Aluminum nitride dipole doping film for adapting multi-v-devices
The implementation of an AlN dipole dopant film with an AlO hard mask addresses the challenge of adjusting threshold voltages in densely integrated semiconductor devices, enhancing efficiency and reducing nitrogen diffusion in high-k dielectric layers.
Patent Information
- Application Number
- DE102024100084
- Authority / Receiving Office
- DE · DE
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-07-03
- Filing Date
- 2024-01-03
- Publication Date
- 2024-10-02
AI Technical Summary
As semiconductor devices continue to reduce minimum element sizes for increased integration density, challenges arise in efficiently adjusting the threshold voltages of transistors, particularly due to the limitations of existing dopant films in high-k dielectric layers.
The use of an aluminum nitride (AlN) dipole dopant film with a lower binding energy, combined with an aluminum oxide (AlO) hard mask, is introduced to dope high-k dielectric layers in gate dielectrics, allowing for more efficient adjustment of threshold voltages in transistors through controlled diffusion of aluminum.
The AlN dipole dopant film provides enhanced efficiency in adjusting threshold voltages of transistors, reducing nitrogen diffusion into high-k dielectric layers and improving the matching of threshold voltages across different transistor types.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
Description PRIORITY CLAIM AND CROSS-REFERENCE
[0001] This application claims priority to U.S. Provisional Patent Application No. 63 / 493,008, filed on April 30, 2001. March 2023 entitled ´´AIN Dipole with Ex-Situ / In-Situ Al O Hardmask for Multi-Vt Device Offering´´, which was 2 3 Reference is incorporated into the present application.This text has been copied by the DPMA from the original sources. It does not contain any drawings. The tables and formulas may be of unsatisfactory quality. BACKGROUND
[0002] Semiconductor devices are used in a variety of electronic applications, such as personal computers, Mobile phones, digital cameras and other electronic devices. Semiconductor devices are typically by sequential deposition of insulating or dielectric layers, conductive layers and Semiconductor layers over a semiconductor substrate and structuring the different material layers using by lithography to form circuit components and elements thereon.
[0003] The semiconductor industry continues to improve the integration density of various electronic components (e.g. Transistors, diodes, resistors, capacitors, etc.) by continuously reducing the minimum element size, which allows more components to be integrated into a given area. If the minimum element sizes are reduced However, additional problems arise that should be addressed. BRIEF DESCRIPTION OF THE DRAWINGS
[0004] Aspects of the present disclosure are best understood from the following detailed description in in conjunction with the accompanying drawings. It should be noted that, in accordance with industry practice, various features are not shown to scale. In fact, the dimensions of the various Features may be arbitrarily enlarged or reduced for the sake of clarity. Figs. 1-4, 5A, 5B, 6A, 6B, 7A, 7B, 8A, 8B, 9A, 9B, 10A, 10B, 10C, 11A, 11B, 12A, 12B, 13A, 13B, 14-26, 27A, 27B, 28A, 28B, 29A, 29B, 30A and 30B illustrate the intermediate stages in the formation of gate all-around Transistors (GAA transistors) according to some embodiments. Figures 31-33 illustrate the tools for ex-situ and in-situ AlN and AlO film deposition processes according to some embodiments. Figures 34-39 illustrate the performance data of the transistors made using AlN dipole dopant films, compared to the transistors formed using AlO dipole dopant films are formed, according to some embodiments. Fig. 40 illustrates a chemical vapor deposition process (CVD process, Chemical Vapor Deposition process) with multiple pulses according to some embodiments. Fig. 41 schematically illustrates the adjustment of the threshold voltages of several transistors by Dipole dopant films having different thicknesses according to some embodiments. Figures 42-43 schematically illustrate two processes for forming multiple Vt devices (transistors) according to some embodiments. Fig. 44 illustrates a process flow for forming multiple Vt devices according to some Embodiments. DETAILED DESCRIPTIONThis text has been copied by the DPMA from the original sources. It does not contain any drawings. The tables and formulas may be of unsatisfactory quality.
[0005] The following disclosure provides many different embodiments or examples for implementing various features of the invention. Specific examples of components and arrangements are described below to simplify the present disclosure. These are, of course, only examples and are intended not be limiting. For example, the formation of a first element over or on a second element in the following description include embodiments in which the first and second elements are in direct contact are formed, and also include embodiments in which additional elements are formed between the first and the second element, so that the first and second elements may not be in direct In addition, the present disclosure may use reference numerals and / or letters in the various Repeat examples. This repetition is for simplicity and clarity and does not in itself indicate any relationship between the various embodiments and / or configurations discussed.
[0006] Furthermore, spatially related terms such as ´´underlying´´, ´´beneath´´, ´´lower´´, ´´overlying´´, ´´upper´´ and the like herein for a more convenient description to describe the relationship of one element or feature to another element(s) or feature(s), as illustrated in the figures, who uses The spatially related terms are intended to describe different orientations of the device in use or operation in addition to the orientation shown in the figures. The device can be rotated differently (90 degrees or with other orientations) and the spatially related descriptors used herein can therefore be interpreted equally.
[0007] A method for adjusting the threshold voltages of transistors is provided. According to some Embodiments of the present disclosure, an aluminum nitride dipole dopant film (AlN dipole dopant film) used to dope the high-k dielectric layers in the gate dielectrics of transistors. An aluminum oxide (AlO, which can be AlO) can be used as a hard mask. The AlN dipole dopant film has a 2 3 Binding energy (approximately 2.02 eV), which is lower than the binding energy (approximately 4.61 eV) of AlO dipole dopant films, is therefore more efficient in introducing an aluminum dipole into the high-k dielectric layers than the AlO dipole dopant films. It should be noted that although gate-all-around transistors (GAA transistors) used as an example, the concept of the present disclosure can be applied to other types of transistors such as planar transistors, fin field-effect transistors (FinFETs), complementary Field-effect transistors (CFETs, Complementary Field-Effect Transistors), and the like.
[0008] The embodiments discussed herein serve to provide examples for making or Use of the subject matter of this disclosure, and a person skilled in the art will readily understand modifications, which can be made without departing from the intended scope of various embodiments. In the different views and illustrative embodiments, like reference numerals are used to to refer to the same elements. Although the method embodiments can be discussed in such a way that they a specific order, other method embodiments can be carried out in any logical order. 1-4, 5A, 5B, 6A, 6B, 7A, 7B, 8A, 8B, 9A, 9B, 10A, 10B, 10C, 11A, 11B, 12A, 12B, 13A, 13B, 14-26, 27A, 27B, 28A, 28B, 29A, 29B, 30A and 30B illustrate the intermediate stages in the formation of GAA transistors according to some embodiments.
[0010] Referring to Fig. 1, a perspective view of a wafer 10 is shown. The wafer 10 has a Multilayer structure having a multilayer stack 22 on a substrate 20. According to some This text has been copied by the DPMA from the original sources. It does not contain any drawings. The tables and formulas may be of unsatisfactory quality. Embodiments, the substrate 20 is a semiconductor substrate, which may be a silicon substrate, a silicon germanium substrate (SiGe substrate) or the like, although other substrates and / or structures, such as semiconductor-on-insulator (SOI, Semiconductor-On-Insulator), strained SOI, silicon germanium on insulator, or the like can be used The substrate 20 may be doped as a p-type semiconductor, although in other embodiments it may be doped as an n- semiconductor can be doped.
[0011] According to some embodiments, the multilayer stack 22 is formed by a series of deposition processes for depositing alternating materials. The respective process is designated as process 202 in process flow 200 illustrated in Fig. 44. According to some embodiments, the multilayer stack 22 comprises first Layers 22A formed from a first semiconductor material and second layers 22B formed from a second semiconductor material that is different from the first semiconductor material.
[0012] According to some embodiments, the first semiconductor material of a first layer 22A is SiGe, Ge, Si, GaAs, InSb, GaSb, InAlAs, InGaAs, GaSbP, GaAsSb or the like. According to some Embodiments, the deposition of the first layers 22A (for example SiGe) is carried out by epitaxial growth, and The corresponding deposition process can be vapor phase epitaxy (VPE), molecular beam epitaxy (MBE, Molecular Beam Epitaxy), chemical vapor deposition (CVD), low-pressure CVD (LPCVD, Low Pressure CVD), Atomic Layer Deposition (ALD), Ultra-high Vacuum CVD (UHVCVD, Ultra High Vacuum CVD), reduced pressure CVD (RPCVD, Reduced Pressure CVD) or the like. According to some embodiments, the first layer 22A is formed with a first thickness in the range of between approximately 30Å and approximately 300Å. However, any suitable thickness may be used without affecting the scope of the Embodiments to leave.
[0013] After the first layer 22A has been deposited over the substrate 20, a second layer 22B is deposited over the first layer 22A. According to some embodiments, the second layers 22B are made of a second Semiconductor material such as Si, SiGe, Ge, GaAs, InSb, GaSb, InAlAs, InGaAs, GaSbP, GaAsSb, combinations of these, or the like, wherein the second semiconductor material from the first semiconductor material of the first layer 22A. For example, according to some Embodiments in which the first layer 22A is silicon germanium, the second layer 22B is formed of silicon or vice versa. It should be noted that any suitable combination of materials for the first Layers 22A and the second layers 22B can be used.
[0014] According to some embodiments, the second layer 22B is epitaxially grown on the first layer 22A under using a deposition technique similar to that used to form the first layer 22A. According to some embodiments, the second layer 22B is formed with a similar thickness to that of the first Layer 22A is formed. The second layer 22B may also be formed with a thickness that differs from the first layer 22A. According to some embodiments, the second layer 22B may, for example, have a second thickness in range of between approximately 10Å and approximately 500Å.
[0015] After the second layer 22B has been formed over the first layer 22A, the deposition process repeated to form the remaining layers in the multilayer stack 22 until a desired top layer of the multilayer stack 22. According to some embodiments, the first layers 22A have thicknesses which are the same or similar to each other, and the second layers 22B have thicknesses which are are the same or similar. The first layers 22A may also have the same thicknesses as or different thicknesses than those of the second layers 22B. According to some embodiments, the first layers 22A are formed in the This text has been copied by the DPMA from the original sources. It does not contain any drawings. The tables and formulas may be of unsatisfactory quality. subsequent processes and are alternatively referred to as sacrificial layers 22A throughout the description. According to alternative embodiments, the second layers 22B are sacrificial layers and are described in the following processes removed.
[0016] According to some embodiments, some pad oxide layer(s) and hard mask layer(s) (not shown) formed over the multilayer stack 22. These layers are structured and are used for the subsequent Structuring of the multilayer stack 22.
[0017] Referring to Fig. 2, the multilayer stack 22 and a portion of the underlying substrate 20 is structured in (an) etching process(es) so that trenches 23 are formed. The respective process is designated as process 204 in the process flow 200 shown in Fig. 44. The trenches 23 extend into the substrate 20. The remaining sections of the multilayer stacks are referred to below as multilayer stacks 22'. Multilayer stacks 22', some sections of the substrate 20 are left and are referred to below as substrate strips 20' The multilayer stacks 22' comprise semiconductor layers 22A and 22B. The following are the Semiconductor layers 22A are alternatively referred to as sacrificial layers and the semiconductor layers 22B are alternatively referred to as Nanostructures. The sections of the multilayer stacks 22' and the underlying substrate strips 20' are collectively referred to as semiconductor strips 24.
[0018] In the previously illustrated embodiments, the GAA transistor structures may be implemented by any suitable method. For example, the structures can be structured using one or more Photolithography processes including double patterning or multiple patterning processes. In general, double patterning or multi-patterning processes combine photolithography and self-aligned processes, which makes it possible to create structures that, for example, have distances smaller than what can otherwise be obtained using a single direct photolithography process. For example, in one embodiment, a sacrificial layer is formed over a substrate and using a photolithography process. Spacers are patterned along the patterned sacrificial layer using a self-aligned process. The sacrificial layer is then removed, and the remaining spacers can then be used to structure the GAA structure.
[0019] Fig. 3 illustrates the formation of isolation regions 26, which are also referred to as Shallow Trench Isolation Regions (STI regions). The respective process is as process 206 in the process flow 200 shown in Fig. 44. The STI areas 26 may be a lining oxide (not shown), which may be a thermal oxide formed by the thermal oxidation a surface layer of the substrate 20. The lining oxide may also be a deposited Silicon oxide layer, which can be deposited using for example ALD, chemical vapor deposition with high density Plasma (HDPCVD, High-Density Plasma Chemical Vapor Deposition), CVD, or the like. The STI areas 26 may also comprise a dielectric material over the lining oxide, wherein the dielectric material is Use of flowable chemical Flowable Chemical Vapor Deposition (FCVD), spin coating, HDPCVD or similar A planarization process, such as a chemical mechanical polishing (CMP) process or a mechanical grinding process can then be carried out to prepare the upper surface of the dielectric material flatten, and the remaining sections of the dielectric material are STI regions 26.
[0020] The STI regions 26 are then recessed so that the upper sections of the semiconductor strips 24 are higher than the upper surfaces 26T of the remaining portions of the STI regions 26 protrude to form protruding fins 28. This text has been copied by the DPMA from the original sources. It does not contain any drawings. The tables and formulas may be of unsatisfactory quality. The multilayer stacks 22' and the upper sections of the substrate strips 20' have protruding fins 28. The Recessing of the STI areas 26 can be carried out by a dry etching process, for example, NF and NH 3 3 used as etching gases. Plasma can be generated during the etching process. Argon may also be present. According to alternative embodiments of the present disclosure, the recessing of the STI regions 26 is achieved by a A wet etching process is performed. The etching chemical can include, for example, HF.
[0021] Referring to Fig. 4, dummy gate stacks 30 and gate spacers 38 are provided on the top surfaces and the side walls of (protruding) fins 28. The respective process is designated as process 208 in the process flow 200 shown in Fig. 44. The dummy gate stacks 30 may include dummy gate dielectrics 32 and dummy Gate electrodes 34 over the dummy gate dielectrics 32. The dummy gate dielectrics 32 can be Oxidizing the surface portions of the projecting fins 28 to form oxide layers, or by Deposition of a dielectric layer, such as a silicon oxide layer. The dummy gate electrodes 34 can be formed, for example, using polysilicon or amorphous silicon, and it can also other materials, such as amorphous carbon, can be used.
[0022] Each of the dummy gate stacks 30 may also include one (or a plurality of) hard mask layers 36 over the dummy Gate electrode 34. The hard mask layers 36 may be made of silicon nitride, silicon oxide, silicon carbonitride, Silicon oxycarbonitride or multilayers thereof. The dummy gate stacks 30 may be a single or a plurality of projecting fins 28 and the STI areas 26 between the projecting fins 28. The Dummy gate stacks 30 also have longitudinal directions perpendicular to the longitudinal directions of the protruding fins 28. Forming the dummy gate stacks 30 includes forming a dummy gate dielectric layer, depositing a Dummy gate electrode layer over the dummy gate dielectric layer, depositing one or more Hard mask layers, and then patterning the formed layers by patterning process(es).
[0023] Next, gate spacers 38 are formed on the sidewalls of the dummy gate stacks 30. According to In some embodiments of the present disclosure, gate spacers 38 are made of a dielectric material, such as silicon nitride (SiN), silicon oxide (SiO ), silicon carbonitride (SiCN), silicon oxynitride (SiON), silicon oxycarbonitride 2 (SiOCN), or the like and may have a single layer structure or a multi-layer structure including a plurality of dielectric layers. The formation process of the gate spacers 38 may Depositing one or more dielectric layers, and then performing an anisotropic / anisotropic etching process(es) on the dielectric layer(s). The remaining sections of the Dielectric layer(s) are gate spacers 38.
[0024] Figures 5A and 5B illustrate the cross-sectional views of the structure shown in Figure 4. Figure 5A illustrates the reference cross-section A1-A1 in Fig. 4, which cross-section shows the sections of the projecting fins 28 which are not covered by gate stacks 30 and gate spacers 38, and perpendicular to the gate length direction. Fin spacers 38, which are located on the side walls of the projecting fins 28, are Fig. 5B illustrates the reference cross-section BB in Fig. 4, where this reference cross-section parallel to the longitudinal directions of the projecting fins 28. Fin spacers 39 are also illustrated.
[0025] Referring to Fig. 6A and Fig. 6B, the portions of the projecting fins 28 which are not directly under the dummy gate stacks 30 and the gate spacers 38 are recessed by an etching process in order to Recesses 42. The respective process is illustrated as process 210 in the process flow 200 shown in Fig. 44 For example, a dry etching process using CF , CF , SO , the mixture of HBr, Cl and 2 6 4 2 2This text has been copied by the DPMA from the original sources. It does not contain any drawings. The tables and formulas may be of unsatisfactory quality. O , the mixture of HBr, Cl , O and CH F , or the like to form multilayer semiconductor stack 22' 2 2 2 2 2 and the underlying substrate strips 20'. The undersides of the recesses 42 lie at least on the same height as or may be lower (as shown in Fig. 6B) than the sub sides of the multilayer semiconductor stack 22'. The etching may be anisotropic, so that the side walls of the multilayer Semiconductor stacks 22' opposite the recesses 42 are vertical and straight, as shown in Fig. 6B.
[0026] Referring to Fig. 7A and Fig. 7B, sacrificial semiconductor layers 22A are laterally recessed to to form lateral recesses 41, which extend from the edges of the respective overlying and underlying Nanostructures 22B are left out. The respective process is illustrated as process 212 in the process flow 200, which shown in Fig. 44. The lateral recessing of the sacrificial semiconductor layers 22A can be achieved by a wet etching process under Using an etchant that is more selective with respect to the material (for example, silicon germanium (SiGe)) of the sacrificial semiconductor layers 22A is the material (for example (Si)) of the nanostructures 22B and the substrate 20. For example, in an embodiment in which the sacrificial semiconductor layers 22A are formed from silicon germanium and the nanostructures 22B are formed of silicon, the wet etching process can be carried out using an etchant, such as hydrochloric acid (HCl). The wet etching process can be carried out using a immersion process, a spraying process or the like and can be carried out using any suitable process temperatures (for example, between approximately 400°C and approximately 600°C) and a suitable Process time (for example, between approximately 100 seconds and approximately 1,000 seconds). According to In alternative embodiments, the lateral recessing of the sacrificial semiconductor layers 22A is achieved by an isotropic Dry etching process or a combination of a dry etching process and a wet etching process.
[0027] Figures 8A and 8B illustrate the formation of inner spacers 44. The respective process is described as Process 214 in the process flow 200 shown in Fig. 44. The formation process includes the Depositing a spacer layer extending into the recesses 41 and performing a Etching process to remove the portions of the inner spacer layer outside the recesses 41, thereby inner spacers 44 are left in the recesses 41. The inner spacers 44 can be made of SiOCN, SiON, SiOC, SiCN, or the like. The inner spacers 44 may also porous, so that they have a lower k value, for example, less than about 3.5. According to In some embodiments, the etching of the spacer layer may be performed by a wet etching process, in which the etching chemical H SO , dilute HF, ammonia solution (NH OH, ammonia in water) or the like 2 4 4 or combinations thereof.
[0028] Referring to Fig. 9A and Fig. 9B, epitaxial source / drain regions 48 are formed in the recesses 42 The respective process is illustrated as process 216 in the process flow 200 shown in Fig. 44. According to some embodiments, the source / drain regions 48 may apply a voltage to the nanostructures 22B which are used as the channels of the corresponding GAA transistors, thereby improving the performance According to some embodiments, the corresponding transistor is n-type and the epitaxial source / drain Regions 48 are accordingly formed by doping with an n-type dopant. For example, silicon phosphorus (SiP), silicon carbon phosphorus (SiCP) or the like to form the epitaxial source / drain regions 48 After the recesses 42 are filled with the epitaxial regions 48, further epitaxial growth of the Epitaxial regions 48, that the epitaxial regions 48 extend horizontally, and facets can be formed. The Further growth of the epitaxial regions 48 may also cause adjacent epitaxial regions 48 to bond together merge.This text has been copied by the DPMA from the original sources. It does not contain any drawings. The tables and formulas may be of unsatisfactory quality.
[0029] Figures 10A, 10B and 10C illustrate the cross-sectional views of the structure after formation a contact etch stop layer (CESL) 50 and an inter-layer dielectric (ILD) Dielectric) 52. Fig. 10A, Fig. 10B and Fig. 10C are each prepared using the same cross-section as the cross-sections A2- A2, BB and A1-A1 in Fig. 4. The respective process is illustrated as process 218 in the process flow 200, which shown in Fig. 44. The CESL 50 may be formed of silicon oxide, silicon nitride, silicon carbonitride or the like and may be formed using CVD, ALD, or the like. The ILD 52 may comprise a dielectric material which may be produced using, for example, FCVD, spin coating, CVD or any other suitable deposition process. The ILD 52 may be made of an oxygen-containing dielectric material which can be a silicon oxide-based material prepared using tetraethylorthosilicate (TEOS) as precursor, phosphosilicate glass (PSG), borosilicate glass (BSG), boron-doped phosphosilicate glass (BPSG), undoped Silicate glass (USG) or the like.
[0030] In the subsequent processes, replacement gate stacks are formed to replace the dummy gate stacks 30. With reference to the Fig. 11A and Fig. 11B, a planarization process, such as a CMP process or a mechanical grinding process, performed to level the upper surface of the ILD 52. The respective process is designated as process 220 in the process flow 200 shown in Fig. 44. According to some embodiments, the planarization process may Remove hard masks 36 to expose the dummy gate electrodes 34, as shown in Fig. 11B. According to alternative Embodiments, the planarization process may expose the hard masks 36 and stops thereon. According to some Embodiments, after the planarization process, the upper surfaces of the dummy gate electrodes 34 (or the hard masks 36), the gate spacer 38 and the ILD 52 within process variations on the same Height.
[0031] Next, the dummy gate electrodes 34 (and the hard masks 36, if they remain) are deposited in one or several etching processes, so that recesses 58 are formed, as shown in Fig. 12A and Fig. 12B. The The respective process is illustrated as process 222 in the process flow 200 shown in Fig. 44. The sections of the Dummy gate dielectrics 32 in the recesses 58 are also removed. According to some embodiments, the dummy gate electrodes 34 and the dummy gate dielectrics 32 are removed by dry etching processes. For example, the etching process is carried out using (a) reaction gas(es) that the dummy gate electrodes 34 selectively etch at a faster rate than the ILD 52. Each recess 58 exposes portions of the multilayer stacks 22' and / or lies above those that comprise the future channel regions in subsequently completed Nano-FETs. corresponding sections of the multilayer stacks 22' are located between adjacent pairs of the epitaxial source / Drain areas 48.
[0032] Sacrificial layers 22A are then removed so that the recesses 58 between the nanostructures 22B are widened and the resulting structure is shown in Fig. 13A and Fig. 13B. The respective process is designated as process 224 in the process flow 200 shown in Fig. 44. The sacrificial layers 22A can be formed by performing a isotropic etching process, such as a wet etching process, using etchants that are selective with respect to the Materials of the sacrificial layers 22A are removed. The nanostructures 22B, the substrate 20, the STI regions 26 remain relatively unetched compared to the sacrificial layers 22A. According to some embodiments in which the Sacrificial layers 22A comprise, for example, SiGe and the nanostructures 22B comprise, for example, Si or SiC, Tetramethylammonium hydroxide (TMAH), ammonium hydroxide (NH OH) or the like can be used to 4 To remove sacrificial layers 22A.This text has been copied by the DPMA from the original sources. It does not contain any drawings. The tables and formulas may be of unsatisfactory quality.
[0033] The preceding processes can be used to form multiple GAA transistors. In the In the following discussion, three device regions are illustrated, each of which is dedicated to forming a transistor therein For example, Fig. 14 illustrates three device areas 59-1, 59-2 and 59-3, and the Structures are formed using the processes discussed in the previous paragraphs. Each of the Device regions 59-1, 59-2 and 59-3 may be an n-type transistor region or a p-type transistor region in any combination. In the examples discussed below, it is assumed for the sake of simplicity that the device regions 59-1, 59-2 and 59-3 are all p-transistor regions.
[0034] Referring to Fig. 14, gate dielectrics 62 are formed. The respective process is described as process 226 in the Process flow 200 shown in Fig. 44. According to some embodiments, each of the gate Dielectrics 62 have an interface layer 62A and a high-k dielectric layer 62B on the interface layer 62A. The interface layer 62A may be formed of or comprise silicon oxide formed by a conformal deposition process, such as ALD or CVD. According to alternative embodiments, the interface layer 62A is formed by thermal oxidation. When formed by thermal oxidation, the Portions of the interface layer 62A are not formed on the upper surfaces of the STI regions 26. According to some In some embodiments, the high-k dielectric layers 62B comprise one or more dielectric layers. For example, the high-k dielectric layer(s) 62B may comprise a metal oxide or a silicate of hafnium, aluminum, Zirconium, lanthanum, manganese, barium, titanium, lead, combinations thereof and / or multilayers thereof.
[0035] Further referring to Fig. 14, a dipole dopant film 64 is formed on the gate dielectric 62 by a conformal deposition process, such as CVD, ALD or the like. The respective process is known as Process 228 in the process flow 200 shown in Fig. 44. The dipole dopant film 64 may have a p- dopant which, when incorporated into the gate dielectrics of p-type transistors, reduces the effective can increase the work function and thus reduce the threshold voltages of the corresponding p-type transistors. incorporated into the gate dielectrics of n-type transistors, the p-type dopant can reduce the effective exit area and thus increase the threshold voltages of the corresponding n-type transistors. According to some In some embodiments, the p-dopant may comprise aluminum (Al), zinc (Zn), and / or the like. According to some In other embodiments, the dipole dopant film 64 may comprise an n-type dopant such as La, Sr, Y, Er, Sc, Mg, or the like or combinations thereof. The effect of the n-dipole dopant on the effective work function and the threshold voltages of the n- and p-transistors are opposite to that of the p-dipole dopant.
[0036] According to some embodiments, when the dipole dopant film 64 comprises aluminum as a p-type dipole dopant the aluminum may be in the form of a compound such as aluminum nitride (as deposited). The thickness T1 of the dipole dopant film 64 may range between about 5 Å and about 20 Å.
[0037] The hard mask 66 can be conformally deposited on the dipole dopant film 64. The respective process is as process 230 in the process flow 200 shown in Fig. 44. According to some embodiments The hard mask 66 comprises aluminum oxide (AlO, which may include AlO). The hard mask 66 may be formed by a 2 3 conformal deposition process, such as CVD, ALD, or the like. The thickness T2 of the Hard mask 66 may be in the range of between about 5Å and about 30Å. The thickness T2 may also be smaller than the Thickness T1, so that the dipole dopant films 64 on the adjacent nanostructures 22B are merged Although Fig. 14 and the following Figs. 18 and 24-26 illustrate that the dipole dopant films 64 on the neighboring nanostructures 22B are separated from each other, they can also fuse together. This It is also desirable to increase the amount of diffused dipole dopant into the high-k dielectric layers 62B. This text has been copied by the DPMA from the original sources. It does not contain any drawings. The tables and formulas may be of unsatisfactory quality. The total thickness T1+T2 of the dipole dopant film 64 and the hard mask 66 can be in the range of between approximately 10 Å and approximately 35 Å.
[0038] The hard mask 66 may have one or both of the following functions. It may be used as a hard mask for etching the dipole dopant film 64. It can also help to reduce nitrogen in the subsequent dipole drive-in process so that the nitrogen in the dipole dopant film 64 does not adversely affect the underlying high-k dielectric layers 62B. In addition, the formation of the hard mask 66, which comprises aluminum oxide, convert at least a part of the dipole dopant film 64 into AlON, and the oxygen in the dipole dopant film 64 also has the function of capturing nitrogen and preventing the nitrogen atoms from entering the underlying High-k dielectric layers 62B diffuse onto.
[0039] The dipole dopant film 64 and the hard mask 66 can be formed by an ex-situ process or an in-situ process According to some embodiments, the dipole dopant film 64 and the hard mask 66 are formed by a Ex-situ process using the tools shown in Fig. 31 and Fig. 32. With reference to Fig. 31 provides an example deposition tool 102 for depositing the dipole dopant film 64 (AlN). The deposition tool 102 has lock chambers 104 for loading wafers, a buffer 106 for transporting of wafers and a plurality of deposition chambers 108, each for depositing the dipole dopant film 64 on a wafer. The deposition tool 102 may be a CVD chamber, an ALD chamber or the like.
[0040] After the dipole dopant film 64 is deposited in the deposition tool 102, the corresponding Wafer is removed from the deposition tool 102 by a vacuum interruption process and exposed to air. Consequently, the oxygen and moisture in the air can oxidize the dipole dopant film 64. When the dipole Dopant film 64 AlN, either the outer surface part or the entirety of the dipole dopant film 64 oxidized to form AlON. The inner part of the dipole dopant film 64 can be oxidized to form AlON, or can remain as AlN.
[0041] Fig. 32 illustrates the deposition tool 112 for depositing the hard mask 66 (which, for example, AlO). The deposition tool 112 has lock chambers 114 for loading wafers, a buffer 116 for transporting wafers and a plurality of deposition chambers 118, each for depositing the Hard mask 66 can be used. Since the deposition of AlO requires an oxygen-containing gas or a water-containing gas, the dipole dopant film 64 can be oxidized, for example, to form AlON. If the dipole Dopant film 64 AlN, either the outer surface part or the entirety of the dipole dopant film 64 oxidized to form AlON. The inner part of the dipole dopant film 64 can be oxidized to form AlON, or can remain as AlN.
[0042] According to alternative embodiments, instead of performing the ex-situ deposition processes of Dipole dopant film 64 and the hard mask 66 by an in-situ deposition The in-situ deposition process can be carried out using a tool 122, as shown in Fig. 33 shown. The deposition tool 122 may include lock chambers 124 for loading wafers, a Buffer 126 for transporting wafers, a plurality of deposition chambers 128A, each for depositing of the dipole dopant film 64, and a plurality of deposition chambers 128B, each for depositing a hard mask 66, such as AlO.
[0043] In the in-situ deposition process, the dipole dopant film 64 is first deposited in one of the deposition chambers 128A, followed by the deposition of the hard mask 66 in one of the deposition chambers 128B. This text has been copied by the DPMA from the original sources. It does not contain any drawings. The tables and formulas may be of unsatisfactory quality. Vacuum interruption between the deposition of the dipole dopant film 64 and its overlying hard mask 66 Since the deposition of AlO involves an oxygen-containing gas or a hydrogen-containing gas, the Dipole dopant film 64, for example, is oxidized to form AlON. If the dipole dopant film 64 contains AlN, either the outer surface part or the entirety of the dipole dopant film 64 is oxidized to form AlON. inner part of the dipole dopant film 64 may be oxidized to form AlON or may remain as AlN.
[0044] Fig. 40 illustrates an exemplary process for depositing the dipole dopant film 64 containing AlN according to some embodiments. The deposition may be performed using multi-pulse CVD be performed, although other processes such as single-pulse CVD, ALD, or the like may be used The deposition can be carried out using a nitrogen-containing precursor and an aluminum-containing precursor. The nitrogen-containing precursor may include NH , N / H , hydrazine (NH ) and / or the like. 3 2 2 2 4 The aluminum-containing precursor can be aluminum trichloride (AlCl ), trimethylaluminum (TMA), triethylaluminum (TEA) and 3 Tri-tert-butyl-aluminum (TTBA) and / or the like.
[0045] In multi-pulse CVD, the plasma is switched off. As shown in Fig. 40, the deposition of AlN may comprise one or a plurality of pulsation cycles of the nitrogen-containing precursor (such as NH ). In each 3 Pulsation cycle of the nitrogenous precursor, the nitrogenous precursor is executed. During a pulsation period of the nitrogen-containing precursor are a plurality of pulsation cycles of the aluminum-containing precursor (such as AlCl ) 3 present, with each cycle switching on and then switching off the flow of the aluminum-containing precursor includes.
[0046] Multi-pulse CVD can help to remove the by-products formed during the deposition of AlN are produced, whereby the by-products can have a detrimental effect on the subsequent processes and the spaces between the nanostructures 22B and can adversely prevent AlN from entering the spaces The by-products may include HCl, NH , NH or the like. By adjusting the 2 3 The ratio of the pulsation length of the nitrogen-containing precursor to the pulsation length of the aluminum-containing precursor can Atomic percentage ratio of N / Al can be adjusted. For example, a longer pulsation of the nitrogen-containing precursor can increase the atomic percentage ratio N / Al and a longer pulsation of the aluminum-containing precursor can Reduce the atomic percentage ratio N / Al.
[0047] The deposition of AlO can be carried out using an aluminum-containing precursor which consists of the same group of candidate precursors for depositing AlN and an oxygen-containing precursor, such as O , O , HO and / or the like. The deposition process can be ALD, CVD 2 3 2 or the like.
[0048] Referring again to Fig. 14, a patterned etch mask 68 is formed. According to some Embodiments, the structured etching mask 68 comprises a lower layer 68BL, a middle layer 68ML and an upper layer (not shown). The top layer may comprise a patterned photoresist and is used to middle layer 68ML and the lower layer 68BL, thereby forming the patterned etching mask 68, as shown in Fig. 14. The etching mask 68 has a portion in the device area 59-1, and the portions of the Etching mask 68 in device areas 59-2 and 59-3 are removed.
[0049] Referring to Fig. 15, an etching / structuring process(es) is / are performed to form the sections the hard mask 66 and the dipole dopant film 64. The respective process is referred to as process 232 in the process flow 200, which is shown in Fig. 44. During etching, the middle layer 68ML can be consumed and is thus not shown in Fig. 15. According to some embodiments, as shown in Fig. 15, both the hard mask 66 This text has been copied by the DPMA from the original sources. It does not contain any drawings. The tables and formulas may be of unsatisfactory quality. as well as the dipole dopant film 64 are etched using the patterned etch mask 68 to define structures. The remaining etch mask 68 is then removed. According to alternative embodiments, the patterned etch mask 68 used to make the Hart mask 66 and is then removed to expose the hard mask 66. The patterned hard mask 66 is then used as the etching mask is used to etch the dipole dopant film 64.
[0050] Fig. 16 illustrates the driving-in process 70 by means of a tempering process. The respective process is referred to as process 234 in the process flow 200 shown in Fig. 44. The driving process 70 can be carried out in a process gas, such as N , He, NH , Ar or the like, or the mixture thereof. According to some 2 3 Embodiments, the driving process 70 is performed by a soaking annealing process, a rapid thermal spike tempering process or the like. If the soaking tempering process is adopted, the tempering time in the range of between approximately 5 seconds and approximately 5 minutes. The annealing temperature can be in the range of between approximately 550°C and approximately 900°C.
[0051] The drive-in process 70 drives the dipole dopant (such as aluminum) into the dipole dopant films 64 into the respective underlying high-k dielectric layers 62B in the device region 59-1. The threshold voltage of the resulting transistor is thus adjusted, for example reduced for a p-transistor and increased for an n- transistor. The use of AlN leads to an improved diffusion rate of Al into the high-k Dielectric layer 62B. For example, Figures 34 to 39 illustrate some results that demonstrate the use of AlN as the dipole dopant film with the use of AlO as the dipole dopant film.
[0052] Fig. 34 illustrates the results of X-ray photoemission spectroscopy (XPS, X-ray Photoemission Spectroscopy) obtained from AlN and AlO, where the count per second (CPS) of the Aluminium signal in high-k dielectric layers (after the drive-in process) as a function of binding energy Line 130A is the result obtained using AlN, while line 130B is the result obtained obtained using AlO. The results reveal that AlN has a lower binding energy than AlO. Accordingly, it is easier to break the Al-N bonds in AlN during the driving-in process than the Al-O bonds in AlO to break. Therefore, if an AlN layer and an AlO layer of the same thickness are used for dipole doping the high-k dielectric layer under the AlN layer will have more doped aluminum atoms than the high-k Dielectric layer under the AlO layer.
[0053] Fig. 35 illustrates the XPS results obtained on AlN and AlO, where the CPS of the Nitrogen signal in the high-k dielectric layers (after the drive-in process) as a function of the binding energy Line 132A is the result obtained using AlN, while line 132B is the result obtained obtained from AlO. Line 132A essentially overlaps line 132B. The results reveal that, Although AlN has more N than AlO, essentially the same amount of N is transferred into the underlying high-k dielectric layers, regardless of whether AlN or AlO is used. Since nitrogen is the high-k dielectric layers is undesirable due to its performance degradation, a lower Nitrogen uptake into the high-k dielectric layers is desirable. This result can be derived from the oxygen in the AlON (the oxidized dipole dopant film), where the oxygen captures the nitrogen atoms so that they do not diffuse into the high-k dielectric layers.
[0054] Fig. 36 illustrates the shift of the flat band voltages of AlN and AlO in p-type transistors as a Function of the capacitance equivalent thickness (ΔCET). This graph shows how the thickness change in the dipole Dopant film 64 affects the change in the threshold voltages of the p-type transistors. It shows that when AlO This text has been copied by the DPMA from the original sources. It does not contain any drawings. The tables and formulas may be of unsatisfactory quality. used, an AlO dipole film with a thickness of approximately 32.5 Å (point 134B) is needed to achieve a shift of approximately 95 mV in the flat band voltage. On the other hand, if AlN is used, the thicknesses of the AlN dipole dopant films are 6 Å, 10 Å and 30 Å (points 134A) to achieve the shift of approximately 80 mV, 100 mV and approximately 105 mV in the flat band voltages. This indicates that the AlN in the Adjusting the threshold voltages of the p-transistors is much more effective.
[0055] Fig. 37 illustrates the shift of the flat band voltages of AlN and AlO as a function of ΔCET. Fig. 37 is similar to Fig. 36 except that Fig. 37 shows the results obtained using n-type transistors This graph shows how the thickness change in the dipole dopant film 64 affects the change in the threshold voltages of the n-type transistors. It shows that when AlO is used, an AlO dipole film with a thickness of approximately 32.5 Å (point 136B) is needed to produce a shift of approximately 16 mV in the flat band voltage. On the other hand, if AlN is used, the thicknesses of the AlN dipole dopant films would be 6 Å, 10 Å and 30 Å (points 136A) to respectively account for the shift of approximately 15 mV, 27 mV and approximately 31 mV in the Flat band voltages to This indicates that AlN is also much more effective in adjusting the threshold voltages of the n- transistors.
[0056] Fig. 38 illustrates the comparison of the shift of the flat band voltages of AlN in p-type transistors with the shift of the flat band voltages of AlN in n-type transistors. Fig. 38 shows that when AlO is used (point 138B), the ratio of the shift in the flat band voltage (which affects the threshold voltage in the n-type transistor to the shift in the flat band voltages in the p-type transistors is approximately 0.18 When AlN is used (points 138A), the ratio of the displacement in the flat band tension in the n-transistor to the shift in the flat-band voltages in the p-transistors (points 138A) is approximately 0.28. This indicates that AlN is better than AlO because when AlN is used, the adjustment of the threshold voltages of the n-type transistors is closer to matching the threshold voltages of the p-type transistors (although they are still smaller than this).
[0057] Fig. 39 illustrates the comparison of the shift of flat band stresses of AlN and AlO under Use of ex-situ deposition with the shift of flat band voltages of AlN and AlO using of in-situ deposition. The points 140A1 are obtained when AlN and AlO are deposited in-situ, and the Points 140A2 are obtained when AlN and AlO are deposited ex-situ. Point 140B is obtained when AlO used alone as the dipole film. The results indicate that the ex-situ deposition and the in-situ deposition show similar results, with ex-situ deposition showing a slightly higher shift of flat band voltages has.
[0058] After driving in the dipole dopant, the hard mask 66 and the dipole dopant film 64, as shown in Fig. 16 shown, removed in etching processes, and the resulting structure is shown in Fig. 17. The respective process is known as process 236 in the process flow 200 shown in Fig. 44. The processes shown in Figs. 14 to 17 are collectively referred to as the first dipole dopant uptake process.
[0059] Figures 18 to 21 illustrate a second dipole dopant uptake process according to some Embodiments. The processes, structures and materials in the second dipole dopant uptake process are described in Essentially the same as those used in the dipole dopant uptake process, with the exception that in this process the dipole dopant is introduced into the high-k dielectric layers 62B in both device regions 59-1 and 59-2 instead of the device region 59-1 alone. Accordingly, more dipole dopants are doped into the This text has been copied by the DPMA from the original sources. It does not contain any drawings. The tables and formulas may be of unsatisfactory quality. High-k dielectric layers 62B in the device region 59-1 are doped, and thus the adaptation of the Work function and threshold voltages of the transistor in the device region 59-1 and is larger than the Adjusting the work function and threshold voltages of the transistor in the device region 59-2. The processes are briefly discussed here, and the details can be found in the discussion of the processes shown in Figures 14-17.
[0060] Fig. 18 illustrates the deposition of the dipole dopant film 64' and the hard mask 66' and the formation of the Etching mask 68', which has the lower layer 68BL' and 68ML'. The respective process is shown as processes 238 and 240 in the process flow 200 shown in Fig. 44. The etching mask 68' covers the sections of the dipole dopant film 64' and the hard mask 66' in the device regions 59-1 and 59-2 and leaves the device region 59-3 open.
[0061] As shown in Fig. 19, the dipole dopant film 64' and the hard mask 66' are next patterned and their sections in the device area 59-3 are removed in an etching process. The respective process is known as process 242 in the process flow 200 shown in Fig. 44. The etching mask 68', if one remains, can be removed The hard mask 66' can also be removed. As shown in Fig. 20, the drive-in process 70' carried out to introduce the dipole dopant into the sections of the high-k dielectric layers 62B in both Device areas 59-1 and 59-2. The respective process is designated as process 244 in the process flow 200 illustrated in Fig. 44. The details of the driving process 70' may be substantially the same as those of the collection process 70.
[0062] Since the portion of the high-k dielectric layer 62B in the device region 59-1 already has the Dipole dopant is added in the first dipole dopant uptake process, the concentration of the Dipole dopant in the device region 59-1 is increased more than that in the device region 59-2. In the Device region 59-3, no dipole dopant is introduced into the corresponding portion of the high-k dielectric layer 62B doped. After the drive-in process 70', the dipole dopant film 64' and the hard mask 66' are etched in (an) etching process(es) removed. The respective process is illustrated as process 246 in the process flow 200 shown in Fig. 44. The The resulting structure is shown in Fig. 21.
[0063] Figures 22 to 24 illustrate the dipole dopant uptake processes according to alternative embodiments. Embodiments are similar to the embodiments in Figs. 14 to 21 with the exception that instead of the Driving in dipole dopants after deposition of each dipole dopant film and then removing the dipole dopant film, the drive-in process is carried out after all dipole dopant films have been deposited, and all Dipole dopant films are removed in the same removal process.
[0064] Fig. 22 illustrates the formation of the dipole dopant film 64 and the formation of the etching mask 68 (including the lower layer 68BL and the middle layer 68ML) according to some embodiments. The hard mask is not formed at this time. Next, the dipole dopant film 64 is patterned as shown in Fig. 23. The Etching mask 68 is removed.
[0065] Fig. 24 illustrates the deposition of the dipole dopant film 64' and the hard mask 66. The etching mask 68' is then formed to cover the device regions 59-1 and 59-2. A patterning process is then performed to etch the portions of the dipole dopant film 64' in the device region 59-3, followed by the Removal of the remaining etching mask 68'. The resulting structure is shown in Fig. 25.This text has been copied by the DPMA from the original sources. It does not contain any drawings. The tables and formulas may be of unsatisfactory quality.
[0066] Fig. 26 illustrates the drive-in process 70 for driving the dipole dopant into the dipole films 64' and 64 in the sections of the high-k dielectric layer 62B in the device regions 59-1 and 59-2. The thicker dipole Dopant films 64 and 64' in the device region 59-1 have a total thickness greater than the thickness of the dipole dopant film 64' in the device region 59-2. The concentration (and atomic percent) of the Dipole dopant driven into the portion of the high-k dielectric layer 62B in the device region 59-1, is thus higher than that in the portion of the high-k dielectric layer 62B in the device region 59-2. In the Device region 59-3 is no dipole dopant in the corresponding section of the high-k dielectric layer 62B endowed.
[0067] After the drive-in process 70, the hard mask 66 and the dipole films 64' and 64 are removed. The resulting Structure is essentially the same as shown in Fig. 21.
[0068] Figures 27A and 27B to 30A and 30B illustrate the formation of the remaining gate stacks and Contact plug according to some embodiments. The respective process is designated as process 248 in the process flow 200 illustrated in Fig. 44. The following figure numbers in Figs. 27A and 27B to 30A and 30B may have the corresponding numbers followed by the letter A or B. The letter A indicates that the corresponding figure shows a cross-section which is the same as the cross-section A2-A2 in Fig. 4, and the letter B indicates that the corresponding figure shows a reference cross-section which is the same as the reference cross-section BB in Fig. 4 Each of the structures in Fig. 18 or Fig. 26 in the device areas 59-1, 59-2 and 59-3 can be subjected to the processes in Figs. 27A and 27B to 30A and 30B to complete the formation of a transistor, wherein the transistors have an adjusted or unadjusted threshold voltage.
[0069] Referring to Figs. 27A and 27B, stacked conductive layers 76 and filler metal 78 formed. According to some embodiments, an optional high-k dielectric layer may be formed over the high-k Dielectric layer 62B may be formed before the stacked conductive layers 76 are formed. According to some Embodiments, the conductive layers 76 and the filler metal 78 are deposited in the device regions 59-1, 59-2 and 59-3 in common processes and using common materials or different materials in different processes. According to alternative embodiments, the conductive layers 76 and the Filler metal 78 are formed by separate processes and can be made of the same material or different materials For example, if the transistors formed in the device regions 59-1, 59-2 and 59-3 have opposite conductivity types, the working exit layers in the device regions 59-1, 59-2 and 59-3 are made of different materials and produced in separate processes. According to alternative Embodiments, the transistors formed in the device region 59-1, 59-2 and 59-3 are of the same conductivity type (p-type or n-type), but have different performance requirements, such as different threshold voltages. Accordingly, the stacked conductive layers 76 in the Device areas 59-1, 59-2 and 59-3 also formed from different processes and / or different materials be.
[0070] The conductive layers 76 may include a working exit layer and may include other layers, such as Cover layers, blocking layers, or the like. For example, if one or both of the Device regions 59-1, 59-2 and 59-3 is a p-type transistor region, the corresponding working exit layer may be TiN, TaN, TiSiN, WCN, MOCN or combinations thereof. If one or both of the devices regions 59-1, 59-2 and 59-3 is an n-transistor region, the corresponding working exit layer can be TiAlC, TiAlN, TaAlC, TaAlN or the like or combinations thereof. The filler metal 78 may be formed to This text has been copied by the DPMA from the original sources. It does not contain any drawings. The tables and formulas may be of unsatisfactory quality. remaining recesses 58 (Fig. 13A and Fig. 13B) if they are not yet completely filled. Filler metal 78 may comprise a metal-containing material such as cobalt, ruthenium, aluminum, tungsten, combinations thereof and / or multiple layers thereof.
[0071] Referring to Figs. 28A and 28B, after filling the recesses 58, a Planarization process, such as a CMP process or a mechanical grinding process, is carried out to to remove excess portions of the gate dielectrics and the material of the gate electrodes 80, wherein the excess sections are located above the upper surface of the ILD 52. The remaining sections of the conductive Layers 76 and the filler metal 78 form gate electrodes 80. The gate electrodes 80 and the gate dielectrics 62 are collectively referred to as gate stack 82.
[0072] As shown in Figs. 29A and 29B, the gate stacks 82 are next recessed so that Recesses directly above the gate stacks 82 and between opposing portions of the gate spacers 38 A gate mask 84, which may include one or more layers of dielectric material, such as silicon nitride, silicon oxynitride or the like, is filled into each of the recesses, followed by a Planarization process to remove excess sections of the dielectric material located above the ILD 52 extend.
[0073] As further illustrated by Figures 29A and 29B, the ILD 86 is disposed over the ILD 52 and over the gate Masks 84 are deposited. An etch stop layer (not shown) may be deposited before the formation of the ILD 86 or According to some embodiments, the ILD 86 is formed by FCVD, CVD, PECVD, or the like. The ILD 86 is formed of a dielectric material selected from silicon oxide, PSG, BSG, BPSG, USG or the like can be.
[0074] In Fig. 30A and Fig. 30B, the ILD 86, the ILD 52, the CESL 50 and the gate masks 84 are etched to recesses (occupied by contact plugs 88A and 88B), with areas of the epitaxial source / drain Regions 48 and / or the gate stack 82 are exposed. The recesses can be formed by etching using a anisotropic etching process, such as RIE, NBE, or the like. According to some embodiments, the recesses by etching through the ILD 86 and the ILD 52 using a first etching process, etching by the gate masks 84 using a second etching process and etching by the CESL 50 possibly under using a third etching process.
[0075] After the recesses are formed, silicide regions 90 (Fig. 30B) are deposited over the epitaxial source / drain regions 48. According to some embodiments, the silicide regions 90 are formed by first metal layer (not shown) is deposited, which is connected to the semiconductor materials of the underlying epitaxial source / drain regions 48 (for example silicon, silicon germanium, germanium) to form silicide and / or germanide regions, and then a heat annealing process is performed to form the silicide regions 90. The metal may include nickel, cobalt, titanium, tantalum, platinum, tungsten, or the like. The unreacted portions of the deposited metal are then removed, for example by an etching process.
[0076] Contact plugs 88B are then formed over the silicide regions 90. Contacts 88A (may also called gate contact plugs) are formed in the recesses and are located above the gate Electrodes 80 and touch them. Although Fig. 30B illustrates that the contact plugs 88A and 88B are in a same cross-section, in various embodiments the contact plugs 88A and 88B can be in different cross-sections, thereby reducing the risk of a short circuit between them. The GAA transistors 92- 1, 92-2 and 92-3, which are represented by the GAA transistor 92, are thus each in the Device areas 59-1, 59-2 and 59-3 are formed (Fig. 21 or Fig. 26).This text has been copied by the DPMA from the original sources. It does not contain any drawings. The tables and formulas may be of unsatisfactory quality.
[0077] In the previously discussed embodiments, as shown in Figs. 14 to 26, three device areas where the device regions have different dipole dopant concentrations (and different atomic percent) by controlling the number of dopant uptake processes and the thicknesses of the dipole dopant films This concept can be generalized to include a larger number of For example, Fig. 41 illustrates a concept of adjusting multiple Transistors so that they have different threshold voltages Vt1, Vt2, Vt3, Vt4, Vt5 and Vt6. This can by controlling the total number of dipole dopant films 64 each with the thicknesses T1', T2', T3', T4', T5' and T6' It should be noted that if multiple dipole dopant films are adopted for a transistor, the collection of the Dipoldo animal material in different driving processes or in the same driving process. For example The thickness T2' can be achieved by two dipole dopant films. Driving in the dipole dopant with the thickness T2' can be achieved by depositing two dipole dopant films, each from a drive-in process or from a accompanied by the same collection process.
[0078] Fig. 42 illustrates an embodiment in which a plurality of transistors X1 to Xn are present, where the integer n is any number greater than 1. Through deposition and structuring processes, the dipole dopant doping corresponding to the transistors by depositing and structuring a plurality of dipole dopant films DL1 to DLn in a plurality of loops. For example, in the first loop, the Dipole dopant film DL1 is deposited and removed from the transistors X2 to Xn. In the second loop, the dipole Dopant film DL2 is deposited and removed from transistors X3 to Xn. This process is continued, with each of the loops has its corresponding dipole dopant film removed from one transistor region less than the previous loop. This may result in n+1 stages (including the stage without dipole film) of total thicknesses of the dipole Dopant films. After the drive-in process, n+1 dipole dopant concentration levels (including one transistor in which no dipole dopant is incorporated) and N+1 Vt adjustment stages must be present.
[0079] Fig. 43 illustrates an embodiment in which a plurality of loops are performed. Each corresponding dipole dopant film undergoes a deposition process, a structuring process, a drive-in process and a removal process. Each of the loops can have sections that can be used in other combinations of transistors were left behind than other loops. Accordingly, a majority of stages of the Vt- n Adjustment must be present, such as 2 Vt adjustment levels.
[0080] The embodiments of the present disclosure have some advantageous features. By adopting of AlN layers as dipole dopant films to provide dipole dopants, a higher degree of Dipole doping and the efficiency of Vt matching is improved by dipole dopant doping. The Vt- Adjustment is volume-free because the dipole dopant films are removed. The formation of AlO can help to so that it does not diffuse into the high-k dielectric layers, thus reducing the adverse effect of Nitrogen reduced.
[0081] According to some embodiments of the present disclosure, a method comprises forming a first Gate dielectric in a first semiconductor region; depositing a first aluminum nitride layer on the first Gate dielectric; depositing an aluminum oxide layer on the first aluminum nitride layer; performing a first annealing process for driving aluminum in the first aluminum nitride layer into the first gate Dielectric; removing the aluminum oxide layer and the first aluminum nitride layer; and forming a gate Electrode on the first gate dielectric. In one embodiment, the first aluminum nitride layer and the Aluminum oxide layer deposited ex-situ with a vacuum interruption in between.This text has been copied by the DPMA from the original sources. It does not contain any drawings. The tables and formulas may be of unsatisfactory quality.
[0082] In one embodiment, the first aluminum nitride layer and the aluminum oxide layer are deposited in-situ in a same vacuum environment. In one embodiment, the first aluminum nitride layer is deposited by a chemical vapor deposition process. In one embodiment, the chemical vapor deposition comprises Vapor deposition process a chemical vapor deposition process with multiple pulses. In one embodiment the multi-pulse chemical vapor deposition process involves pulsing a nitrogen-containing precursor; and when the nitrogenous precursor is pulsed, performing a plurality of pulsing processes to produce a aluminum-containing precursor. In one embodiment, the first annealing process is carried out when the aluminum oxide layer is located on the first aluminum nitride layer.
[0083] In one embodiment, the method further comprises forming a patterned etch mask over the aluminum oxide layer; structuring the aluminum oxide layer using the patterned etching mask to structures; and structuring the first aluminum nitride layer using the aluminum oxide layer as an etching mask. In one embodiment, the method further comprises forming a second Gate dielectric in a second semiconductor region, wherein the second semiconductor region surrounds the first semiconductor region overlapped and spaced therefrom, and wherein the first aluminum nitride layer and the aluminum oxide layer also formed in the second semiconductor region. In one embodiment, the aluminum oxide layer has a portion which is filled in a space between the first semiconductor region and the second semiconductor region.
[0084] In one embodiment, the entire aluminum oxide layer is located outside a space between the first semiconductor area and the second semiconductor region. In one embodiment, the method further comprises, prior to the first annealing process, Depositing a second aluminum nitride layer on the first aluminum nitride layer, wherein the aluminum oxide layer deposited on the second aluminum nitride layer. In one embodiment, the method further comprises Depositing a second aluminum nitride layer, wherein the first annealing process is carried out before the second aluminum nitride layer is deposited.
[0085] According to some embodiments of the present disclosure, a method comprises forming a first Gate dielectric in a first semiconductor region and a second gate dielectric in a second semiconductor region; depositing a first aluminum nitride layer on the first gate dielectric; depositing a second aluminum nitride layer on the first gate dielectric; driving aluminum in the first aluminum nitride layer and the second aluminum nitride layer into the first gate dielectric; depositing the second Aluminum nitride layer on the second gate dielectric; the driving of aluminum in the second aluminum nitride layer into the second gate dielectric; and forming a first gate electrode on the first gate dielectric and a second gate electrode on the second gate dielectric.
[0086] In one embodiment, when aluminum is present in the first aluminum nitride layer and the second aluminum nitride layer is driven into the first gate dielectric, the second aluminum nitride layer is located above the first aluminum nitride layer. In one embodiment, the method further comprises, before the second aluminum nitride layer is deposited, removing the first aluminum nitride layer, wherein the aluminum in the first aluminum nitride layer and the second aluminum nitride layer in separate drive-in processes into the first gate dielectric. In one embodiment, the method further comprises depositing a Aluminum oxide layer over the first aluminum nitride layer, wherein when the aluminum in the first aluminum nitride layer is driven into the first semiconductor region, the aluminum oxide layer over the first Aluminum nitride layer is located.This text has been copied by the DPMA from the original sources. It does not contain any drawings. The tables and formulas may be of unsatisfactory quality.
[0087] According to some embodiments of the present disclosure, a method comprises forming a first nanostructure and a second nanostructure overlapping the first nanostructure, wherein the first nanostructure is a space from the second nanostructure; forming a first gate dielectric and a second Gate dielectric on the first nanostructure and the second nanostructure, respectively; depositing a Aluminum nitride layer comprising a first portion on the first gate dielectric and a second portion on the second gate dielectric; depositing an aluminum oxide layer on the aluminum nitride layer; Driving aluminum in the aluminum nitride layer into the first gate dielectric and the second gate dielectric; and removing the aluminum oxide layer and the aluminum nitride layer. In one embodiment, the first section the aluminum nitride layer is connected to the second portion of the aluminum nitride layer. In one embodiment, the first section of the aluminum nitride layer separated from the second section of the Aluminum nitride layer separated.
[0088] The foregoing explains features of various embodiments so that a person skilled in the art can understand the aspects of A person skilled in the art should recognize that he or she may better understand the present disclosure easily used as a basis for designing or modifying other processes and structures to achieve the same purposes and / or achieve the same advantages of the embodiments presented herein. A person skilled in the art should also realize that such equivalent constructions do not depart from the spirit and scope of the present disclosure and may make various changes, substitutions and alterations herein without departing from the nature and scope of this disclosure. QUOTES CONTAINED IN THE DESCRIPTION
[0000] This list of documents submitted by the applicant was generated automatically and is intended solely for This list is not part of the German patent or trademark law. Utility model application. The DPMA assumes no liability for any errors or omissions. Cited patent literature
[0000] US 63493008
[0001] Patent claims 1. Procedure comprising: Forming a first gate dielectric in a first semiconductor region; depositing a first aluminum nitride layer on the first gate dielectric; Depositing an aluminum oxide layer on the first aluminum nitride layer; Performing a first annealing process to transfer aluminum in the first aluminum nitride layer into the first gate to drive dielectric; Removing the aluminum oxide layer and the first aluminum nitride layer; and Forming a gate electrode on the first gate dielectric.This text has been copied by the DPMA from the original sources. It does not contain any drawings. The tables and formulas may be of unsatisfactory quality. 2. The method according to claim 1, wherein the first aluminum nitride layer and the aluminum oxide layer are deposited ex-situ with a Vacuum interruption in between. 3. The method according to claim 1, wherein the first aluminum nitride layer and the aluminum oxide layer are deposited in-situ in a same vacuum environment. 4. The method of claim 1, wherein the first aluminum nitride layer is deposited by a chemical vapor deposition process is separated. 5. The method of claim 4, wherein the chemical vapor deposition process comprises a chemical vapor deposition process with multiple pulses. 6. The method of claim 5, wherein the multi-pulse chemical vapor deposition process comprises: Pulsing of a nitrogenous precursor; and when the nitrogenous precursor is pulsed, performing a plurality of pulsing processes to perform a aluminum-containing precursor. 7. Method according to one of the preceding claims, wherein the first tempering process is carried out when the Aluminum oxide layer on the first aluminum nitride layer. 8. Method according to one of the preceding claims, further comprising: Forming a patterned etch mask over the aluminum oxide layer; Structuring the aluminum oxide layer using the structured etch mask to define structures; and Patterning the first aluminum nitride layer using the aluminum oxide layer as an etch mask. 9. The method according to any one of the preceding claims, further comprising forming a second gate dielectric in a second semiconductor region, wherein the second semiconductor region overlaps the first semiconductor region and is spaced, and wherein the first aluminum nitride layer and the aluminum oxide layer are also in the second semiconductor area. 10. The method according to claim 9, wherein the aluminum oxide layer has a portion extending into a space between the first semiconductor region and the second semiconductor region. 11. The method of claim 9, wherein the entire aluminum oxide layer is outside a space between the first semiconductor region and the second semiconductor region. 12. Method according to one of the preceding claims, further comprising: before the first annealing process, depositing a second aluminum nitride layer on the first aluminum nitride layer, wherein the aluminum oxide layer is deposited on the second aluminum nitride layer. 13. The method according to any one of the preceding claims 1 to 11, further comprising: Depositing a second aluminum nitride layer over the first gate dielectric, wherein the first annealing process is carried out before the second aluminum nitride layer is deposited. 14. Procedure comprising: Forming a first gate dielectric in a first semiconductor region and a second gate dielectric in a second semiconductor region; depositing a first aluminum nitride layer on the first gate dielectric; depositing a second aluminum nitride layer on the first gate dielectric; Driving aluminum in the first aluminum nitride layer and the second aluminum nitride layer into the first gate-This text has been copied by the DPMA from the original sources. It does not contain any drawings. The tables and formulas may be of unsatisfactory quality. Dielectric; depositing the second aluminum nitride layer on the second gate dielectric; Driving aluminum in the second aluminum nitride layer into the second gate dielectric; and Forming a first gate electrode on the first gate dielectric and a second gate electrode on the second Gate dielectric. 15. The method according to claim 14, wherein when aluminum is present in the first aluminum nitride layer and the second aluminum nitride layer is driven into the first gate dielectric, the second aluminum nitride layer is above the first aluminum nitride layer. 16. The method of claim 14, further comprising, before depositing the second aluminum nitride layer, removing the first aluminum nitride layer, wherein the aluminum in the first aluminum nitride layer and the second Aluminum nitride layer is driven into the first gate dielectric in separate drive-in processes. 17. The method of claim 14, further comprising depositing an aluminum oxide layer over the first Aluminium nitride layer, wherein when aluminium in the first aluminium nitride layer is introduced into the first semiconductor region driven, the aluminum oxide layer is located above the first aluminum nitride layer. 18. Procedure comprising: Forming a first nanostructure and a second nanostructure overlapping the first nanostructure, wherein the first nanostructure is spaced from the second nanostructure by a space; Forming a first gate dielectric and a second gate dielectric on the first nanostructure and the second nanostructure; Depositing an aluminum nitride layer comprising a first portion on the first gate dielectric and a second portion on the second gate dielectric; Depositing an aluminum oxide layer on the aluminum nitride layer; Driving aluminum in the aluminum nitride layer into the first gate dielectric and the second gate dielectric; and Removing the aluminum oxide layer and the aluminum nitride layer. 19. The method of claim 18, wherein the first portion of the aluminum nitride layer is bonded to the second portion of the aluminum nitride layer. 20. The method of claim 18, wherein the first portion of the aluminum nitride layer is separated by the aluminum oxide layer of separated from the second section of the aluminum nitride layer.
Claims
A method comprising: forming a first gate dielectric in a first semiconductor region; depositing a first aluminum nitride layer on the first gate dielectric; depositing an aluminum oxide layer on the first aluminum nitride layer; performing a first annealing process to drive aluminum in the first aluminum nitride layer into the first gate dielectric; removing the aluminum oxide layer and the first aluminum nitride layer; and forming a gate electrode on the first gate dielectric.The method of claim 1, wherein the first aluminum nitride layer and the aluminum oxide layer are deposited ex-situ with a vacuum interruption therebetween.The method of claim 1, wherein the first aluminum nitride layer and the aluminum oxide layer are deposited in-situ in a same vacuum environment.The method of claim 1, wherein the first aluminum nitride layer is deposited by a chemical vapor deposition process.The method of claim 4, wherein the chemical vapor deposition process comprises a multiple pulse chemical vapor deposition process.The method of claim 5, wherein the multiple pulse chemical vapor deposition process comprises: pulsing a nitrogen-containing precursor; and when the nitrogen-containing precursor is pulsed, performing a plurality of pulsing processes to produce an aluminum-containing precursor.A method according to any preceding claim, wherein the first annealing process is performed when the aluminum oxide layer is on the first aluminum nitride layer.The method of any preceding claim, further comprising: forming a patterned etch mask over the aluminum oxide layer; patterning the aluminum oxide layer using the patterned etch mask to define structures; and patterning the first aluminum nitride layer using the aluminum oxide layer as an etch mask.The method of any preceding claim, further comprising forming a second gate dielectric in a second semiconductor region, wherein the second semiconductor region overlaps and is spaced from the first semiconductor region, and wherein the first aluminum nitride layer and the aluminum oxide layer are also formed in the second semiconductor region.The method of claim 9, wherein the aluminum oxide layer has a portion filled in a space between the first semiconductor region and the second semiconductor region.The method of claim 9, wherein the entire aluminum oxide layer is located outside a space between the first semiconductor region and the second semiconductor region.The method of any preceding claim, further comprising: prior to the first annealing process, depositing a second aluminum nitride layer on the first aluminum nitride layer, wherein the aluminum oxide layer is deposited on the second aluminum nitride layer.The method of any of the preceding claims 1 to 11, further comprising: depositing a second aluminum nitride layer over the first gate dielectric, wherein the first annealing process is performed before the second aluminum nitride layer is deposited.A method comprising: forming a first gate dielectric in a first semiconductor region and a second gate dielectric in a second semiconductor region; depositing a first aluminum nitride layer on the first gate dielectric; depositing a second aluminum nitride layer on the first gate dielectric; driving aluminum in the first aluminum nitride layer and the second aluminum nitride layer into the first gate dielectric; depositing the second aluminum nitride layer on the second gate dielectric; driving aluminum in the second aluminum nitride layer into the second gate dielectric; and forming a first gate electrode on the first gate dielectric and a second gate electrode on the second gate dielectric.The method of claim 14, wherein when aluminum in the first aluminum nitride layer and the second aluminum nitride layer is driven into the first gate dielectric, the second aluminum nitride layer is above the first aluminum nitride layer.The method of claim 14, further comprising, before depositing the second aluminum nitride layer, removing the first aluminum nitride layer, wherein the aluminum in the first aluminum nitride layer and the second aluminum nitride layer is driven into the first gate dielectric in separate drive processes.The method of claim 14, further comprising depositing an aluminum oxide layer over the first aluminum nitride layer, wherein when aluminum in the first aluminum nitride layer is driven into the first semiconductor region, the aluminum oxide layer is located over the first aluminum nitride layer.A method comprising: forming a first nanostructure and a second nanostructure overlapping the first nanostructure, the first nanostructure being spaced from the second nanostructure by a space; forming a first gate dielectric and a second gate dielectric on the first nanostructure and the second nanostructure, respectively; depositing an aluminum nitride layer comprising a first portion on the first gate dielectric and a second portion on the second gate dielectric; depositing an aluminum oxide layer on the aluminum nitride layer; driving aluminum in the aluminum nitride layer into the first gate dielectric and the second gate dielectric; and removing the aluminum oxide layer and the aluminum nitride layer.The method of claim 18, wherein the first portion of the aluminum nitride layer is bonded to the second portion of the aluminum nitride layer.The method of claim 18, wherein the first portion of the aluminum nitride layer is separated from the second portion of the aluminum nitride layer by the aluminum oxide layer.
Citation Information
Patent Citations
METHOD FOR DOTING HIGH-K / METAL GATES TO SET THRESHOLD VOLTS
DE102019125922B3
DIPOLIG-FABRICATED HIGH-K-GATE DIELECTRIC AND METHOD FOR FORMING THE SAME
DE102020130401A1
Methods for threshold voltage tuning and structures formed thereby
US20190318967A1
Dipole Patterning for CMOS Devices