 minutes. The polarizing electric field must not be less than 0.9 times the coercive field of the sintered body.
[0038] After the polarization treatment, the temporary electrodes are removed from the sintered body. A piezoelectric composite (piezoelectric body) with a desired shape can be formed by processing the sintered body.
[0039] While preferred embodiments of the present invention have been described so far, the present invention is not limited to the above-mentioned embodiments. For example, the piezoelectric composition according to the present invention may be a piezoelectric thin film. EXAMPLES
[0040] The present invention will be described in detail below using examples and comparative examples. However, the present invention is not limited to the following examples. (Example A1)
[0041] Bi2O3 powder, Fe2O3 powder, BaCO3 powder, and TiO2 powder were used as starting materials. The BaCO3, TiO2, Bi2O3, and Fe2O3 were weighed so that the molar ratios of Bi, Fe, Ba, and Ti in all the starting materials matched the molar ratios of Bi, Fe, Ba, and Ti in the following Chemical Formula 1. In the case of Example A1, the values of x, y, m, and n in the Chemical Formula 1 were shown in Table 1 below. x[Bi m FeO3]-y[Ba n TiO3] (1)
[0042] All raw materials and pure water were mixed in a ball mill for 10 hours. The raw materials were dried after mixing, and then pressed to obtain a temporary green compact. The temporary green compact was heated to 800°C to obtain a temporary sintered body. The temporarily sintered body was pulverized by a ball mill. The pulverized, temporarily sintered body was dried to obtain raw material particles. A mixture of the raw material particles and a binder (polyvinyl alcohol) was compression-molded to obtain a green compact. The binder was removed by heating the green compact.
[0043] After the debinding treatment, a sintered body was obtained by the following sintering step.
[0044] As a sintering step, a first sintering process and a second sintering process were carried out after the first sintering process. In the first sintering process, the temperature of the green body was increased from room temperature to a first sintering temperature at a temperature increase rate V T In the first sintering process, the green body was heated in the air to the first sintering temperature T S1 The time of the first sintering process was 1 hour. In the second sintering process, the green compact was heated to a second sintering temperature T S2 heated. The time of the second sintering process was 10 hours. The temperature rise rate V T , the first sintering temperature T S1 and the second sintering temperature T S2 of Example A1 are shown in Table 1 below.
[0045] The sintered body was machined into a sintered body plate using a double-sided lapping machine and a cut-off saw. The dimensions of the sintered body after machining were 16 mm long x 16 mm wide x 0.5 mm thick.
[0046] Ag electrodes were formed on both surfaces of the sintered body using a vacuum deposition system. The thickness of each electrode was 1.5 µm. The dimensions of each electrode were 15 mm × 15 mm.
[0047] An electric field was applied to the sintered body, which was placed between the pair of electrodes, to polarize the sintered body. The intensity of the electric field applied to the sintered body was 1.5 to 2 times the coercive field. The electric field was applied to the sintered body for 15 minutes. The above-mentioned polarization treatment was carried out in a silicone oil bath at a temperature of 120°C.
[0048] Using the above method, a piezoelectric composition of Example A1 was obtained. As a result of analysis based on an X-ray fluorescence analysis method, the molar ratios of Bi, Fe, Ba, and Ti in the piezoelectric composition were consistent with the molar ratios of Bi, Fe, Ba, and Ti in Chemical Formula 1. That is, the values of x, y, m, and n in Chemical Formula 1 were as shown in Table 1 below.
[0049] An X-ray diffraction pattern was measured by an out-of-plane measurement (2θ / θ method) on the surface of the piezoelectric composite after polarization treatment. Cu was used as the X-ray source in the X-ray diffraction measurement. A characteristic Cu X-ray beam was applied to the surface of the piezoelectric composite. The surface of the piezoelectric composite where the X-ray diffraction pattern was measured was perpendicular to the polarization direction. The polarization direction is the direction of a direct current electric field in the polarization treatment. By software processing the measured X-ray diffraction pattern, bands of diffracted X-rays of a CuKα2 line were removed from the X-ray diffraction pattern. That is, an X-ray diffraction pattern originating from a CuKα1 line was extracted from the measured X-ray diffraction pattern.The wavelength of the CuKα1 line is 1.540593 Å. The X-ray diffraction pattern described below is an X-ray diffraction pattern derived from the CuKα1 line. The X-ray diffraction pattern confirmed that the piezoelectric composition has a perovskite structure. The X-ray diffraction pattern had a first peak and a second peak in the range of diffraction angle 2θ of 38.6° or more and 39.6° or less. The diffraction angle 2θ of the first peak was smaller than the diffraction angle 2θ of the second peak. The diffraction angle 2θ of the intensity of the first peak was about 38.909°. The diffraction angle 2θ of the intensity of the second peak was about 39.367°. I. H / I L was derived from intensity I L of the first peak and the intensity I H of the second peak. The I H / I L of Example A1 is shown in the following Table 1.
[0050] The piezoelectric constant d 33 (Unit: pC / N) of the piezoelectric composition after polarization treatment was measured with a d 33 -meters. The d 33 -Meter is a device for measuring d 33 according to the Berlincourt method according to JIS (Japanese Industrial Standards) R1696. In the Berlincourt method, the 33 by utilizing the direct piezoelectric effect when a vibration is applied to a piezoelectric composition. Therefore, in the Berlincourt method, in contrast to a measurement method that uses the inverse piezoelectric effect, when an electric field is applied to a piezoelectric composition, there is no influence of electrostriction, and an intrinsic d 33 of the piezoelectric composition. The d 33 of Example A1 is shown in the following Table 1.
[0051] A piezoelectric device was fabricated by forming electrodes on both surfaces of the piezoelectric composition after polarization treatment. The entire piezoelectric device was placed in a thermostatic chamber. The depolarization temperature T d (Unit: °C) of the piezoelectric composition was determined by continuously measuring the piezoelectric constant (d 33 ) of the piezoelectric composition was determined while the temperature of the piezoelectric device in the thermostat chamber was raised starting at room temperature. The depolarization temperature T d is the temperature of the piezoelectric composition when the d 33 of the piezoelectric composition is 0. For the measurement of the d 33 An impedance analyzer was used. The T d of Example A1 is shown in the following Table 1.
[0052] (Examples A2 to A10, B1 to B15, C1 to C15, D1 to D15 and E1 to E11 as well as comparative examples 1 to 5).
[0053] In the case of Examples A2 to A10, B1 to B15, C1 to C15, D1 to D15 and E1 to E11 as well as Comparative Examples 1 to 5, x, y, m and n were adjusted to the values given in Tables 1 to 5 below by weighing the starting materials.
[0054] In the case of Examples A2 to A10, B1 to B15, C1 to C15, D1 to D15 and E1 to E11 and Comparative Examples 1 to 5, the temperature rise rate V T , the first sintering temperature T S1 and the second sintering temperature T S2 shown in the following tables 1 to 5.
[0055] The respective piezoelectric compositions of the above examples and comparative examples were prepared using the same method as in Example A1, except for the above points. Analysis and measurements were performed using the same method as in Example A1 on the respective piezoelectric compositions of the above examples and comparative examples.
[0056] In each of Examples A2 to A10, B1 to B15, C1 to C15, D1 to D15, and E1 to E11 and Comparative Examples 1 to 5, the molar ratios of Bi, Fe, Ba, and Ti of the piezoelectric composition were consistent with the molar ratios of Bi, Fe, Ba, and Ti in Chemical Formula 1. The values of x, y, m, and n in Chemical Formula 1 were consistent with the values shown in Tables 1 to 5 below.
[0057] In each of Examples A2 to A10, B1 to B15, C1 to C15, D1 to D15, and E1 to E11, and Comparative Examples 1 to 5, it was confirmed that the piezoelectric composition has a perovskite structure. In all Examples and Comparative Examples except Comparative Example 1, the X-ray diffraction pattern had a first peak and a second peak in the range of the diffraction angle 2θ of 38.6° or more and 39.6° or less, with the diffraction angle 2θ of the first peak being smaller than the diffraction angle 2θ of the second peak. The corresponding I H / I L Examples and Comparative Examples except Comparative Example 1 are shown in the following Tables 1 to 5. The X-ray diffraction patterns of Example C1 and Comparative Example 1 are shown in Fig. 6. As shown in Fig. 6, the X-ray diffraction pattern of Comparative Example 1 had no first peak. That is, the I Lof comparative example 1 was zero. Therefore, it was impossible to H / I L of comparative example 1.
[0058] In the cases of Examples A2 to A10, B1 to B15, C1 to C15, D1 to D15 and E1 to E11 as well as Comparative Examples 1 to 5, the 33 and T d Values listed in Tables 1 to 5 below. d 33 should be 100 pC / N or more. Preferably, the 33 200 pC / N or more. T d should be 260°C or more. Preferably, T d 300°C or more.
[0061] Table 1] Table 1 I H / I L x y m n V T (°C / min) T S1 (°C) T S2 (°C) d 33 (pC / N) T d (°C) Comparison example 1 - 0,9 0,1 1,00 1,00 5 850 850 15 651 Comparison example 2 7,60 0,8 0,2 1,00 1,00 5 900 900 43 581 Comparison example 3 3,80 0,7 0,3 1,00 1,00 5 1000 1000 80 450 Comparison example 4 3,00 0,6 0,4 1,00 1,00 5 1100 1100 62 363 Comparison example 5 2,50 0,5 0,5 1,00 1,00 5 1150 1150 20 281 Example A1 1,52 0,9 0,1 0,93 1,00 300 1100 900 102 623 Example A2 1,43 0,9 0,1 0,94 1,00 300 1100 900 103 643 Example A3 1,38 0,9 0,1 1,00 1,00 300 1100 900 105 632 Example A4 1,27 0,9 0,1 1,02 1,02 300 1100 900 111 612 Example A5 1,33 0,9 0,1 1,06 1,00 300 1100 900 110 611 Example A6 1,38 0,9 0,1 1,07 1,00 300 1100 900 108 631 Example A7 1,49 0,9 0,1 1,00 0,93 300 1100 900 107 612 Example A8 1,46 0,9 0,1 1,00 0,94 300 1100 900 102 633 Example A9 1,38 0,9 0,1 1,00 1,06 300 1100 900 106 624 Example A10 1,41 0,9 0,1 1,00 1,07 300 1100 900 104 619
[0062] Table 2] Table 2 I H / I L x y m n V T (°C / min) T S1 (°C) T S2 (°C) d 33 (pC / N) T d (°C) Example B1 1,33 0,8 0,2 0,93 1,00 300 1150 950 150 571 Example B2 1,28 0,8 0,2 0,94 1,00 300 1150 950 160 568 Example B3 1,14 0,8 0,2 1,00 1,00 300 1150 950 152 558 Example B4 1,13 0,8 0,2 1,06 1,00 300 1150 950 160 551 Example B5 1,23 0,8 0,2 1,07 1,00 300 1150 950 164 557 Example B6 1,28 0,8 0,2 1,00 0,93 300 1150 950 155 558 Example B7 1,27 0,8 0,2 1,00 0,94 300 1150 950 162 546 Example B8 1,12 0,8 0,2 1,00 1,06 300 1150 950 158 546 Example B9 1,23 0,8 0,2 1,00 1,07 300 1150 950 163 541 Example B10 1,11 0,8 0,2 1,02 1,02 300 1150 950 166 561 Example B11 1,10 0,8 0,2 1,04 1,04 15 1100 1000 165 571 Example B12 1,06 0,8 0,2 1,04 1,04 15 1100 900 201 569 Example B13 1,05 0,8 0,2 1,04 1,04 300 1200 950 203 567 Example B14 1,06 0,8 0,2 1,04 1,04 1000 1300 1000 202 571 Example B15 1,12 0,8 0,2 1,05 1,05 300 1200 950 167 539
[0063] Table 3] Table 3 I H / I L x y m n V T (°C / min) T S1 (°C) T S2 (°C) d 33 (pC / N) T d (°C) Example C1 0,76 0,7 0,3 0,93 1,00 300 1200 950 170 437 Example C2 0,72 0,7 0,3 0,94 1,00 300 1200 950 169 436 Example C3 0,73 0,7 0,3 1,00 1,00 300 1200 950 195 441 Example C4 0,72 0,7 0,3 1,06 1,00 300 1200 950 197 428 Example C5 0,72 0,7 0,3 1,07 1,00 300 1200 950 178 437 Example C6 0,71 0,7 0,3 1,00 0,93 300 1200 950 163 429 Example C7 0,68 0,7 0,3 1,00 0,94 300 1200 950 180 419 Example C8 0,67 0,7 0,3 1,00 1,06 300 1200 950 194 423 Example C9 0,64 0,7 0,3 1,00 1,07 300 1200 950 185 433 Example C10 0,67 0,7 0,3 1,02 1,02 300 1200 950 216 426 Example C11 0,67 0,7 0,3 1,04 1,04 15 1100 1000 220 427 Example C12 0,53 0,7 0,3 1,04 1,04 15 1100 900 245 431 Example C13 0,49 0,7 0,3 1,04 1,04 300 1200 950 250 433 Example C14 0,49 0,7 0,3 1,04 1,04 1000 1300 1000 248 429 Example C15 0,55 0,7 0,3 1,05 1,05 300 1200 950 218 419
[0064] Table 4] Table 4 I H / I L x y m n V T (°C / min) T S1 (°C) T S2 (°C) d 33 (pC / N) T d (°C) Example D1 1,14 0,6 0,4 0,93 1,00 300 1250 950 182 354 Example D2 1,12 0,6 0,4 0,94 1,00 300 1250 950 191 347 Example D3 1,11 0,6 0,4 1,00 1,00 300 1250 950 188 341 Example D4 1,11 0,6 0,4 1,06 1,00 300 1250 950 161 339 Example D5 1,10 0,6 0,4 1,07 1,00 300 1250 950 166 335 Example D6 1,15 0,6 0,4 1,00 0,93 300 1250 950 183 327 Example D7 1,13 0,6 0,4 1,00 0,94 300 1250 950 191 354 Example D8 1,12 0,6 0,4 1,00 1,06 300 1250 950 165 344 Example D9 1,09 0,6 0,4 1,00 1,07 300 1250 950 171 329 Example D10 1,06 0,6 0,4 1,02 1,02 300 1250 950 193 347 Example D11 1,06 0,6 0,4 1,04 1,04 15 1100 1000 200 346 Example D12 1,05 0,6 0,4 1,04 1,04 15 1100 900 231 348 Example D13 1,05 0,6 0,4 1,04 1,04 300 1200 950 241 342 Example D14 1,05 0,6 0,4 1,04 1,04 1000 1300 1000 239 345 Example D15 1,06 0,6 0,4 1,05 1,05 300 1200 1100 198 351
[0065] Table 5] Table 5 I H / I L x y m n V T (°C / min) T S1 (°C) T S2 (°C) d 33 (pC / N) T d (°C) Example E1 1,26 0,5 0,5 0,93 1,00 300 1300 1000 150 260 Example E2 1,23 0,5 0,5 0,94 1,00 300 1300 1000 163 267 Example E3 1,17 0,5 0,5 1,00 1,00 300 1300 1000 168 265 Example E4 1,10 0,5 0,5 1,02 1,02 300 1300 1000 155 271 Example E5 1,12 0,5 0,5 1,06 1,00 300 1300 1000 162 268 Example E6 1,13 0,5 0,5 1,07 1,00 300 1300 1000 166 264 Example E7 1,18 0,5 0,5 1,00 0,93 300 1300 1000 159 264 Example E8 1,16 0,5 0,5 1,00 0,94 300 1300 1000 159 264 Example E9 1,15 0,5 0,5 1,00 1,06 300 1300 1000 155 271 Example E10 1,14 0,5 0,5 1,00 1,07 300 1300 1000 162 273 Example E11 0,10 0,4 0,6 1,00 1,00 300 1300 1000 170 200
[0066] [Industrial Applicability]
[0059] The piezoelectric composition according to the present invention is used, for example, for a piezoelectric actuator.
[0067] [Reference character list] 2 SUBSTRATE, 4 FIRST ELECTRODE, 6 PIEZOELECTRIC BODY (PIEZOELECTRIC COMPOSITION), 8 SECOND ELECTRODE, uc UNIT CELL OF THE PEROVSKITE STRUCTURE.
Claims
[1] Piezoelectric composition comprising an oxide having a perovskite structure, the oxide contains bismuth, barium, iron and titanium, an X-ray diffraction pattern of the piezoelectric composition after a polarization treatment has a first peak and a second peak in the range of a diffraction angle 2θ of 38.6° or more and 39.6° or less, the diffraction angle 2θ of the first peak is smaller than the diffraction angle 2θ of the second peak, an intensity of the first peak as I L is shown, an intensity of the second peak as I H is shown and I H / I L 0.10 or more and 1.52 or less. [2] The piezoelectric composition according to claim 1, wherein at least part of the oxide is represented by x[Bi m FeO3]-y[Ba n TiO3]; x is 0.6 or more and 0.8 or less; y is 0.2 or more and 0.4 or less; x + y is 1; m is 0.96 or more and 1.06 or less and n is 0.96 or more and 1.06 or less. [3] The piezoelectric composition according to claim 2, wherein m is 1.02 or more and 1.05 or less, and n is 1.02 or more and 1.05 or less. [4] The piezoelectric composition according to any one of claims 1 to 3, wherein at least a part of the oxide is a rhombohedral crystal. [5] The piezoelectric composition according to any one of claims 1 to 4, comprising a rhombohedral crystal of an oxide containing bismuth and iron. [6] The piezoelectric composition according to any one of claims 1 to 5, wherein a piezoelectric constant d 33 the piezoelectric composition is 150 pC / N or more. [7] A piezoelectric device (10) comprising: a substrate (2), a first electrode (4) stacked on a surface of the substrate, a piezoelectric body (6) stacked on a surface of the first electrode, and a second electrode (8), which is stacked on a surface of the piezoelectric body, wherein the piezoelectric body contains the piezoelectric composition according to any one of claims 1 to 6.
Citation Information
Patent Citations
Piezoelectric material, piezoelectric device, liquid discharging head, ultrasonic motor and dust removal apparatus
JP2013191751A