Method for sintering with stabilizing agents at an interface of a fastening object to stabilize a lateral position of the fastening object relative to a base component and assembly produced with stabilizing agents
By applying a sintered layer with stabilizing projections to the interface of fastening objects, the method addresses alignment and stability issues in sintering processes, enhancing manufacturing efficiency and heat transfer in power module assemblies.
Patent Information
- Application Number
- DE102023109136
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-04-12
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2043-04-12
AI Technical Summary
The current methods for sintering fastening objects to base components in power module assemblies, such as semiconductor power modules, face challenges with alignment and stability during the solidification step, leading to misalignment, increased manufacturing time and complexity, and potential overheating due to inefficient heat transfer.
A method involving the application of a sintered layer to the base component, provision of stabilizing agents on the interface, and arranging the fastening object with projections that protrude into the sintered layer to stabilize the lateral position, eliminating the need for additional alignment frames and ensuring precise positioning during the solidification process.
This approach enhances manufacturing efficiency by reducing the need for alignment frames, saving energy, and improving heat transfer while preventing misalignment and overheating, thereby increasing production capacity and reliability of the assembly.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[0001] The present invention relates to a method for sintering an interface of a mounting object, e.g. a semiconductor power module, to a mounting side of a base component, e.g. to a heat sink, a heatsink and / or (a part for) a cooler.
[0002] The method is applicable to the manufacture of power module assemblies. Such a power module assembly (hereinafter referred to as "assembly") may comprise multiple attachment objects attached to the base component. Typically, the assembly is configured to be part of an electrical circuit, e.g., a powertrain circuit of an electric vehicle. Demand for electric vehicles, especially electric cars, is increasing rapidly these days.
[0003] The power module, and in particular its mounting objects, are adapted to provide the required electrical functionalities. At least some of the mounting objects may be semiconductor power modules. These may include insulated-gate bipolar transistors (IGBTs) and / or metal-oxide-semiconductor field-effect transistors (MOSFETs).
[0004] During operation of electrical circuits, the mounting objects generate heat, particularly from electrical currents. To prevent overheating and damage to the mounting objects, they are fixed to the base component. The base component is often a heat sink, a heat sink, and / or (a part of) a cooler. The base component absorbs a significant portion of the heat generated by the mounting objects and dissipates it. For example, the base component dissipates the heat to the ambient air via cooling fins.
[0005] The fastening objects should be attached to the base component in such a way that enables sufficient heat transfer from the fastening objects to the base component. In particular, the fastening objects can be attached to the base component by pressure sintering. A sintering layer of sintered material is provided between the fastening objects and the base component. In a subsequent solidification step, the sintered material is heated to a maximum sintering temperature. Furthermore, the fastening objects and the base component are pressed together, e.g., along a normal direction that can be perpendicular to the fastening side. The solidification step compacts and solidifies the sintered material. A sintered layer is formed from the sintered layer between the fastening objects and the base component. The sintered layer permanently fixes the fastening objects to the base component.
[0006] The consolidation step can be a bottleneck in assembly manufacturing. It requires the use of a pressure sintering tool, which presses the attachment objects and the base component together while heating the sintering material.
[0007] Each fixture should be correctly positioned (i.e., at the individually designated location and with the individually designated spatial orientation) on the base component. To utilize the maximum production capacity of the pressure sintering tool, the sinter layer is applied to the base component, and the fixtures are positioned on the sinter layer before the start of the solidification step and outside the pressure sintering tool. An assembly to be sintered is assembled and then moved into the pressure sintering tool. In the assembly, the fixtures are correctly positioned on the sinter layer. Their interfaces face the sinter layer.
[0008] The pressure sintering tool is not occupied during the assembly of the assembly and can perform the solidification step for another assembly in the meantime.
[0009] Simply placing the attachment objects on the sintered layer isn't enough. The surface of the sintered layer isn't very sticky, especially after some pre-drying (if any). In the assembly, there's no significant adhesion of the attachment objects to the sintered layer.
[0010] Furthermore, it may happen that the shape of the interface of the fastening object does not match the shape of the base component on the fastening side where the fastening object is to be fastened. If the fastening object is placed on the sintered layer before the solidification step, its interface will not fit snugly on the sintered layer. This may lead to unstable support of the fastening object on the sintered layer. For example, the interface of the fastening object may be convex. As a result, there is only a small contact area between the interface and the sintered layer. The fastening object may wobble. Of course, other cases of shape mismatches may also occur.
[0011] Without additional measures, there is a high risk in such cases that the fastening objects will move away from their individually intended positions and / or deviate from their individually intended spatial orientations as the assembly is moved into the compression mold. The fastening objects can wobble and easily lose their correct position. Something is needed to hold them precisely in position while the assembly is moved, e.g., into the pressure sintering mold. Additionally or alternatively, unintentional misalignments and lateral displacements of the fastening objects relative to the base component can occur even at an early stage of the solidification step, when the fastening objects are pressed against the base component and the convex interfaces are flattened by the increasing pressure.
[0012] The current approach is to use an alignment frame structure that holds the fastening objects in the assembly in their correct position, particularly during the transfer of the assembly into the pressure sintering tool and during the solidification step performed in the pressure sintering tool. The alignment frame structure comprises a frame that surrounds the base component in the circumferential direction, e.g., at least in a plane perpendicular to the normal direction. The alignment frame structure may have recesses for receiving the fastening objects in their correct position. Additionally or alternatively, it may have pins that engage corresponding holes in the base component and / or the fastening object.
[0013] The use of the alignment frame structure, especially during transfer to the pressure sintering tool and during the solidification step, increases manufacturing time, manufacturing costs, and manufacturing complexity. The alignment frame structure is used only temporarily. It is removed from the assembly after the solidification step. A suitable alignment frame structure must be developed for each assembly layout. The current approach is suitable for small-batch production but is too complicated for high-volume production.
[0014] Furthermore, the alignment frame is complex and delicate, resulting in a significant risk of failure.
[0015] US 2015 / 0 146 399 A1 discloses a method for attaching a semiconductor chip to a substrate by means of pressure sintering. Mechanical locking elements can be formed on a top side of the substrate and / or on a bottom side of the semiconductor chip to increase the shear strength of the attachment of the semiconductor chip to the substrate in the finished assembly. The locking elements can be formed by chemical etching, sputter etching, or selective coating.
[0016] JP 2020-155497 A describes a connection between two plate-shaped elements by means of a sintering process. Grooves are formed on one of the plate-shaped elements at a connecting surface for connecting to the other plate-shaped element via a sintered layer. These grooves form gas passages for evaporating solvent in a sintering paste.
[0017] US 2016 / 0 113 107 A1 discloses an electrical module comprising a substrate, a power semiconductor chip, and a bonding material. The power semiconductor chip is attached to a conductor layer of the substrate by the bonding material. Spacers are provided in the bonding material between the conductor layer and the power semiconductor chip to keep the power semiconductor chip at a distance from the conductor layer.
[0018] WO 2020 / 182361 A1 explains a method for producing a cohesive bond between a first component of a power semiconductor module and a second component. A material preform may comprise a stabilizing agent that ensures a specific gap between the surfaces being bonded during a period when a solder material of the material preform is at an elevated temperature and therefore in a liquid state.
[0019] The invention is based on the object of facilitating the production of assemblies as described above.
[0020] This object is achieved by a method according to claim 1.
[0021] The process is used to sinter an interface of a fastening object to a fastening side of a base component. It comprises the following steps: - Applying a sintered layer to the fastening side; - Providing stabilizing agents on the interface; and - Arranging the fastening object directly on the sintered layer, wherein the interface faces the sintered layer and wherein the stabilizing means protrudes into the sintered layer to stabilize a lateral position of the fastening object relative to the base component, thereby forming an assembly to be sintered.
[0022] The stabilizing agent interacts with the sinter layer and helps secure the fastening object in its correct position within the assembly. It stabilizes the position of the fastening object relative to the sinter layer and thus relative to the base component. It eliminates the need for an additional alignment frame structure to secure the correct position of the fastening object within the assembly, e.g., during transfer of the assembly into the pressure sintering tool or during a solidification step for solidifying the sinter material of the sinter layer into a sintered layer. This facilitates manufacturing.
[0023] Since no alignment frame structure is inserted into the pressure sintering tool with the assembly, the pressure sintering tool can be smaller. Energy is saved because no heat is wasted on at least partially heating the material of such an alignment frame structure in the pressure sintering tool during the solidification step.
[0024] When the fastening object is placed in its correct position on the sintered layer, its interface faces the sintered layer. The interface can be at least partially in direct contact with the sintered layer. The stabilizing agent, which protrudes into the sintered layer, provides a positive connection between the stabilizing agent and the sintered layer. This naturally stabilizes the fastening object, ensuring that it remains in its correct position. The stabilizing agent engages the sintered layer, and the sintered layer ultimately exhibits a predetermined mechanical stability. This engagement reduces the risk of the fastening object moving from its correct position in the assembly and / or becoming jammed.
[0025] Of course, the method can relate to sintering the interfaces of multiple fastening objects, for example the interfaces of at least two fastening objects, onto the fastening side of the base component. References to "the fastening object" and its fastening to the base component can refer individually to one, several, or all fastening objects. The fastening of the various fastening objects can have different modifications according to the present disclosure. Preferably, the various fastening objects are fixed using the same solidification step. According to one aspect, all fastening objects can be fastened to the base component in the same way. The fastening objects can be positioned at a distance from one another in the assembly to be sintered (and accordingly in the resulting assembly).
[0026] According to one aspect, the assembly to be sintered is assembled outside the pressure sintering tool and subsequently moved into the pressure sintering tool. The assembly to be sintered can be moved into the pressure sintering tool without using an alignment frame means that engages the base component and the fastening object. In particular, the fastening object can only be aligned with the base component. - about the sinter layer - and optionally additionally directly through the stabilizing means, which protrude through the sintered layer and lie directly on the fastening side, there is a mechanical engagement while the assembly (to be sintered) is moved into the pressure sintering tool.
[0027] In one embodiment, the stabilizing means comprise at least one projection protruding from the interface. Without the additional stabilizing means, the interface is at least substantially planar after the solidification step. However, due to the convex shape of the interface before the solidification step (particularly in the assembly), it is possible that at least one region of the interface does not directly abut the sintered layer in the assembly to be sintered (non-adjacent section), while at least another region of the interface directly abuts the sintered layer (adjacent section). Since the at least one projection protrudes from the interface, it protrudes in the direction of the base component in the assembly to be sintered.
[0028] If multiple protrusions are provided, the reference to "the protrusion" may refer to at least one, several, or all of the protrusions. It is possible for different protrusions to be implemented according to various disclosed modifications.
[0029] The projections can protrude from the interface, e.g., in the normal direction, by at least 125 µm. Taking into account the expected maximum convexity of the interface, this ensures an acceptable probability that the projection will still protrude into the sintered layer even if the projection is located in the non-adjacent section.
[0030] If at least one projection is located in the adjacent section, it extends deeply into the sintered layer. This exhibits a comparatively strong engagement with the sintered layer.
[0031] Even if the at least one projection is located in the non-adjacent section, it can still partially protrude into the sintered layer. Thus, there are now at least two different locations where the fastening object engages with the sintered layer: the at least one adjacent area and the at least one projection. This reduces the risk of the fastening object being rotated from its individually intended spatial orientation, e.g., while the assembly is being moved and / or while the assembly is being pressure sintered. Naturally, this also further reduces the risk of the fastening object being displaced from its individually intended position relative to the base component.
[0032] In one embodiment, the stabilizing means comprise at least two projections that protrude from the interface, wherein the at least two projections are spaced apart from one another. Since the projections protrude from the interface, they protrude in the assembly toward the base component. Since the at least two projections in the assembly protrude into the sintered layer, both the individually desired position and the individually desired orientation of the fastening object in the assembly to be sintered are particularly reliably ensured, even in the case where the adhesion of the interface to the sintered layer—ignoring the stabilizing means—is particularly low.
[0033] The stabilizing means may comprise a plurality of projections projecting from the interface. The risk of the correct position of the fastening object not being maintained is further reduced with an increasing number of projections. For example, there may be at least 3 projections or even at least 24 projections.
[0034] In one embodiment, the stabilizing means comprise at least three projections projecting from the interface. The at least three projections can be spaced apart from one another. This ensures that the fastening object rests on the sintered layer at at least three different locations. In other words, the fastening object is supported on the sintered layer at at least three locations. This prevents the fastening object from wobbling on the sintered layer, even if the interface is convex.
[0035] According to a further aspect, at least one projection is arranged at each corner region of the interface. For example, the interface can be rectangular and have four corner regions.
[0036] According to one aspect, parts (e.g., protrusions) of the stabilizing agent can be clustered at and / or near at least one area where an increased risk of crack formation in the sintered layer is to be expected. Such locations are, for example, edges and corners of the fastening object and the sintered layer, e.g., lateral ends (edges) and, in particular, corners of the sintered layer in planes perpendicular to the normal direction, or areas of the sintered layer adjacent to lateral ends (and, in particular, corners) of the interface of the fastening object. In final assembly, the combination of the sintered layer and the stabilizing agents (or their residues, if any) forms a composite material, at least locally. This inhibits crack formation and / or crack propagation in the sintered layer.
[0037] The stabilizing means may, for example, comprise a plurality of protrusions projecting from the interface and lined up along an outer circumferential portion of the interface. The protrusions may be arranged at equal intervals along the circumference. It is also possible for a spatial density of the protrusions to be increased in at least one region where the risk of crack formation in the sintered layer is particularly high. For example, the protrusions are provided substantially equidistantly along the edges of the sintered layer and / or adjacent to the edges of the interface, but with a denser spatial (narrower) arrangement at the corners of the sintered layer and / or adjacent to the corners of the interface.
[0038] The protrusions (or their remnants) locally improve the thermal shock resistance ("TC resistance") of the sintered layer. TC resistance is the resistance to damage caused by thermal shock. During operation of the assembly, the attachment object (e.g., in the form of a molded semiconductor power module) can generate heat. The temperatures of the attachment object, the sintered layer, and the attachment side can vary during operation. This results in thermal cycling of the sintered layer between the attachment object and the attachment side. The thermally induced stresses are higher at the edges and especially at the corners of the sintered layer and / or the interface. These thermal cycling stresses can lead to crack formation and crack propagation in the sintered layer.
[0039] The arrangement of many protrusions, such as wire bond structures, at the edges of the fastening object, e.g., an overmolded module with a DCB structure (see below), inhibits crack propagation from the edges (where cracking is expected to occur with increased probability) in a similar way to what happens with composite materials such as fiber-reinforced plastic, e.g., glass fiber reinforced plastic. Normally, cracks grow more easily in a homogeneous material. In a material enriched with objects that exhibit differing physical properties (such as the protrusions or their remnants, or glass fibers in the case of glass fiber reinforced plastic), the sharp tip of a crack is repeatedly blunted, slowing crack propagation.
[0040] In one aspect, the lateral distance between adjacent protrusions may be less than 0.5 mm. The lateral distance may be measured where the protrusions are attached to the interface.
[0041] The projections can locally influence the heat conduction in the sintered layer and / or in the sintered layer.
[0042] The stabilizing means may consist of elements attached to the interface and / or of elements formed directly in one piece with the interface.
[0043] The method may comprise (the step of) forming at least part of the stabilizing means on the interface by wire bonding, e.g., using a wire bonder. The position of the parts of the stabilizing means formed by this technique can be controlled very precisely. The technique can be easily integrated into existing manufacturing practices. It is particularly suitable for very precisely grouping the parts (e.g., protrusions) of the stabilizing means at specific locations. It is a cost-effective and time-saving method for attaching the stabilizing means to the interface. The bond wires used for wire bonding are compatible with the sintering process and do not interfere with the sintering process.
[0044] The thickness of a bonding wire used can range from 90 µm to 200 µm, for example, from 100 µm to 140 µm. This allows for the creation of very fine structures.
[0045] In one embodiment, the stabilizing agent comprises at least one wire bond structure. The wire bond structure can be formed by wire bonding, as explained above. It can be fixed at the interface by ultrasonic welding.
[0046] The at least one projection may, for example, be a wire bond structure formed by the wire bonder.
[0047] Accordingly, the at least two projections can each be formed as wire bond structures by the wire bonder.
[0048] In particular, the at least one wire bond structure can be a bond-off. A bond-off is a wire bond structure attached to an interface with a free end portion of a bond wire. In other words, the free end portion of the bond wire is not directly attached to the interface, while another portion of the bond wire, e.g., at least the other end of the bond wire, is attached to the interface, e.g., by melting using an ultrasonic welding process.
[0049] The sharp bond-off can easily penetrate into the sinter layer, even after the pre-drying of the sinter layer has already been completed.
[0050] At least one, several, or all of the wire bond structures may be bond-offs. At least one, several, or all of the protrusions may be bond-offs.
[0051] In one embodiment, the at least one wire bond structure may be a ball bond. Generally, at least one, several, or all of the wire bond structures may be ball bonds.
[0052] In one embodiment, the stabilizing agents are made of sinterable materials. By "sinterable materials" we mean materials that bond well with the sintered layer during the solidification step. For example, the wire bond structure(s) can be produced using wires made of sinterable materials, e.g., copper, silver, and / or aluminum (including alloys based on at least one of these materials). In particular, the stabilizing agent can be made of a material that is sintered together with the sintered material in the solidification step. In one embodiment, the stabilizing agent consists of a material that can be sintered together with the sintered layer in the solidification step, but is different from a metallic portion of the sintered material.On the one hand, this is advantageous for a strong, permanent fixation of the fastening object to the base component after the solidification step, but on the other hand, it is also advantageous for inhibiting crack formation and / or propagation in the sintered layer.
[0053] In one embodiment, at least one, several, or all of the protrusions may comprise a patch of adhesive. In another aspect, at least one, several, or all of the protrusions may have a sharp ridge at the interface. The sharp ridge may be formed by cutting and / or scraping into the interface. In another aspect, at least one, several, or all of the protrusions result from the attachment of a solid protrusion object, e.g., made of metal, to the interface.
[0054] It is possible that the stabilizing means comprise projections of different types.
[0055] According to a further aspect, the method may comprise (a step of) applying the sintering material to the attachment side to form the sintering layer.
[0056] If the assembly includes multiple fastening objects, the sintered layer may comprise multiple sections, e.g., one section for each fastening object. Different sections of the sintered layer may be spaced apart from each other.
[0057] The sintering material may comprise (in particular consist of) a sintering paste and / or a sintering pad (also referred to as a sintering preform).
[0058] The sintered material may contain metallic particles and at least one volatile component. The metallic particles may contain or be silver particles and / or copper particles. The volatile component(s) may be organic. The density of the sintered material may be in the range of 2.5 g / cm 3 up to 3.5 g / cm3 lay.
[0059] The sintering material (or the sintering paste and / or the sintering pad) can be pre-dried. In particular, the method can comprise a step of pre-drying the sintering material, e.g., after application and before placing the fastening object on the fastening side with the sintering layer in between. During pre-drying, at least part of the volatile organic component can evaporate.
[0060] The sintering material can be applied in a wet state in the application step before pre-drying.
[0061] Pre-drying makes the sintered material more like a solid material than in its wet state. The sintering paste can adhere to the mounting surface because it is a paste. The pre-dried sinter layer can bond firmly to the mounting surface. Because the pre-drying makes the sintered material more like a solid material, it exhibits even greater resistance to the stabilizing agent being pulled parallel to the mounting surface.
[0062] The pre-dried sinter layer may be porous after evaporation of the volatile component(s). Therefore, the stabilizing agent can penetrate the sinter layer even after pre-drying.
[0063] The thickness of the sintered layer (in the normal direction) can be in the range of 80 µm to 200 µm, e.g. 100 µm.
[0064] The process may include a step in which the fixture is placed onto the applied sinter layer by a robot. This enables high production capacity and cost-effective, high-precision production. Since a complex alignment frame structure is not required, it is much easier to use a robot for this task.
[0065] Pre-drying can occur before, during, and / or after placing the fastening object on the sintered layer. Pre-drying can be completed at the latest before the assembly is inserted into the pressure sintering tool, in particular before the assembly is moved for insertion into the pressure sintering tool. For example, pre-drying can be considered complete when at least 70 wt.% of the volatile compound has evaporated.
[0066] For example, the fastening object can be placed on the pre-dried sintered material. Specifically, the placing (the step of placing) of the fastening object on the applied sintered layer is performed after the pre-drying is complete (e.g., when at least 70 wt.% of the volatile compound has evaporated).
[0067] The solidification step can be carried out with the pre-dried sintered material.
[0068] According to one aspect, the method comprises (the step of) inserting the assembly to be sintered into the pressure sintering tool, wherein the arrangement of the fastening object on the sintering layer occurs before the collocation material to be sintered is inserted into the pressure sintering tool. In other words, the method may include (the step of) moving the collocation to be sintered into the pressure sintering tool. In particular, the assembly to be sintered may be inserted into the pressure sintering tool without an alignment frame structure for holding the fastening objects in their correct position in the assembly.
[0069] According to a further aspect, the method comprises a solidification step for solidifying the sintered layer in the assembly to be sintered. This rigidly and permanently connects the fastening object to the base component.
[0070] The solidification step may include sintering the sinter layer (for permanently fixing the at least one fastening object to the base component) with a maximum sintering temperature in a range of 200 °C to 300 °C and / or with a maximum sintering pressure in a range of 10 MPa to 40 MPa. This ensures proper sintering and thus a rigid and firm fixation of the fastening object to the base component.
[0071] The solidification step can be carried out using the pressure sintering tool.
[0072] In one embodiment, the thickness of the sintered layer (e.g., along the normal direction) is a maximum of 70 µm. Additionally or alternatively, the thickness of the sintered layer can be at least 20 µm. The thickness of the sintered layer can be 50 µm ± V. V can be, for example, 10 µm or 6 µm. The thickness of the sintered layer can be less than the thickness of the previous sintered layer. The density of the sintered layer can be higher than the density of the previous sintered layer. The sintered layer can consist of at least 90 wt.%, possibly at least 96 wt.%, metal, e.g., of the metallic material portion of the sintered material. The density of the sintered layer can at least substantially correspond to a density of the metallic material portion of the sintered material.
[0073] According to the invention, the stabilizing agent is at least partially permanently compressed (at least partially reduced in height) in the solidification step. As already mentioned above, the stabilizing agents can consist of projections formed from a bonding wire with a diameter of 125 µm. Furthermore, the sintered layer should be thin to enable good heat transfer from the fastening object to the base component, e.g., with a thickness of at most 70 µm. Even if the interface of the fastening object initially has a convex shape, it has become flat at an advanced stage of the solidification step. The forces pressing the fastening object against the base component and the resulting counterforces from the sintered layer and the stabilizing agents clamped between the interface and the base component flatten the interface.Furthermore, due to the relative friction between the fastening object, the sintered layer, and the base component, and due to the advanced solidification (hardening) of the sintered layer, the stabilizing agents are no longer needed to hold the fastening object in its correct position. It is therefore unproblematic that the stabilizing agents are at least partially permanently compressed during the solidification process. It has also been shown that this does not impair the sintering process.
[0074] According to one aspect, the stabilizing agent may be made of a different material than the interface. For example, the hardness and / or yield strength of the stabilizing agent may be lower than the hardness and / or yield strength of the interface material. This reduces the risk of damaging the interface when the stabilizing agents are compressed during the solidification step.
[0075] According to a further aspect, the fastening object is or comprises at least one of the following elements: - a heat-generating component, - an electronic component, e.g. a semiconductor component, and - a semiconductor power module.
[0076] In particular, the attachment object can be the semiconductor power module. The semiconductor power module can contain at least one semiconductor component.
[0077] The electronic component and the semiconductor power module generate heat during operation and can therefore also be considered heat-generating components.
[0078] The semiconductor component may comprise or consist of a semiconductor switch, an insulated-gate bipolar transistor (IGBT), a metal-oxide-semiconductor field-effect transistor (MOSFET) and / or the like.
[0079] In particular, the attachment object may include or consist of a molded-in module. The molded-in module may be a semiconductor power module with a resin cover. The resin cover may be manufactured by transfer resin molding. When multiple attachment objects are attached to the base component, at least one of them, some of them, or all of them may include or consist of a molded module.
[0080] The semiconductor power module as such may contain various layers and / or components.
[0081] The semiconductor power module may contain one, several or all of the following elements: - an integrated heat sink, - an insulating layer, - an (internal) circuit layer, - a fixing layer (e.g. an internal sintered layer) for fixing the semiconductor component to the insulation layer and / or the circuit layer, - the semiconductor part, - Bond wires, and - the resin cover (“cast module”).
[0082] The insulating layer may be made of ceramic material. The (internal) circuit layer may be attached to the insulating layer. Additionally or alternatively, the integrated heat sink may be attached to the insulating layer. The integrated heat sink may be arranged at the interface. In particular, it may form the interface. The insulating layer may be arranged between the integrated heat sink and the (internal) circuit layer.
[0083] In one embodiment, the mounting object (e.g., the semiconductor power module) comprises a direct copper bonded (DCB) structure. It may include a substrate, e.g., a ceramic substrate, forming the insulating layer. Furthermore, the DCB structure may include the insulating layer and the (internal) circuit layer or the integrated heat sink, or both.
[0084] According to another aspect, the base component is or comprises a heat sink, a heat sink and / or (a part for) a cooler.
[0085] In one embodiment, the mounting side of the base component is made of metal. Additionally or alternatively, the interface is made of metal. This enables effective transfer and dissipation of the heat generated in the mounting object.
[0086] The above-mentioned problem is further solved by an assembly having the features of claim 13.
[0087] The assembly comprises a base component and a fastening object, wherein a sintered layer between an interface of the fastening object and a fastening side of a base component fixes the fastening object to the base component, wherein a stabilizing agent formed at the interface or at least residues thereof protrude into the sintered layer.
[0088] The features and advantages described with regard to the method also apply to the assembly, and vice versa. For example, as described above, the stabilizing agents, e.g., projections, or their residues can inhibit crack formation and / or propagation.
[0089] According to one aspect, the fastening object may have been (permanently) fastened to the base component using the method disclosed herein.
[0090] The assembly may be configured to have electrical functionalities. For example, it may be adapted to switch electrical currents.
[0091] The assembly may be configured to be electrically connected to other electrical and / or electronic components.
[0092] In one embodiment, the assembly is configured to form part of an electrical circuit.
[0093] The assembly may be configured to be part of a powertrain circuit, e.g., in an electric vehicle. Electric vehicles may include electric cars, trucks, electric trains, watercraft (e.g., boats and ships), aircraft, and / or the like. The powertrain circuit may be a circuit for an electric motor, an electric drivetrain, a hybrid electric drivetrain, a battery-electric drivetrain, and / or the like. The assembly may, for example, be a multi-chip automotive drive module. In general, the powertrain circuit may be configured for mobile, semi-mobile, and / or stationary applications. For example, drive circuits for compressors, cable cars, stationary cranes, pumps, and the like may also be considered.
[0094] In one aspect, the assembly is configured to form part of an inverter circuit. The assembly can be used in inverters, e.g., in the powertrain circuit.
[0095] According to one aspect, the assembly is a half-bridge power assembly.
[0096] The present disclosure further describes a sintered assembly for attaching an interface of a fastening object to a fastening side of a base component by sintering, comprising the basic component; the fortification object; and a sintered layer arranged between the attachment side and the interface; wherein stabilizing means for stabilizing a lateral position of the fastening object relative to the base component are formed at the interface, wherein the stabilizing means protrude into the sintered layer in order to stabilize the lateral position of the fastening object relative to the base component.
[0097] The features and advantages described with regard to the process and the assembly apply accordingly to the assembly to be sintered and vice versa.
[0098] The composition to be sintered can be adapted for the production of the assembly.
[0099] Further features, advantages, and possible applications of the invention will become apparent from the following description of exemplary embodiments and the drawings. All features described and / or illustrated herein, alone or in any combination, constitute the subject matter of the invention, regardless of how they are combined in the claims or in their references to preceding claims.
[0100] Preferred embodiments of the invention will now be described with reference to the drawings in which: Fig. 1 shows a cross-sectional view of a base component with a sintered layer applied to a fastening side of the base component and a semiconductor power module to be placed on the sintered layer, wherein the semiconductor power module has stabilizing means protruding from an interface of the semiconductor power module for engaging in the sintered layer, in particular for insertion into the sintered layer; Fig. 2 shows a cross-sectional view of an assembly to be sintered, comprising the base component with the sinter layer and the Fig. 1, wherein the semiconductor power module is placed on the sintered layer, wherein the stabilizing means protrude into the sintered layer and thus stabilize a lateral position of the semiconductor power module relative to the base component; Fig. 3 shows a cross-sectional view of an assembly consisting of the Fig. 2 shown assembly to be sintered is formed by pressure sintering; Fig. 4 a view of the interface of the semiconductor power module of Fig. 1 shows; Fig. 5 shows a flow diagram of a process for sintering the interface of the semiconductor module to the mounting side of the base component; and Fig. 6A to 6E show different embodiments of projections of the stabilizing means.
[0101] Fig. 1 is a cross-sectional view showing a base member 10 and a fastening object to be fastened to a fastening side 11 of the base member 10 by pressure sintering to finally produce an assembly 60 which is Fig. 3 is shown.
[0102] In this example, the attachment object is a semiconductor power module 30, more specifically, a semiconductor power module 30 with a resin cover 40 (which may also be referred to as an encapsulated semiconductor power module).
[0103] The semiconductor power module 30 comprises a direct bonded copper structure (DCB structure, DCB is an abbreviation for "direct bonded copper") with a ceramic insulating layer 34, an integrated heat sink 33, and an internal circuit layer 35. A side of the integrated heat sink 33 facing away from the insulating layer 34 forms the interface 31. The integrated heat sink 33 is formed on one side of the insulating layer 34 and attached to the latter. The internal circuit layer 35 is attached to an opposite side of the insulating layer 34 (e.g., a top side in Fig. ) is formed and attached. The semiconductor components 37 are attached to the internal circuit layer 35 by an internal sintered layer 36. The internal sintered layer 36 may include separate sections for some or all of the semiconductor components 37. The semiconductor components 37 include, for example, IGBTs and / or MOSFETs. The semiconductor power module 30 may further include internal wiring 38, e.g., for establishing electrical connections between the semiconductor component 37 and the internal circuit layer 35. Furthermore, the semiconductor power module 30 may include electrical terminals 39. The electrical terminals 39 may be used to establish electrical connections with further attachment objects (not shown), e.g., further semiconductor power modules attached to the same base component 30, and / or with other electrical components.
[0104] The optional resin cover 40 covers the entire semiconductor power module 30 except for the integrated heat sink 33 at the interface 31.
[0105] The resin cover 40 provides electrical insulation, protection against moisture and protection against mechanical and chemical damage.
[0106] The semiconductor power module 30 is suitable for providing at least one electrical functionality in the finished assembly 60, e.g., for switching electrical currents. During operation, the semiconductor power module 30 generates heat. By attaching the semiconductor power module 30 to the base component 10, heat dissipation is improved and overheating of the semiconductor power module 30 during operation is prevented.
[0107] In the assembly 60, the base component 10 is used to dissipate the heat generated by the semiconductor power module 30. For example, the base component 10 can be a heat sink with cooling fins, e.g., elongated cooling fins and / or pin fins (not shown). Additionally or alternatively, the base component 10 can be a cooler or a part for forming a cooler. The base component 10 can have a channel structure for guiding a fluid, e.g., a coolant.
[0108] The base component 10 can be made of aluminum and / or copper (including corresponding alloys). In one embodiment (not shown), the base component 10 is made of aluminum (including aluminum alloys) and has an insert in the contact area, wherein the insert is made of copper (including copper alloys).
[0109] The fastening object is firmly and permanently connected to the base component 10 by pressure sintering.
[0110] The fastening side 11 of the base component 10 is substantially flat, at least in a contact area where the fastening object (the semiconductor power module 30) is fastened. A normal direction N runs perpendicular to this contact area. In this example, the entire fastening side 11 is flat, and the normal direction N is perpendicular to the entire fastening side 11.
[0111] An example of a corresponding method for (pressure) sintering the interface 31 of the fastening object (e.g. the semiconductor power module 30) to the fastening side 11 of a base component 10 is described below with reference to Fig. 5 and the other figures are described in more detail.
[0112] In a sinter layer application step S20, a sinter material is applied to the fastening side 11 of the base component 10 to form a sinter layer 20, which is pressure-sintered in a subsequent consolidation step S60. The sinter layer 20 is formed at least in the contact area of the fastening side 11 for fastening the fastening object. In this example, the sinter layer 20 is formed using a sinter paste. The sinter paste is applied to the fastening side 11, at least to the contact surface. It comprises finely distributed metal, e.g., silver, copper, and / or another metal. In this example, silver and / or copper is / are used as the metal (including corresponding alloys). In the sinter layer application step S20, the sinter paste is applied in a wet state. The sinter paste contains liquid organic volatile components. This facilitates proper application of the sinter paste.The density of the sintering paste can be in the range of 2.5 g / cm. 3 up to 3.5 g / cm 3 lay.
[0113] Fig. 1 shows the base component 10 with a section (a patch) of the sintered layer 20 applied to the fastening side 11. Of course, the section can also be larger, particularly if several fastening objects are to be pressure-sintered onto the base component 10 with the same section. Additionally or alternatively, the sintered layer 20 can comprise several sections (patches) for pressure-sintering different fastening objects onto the base component 10.
[0114] The sintered layer 20 may be subjected to a pre-drying step S30. In the pre-drying step S30, at least a portion of the volatile components evaporates. In other words, the sintered layer 20 is at least partially dried during the pre-drying step S30. The pre-drying step S30 may involve the base component 10 with the applied sintered layer 20 resting for at least a predetermined time. As the sintered layer 20 dries, it becomes more of a solid, yet sponge-like material (with voids therein). The sintered layer 20 is also firmly bonded to the fastening side 11.
[0115] The (pre-dried) sintered layer 20 can have a thickness (in the normal direction N) in the range of 80 µm to 200 µm. The thickness may not be influenced by the pre-drying step S30, at least not significantly. For example, the thickness after pre-drying may deviate by less than 20% from the thickness before pre-drying.
[0116] Fig. 2 shows an assembly 50 to be sintered. The assembly 50 comprises the base component 10, the sintered layer 20 applied to the fastening side 11 and the fastening object (here in the form of the semiconductor power module 30) placed in the correct position on the sintered layer 20.
[0117] The interface 31 of the attachment object, here the semiconductor power module 30, is often convex. This is shown in the Fig. 1 and Fig. 2. The convex shape may result from different thermal expansion coefficients of the elements that comprise the semiconductor power module 30.
[0118] In conventional embodiments (not shown), the interface 31 of the semiconductor power module 30 is flat and smooth, except for the convex curvature. Due to the convex curvature, only a small area of the interface 31 (only a small area of the underside of the integrated heat sink 33) lies directly on the sinter layer 20. Therefore, the power semiconductor module can easily wobble, twist, and / or shift laterally relative to the base component 10. This would impair proper manufacturing. Therefore, the assembly 50 would typically preclude a specially designed alignment frame structure to hold the semiconductor power module 30 in its correct lateral position, as intended for the finished assembly 60. "Laterally" can mean perpendicular to the normal direction N (parallel to the mounting side 11 in Fig. 2).
[0119] According to the present invention, the method comprises a step S10 in which stabilizing means are provided at the interface 31. The stabilizing means are designed such that they protrude into the sintered layer 20 when the fastening object (i.e., the semiconductor power module 30) is placed on the (optionally pre-dried) sintered layer 20 and stabilize the lateral position of the fastening object relative to the base component 10. Thus, it is not necessary to use an additional alignment frame structure to stabilize the fastening object in its correct lateral position relative to the base component 10. The assembly 50 to be sintered does not have such an additional alignment frame structure and is handled without one.
[0120] In this example, step S10 includes providing a plurality of protrusions 32 at the interface 31. The protrusions 32 protrude from the interface 31 (in this example, from the bottom of the integrated heat sink 33).
[0121] The projections 32 can be manufactured using an ultrasonic wire bonder. The projections 32 can be wire bond structures. In particular, they can be formed as so-called bond-offs. To produce such a bond-off, the wire bonder fixes one end of a bond wire to the interface 31 (to the integrated heat sink 33) using ultrasonic waves. The bond wire is then cut to sever a bond wire segment that is attached to the interface 31.
[0122] The diameter of the bonding wire and thus of the bonding wire segments forming the projections 32 (the stabilizing means) may be, for example, 125 µm.
[0123] The stabilizing agent can be made of a sinterable material. It can consist of a sinterable metal, e.g., copper, silver, and / or gold (including alloys based on one or more of these metals). The bonding wire can be made of the corresponding material.
[0124] In a placement step S40, the fastening object is placed on the sintered layer 20. The placement step S40 may include an automatic alignment of the fastening object with respect to the base component 10. For example, the fastening object may be placed in its correct position on the sintered layer 20 with the aid of at least one robot. The correct position is the lateral position as shown in the Fig. 3 shown finished assembly 60.
[0125] It is possible that the assembly step S40 comprises placing several fastening objects on the sintered layer 20 in their respective correct positions.
[0126] The placement step S40 results in the formation of the assembly 50 to be sintered, as shown in Fig. 2 shown.
[0127] In the assembly 50, the stabilizing means (in this example, the projections 32) extend deeply into the sintered layer 20. More precisely, in this example, the sharp bond-offs are pressed into the pre-dried sintered layer 20. They are inserted into the sintered layer 20.
[0128] The pre-dried sinter layer 20 resembles snow in that it can be further compressed and resists the displacement of the stabilizing means laterally to the normal direction N (ie parallel to the fastening side 11).
[0129] The stabilizing means extending into the sintered layer 20 stabilize the correct position of the fastening object relative to the sintered layer 20 and thus relative to the base component 10. This allows the assembly 50 to be sintered to be handled without the fastening object being laterally displaced or twisted from its correct position, without the use of an additional alignment frame structure. Since a plurality of projections 32 are provided in this example, the fastening object cannot wobble.
[0130] In a transfer step S50, the assembly 50 to be sintered is moved and placed into a pressure sintering tool. The transfer step S50 is performed without an additional alignment frame structure.
[0131] In the consolidation step S60, the sintered layer 20 is converted into a sintered layer 20a. This firmly, rigidly, and permanently bonds the attachment object (in this example, the semiconductor power module 30) to the base component 10. The consolidation step 60 is performed in the pressure sintering tool. The consolidation step 60 involves pressing the attachment object and the base component 10 against each other, for example, along the normal direction N. The sintered layer 20 is squeezed between the interface 31 and the attachment side 11. Furthermore, heat is applied, e.g., by the pressure sintering tool, to heat the sintered layer 20. The combined action of pressure and heat on the sintered layer 20 converts it into the sintered layer 20a. The stabilizing agents do not impair the sintering process.
[0132] During the solidification step S60, the sintered layer 20 is heated to a maximum sintering temperature in the range of 200°C to 300°C. The pressure exerted on the sintered layer 20 can be in a range of 10 MPa to 40 MPa.
[0133] The temperature may be maintained in the said sintering temperature range and / or the pressure exerted on the sintered layer 20 may be maintained in the said sintering pressure range for a duration in the range of 2 minutes to 10 minutes in the solidification step S60.
[0134] The thickness of the sintered layer 20a (in the normal direction N) may be less than that of the previous sintered layer 20. For example, the thickness of the sintered layer 20a may be in the range of 40 µm to 60 µm, for example 50 µm.
[0135] The sintered layer 20a as such (neglecting the stabilizing agents or their residues 32a) consists of the metallic portion contained in the original sintering paste. The density of the sintered layer 20a is higher than the density of the previous (pre-dried) sintered layer 20. The density of the sintered layer 20a corresponds, for example, to the density of the metallic portion (e.g., approximately 10.5 g / cm 3 if the metal content is silver, or about 9 g / cm 3 if it is copper).
[0136] Fig. 3 shows a finished assembly 60, which consists of the Fig. 2, the assembly 50 to be sintered being produced, the production comprising the solidification step S60.
[0137] In this example, the original diameter of the bonding wire (and thus of the protrusions 32) is larger than the thickness of the sintered layer 20a. Therefore, the stabilizing means (the protrusions 32) are deformed during the solidification step S60. Remains 32a of the stabilizing means are embedded in the finished sintered layer 20a.
[0138] The material of the stabilizing means can be softer (e.g., lower hardness and / or yield strength) than a material of the integrated heat sink 33 and / or than a material of the base component 10 on the fastening side. This allows the stabilizing means to be deformed in the hardening step S60 without damaging the fastening object and / or the base component 10.
[0139] The material of the stabilizing agent and its residues 32a, on the one hand, and the material of the sintered layer 20a, on the other hand, may be different. Therefore, the stabilizing agents or the residues 32a (in the event that the stabilizing agents are significantly deformed during the solidification step S60) form, at least locally, a composite material in the finished assembly 60 according to Fig. 3.
[0140] The stabilizing agents or the residues 32a in the sintered layer 20a can locally influence the thermal conductivity between the fastening object and the base component 10.
[0141] As explained above, the fastening object can generate heat during operation, e.g., when the assembly 60 switches electrical currents. The amount of heat generated per unit of time and thus the temperatures of the fastening object, e.g., at the integrated heat sink 33, vary depending on the operating state. Due to different thermal expansion coefficients, the rigid connection between the fastening object and the base component 10 via the sintered layer 20a is subjected to thermal cycling. This can lead to the formation and propagation (growth) of cracks in the sintered layer 20a.
[0142] The local composite structure in the sintered layer 20a, resulting from the embedded stabilizing agents or their residues 32a, locally inhibits the formation and propagation of cracks in the sintered layer 20a. The boundaries between the different materials can redistribute local stresses and strains and act as a stop to crack propagation.
[0143] According to one aspect, the stabilizing means, e.g., in the form of the projections 32 produced as bond-offs, are bundled at and / or near regions where an increased risk of crack formation in the sintered layer 20a is to be expected. Such regions are, for example, the regions in the sintered layer 20a below the edge regions (in a plane parallel to the normal direction N) of the integrated heat sink 33, i.e., below edge regions and, in particular, below corner regions of the integrated heat sink 33. The stabilizing means can thus be bundled at the corresponding regions of the integrated heat sink 33.
[0144] Fig. shows a view of the underside of the fastening object before performing the solidification step S60. The projections 32 are provided on the underside of the integrated heat sink 33. More specifically, they are arranged equidistantly along an outer peripheral portion 31a of the underside of the integrated heat sink 33. Therefore, the projections 32, or at least their remnants 32, are in the Fig. 3, the finished assembly 60 is arranged in the areas of the sintered layer 20a where the risk of cracking is greatest. This improves the resistance of the assembly 60, in particular of the sintered layer 20, to temperature fluctuations and thus increases the reliability of the assembly 60. As shown in Fig. As shown in Figure 4, a lower part of the resin cover 40 may laterally enclose the peripheral regions of the integrated heat sink 33. It can be assumed that the lower part of the resin cover 40 is not part of the interface 31 as such, since the resin material does not form a strong bond with the sintered layer 20a.
[0145] Of course, the method may include pressure sintering the interfaces of multiple attachment objects, e.g., multiple semiconductor power modules 30, onto the attachment side 11 of the base component. Accordingly, the assembly 50 may include multiple attachment objects.
[0146] The assembly 60 is configured to form part of an electrical circuit, e.g., a drive train circuit for mobile, semi-mobile, and / or stationary applications. The electrical connections 39 can be used to integrate the assembly 60 into the electrical circuit.
[0147] The Fig. 6A to 6E show various embodiments of the projections 32 provided on the interface 31.
[0148] In Fig. 6A, the single projection 32 is formed as a short wire bond (bond-off) as described above.
[0149] Fig. 6B shows an embodiment of the protrusion 32 formed by ball bonding. In this case, the protrusion 32 has a ball portion 321 attached to the interface 31 and an extension 322 protruding from the ball portion 321 further away from the interface 31. In a first step, the ball portion 321 is formed at the interface 31. For this purpose, the bonding wire is guided through a capillary of the bonding tool and subjected to a high electrical voltage. This melts one end of the bonding wire at a tip of the capillary. Due to the surface tension of the molten metal, the ball portion 321 is preformed at the end of the bonding wire. The preformed ball portion 321 cools and at least partially solidifies. The preformed ball portion 321 is pressed against the interface 31 and attached thereto, e.g., by ultrasonic welding.In a second step, the capillary is lifted from the interface 31, while the bonding wire is guided further through the capillary. The bonding wire is then cut off. This creates the additional extension 322 on the spherical section 321.
[0150] In the Fig. 6C, the projection 32 is formed by a solid (metallic) object 323 that is attached to the interface 31. This ensures a projection 32 with a very precise shape. The solid object 323 may have a sharp tip (as in Fig. 6C). The solid object 323 is provided as a separate element (e.g., prefabricated) and then welded, bonded, and / or soldered to the interface 31. The solid object 323 can be attached, for example, by an ultrasonic welding process.
[0151] Another approach is in Fig. . In this case, the protrusion 32 is an adhesive dot 324. The adhesive dot 324 has a sharp point. To create the adhesive dot 324, a material can be applied to the interface 31 as a viscous liquid and then solidified. In one embodiment, the adhesive dot 324 is formed from hot-melt adhesive.
[0152] Fig. 6E shows another embodiment of the protrusion 32. In this case, the protrusion 32 is a sharp ridge 325. An exemplary sharp tool 326 for forming the ridge 325 is shown by a dashed line. The sharp tool 326 is pressed into the interface 31 of the fastening object 30, so that a small portion of the interface 31 is raised as a sharp protrusion 32. List of reference symbols: 10 Basic component 11 Mounting side 20 sintered layer 20a sintered layer 30 semiconductor power module (fixing object) 31 Interface 31a circumferential section 32 Stabilizers (Protrusion) 32a Residues (of stabilizing agents) 33 integrated heat distributor 34 Insulating layer 35 internal circuit layer 36 internal sintered layer 37 semiconductor component 38 Internal wiring 39 electrical connections 40 resin cover 50 (to be sintered) compilation 60 assembly 321 spherical section 322 appendages 323 fixed object 324 adhesive dots 325 ridge 326 tools N Normal direction S10 (Step of) Provision of stabilization funds S20 Sinter layer application step S30 Pre-drying step S40 Placement step S50 transfer step S60 Solidification step
Claims
[1] Method for sintering an interface (31) of a fastening object (30) to a fastening side (11) of a base component (10), comprising the following steps: • Applying a sintered layer (20) to the fastening side (11); • Providing stabilizing agents (32) on the interface (31); • Arranging the fastening object (30) directly on the sintered layer (20), wherein the interface (31) faces the sintered layer (20) and wherein the stabilizing means (32) protrude into the sintered layer (20) to stabilize a lateral position of the fastening object (30) relative to the base component (10), thereby forming an assembly (50) to be sintered; and • a solidification step (S60) for solidifying the sintered layer (20) in the assembly (50) to be sintered; characterized bythat the stabilizing means (32) are at least partially permanently compressed in the solidification step (S60). [2] Method according to one of the preceding claims, characterized by that the stabilizing means comprise at least one projection (32) projecting from the interface (31). [3] Method according to claim 2, characterized by that the stabilizing means have at least two projections (32) which project from the interface (31), wherein the at least two projections (32) are spaced apart from one another. [4] Method according to claim 3, characterized by that the stabilizing means comprise a plurality of projections (32) which protrude from the interface (31) and are arranged along an outer peripheral portion (31a) of the interface (31). [5] Method according to one of the preceding claims, characterized bythat at least part of the stabilizing means (32) is formed on the interface (31) by means of a wire bonder. [6] Method according to claim 5, characterized by that the stabilizing means (32) have at least one wire bond structure. [7] Method according to one of the preceding claims, characterized by the step of inserting the assembly (50) to be sintered into a pressure sintering tool, wherein the fastening object (30) is placed on the sintered layer (20) before the assembly (50) to be sintered is inserted into the pressure sintering tool. [8] Method according to one of the preceding claims, characterized by that the solidification step (S60) comprises sintering the sintered layer (20) with a maximum sintering temperature in the range of 200 °C and 300 °C and / or with a maximum sintering pressure in the range of 10 MPa to 40 MPa. [9] Method according to one of the preceding claims, characterized bythat the stabilizing means (32) consist of a different material than the interface (31). [10] Method according to one of the preceding claims, characterized by that the fastening object is or includes at least one of the following: - a heat-generating component (30, 35, 37, 38, 39); - an electronic component (30, 37); and - a semiconductor power module (30). [11] Method according to one of the preceding claims, characterized by that the base component (10) is a heat dissipator, a heat sink and / or a cooler. [12] Method according to one of the preceding claims, characterized by that the fastening side (11) of the base component (10) is made of metal and / or that the interface (31) is made of metal. [13] Assembly (60) with a base component (10) and a fastening object (30), wherein a sintered layer (20a) between an interface (31) of the fastening object (10) and a fastening side (11) of a base component (10) fixes the fastening object (30) to the base component (10), wherein the assembly (60) was formed by pressure sintering from an assembly (50) to be sintered, the latter comprising the base component (10), the fastening object (30) and a sintered layer (20) arranged between the fastening side (11) and the interface, as well as stabilizing means (32) formed at the interface (31) for stabilizing a lateral position of the fastening object (30) relative to the base component (10), wherein the stabilizing means in the assembly (50) to be sintered projected into the sintered layer (20) in order to stabilize the lateral position of the fastening object (30) relative to the base component (10), wherein the sintered layer (20) was converted into a sintered layer (20a) in a solidification step (S60), wherein in the assembly (60) the stabilizing means (32) formed at the interface (31) or at least residues (32a) of the stabilizing means (32) protrude into the sintered layer (20a), wherein the fastening object (10) is a semiconductor power module (30) and contains an integrated heat sink (33) which is arranged at the interface (31) of the fastening object (10), characterized by that a material of the stabilizing means (32) is softer than a material of the integrated heat dissipator (33) and than a material of the base component (10) on the fastening side (11) and that the stabilizing means (32) were at least partially permanently compressed in the solidification step (S60).
Citation Information
Patent Citations
Joined body
JP2020155497A
Packaged semiconductor devices and methods of their fabrication
US20150146399A1
Power module
US20160113107A1
Method for making a cohesive connection by fluxless chip- or element soldering, gluing or sintering using a material preform
WO2020182361A1