Method for machining a metal tube
Conductive heating and press hardening of metal pipes address the challenge of producing tailored tempered parts by enabling rapid, targeted heating and cooling to achieve desired material properties with reduced energy and equipment, suitable for automotive applications.
Patent Information
- Application Number
- DE102020100461
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-01-10
- Publication Date
- 2024-11-28
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
There is a need for improved methods to process metal pipes with varying hardness properties across the component, particularly in the automotive industry, as existing technologies struggle to efficiently achieve tailored tempered parts using conventional heating methods.
A method involving conductive heating of specific areas of a metal pipe, followed by press hardening, allows for rapid and targeted heating and cooling to create sharply defined zones with varying material structures, using electrodes to control the heating and cooling process.
Enables the production of metal pipes with sharply defined high-strength and ductile areas, achieving desired material properties like tensile strength over 1,500 MPa and elongations of >5%, while reducing energy input and equipment requirements.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[0001] The invention relates to a method for processing a metal pipe by press hardening at least one region of the metal pipe.
[0002] There is a high demand for hot-form-hardened components, for example, in the automotive industry. There is a particular need for hot-form-hardened components whose hardness properties vary across the component (so-called tailored tempered parts). While various approaches already exist for components manufactured from flat sheet metal, there is still room for improvement in the provision of hot-form-hardened tubular profiles. EP 2 446 977 A1 discloses a hot-form hardening process for tubular profiles. US 2017 / 0 043 642 A1 discloses a heat treatment process for a hollow stabilizer. DE 102 07 132 A1 discloses a method for reinforcing a workpiece in at least one partial area.
[0003] The invention is based on the object of providing improved possibilities for processing a metal pipe by press hardening.
[0004] This object is achieved by a method according to claim 1. This comprises processing a metal tube by press hardening at least one region of the metal tube, comprising the steps: a) Providing the metal pipe, b) conductive heating of at least one area of the metal tube, c) Press hardening of the area of the metal tube heated by conductive heating.
[0005] It is advantageous that conductive heating technology is used to heat at least one region of the metal tube, which offers a number of advantages over conventional processes. For example, compared to furnace heating of the metal tube, the processing can be accelerated and carried out with significantly less energy. Furthermore, a more targeted, segmented heat input can be achieved in individual regions of the metal tube, allowing the creation of sharply defined conductively heated regions, which can then be specifically and sharply defined and given the desired properties through press hardening. In this way, metal tubes can be produced with strength properties that vary greatly in certain sections as required, for example, with high-strength and adjacent ductile regions.
[0006] In addition, the equipment required for conductive heating is comparatively low compared to other heating processes, such as furnace heating.
[0007] In the method according to the invention, the step of heating the at least one region of the metal tube can advantageously be carried out exclusively by conductive heating or by a combination of conductive heating and another heat supply method. The conductive heating of the at least one region of the metal tube can be carried out by conductively heating the region by means of an electric current passed through this region by means of electrodes that electrically contact this region, i.e., by resistance heating. Compared to other types of heating, conductive heating has the advantage that it can be carried out very quickly, for example, within a period of 0.5 to 5 seconds.This in turn has the advantage that due to this rapid heating, only a low heat conduction occurs between different areas of the metal pipe, which is also advantageous for sharply defined press-hardened areas of the metal pipe.
[0008] According to an advantageous embodiment of the invention, it is therefore provided that, during press hardening, sharply defined zones of different material structures are created on the metal tube. According to an advantageous embodiment of the invention, the conductive heating of at least one region of the metal tube is carried out within a period of less than 10 seconds.
[0009] Press hardening, also known as hot forming, is a process for hot forming sheet metal, used in industries such as automotive. During press hardening, a sheet metal blank is heated to an initial press hardening temperature, also known as the AC3 temperature, and then cooled in a defined manner during the forming process, which is carried out by pressing. For this purpose, a hot forming tool is used in which the sheet metal blank is simultaneously formed and cooled, and thus hardened, so that the desired, usually three-dimensional press-hardened sheet metal component is created. The sheet metal blank is usually a flat, level sheet metal component, which can be cut out of a steel coil, for example. In the process according to the invention, a previously manufactured metal tube is used as the sheet metal blank.
[0010] During press hardening, targeted cooling, e.g., via cooled press tools, creates a martensitic microstructure, which leads to the desired material properties, such as tensile strength above 1,500 MPa and elongations in the range of >5%. The aforementioned tensile strengths are often only necessary in certain areas of the sheet metal component; in some cases, it is desirable to achieve higher elongations in other areas.
[0011] The temperature gradient can, in particular, be the cooling temperature gradient assigned to a press hardening process for the respective metal material of the metal pipe. If press hardening of the area of the metal pipe heated by conductive heating is to be carried out, the conductive heating is carried out to an initial temperature suitable for such a press hardening process. If heat treatment of the area is to be carried out, the conductive heating can be carried out to an intermediate temperature below the press hardening initial temperature, for example if an area of the metal pipe not processed by press hardening is to be heat treated. Heating to the press hardening initial temperature can also initially be carried out by means of conductive heating, in which case, during the heat treatment, which is intended, for example, to increase the ductility of the area, the cooling is carried out with a lower temperature gradient than during the press hardening process.In this way, a transformation into a martensitic structure is avoided.
[0012] For example, if such a heat treatment has produced an area of the metal tube with increased ductility, this area can be reshaped after the heat treatment step, for example by cold forming.
[0013] In the present invention, the press hardening process can be applied to any metal material of the metal pipe. In particular, press hardening is not limited to steel materials, but can also be applied to other metal materials, such as aluminum. Heat treatment is generally a process in which the material of the metal pipe is first heated and then deliberately cooled to cause a structural transformation in the metal material. The term "heat treatment" should therefore not be confused with the term "heating."
[0014] The initial press hardening temperature can be, for example, the AC3 temperature, e.g., 950°C. The final press hardening temperature is typically a temperature around room temperature, e.g., 20°C. The intermediate temperature can be selected, for example, approximately halfway between the initial press hardening temperature and the final press hardening temperature, with different temperature ranges being possible depending on the sheet material used. For example, an intermediate temperature in the range of 400 to 500°C is suitable. The intermediate temperature can, in particular, be in a range where the metal tube is not yet brought to the annealing range.
[0015] The pressing force during press hardening does not need to be excessively high, especially for metal pipes. In any case, the forming tool creates a deformation force that results in the desired transformation to a martensitic structure.
[0016] For example, alternating current can be used to generate the conductive current flow through the metal pipe.
[0017] According to an advantageous embodiment of the invention, at least one region of the metal tube is conductively heated with direct current. This allows conductive heating of the region to be carried out even more efficiently. In particular, interference due to impedances of the arrangement and skin effects are avoided.
[0018] The metal tube can have any shape, in principle. It can be a straight tube or a tube with one or more bends. The cross-sectional shape of the tube can also be arbitrary, for example, circular, oval, square, or any irregular shape. The metal tube can therefore be any elongated body that is hollow inside.
[0019] According to an advantageous embodiment of the invention, the area of the metal tube heated by conductive heating is cooled during press hardening with a minimum temperature gradient defined from an initial temperature generated by conductive heating to a final temperature. The cooling process is thus carried out comparatively quickly, determined by the minimum temperature gradient, but at least with a temperature difference per unit of time that corresponds to the minimum temperature gradient. This allows a targeted material microstructure transformation to be achieved, for example, the desired transformation to martensite during press hardening. The minimum temperature gradient can be, for example, 27°C per second.
[0020] If heat treatment is performed, it can also be carried out in such a way that an area of the metal tube that initially has a high degree of hardness (low ductility) is transformed into an area of lower hardness (higher ductility). For example, a martensite transformation caused by a previous press hardening process can be reversed by the heat treatment. In the method according to the invention, this can be carried out specifically in one or more areas of the metal tube, meaning that the entire metal tube does not necessarily have to undergo this treatment.
[0021] According to the invention, several consecutive regions in the longitudinal direction of the metal tube are conductively heated by separate electrodes and then processed by press hardening. This allows for highly efficient processing of the metal tube in several regions. The consecutive regions can be first conductively heated and then processed by press hardening, optionally simultaneously and / or sequentially. The consecutive regions of the metal tube can be adjacent to one another or spaced apart from one another, for example, by regions of the metal tube not subjected to this processing.
[0022] According to an advantageous embodiment of the invention, the region of the metal tube heated by conductive heating is cooled during press hardening by means of a forming tool that is brought into contact with the region and / or by passing a cooling medium through the metal tube. During press hardening, the forming tool can in particular be a press-hardening tool, for example a forming tool with an upper and a lower tool, between which the metal tube or at least the conductively heated region is pressed. The cooling of the conductively heated region of the metal tube can be achieved solely by the cooling effect of the forming tool if this is designed as a non-cooled forming tool. The forming tool can also be designed as a cooled forming tool in which a cooling medium is passed through at least parts of the forming tool, for example through the upper tool and / or the lower tool.Alternatively or additionally, cooling can be achieved by passing a cooling medium through the metal tube, which reduces the equipment required for the mold. The cooling medium can be water, for example.
[0023] According to an advantageous embodiment of the invention, the conductive heating is carried out by means of at least two electrodes arranged at a distance from one another and resting against the metal tube, wherein one or more end-side electrodes are arranged on the end side of the metal tube and / or one or more peripheral electrodes are arranged on the circumference of the metal tube. In this way, electrode designs adapted to the processing requirements can be used, so that not necessarily the entire metal tube has to be conductively heated, but for example only an end region or a region in the middle of the metal tube. The end-side electrodes can be designed as one-piece plate electrodes or ring electrodes. The peripheral electrodes can be designed as ring electrodes, for example as a one-piece or multi-piece ring electrode.In the multi-part embodiment, the circumferential electrode can comprise multiple circumferential segments, each surrounding a circumferential sector of the metal tube. One, several, or all of the electrodes can be integrated into the forming tool or arranged separately from the forming tool.
[0024] According to an advantageous embodiment of the invention, one or more electrodes are cooled by means of a cooling liquid during conductive heating. This has the advantage that unwanted heating of the electrodes can be avoided or at least reduced. This prevents the specific resistance of the electrode from changing significantly due to the heating, so that the characteristics of the conductive heating can be kept largely constant without such unwanted heating processes of the electrodes.
[0025] The object mentioned above is also achieved by a device for carrying out the step of conductively heating at least one region of the metal tube in a method of the type described above, wherein the device has one or more end-face electrodes arranged on the end face of the metal tube and / or one or more circumferential electrodes arranged on the circumferential face of the metal tube for introducing the electric current into the metal tube and / or discharging the electric current from the metal tube. This also allows the previously explained advantages to be realized.
[0026] The electrodes can, for example, be designed as a feed electrode, through which the electrical current is introduced into the metal tube, as a discharge electrode, through which the electrical current is discharged from the metal tube, or as a bypass electrode. The bypass electrode can be used to electrically bridge a section of the metal tube located between the feed electrode and the discharge electrode. The bypass electrode diverts the current flow through the section of the metal tube bridged by the bypass electrode, bypassing the metal tube in sections, so that this section is not conductively heated.
[0027] Such a device is also suitable for retrofitting existing molds or presses, since laying electrical cables requires significantly less effort than providing cooling channels.
[0028] According to an advantageous embodiment of the invention, at least one circumferential electrode is designed as a segmented electrode having a plurality of circumferential segments surrounding the circumference of the metal tube, each of which surrounds a circumferential sector of the metal tube. Each circumferential segment has an at least predominantly concave contact surface that serves to galvanically contact the associated circumferential sector of the metal tube. The circumferential electrode can be formed, for example, from two, three, four, five, six, or a larger number of circumferential segments.
[0029] According to an advantageous embodiment of the invention, at least one electrode has a contact surface for galvanically contacting the metal tube, which contact surface has a surface-structured design. The surface structuring of the contact surface provides an uneven, structured contact area with a plurality of spaced-apart contact surfaces, which form a plurality of individual, spaced-apart contact points between the electrode and the metal tube. The surface structuring can be designed, for example, as increased roughness, as a plurality of protruding teeth, or as a similar structure. In this way, the galvanic transition surfaces from the electrode to the metal tube are deliberately reduced and reduced to comparatively small areas.This has the advantage that the metal tube can also be conductively heated in the area below the electrode, where the surface-structured contact surface rests against the metal tube. This is due to the fact that the reduced contact surfaces create so-called hotspots, which lead to the heating of the metal tube below the contact surface. The surface-structured contact surface can, in particular, be an inner circumferential surface of a circumferential segment of the segmented electrode.
[0030] According to an advantageous embodiment of the invention, it is provided that at least one electrode is designed as a liquid-cooled electrode.
[0031] The invention is explained in more detail below using exemplary embodiments and drawings.
[0032] It shows Fig. 1 to 5 each show a metal tube in side view with different embodiments of electrodes for carrying out conductive heating and Fig. 6 and Fig. 7 each show a device for press hardening and a metal tube with different designs of electrodes for conductive heating and Fig. 8 a bent metal tube with electrodes for conductive heating.
[0033] The Fig. 1 shows, in the center, a metal pipe 1 that is to be conductively heated in a region 2. In this case, the region 2 extends over the entire length of the metal pipe 1. To carry out the conductive heating, front-side electrodes 3 are arranged on the metal pipe 1 at the respective opposite end faces, which are pressed against the respective end face of the metal pipe 1 with a contact force F.
[0034] In the Fig. 1 and the other exemplary embodiments are based on a metal tube 1 with a circular cross-section. However, the metal tube 1 can have any cross-sectional shape. In the case of a metal tube 1 with a circular cross-section, the end-face electrodes 3 can be designed as circular plate electrodes, as shown on the left and right in the Fig. 1. The electrodes 3 are connected to an electrical energy source 4. Via the electrical energy source 4, an electrical current flow is generated by the electrodes 3 from one electrode 3 to the other electrode 3 in the metal tube 1. The electrical current flow conductively heats the area 2. After reaching a desired initial temperature through conductive heating, press hardening of the area 2 is carried out.
[0035] The Fig. Figure 2 shows a variant of conductive heating in which only a shorter region 2 of the metal tube 1 is to be conductively heated. By way of example, this region 2 extends from a front end (left) to a region approximately in the middle of the metal tube 1. In this case, the electrodes for conductive heating are designed as a front electrode 3, as previously explained, and as a peripheral electrode 5.
[0036] The circumferential electrode 5 can be designed as a multi-part electrode with several circumferential segments 6. Each circumferential segment 6 surrounds a circumferential sector of the metal tube 1. Each circumferential segment 6 rests with a concave contact surface 8 on the outside of the wall 10 of the metal tube 1. The individual circumferential segments 6 are each pressed against the metal tube 1 with a force F. The individual circumferential segments 6 of a circumferential electrode 5 can either be connected separately to the electrical energy source 4 via electrical lines or can be connected in parallel via connecting lines 7. In this way, a partial area 2 of the metal tube 1 can be conductively heated if, for example, it is desired to process only this partial area 2 of the metal tube 1 by press hardening.
[0037] The Fig. Figure 3 shows an embodiment in which only a central region 2 of the metal tube 1 is to be conductively heated. In this case, no end-side electrodes are used, but rather the peripheral electrodes 5, as previously described with reference to the Fig. 2 described.
[0038] These circumferential electrodes 5 or their circumferential segments 6 can have smooth contact surfaces 8, as in the Fig. 3 can be seen in the middle, or surface-structured contact surfaces 8, as in the Fig. 3 on the right. For example, the surface-structured contact surfaces 8 can be grooved, serrated, have a toothed pattern, or a similar regular or irregular surface structure. As mentioned, this can create local hotspots on the metal tube 1 during conductive heating, so that the area of the metal tube 1 below the contact surfaces 8 is also heated.
[0039] As the Fig. As shown in Figure 4, the electrode configurations of the previously explained Fig. 1 to 3 can be combined in any way, even multiple times. Fig. Figure 4 shows, by way of example, the dual arrangement of respective pairs of circumferential electrodes 5 and the electrical energy source 4 in respective regions 2 of the metal tube, which are spaced apart from one another. Between the regions 2 is a section of the metal tube 1, which is thus not to be heated conductively. A potential U present between these electrode pairs D swims in.
[0040] The Fig. Figure 5 shows a variant of conductive heating, in which the respective end regions 2 of the metal pipe 1 are to be conductively heated, but an intermediate, central region is not. Therefore, similar to the Fig. 1, the front electrodes 3 are arranged at the front ends. A bypass electrode 9 is arranged in the central region, which is not to be conductively heated. This bypass electrode 9 diverts the current fed in by one electrode 3 from the metal tube 1 and feeds it back in at its other end, so that at least no significant current flows through this central region of the metal tube 1. As can be seen, this principle can also be used in combination with circumferential electrodes 5 if the metal tube is not to be conductively heated from the front end.
[0041] The Fig. Figure 6 shows a press hardening of the conductively heated area 2 of the metal tube 1 in a forming tool having an upper tool 11 and a lower tool 12. The conductive heating takes place, as already described with reference to Fig. 1, for example, by front-face electrodes 3 and the electrical energy source 4. Once the desired initial temperature has been reached by means of conductive heating, the press hardening process takes place by moving the upper tool 11 and the lower tool 12 toward each other, thereby performing a pressing process with simultaneous cooling of area 2. In this way, press hardening takes place with cooling of area 2 by the cooling tool 11, 12.
[0042] The Fig. Figure 7 shows an additional or alternative variant for cooling area 2 during the press hardening process. In this case, for example, circumferential electrodes 5, as previously described, are used for conductive heating, or end-face ring electrodes 13, which have a central through-opening. A cooling medium can be supplied through the central through-opening at a supply side 14 and guided through the metal tube 1, and then discharged again at an outlet side 15. In this way, cooling during the press hardening process can be achieved additionally or exclusively by the cooling medium guided through the metal tube 1.
[0043] The Fig.Figure 8 illustrates that the innovative conductive heating of at least one region 2 of the metal tube 1 according to the invention also allows any shaped region 2 of the metal tube 1 to be conductively heated without any problems, for example, curved regions. The bending of the curved region does not pose a problem for the attachment of, for example, the peripheral electrodes 5.
Claims
[1] Method for machining a metal pipe (1) by press hardening at least one region (2) of the metal pipe (1), comprising the steps: a) Providing the metal pipe (1), b) conductive heating of at least one region (2) of the metal tube (1), c) press hardening the area (2) of the metal tube (1) heated by conductive heating, characterized by that several regions (2) lying one behind the other in the longitudinal direction of the metal tube (1) are conductively heated by respective separate electrodes (3, 5, 13) and then processed by press hardening. [2] Method according to claim 1, characterized by that the area (2) of the metal tube (1) heated by the conductive heating is cooled during press hardening with a minimum temperature gradient defined from an initial temperature generated by the conductive heating to a final temperature. [3] Method according to one of the preceding claims, characterized bythat the region (2) of the metal tube (1) heated by the conductive heating is cooled during press hardening by means of a forming tool (11, 12) which is brought into contact with the region (2) and / or by passing a cooling medium through the metal tube (1). [4] Method according to one of the preceding claims, characterized by that the conductive heating takes place by means of at least two electrodes (3, 5, 13) arranged at a distance from one another and lying against the metal tube (1), wherein one or more end-side electrodes (3, 13) are arranged on the end side of the metal tube (1) and / or one or more circumferential electrodes (5) are arranged on the circumferential side of the metal tube (1). [5] Method according to claim 4, characterized by that one or more electrodes (3, 5, 13) are cooled by means of a cooling liquid during the conductive heating. [6] Method according to one of the preceding claims, characterized bythat during press hardening, sharply defined zones of different material structures are produced on the metal tube (1). [7] Method according to one of the preceding claims, characterized by that the conductive heating of at least one region (2) of the metal tube (1) is carried out in a period of less than 10 seconds.
Citation Information
Patent Citations
Method for reinforcing a workpiece with a hole in certain areas
DE10207132A1
Electric resistance heating jig for heat treatment of tubes - has fixed and mobile arms with tongs on respective opposite sides of trolley
DE3027107A1
Hot forming system for metal workpieces
EP1598129A1
Method for producing a tubular profile
EP2446977A1
Apparatus for annealing metal pipe
JP1992099821A